Method for adjusting refractive index

By recording the measurement parameters of the optical components, adjusting the adhesive mixing ratio and adopting a closed-loop control loop, the problem of inaccurate refractive index matching in the prior art is solved, and high-precision production of optical components such as smart glasses is achieved, reducing visual interference.

CN119095720APending Publication Date: 2024-12-06TOOZ TECH GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036441.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-29
Filing Date
2023-04-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to produce optical components with precise matching of refractive index, especially in smart glasses. It is difficult to match the refractive index of the adhesive with the base material to the accuracy of the fourth or fifth position after the decimal point, resulting in visual interference.

Method used

By recording the measurement parameters of the optical element, adjusting the mixing ratio of the multiple starting materials of the adhesive to achieve accurate matching of the refractive index, a closed-loop control loop is used to ensure a tolerance of less than 0.0005 or less than 0.0001.

Benefits of technology

It realizes accurate matching of refractive index of optical components, reduces visual interference, improves production accuracy and consistency, and is suitable for smart glasses and other display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095720A_ABST
    Figure CN119095720A_ABST
Patent Text Reader

Abstract

Aspects of the present disclosure relate to the production of optical components for optical elements for use in display devices (e.g., smart glasses).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Various aspects of the present disclosure relate to optical components for producing optical elements for use in display devices (eg, smart glasses). Background Art

[0002] The prior art discloses adhesives which are suitable as special optical fine adhesives for filling structures, for example for embedding functional layers in smart glasses.

[0003] A key feature of smart glasses is the introduction of virtual content into the field of view. This typically involves the use of injection molded optical components with various high-precision free-form phases, called waveguides. A Fresnel structure produced by injection molding with a translucent coating is used to display the virtual image to the eye, and the viewer is simultaneously able to perceive the environment through the structure without the view being impaired. Alternatively, the structure can also have a partial 100% reflective coating. If the areas with 100% specular reflection are relatively small (e.g. <1 mm in diameter) and the areas in between have a sufficiently high transmittance for ambient light, the viewer is also able to perceive the virtual image superimposed on the environment.

[0004] In order to enable undisturbed viewing in both horizontal and vertical directions through the prism or mirror structures provided in the smart glasses, it is useful that the refractive index of the adhesive used is substantially identical to that of the base material. Furthermore, the adhesive can be part of the optical path of the virtual image. To produce such a device, the refractive indices of the fine adhesive and the optical component must be precisely matched.

[0005] Typically, optical elements for this purpose are produced by gluing and combining optical components, such as transparent housings or overfilled Fresnel structures.

[0006] According to WO 2015 / 121341 A1, adhesives with optical functional properties (e.g., a defined refractive index) can be produced by using adhesive components with optical quality. The desired refractive index or desired dispersion (Abbe number) of such an adhesive can be adjusted to the desired purpose by selecting the components used (particularly their chemical structure). The refractive index of an adhesive (fine adhesive) for optical components can be adjusted for a defined wavelength (e.g., in the case of an optical measurement system) or for a specific wavelength range (e.g., 450nm to 700nm) in the case of multicolor applications, and in particular the refractive index is adjusted to adapt to the optical component to be bonded. In the case of multicolor adjustment of the refractive index, it is important to match the dispersion (wavelength dependence of the refractive power) of the fine adhesive and the optical component to each other as closely as possible. Typically, in this case, a central wavelength is defined, e.g., 546nm (nm) e). The dispersion of fine adhesives can be controlled by the adhesive components used, since the chemical structure of the monomeric substances has a considerable influence on the refractive power and dispersion.

[0007] A particular application is the above-mentioned gluing of optical components, some of which have diffractive, reflective and / or other micro-optical elements on the component surface. If the refractive index is adjusted to, for example, Δn<0.0005, the diffractive structures encapsulated in the adhesive layer are barely visually discernible anymore.

[0008] Thus, depending on the structure to be filled and its relative position with respect to the viewing direction, it may be necessary to match the refractive index between the adhesive and the base material to the fourth or fifth decimal place to ensure a substantially undisturbed viewing impression when a user looks through the structure.

[0009] Adhesives that meet the above requirements (eg the values ​​for the refractive index to the degree described are permanently constant) are rarely available on the market, since even identical adhesives usually fluctuate at least slightly from batch to batch.

[0010] Achieving this refractive index accuracy in synthesis is a complex task. If the system is a 2-component system (2K system) consisting of resin and hardener, or a mixture of two or more 1K systems, each component itself should be manufactured within extremely tight tolerances. The complexity and tolerance management are further increased if resin and hardener batches with different production dates are to be used in daily production while also complying with the maximum permissible refractive index variation.

[0011] If the glass to be bonded or the structure to be filled is produced as an optical component by injection molding, fluctuations in the refractive index of the base glass itself cannot be ruled out. The reason for these fluctuations lies, for example, in the optical properties of the polymer granules used, which also have or may have production-related refractive index variations. Depending on the processing parameters, the process scheme of the injection molding process leads to different refractive indices of finished parts with exactly the same starting materials. These may also be locally different within the part. Examples of processing parameters include temperature and shear conditions during melting in the cylinder screw, injection rate, holding pressure curve, cooling time and mold temperature conditions, which affect the solidification characteristics and therefore also the local optical properties. Since these parameters also affect the geometric dimensions of the injection molded parts, they are typically also used to compensate for fluctuations in the environment and manufacturing to meet the geometric component tolerances. Therefore, the dimensional accuracy of the base glass and the adhesive system and the process-related matching of the refractive index constitute a special challenge. Summary of the invention

[0012] Therefore, there is a need for improved techniques for producing optical components with precisely matched refractive indices. This object is achieved by the features of the independent claims. Embodiments are defined by the features of the dependent claims.

[0013] A method of adjusting the refractive index of an adhesive for an optical element is disclosed, wherein the adhesive is optically transparent and is produced from a plurality of starting materials, wherein the method comprises:

[0014] - producing at least one sample of the optical element using the adhesive,

[0015] - optically analyzing at least one sample of the optical element by recording at least one measurement parameter,

[0016] - adjusting the mixing ratio of the various starting materials of the adhesive based on the results of the optical analysis, and

[0017] - producing a plurality of replicate products of the optical element using a binder having an adjusted mixing ratio of the plurality of starting materials.

[0018] In the method of the present invention, preferably multiple samples of the optical element can be produced successively, wherein the mixing ratio of the multiple starting materials is matched between the production of the multiple samples based on the results of the previous optical analysis of the multiple samples. The adjustment is preferably performed in a gradual, linear or decreasing manner.

[0019] The method may further comprise implementing a closed-loop control loop, wherein the closed-loop control loop compares at least one measured parameter with a corresponding target value and sets the dose of at least one of the plurality of starting materials as a controlled variable when adjusting the mixing ratio. The closed-loop control loop may be implemented, for example, by software executed on a processor based on program code from a memory. A corresponding controller may be used. In particular, a closed-loop control tolerance of such a closed-loop control loop as a variation from a defined refractive index may be less than 0.0005 or less than 0.0001.

[0020] The adhesive may be a two-component adhesive, wherein the plurality of starting materials include a first starting material, a second starting material, a third starting material, and a fourth starting material, and the first component of the two-component adhesive is formed by mixing the first starting material and the second starting material, and the second component of the two-component adhesive is formed by mixing the third starting material and the fourth starting material, and adjusting the mixing ratio of the plurality of starting materials may include adjusting a first part mixing ratio of the first starting material relative to the second starting material in the mixing of the first component, and adjusting the mixing ratio of the plurality of starting materials may include adjusting a second part mixing ratio of the third starting material relative to the fourth starting material in the mixing of the second component. Furthermore, adjusting the mixing ratio may include adjusting a third part mixing ratio of the first component relative to the second component.

[0021] In the method of the present invention, the first component of the two-component adhesive can be mixed with the first starting material and the second starting material in the first mixer, and the second component of the two-component adhesive can be mixed with the third starting material and the fourth starting material in the second mixer. The first component and the second component of the two-component adhesive can be mixed in a third mixer downstream of the first mixer and the second mixer.

[0022] The mixing ratio of the multiple starting materials can be adjusted by changing the amount of at least one of the multiple starting materials, changing the weight of at least one of the multiple starting materials, changing the volume of at least one of the multiple starting materials, and / or changing the flow rate of at least one of the multiple starting materials from a storage container, such as via a metering pump, into a mixing container.

[0023] In the method of the present invention, at least one measurement parameter may include color splitting and / or optical shift of the optical transmission of the optical element, which color splitting and / or the optical shift are determined based on the optical transmission of the test pattern. At least one measurement parameter may include the prismatic effect of the optical element determined based on the optical transmission of the test pattern, and / or the light dispersion of the adhesive at a specific wavelength or in a wavelength range. The optical element may be any type of microstructure and / or macrostructure, which, due to its geometric characteristics, will lead to optically assessable variations in the test image when the refractive index of the adhesive does not meet the conditions. Typical geometric structures are: Fresnel structures, prismatic structures, pyramidal structures, striped or corrugated structures, spherical surfaces, complex surfaces or free-form surfaces - in coherent or segmented form, individually or in array form, etc. The optical element may preferably include a Fresnel structure, and the test pattern in the method may be reflected laterally into the Fresnel structure or the optical element. The Fresnel structure may have, for example, steps along a face, which may then be reflected laterally into the plane of the face.

[0024] In the method of the present invention, the optical element may include a plurality of optical components, and producing at least one sample of the optical element includes bonding the plurality of optical components with an adhesive and initiating curing of the adhesive, wherein the optical analysis is initiated before, during or after initiation of curing.

[0025] Producing at least one sample of an optical element including a plurality of optical components may include bonding the plurality of optical components with an adhesive and initiating curing of the adhesive, wherein a first optical component of the plurality of optical components of the optical element includes a Fresnel structure, and wherein a second optical component of the plurality of optical components of the optical element includes a housing. Alternatively, other types of structures, such as prismatic structures, are also contemplated. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1An illustrative arrangement for optical analysis by the method according to the invention is shown.

[0027] Figure 2 Schematic diagram showing the effect of refractive index variation of illustrative adhesive systems on optical analysis of optical components.

[0028] Figure 3 The effects of an inadequate refractive index adaptation are shown by way of illustration and can be used as a measurement parameter for adjusting the refractive index within the scope of optical analysis.

[0029] Figure 4 A structural scheme of a closed-loop control process as a configuration of the method of the present invention is shown.

[0030] Figure 5 Another schematic structural diagram of a closed-loop control process as a configuration of the method of the present invention is shown.

[0031] Figure 6 is a flow chart of an illustrative method. DETAILED DESCRIPTION

[0032] The above-mentioned characteristics, features and advantages of the present invention and the manner of achieving them will become more clear and obvious with reference to the following description of working examples, which are explained in detail with reference to the accompanying drawings.

[0033] The present invention will be explained in detail below with reference to the accompanying drawings by preferred embodiments. In the accompanying drawings, the same reference numerals represent the same or similar elements. The accompanying drawings are schematic representations of various embodiments of the present invention. The elements shown in the accompanying drawings are not necessarily shown in true proportion. Instead, the various elements shown in the accompanying drawings are reproduced so that their functions and general purposes will be apparent to those skilled in the art.

[0034] The technology used when producing optical elements is described below. The method of the invention for adjusting the refractive index generally comprises recording at least one measurement parameter during an optical analysis, making it possible to detect the quality of the refractive index match, to determine the amount and the mixing ratio of the adhesive, so that the refractive index can be matched as required. In the case of refractive index matching of the Fresnel structure overfilling, a test pattern, such as a black and white test pattern (preferably a pattern consisting of stripes, or a checkerboard pattern, etc.) can be observed through the filled structure with the aid of a camera, and color breakup or optical shifts due to prismatic effects that are still present in the case of non-optimal matching can be evaluated and used as measurement parameters.

[0035] This technology can be used to produce optical elements that can be used, for example, in conjunction with smart glasses. This technology can also be used, for example, in heads-up displays.

[0036] Figure 1An illustrative arrangement in which the method of the invention can be carried out is shown in FIG. 1 , wherein a sample of an optical component or optical element (eg, a filled Fresnel structure G1 ( Figure 1 a) G2( Figure 1 b) or G3( Figure 1 c) a sample made by the adhesive) to view the test pattern and one or more measurement parameters (such as color breakup and / or optical shift) can be detected and evaluated. This then enables a specific adjustment of the refractive index by varying the amount of the components of the adhesive, which means that refractive index matching can be performed or improved. Figure 1 Another working example of the arrangement of the sample, camera and test pattern is shown by way of example in (c). In this case, the light emitted by the test pattern is guided in the waveguide in the direction of the camera until it is coupled out. In special cases, this light path in the glass can correspond exactly to the light path in the application as smart glasses.

[0037] The test pattern itself can also be a self-luminous object, such as a display, or a non-self-luminous object.

[0038] Figure 2 The effect of refractive index variations of illustrative binder systems on optical components is shown by way of example. In addition to the shift of the original image and / or the shifted double image, the different (color) splitting is another measure of the match or mismatch of the refractive index or Abbe number of the base material and the binder, and therefore also a measure of the need for adjusting the refractive index. Thus, direct characterization can be performed over the entire visible wavelength range.

[0039] exist Figure 2 In FIG. 1 , image a) shows a possible test pattern, and images b) to e) show possible images observed by a viewer or camera. Figure 2 In the figure, (a) shows the target image, (b) shows the image shifted to the left, (c) shows the image shifted to the right, (d) shows the image shifted to both sides, and (e) illustrates the color splitting, e.g. red to the right, blue to the left or vice versa. This observation can in principle be carried out before, during or after the curing process. The fully cured state is essential for the final assessment of the adequate matching of the refractive indices. However, if there is sufficient experience with the corresponding adhesive system, it is even possible to draw conclusions about the quality of the final component in the fully cured state based on uncured or only partially cured systems or image defects during the curing process. In particular in the case of very long curing processes, it is particularly valuable to draw the expected results in advance so that process fluctuations can be compensated in time by adjusting the mixing ratio.

[0040] Depending on the sign of the difference between the actual and target values ​​of the refractive index and the geometric ratios of the structure to be filled, the image captured by the camera can show image shifts, widening of the test marks or color splitting compared to the original image.

[0041] If in Figure 2 (b) to Figure 2 Where the image shown in this example in (e) represents the final cured state obtained, the measured parameters recorded corresponding to the shift or color splitting indicate that the desired refractive index match has not yet been obtained, and therefore, an improved match can be found by further using the method of the present invention, i.e. adjusting the mixing ratio and producing multiple repeat products of optical elements using adhesives with matching mixing ratios.

[0042] Figure 3 Similar to Figure 2 , by way of example, shows further test patterns and optical influences that occur as a function of the geometric ratio in the case of an insufficient refractive index match, which can be used as measurement parameters. Accordingly, Figure 3 (a) shows the target image, Figure 3 (b) to Figure 3 (d) shows the corresponding image shift.

[0043] As mentioned above about Figure 2 and Figure 3 It can be seen from the observation that in the method of the present invention, at least one measurement parameter may include a color breakup and / or an optical shift of the optical transmission of the optical element, which color breakup and / or the optical shift are determined based on the optical transmission of the test pattern.

[0044] The method can also be implemented as a closed-loop control process. As an example, Figure 4 The structure shown in schematic form in FIG. 1 is composed of the arrangement described below.

[0045] As described above, the transparent adhesive used is formed of multiple starting materials and can be a two-component (2K) adhesive. For example, the first starting material A1 and the second starting material A2 can form the resin component A, and the third starting material B1 and the fourth starting material B2 can form the curing agent component B.

[0046] exist Figure 4In the example described in , the first component A of the two-component adhesive is formed by mixing the first starting material A1 and the second starting material A2, and the second component B of the two-component adhesive is formed by mixing the third starting material B1 and the fourth starting material B2. At this time, the mixing ratio of the various starting materials is matched in the mixing of the first component A, that is, the first partial mixing ratio of the first starting material A1 to the second starting material A2 is (A1):(A2), and the mixing ratio of the various starting materials is matched in the mixing of the second component B, that is, the second partial mixing ratio of the third starting material B1 to the fourth starting material B2 is (B1):(B2).

[0047] exist Figure 4 In the embodiment shown, the storage container for starting materials A1 / A2 contains the starting materials for resin A, namely the first starting material A1 and the second starting material A2, which form resin A and arrive in storage container A after mixing in mixer M1. Storage container B1 / B2 contains the above-mentioned starting materials for adhesive component B, namely the third starting material B1 and the fourth starting material B2, which arrive in storage container B after mixing in mixer M2. Components A and B together form a reactive system, which is cured over time by thermal and / or photochemical / UV activation, wherein the components in the example shown are contacted in mixer M3. The storage container can be under pressure p1 to p6 in order to ensure that the feed into metering pumps P1 to P6 is in the desired manner. The metering pump is responsible for the precise adjustment of the mixing ratio in its downstream mixer system or mixer M1 to M3 and can be controlled accordingly by controller unit C. For example, the mixer M1 can be configured to mix the starting materials A1 and A2, the mixer M2 can be configured to mix the starting materials B1 and B2, and then arrive at the mixer M3 via pumps P5 and P6, respectively, and the mixer M3 is configured to mix the component A (here the resin) and the component B (here the curing agent). Thus, the adhesive AB is obtained in a reactive form. The method of the present invention can also include adjusting the third part mixing ratio of the first component A relative to the second component B.

[0048] The control commands for the metering pump can be generated based on the optical analysis mentioned (i.e., optical property analysis), and a closed control loop can be constructed in this way. The mixing ratio change causes the reactivity between the components to change, for example, the reactivity between the resin and the curing agent of a 2K adhesive to change. The amount of at least one starting material can be adjusted by changing the weight, changing the volume and / or changing the flow rate of at least one of the multiple starting materials into the storage container.

[0049] The adjustment of the mixing ratio may be controlled via a closed-loop control system, wherein the closed-loop control uses the amount of the adhesive component or starting material mixed with the further adhesive component or starting material as a manipulated variable.

[0050] These components themselves can in turn be formed by a plurality of components, or ingredients or starting materials. The first starting material A1 and the second starting material A2 mentioned for component A can be variants of the same chemical material, for example, variants of resins in this case, and for example the refractive index is different in the region of the third or fourth decimal place. As mentioned above, this difference may be the result of production, or it may be deliberately set so that one of the two variants is lower than the target value of the refractive index established for component A, while the other is higher than the target value. By means of a metering pump, a suitable mixing ratio of A1 and A2 can be established, so that A can be accurately adjusted to the currently required refractive index. As described at the beginning, components A1 and A2 can also be different adhesives, for example two different 1K adhesives.

[0051] The control of the refractive index of component A can also be applied to component B, which can be a hardener for a 2K adhesive in particular. If starting materials B1 and B2 differ, for example, in viscosity and / or reactivity, hardener component B can also be adjusted precisely as required.

[0052] In combination with the second component B of the reactive system (here a curing agent, in the above example, a mixture of the third starting material B1 and the fourth starting material B2), the mixture of components A and B ultimately results in a refractive index that is matched to the optical component or component part.

[0053] Specifically for thermal curing systems, two opposite effects often occur. Viscosity decreases with increasing temperature, which is usually desired for forming a thin and uniform adhesive gap. On the other hand, the curing process is accelerated, which may cause stress and warping depending on the temperature gradient established in the component or adhesive gap, which may adversely affect the optical properties of the component or optical element. Therefore, in this case, practical means for adjusting viscosity and / or reactivity are also desired. This change also affects the refractive index of the entire system A+B, so it is compensated by the above-mentioned readjustment of the mixing ratio of the starting materials (hereinafter referred to as A1 and A2). For example, the resin component (referred to as A above) can affect the optical properties, and the curing agent component B can affect the processing characteristics. Components with different properties (for example, refractive indices that are different (i.e., changed due to production) due to different batches of starting materials (hereinafter referred to as A1 or A2)) can be mixed as needed.

[0054] Here, the method may include recording the refractive index matching quality to determine the refractive index matching quality to be determined via the controller C (e.g., Figure 4 and Figure 5The embodiment of the present invention can further include implementing a closed-loop control loop, wherein the closed-loop control loop compares at least one measured parameter with a corresponding target value and sets a dosage of at least one starting material from the plurality of starting materials as a controlled variable when adjusting the mixing ratio.

[0055] As described above, in the case of refractive index matching overfilling of the Fresnel structure, for example, a black and white test pattern (striped pattern, checkerboard pattern, etc.) can be viewed with the aid of a camera through the filled optical components (Fresnel structures) as samples (referred to as G1, G2 and G3 in the figure). The color breakup or optical shift caused by the prism effect that still exists in the case of non-optimal matching is evaluated and used as a measurement parameter for the refractive index matching. Figure 1 , Figure 4 and Figure 5 An illustrative arrangement for optical analysis is shown in .

[0056] Compared with the above analysis methods, different analysis methods can also be used to construct a closed-loop control loop.

[0057] The method of the present invention can advantageously be formed as a process of constructing a closed-loop control loop. For example, the method can include implementing a closed-loop control loop, wherein the closed-loop control loop compares at least one measured parameter with a corresponding target value and sets the dosage of at least one of the plurality of starting materials as a controlled variable when adjusting the mixing ratio. This applies both to the mixing of components (e.g., resin and curing agent) and to the starting materials of the resin component and the curing agent component.

[0058] Further sub-configurations starting from the above-described configuration are also conceivable, as will be illustrated by the following examples.

[0059] The configurations described so far for 2-component systems also include application to 1-component systems, for example UV-curing 1-component adhesives or mixtures thereof. Here too, it is extremely difficult but necessary to establish a perfect refractive index match and also to track process-related refractive index fluctuations (for example in the polymers used for the base material). Figure 5 In the variant of the invention shown, Figure 4In contrast, starting materials A1 and A2 are not mixed to obtain A, nor are B1 and B2 mixed to obtain B, but all components A1, A2, B1 and B2 are metered directly into only one common mixer unit M1. By changing the volume flow of starting materials A1, A2, B1 and / or B2 individually or together, the refractive index of the entire system can be closed-loop controlled as required in a volume ratio. Correspondingly, the first starting material A1 and the second starting material A2 can also be fed directly into the mixer M1 via pumps P1 and P2, and the starting materials B1 and B2 can also be fed directly into the mixer M1 via pumps P3 and P4, wherein after A and B are mixed, a filled optical component G2 is obtained, which can be a Fresnel structure.

[0060] Figure 5 A simplified arrangement is shown as an example of carrying out the method of the invention. G1 illustrates a sample of a filled structure which may include an optical component, for example a filled Fresnel structure as a component of an optical component or an optical element. A camera K optically analyses the sample G1 by recording at least one measurement parameter, wherein the optical analysis is optionally additionally performed using a pattern as described above. Figure 5 In the variant shown, the components (eg resin and curing agent, hereinafter referred to as A and B) are fed directly to the mixer M1, rather than being prepared as separate components A and B via separate streams in the mixers M1 and M2 (see Figure 4 ). Similar to Figure 4 In the arrangement shown (controlled by a controller C and determined by the analysis results of a sample G1), a first starting material A1 and a second starting material A2 (e.g., when mixed, give a resin A) are fed - optionally at pressures p1 and p2 - into a mixer M1 by means of pumps P1 and P2. A third starting material B1 and a fourth starting material B2 (e.g., when mixed, give a curing agent B) are fed - optionally at pressures p3 and p4 - into a mixer M1 by means of pumps P3 and P4, and are then mixed therein to give an adhesive AB, which is processed to give a filled structure G2. Optionally, the structure G2 can then be subjected to a parallel or subsequent optical analysis by comparison with the structure G1 to perform a refractive index matching. The structures G1 and G2 can be any type of microstructure and / or macrostructure which, due to their geometrical features, will lead to optically assessable variations in the test image in the event that the refractive index of the adhesive does not meet the conditions. Typical geometries are: Fresnel structures, prismatic structures, pyramidal structures, striped or corrugated structures, spherical, complex or free-form surfaces - in coherent or segmented form, individually or in arrays, etc.

[0061] As described above, the refractive index can be adjusted via changes in the weight or feed rate or volume of the adhesive components.

[0062] In this way, the refractive index can be adjusted during the production process and precise adjustment and readjustment can be achieved by the method according to the invention. Figure 4 and Figure 5 The controller (control unit) C shown has an influence.

[0063] The adhesive used in the method of the invention may, for example, be a composition based on epoxy resins and thiols, which can be polymerized under amine catalysis.

[0064] In the case of adhesives, especially structural adhesives, for fine machinery and optical devices, short curing times are increasingly needed. Reactive adhesives with short curing times typically also have short processing times. However, from a technical point of view, sufficiently long processing times are often required, for example, in order to accurately align the workpieces to be bonded. The commercial adhesives that cure at room temperature are polyurethane adhesives and amine-cured epoxy resins. When the processing time is about one hour, the curing time at room temperature until the final strength is reached is in the range of about one day to two days.

[0065] The method for adjusting the refractive index of the present invention is particularly suitable for an optical element in which an optical component and a part thereof are bonded to each other by the adhesive and the adhesive becomes a part of an optical system.

[0066] In the method of the present invention, when the processing time is long enough at the same time, an adhesive or composition with a short curing time can be used, so that complete curing is achieved even at room temperature and the micro-adhesive has excellent bonding strength.

[0067] Adhesives that can be used in the method according to the invention can be found, for example, in DE 10 2012 210 185 A1, WO 2009 / 056196 A1 or WO 2015 / 121341 A1. In this way, individual parts of one or more optical components can be bonded to one another by means of an amine-catalyzed, thiol-cured adhesive or adhesive system based on epoxy resins, analogously to WO 2015 / 121341 A1, particularly analogously to claims 1 to 9 of WO 2015 / 121341 A1, particularly preferably analogously to claim 1. Processing can be carried out, for example, at a temperature in the range of 20° C. to 80° C., preferably in the range of 40° C. to 70° C., more preferably in the range of 45° C. to 65° C.

[0068] The starting material for the binder that can be used in the method of the present invention can be a tertiary amine, similar to WO 2015 / 121341 A1.

[0069] The adhesive composition that can be used in the method of the present invention can be UV-curable and contain a photolatent base, as described, for example, in claim 9 of WO 2015 / 121341 A1. In the context of the present invention, a photolatent base refers to a photolatent base compound according to claim 1 of EP 2145 231 B1, which is referenced herein. In the context of the present invention, a photoinitiator is a compound that decomposes into reactive fragments by absorbing light. These reactive fragments then separate the protective group from the photolatent base in the composition so that a strongly basic amidine structure is formed by the photolatent base, which acts as a base to catalyze the polymerization reaction between the epoxide and the SH group of the thiol ester. In this way, the reaction of the amine-catalyzed thiol with the epoxide is locally accelerated in the UV light action area, thereby greatly shortening the curing time of the composition.

[0070] In addition to the photoinitiator, a dye may also be present.

[0071] When using the composition according to WO 2015 / 121341 A1 as embedding medium or for bonding of glass, it is advantageous if the composition additionally contains alkoxysilanes which optionally additionally have polymerizable groups.

[0072] Furthermore, the composition according to WO 2015 / 121341 A1 can additionally contain plasticizers, solid plasticizers, synthetic resins and / or polymers, such as ethylene-vinyl acetate (EVA) copolymers. In addition, fillers such as quartz powder (Silbond) and fine-grained silicon dioxide can also be used as additives.

[0073] The resin component and also the curing agent of the fine adhesive should preferably be reproducible to a specified accuracy. In order to achieve this accuracy, it is preferred for the method of the invention to use at least two main components, such as thiol esters or thiolcarbamates, which have different refractive indices for the resin component (e.g. epoxy compound, component (A)) and / or for the curing agent component (e.g. thiol ester (B) or oligomeric thiolcarbamate).

[0074] It has been found that the compositions described in WO 2015 / 121341 A1 for fine adhesives with high refractive index adjustment are particularly suitable. It is advantageous here to use the oligomers described above or in this document, in particular oligothiocarbamates (reduced volume shrinkage, low curing stress, viscosity matching the resin component - thus better miscibility of resin and curing agent).

[0075] The method of the present invention can be implemented as follows. For example, the method for producing an optical element that is transparent to a predetermined wavelength range and in which an optically active structure is embedded has the following steps:

[0076] a) providing a first housing which is transparent to a predetermined wavelength range, the first housing being in one piece and having a structured section on its top side,

[0077] b) applying a coating which is optically active for a predetermined wavelength range on top of the structured segments to form an optically active structure,

[0078] c) providing a second housing transparent to the predetermined wavelength range, the second housing being in one piece and having a bottom side whose shape is complementary to the shape of the top side of the first housing, the second housing having or not having a structure complementary to the first housing,

[0079] d) applying a composition transparent to a predetermined wavelength range as an adhesive on the top side of the first housing and / or the bottom side of the second housing, and

[0080] e) bonding the top side of the first shell to the bottom side of the second shell by means of an adhesive,

[0081] Wherein, the refractive index of the optical element is matched by the method of the present invention,

[0082] This allows the production of double-shell optical components in which optically active structures are embedded.

[0083] As mentioned above, the optically active structure can be a Fresnel structure. As mentioned at the beginning, the optically active structure can be any type of microstructure and / or macrostructure which, due to its geometrical characteristics, will cause optically assessable variations in the test image in the event that the refractive index of the adhesive does not meet the conditions. Typical geometric structures are: Fresnel structures, prismatic structures, pyramidal structures, striped or corrugated structures, spherical, complex or free-form surfaces - in coherent or segmented form, individually or in array form, etc.

[0084] This method can be used to produce optical elements with two or more shells (especially with exactly two shells) and mass-produced with the desired accuracy and with suitable optical properties. The optical element can also have more than two shells and two or more parts that are bonded or connected to each other by an adhesive.

[0085] The first housing can be provided in step a) such that, apart from the structured section, the top side takes the form of a smooth surface.

[0086] In addition, after step b), the at least one recess formed by the structured section can be filled with material up to the top side. Preferably, the same material is used as for forming the first shell. In addition, the described composition can be used for filling.

[0087] The filling can be done in one go or in several steps. In particular, the filling is done to obtain a smooth, continuous top side. Thus, the filled structured section forms a continuous surface together with the rest of the top side.

[0088] In the method, based on WO 2015 / 121341 A1, in step d), an adhesive having a refractive index matched by the method according to the invention can be applied as an adhesive layer over the entire top side of the first shell and / or the entire bottom side of the second shell. In particular, the structured section (preferably when it has been filled with material up to the top side) can also be provided with an adhesive layer.

[0089] The first shell may consist of a first polymer material and the second shell may in each case be selected from one or more of a thermoplastic material, a thermosetting material, a mineral material and a combination of a polymer material and a mineral glass.

[0090] As described in WO 2015 / 121341 A1, the optically active structure can take the form of, for example, a reflective and / or diffractive structure. In particular, the optically active structure can take the form of a partially reflective structure and / or a wavelength-dependent reflective structure. The formation of the first shell and / or the second shell can be carried out in at least two consecutive composition steps in each case. This reduces the shrinkage during the production of the first shell or the second shell. In the described structure, for example, the first polymer material and the second polymer material used are those materials whose refractive index difference for at least one wavelength in a predetermined wavelength range does not exceed 0.005, preferably does not exceed 0.002, more preferably does not exceed 0.0005, and even more preferably does not exceed 0.0001. In particular, the refractive index may differ by no more than 0.00005. In the case of such a small refractive index difference, for a predetermined wavelength range, the interface between the two polymer materials effectively disappears from the field of view.

[0091] The polymer material can be selected in this case so as to have the same dispersion in a predetermined wavelength range. The predetermined wavelength range can be the visible wavelength range, the near infrared range, the infrared range and / or the UV range.

[0092] Using the method according to the invention, an optical element can be produced, for example, by the procedure described in WO 2015 / 121341 A1, so that, for example, in a first step, a first semi-finished product is produced from a thermoplastic polymer by injection molding. The first semi-finished product has a first side and a second side. On the second side, a microstructure is formed, which defines the shape of the desired reflective facet.

[0093] The materials used for the two semi-finished products can be different materials. However, preferably, the two semi-finished products use the same material. In particular, the above-mentioned thermoplastic material and / or thermosetting material is suitable.

[0094] With the adhesive described in WO 2015 / 121341 A1, sufficiently long processing times of about 60 to 120 minutes can be achieved with complete curing in about 4 to 6 hours (at room temperature), and excellent bond strengths can be achieved.

[0095] Figure 6 is a flow chart of an illustrative method for adjusting the refractive index of an adhesive for an optical element.

[0096] In frame 3005, a sample of an optical element is produced. For this purpose, a plurality of optical components of the optical element can be bonded to each other. For this purpose, an optically transparent adhesive as described above is used. The optically transparent adhesive has a plurality of starting materials mixed with each other. In the first iteration of frame 3005, an initial mixing ratio of a plurality of starting materials is used.

[0097] For example, at block 3005, the following may be performed: Figure 4 The mixing is carried out by means of an associated technique, wherein, as described above, the first starting material A1 and the second starting material A2 forming the resin A are mixed in a mixer M1 and then arrive in a storage container A, and the third starting material B1 and the fourth starting material B2 are mixed in a mixer M2 and then arrive in a storage container B. Components A and B together form a reactive system that cures over time by thermal and / or photochemical / UV activation, wherein the components in the example shown are contacted in a mixer M3.

[0098] Additionally, at block 3005, the Figure 5 Related technologies, including Figure 4 In contrast, as described above, the components (e.g., resin and curing agent, hereinafter referred to as A and B) are fed directly into the mixer M1, rather than being prepared as separate components A and B via separate streams in the mixers M1 and M2. Figure 4 In the arrangement shown (controlled by the controller C and determined by the analysis results of the sample G1), the first starting material A1 and the second starting material A2 (e.g., when mixed, give the resin A) are fed - optionally at pressures p1 and p2 - by pumps P1 and P2 into a mixer M1. The third starting material B1 and the fourth starting material B2 (e.g., when mixed, give the curing agent B) are fed - optionally at pressures p3 and p4 - by pumps P3 and P4 into the mixer M1, and then mixed in the mixer to give the adhesive AB, which is processed to give the filled structure G2.

[0099] The mixing ratio of the starting materials determines the refractive index. In particular, the refractive index at the initial mixing ratio may vary from the refractive index of one or more of the substrate materials used in the optical element. This may be due to fluctuations in the batches of substrate materials and / or due to fluctuations in the mixing ratio of the starting materials. Environmental conditions may also affect the quality of the refractive index match.

[0100] At block 3010, an optical analysis is performed on the sample produced in the current iteration of block 3005. The purpose of the optical analysis is to determine the quality of the refractive index match between the adhesive and the optical component. For example, at block 3010, as described above, the optical analysis may be performed by recording at least one measurement parameter, such as, for example Figure 1 , Figure 4 and Figure 5 In particular, in block 3010, as Figure 4 and Figure 5 As shown, the sample G1 (which may include, for example, a filled Fresnel structure as an optical component) may be optically analyzed by recording at least one measurement parameter using a camera K, wherein, as described above, the optical analysis may optionally be performed using a camera transmission pattern. The verification technique described in block 3010 may also evaluate the results of the optical analysis, for example Figure 2 and Figure 3 The color splitting, or optical shifting, shown.

[0101] At block 3015, it is then verified whether there is a refractive index match, i.e., whether there is a variation between the refractive index of the adhesive and the refractive index of the optical component forming the optical element. For example, it can be verified whether the variation is within a defined tolerance range, such that the difference can be determined based on the evaluation results of previous optical analysis of multiple samples (e.g., optical shift or color splitting, such as Figure 2 and Figure 3 ) adjusting the mixing ratio of the various starting materials between the production of the multiple samples, preferably in a gradual, linear or decreasing manner.

[0102] When the verification result of frame 3015 is that there is a significant variation between the refractive index of the adhesive and the refractive index of the optical component, the mixing ratio of the starting material can be adjusted in frame 3020. This can be achieved, for example, by closed-loop control. For example, in the case of such closed-loop control adjustment, the sign of the variation and / or the size of the variation can be considered and converted by means of a defined model to adjust the mixing ratio of one or more starting materials and one or more other starting materials. For example, in the case of a large variation in the refractive index, there may be a trend to make a greater adjustment to the mixing ratio. The specific implementation of the adjustment of the mixing ratio depends on the properties of the adhesive used or the starting material used. For example, this dependence can be determined by empirical testing. This logic can be modeled by means of a controller, which actuates, for example, a metering pump based on a program code executed by the controller from a memory. In this way, in particular, a closed-loop control loop can be implemented that minimizes the mismatch of the refractive index and uses the mixing ratio of the starting material as a manipulated variable. This closed-loop control loop can work with a particularly high waiting time, because, for example, optical analysis must wait for a stable state after the curing of the adhesive is initiated.

[0103] However, if the cure characteristics are known, readjustments can be made based on the variation found in the uncured state. In this case, the target parameter would be a specific shift or a specific color split equal to that after application of the adhesive system or in a defined partially cured state.

[0104] With the matched mixing ratio, it is then verified in further iterations of blocks 3005, 3010, 3015 whether there is a refractive index match. This therefore means that a plurality of samples can be produced (e.g. in a progressive, linear or decreasing manner), wherein the mixing ratios of the various starting materials are matched between the production of two samples (in successive iterations of blocks 3005, 3010, 3015), in each case based on the results of the corresponding optical analysis of the previous iteration.

[0105] When the verification at block 3015 ultimately indicates that the refractive index of the adhesive is not significantly different (if at all) from the refractive index of the optical component, ie, the refractive index match is successful, a finished duplicate product having the desired optical properties can be produced at block 3025 .

[0106] Using the above-described method of the present invention, an optical element for a display device or a pair of smart glasses can be produced, which optical element includes multiple optical components and is transparent or partially transparent to a predetermined wavelength range and in which an optically active structure is embedded, wherein the method of the present invention enables matching of the refractive index so that an undistorted view can be seen through the optical element.

Claims

1. A method for adjusting the refractive index of an adhesive for an optical element, wherein: The adhesive is optically clear and is produced from a variety of starting materials, wherein the method comprises: - producing at least one sample of the optical element using the adhesive, - optically analyzing at least one sample of the optical element by recording at least one measurement parameter, - adjusting the mixing ratio of the various starting materials of the adhesive based on the results of the optical analysis, and - producing a plurality of replicate products of the optical element using a binder having an adjusted mixing ratio of the plurality of starting materials.

2. The method according to claim 1, in, Multiple samples of the optical element are produced successively. Wherein, based on the results of the previous optical analysis of the plurality of samples, the mixing ratio of the plurality of starting materials is adjusted between the production of the plurality of samples.

3. The method of claim 2, wherein: The method further comprises: A closed control loop is implemented, wherein the closed control loop compares the at least one measured parameter with a corresponding target value and sets the dosage of at least one starting material from the plurality of starting materials as a controlled variable when adjusting the mixing ratio.

4. The method according to claim 3, in, The closed-loop control tolerance of the closed-loop control loop as a deviation from a defined refractive index is less than 0.0005 or less than 0.0001.

5. A method as claimed in any one of the preceding claims, in, The plurality of starting materials include a first starting material, a second starting material, a third starting material, and a fourth starting material, Wherein, the adhesive is a two-component adhesive, The first component of the two-component adhesive is formed by mixing the first starting material and the second starting material. The second component of the two-component adhesive is formed by mixing the third starting material and the fourth starting material. wherein adjusting the mixing ratio of the plurality of starting materials comprises adjusting a first partial mixing ratio of the first starting material relative to the second starting material in the mixing of the first component, Wherein, adjusting the mixing ratio of the plurality of starting materials includes adjusting a second portion mixing ratio of the third starting material relative to the fourth starting material in the mixing of the second component.

6. The method according to claim 5, in, Adjusting the mixing ratio includes adjusting a third portion mixing ratio of the first component relative to the second component.

7. A method as claimed in any one of the preceding claims, in, The plurality of starting materials include a first starting material, a second starting material, a third starting material, and a fourth starting material, Wherein, the adhesive is a two-component adhesive, The first component of the two-component adhesive is mixed with the first starting material and the second starting material in a first mixer, and The second component of the two-component adhesive is mixed with the third starting material and the fourth starting material in a second mixer. And wherein the first component and the second component of the two-component adhesive are mixed in a third mixer downstream of the first mixer and the second mixer.

8. A method as claimed in any one of the preceding claims, in, The mixing ratio of the multiple starting materials is adjusted by changing the amount of at least one of the multiple starting materials, changing the weight of at least one of the multiple starting materials, changing the volume of at least one of the multiple starting materials, and / or changing the flow rate of at least one of the multiple starting materials from a storage container, for example, via a metering pump into a mixing container.

9. A method as claimed in any one of the preceding claims, in, Performing the optical analysis comprises recording the temporal evolution of the at least one measured parameter over a period of at least 24 hours.

10. The method according to any one of the preceding claims, in, Performing the optical analysis comprises detecting the optical transmission of a test pattern through the optical element by means of a camera.

11. The method according to claim 9 or 10, in, The at least one measurement parameter comprises a color breakup and / or an optical shift of the optical transmission of the optical element, the color breakup and / or the optical shift being determined based on the optical transmission of the test pattern.

12. The method according to claim 9 or 10, in, The at least one measurement parameter includes a prismatic effect of the optical element determined based on an optical transmission of the test pattern.

13. The method according to any one of claims 9 to 12, in, The optical element includes a Fresnel structure, and The test pattern is reflected laterally into the Fresnel structure.

14. A method as claimed in any one of the preceding claims, in, The at least one measured parameter comprises light dispersion of the adhesive at a particular wavelength or within a range of wavelengths.

15. A method as claimed in any one of the preceding claims, in, The optical element comprises a plurality of optical components. wherein producing at least one sample of the optical element comprises bonding the plurality of optical components with the adhesive and initiating curing of the adhesive, The optical analysis is hereby started after the initiation of curing.

16. A method as claimed in any one of the preceding claims, in, The optical element comprises a plurality of optical components. wherein producing at least one sample of the optical element comprises bonding a plurality of optical components with the adhesive and initiating curing of the adhesive, Wherein, a first optical component among the plurality of optical components of the optical element comprises a Fresnel structure, and wherein a second optical component among the plurality of optical components of the optical element comprises a housing.

17. The method of claim 16, wherein: The first optical component is a housing including the Fresnel structure.

18. The method according to any one of claims 15 to 17, wherein: One or more of these optical components are produced by an injection molding process.

19. A method as claimed in any one of the preceding claims, in, The curing reaction of the adhesive is initiated with the aid of UV light and / or heat.

20. A method as claimed in any one of the preceding claims, wherein: The adhesive is a thermally curing or photochemically curing (UV curing) adhesive.

21. A method as claimed in any one of the preceding claims, wherein: The adhesive is produced from a variety of 1-component adhesives as starting material.

22. A method as claimed in any one of the preceding claims, wherein: The adhesive includes an epoxy resin cured via an amine-catalyzed mercaptan, or a polycarbonate resin.