Styrene resin composition for optical use, light guide plate, edge light type surface light source unit, light diffusion plate, and direct down type surface light source unit
By using a specific proportion and type of styrene-based resin, a (meth)acrylate-based monomer copolymer and a hindered amine light stabilizer in the light guide plate, the problem of deterioration and uneven hue after long-term use is solved. , realizes the optical performance stability and dimensional stability of high-brightness LED light sources.
Patent Information
- Application Number
- CN202380036124.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-13
- Filing Date
- 2023-04-27
- Publication Date
- 2024-12-06
AI Technical Summary
The conventional styrene-(meth)acrylate copolymer light guide plates are prone to deterioration (carbonization) of end face parts after long-term use, and the hue is uneven, which affects transparency and dimensional stability.
Copolymers containing styrene-based monomers and (meth)acrylate-based monomers are used, and hindered amine light stabilizers are added to adjust their mass ratio and types to improve the transparency, hue and color of the styrene-based resin for optical use. Dimensional stability, suitable for long-term use of high-brightness LED light sources.
It achieves excellent light stability for LED light sources, avoids carbonization of the end face of the light guide plate, ensures stability of hue and size, and improves transparency and service life.
Smart Images

Figure BDA0005100003170000071 
Figure BDA0005100003170000161 
Figure BDA0005100003170000171
Abstract
Description
Technical Field
[0001] The present invention relates to an optical styrene resin composition, a light guide plate, an edge-light type surface light source unit, a light diffusion plate, and a direct-light type surface light source unit. Background Art
[0002] The backlight sources of liquid crystal display devices include direct-lit type, where the light source is arranged on the front of the display device, and edge-lit type, where the light source is arranged on the side. Edge-lit backlight sources use a component called a light guide plate that guides the light from the light source arranged on the side to the front of the display device. They are used in a wide range of applications, such as televisions, desktop personal computer displays, notebook personal computers, mobile phones, and car navigation displays. In addition, backlight sources using light guide plates are also used as lighting devices or billboards.
[0003] The light transmission distance of the light guide plate is relatively long, and the light loss in the optical path length is large, so it is required to have a particularly high light transmittance. Therefore, the material of the light guide plate uses an acrylic resin represented by polymethyl methacrylate (PMMA). However, PMMA has a high water absorption, so there is a situation where the light guide plate will warp or change in size due to water absorption. In addition, it is easy to thermally decompose during molding, so if it is molded at a high temperature, there is a problem that the molded body is prone to poor appearance. In order to improve these problems, for example, Patent Document 1 proposes using styrene-methyl (meth)acrylate copolymer as a material for the light guide plate.
[0004] On the other hand, the molded product of styrene-methyl (meth)acrylate copolymer has a poorer hue than PMMA, and may cause color unevenness when used as a backlight. In order to improve this problem, Patent Document 2 is proposed as a hue improvement technology for styrene-methyl (meth)acrylate.
[0005] [Prior art documents]
[0006] [Patent Document]
[0007] [Patent Document 1] Japanese Patent Publication No. 2003-075648
[0008] [Patent Document 2] International Publication No. 2016-129675 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] In recent years, with the increase in the resolution of backlight units such as televisions and monitors, high-brightness LEDs (light-emitting diodes) are sometimes used as edge light sources. However, the previous styrene-methyl (meth)acrylate copolymer light guide plates may deteriorate (carbonize) at the end surfaces of the light guide plates after being lit for a long time, depending on the usage environment.
[0011] The present invention has been made in view of the above problems, and an object of the present invention is to provide an optical styrene resin composition having excellent transparency, hue, and dimensional stability and excellent light stability against long-term use of an LED light source.
[0012] Solutions for solving problems
[0013] According to the present invention, there is provided an optical styrene resin composition, which contains a styrene resin (A) which is a copolymer containing a styrene monomer unit and a (meth)acrylate monomer unit, and a hindered amine light stabilizer (B), wherein the copolymer contains 95 to 20% by mass of the styrene monomer unit and 5 to 80% by mass of the (meth)acrylate monomer unit in 100% by mass of the copolymer, and the optical styrene resin composition contains 0.001 to 1.0 parts by mass of the hindered amine light stabilizer (B) relative to 100 parts by mass of the styrene resin (A).
[0014] The present inventors have conducted diligent research and have found that an optical styrene resin composition comprising a styrene resin having a content of styrene monomer units and (meth)acrylate monomer units within a specific range and a hindered amine light stabilizer within a specific range can simultaneously satisfy transparency, hue, dimensional stability, and light stability for long-term use with an LED light source, thereby completing the present invention.
[0015] Various embodiments of the present invention are described below. The embodiments described below can be combined with each other.
[0016] [1] An optical styrene resin composition comprising a styrene resin (A) which is a copolymer containing a styrene monomer unit and a (meth)acrylate monomer unit, and a hindered amine light stabilizer (B), wherein the copolymer contains 95 to 20% by mass of the styrene monomer unit and 5 to 80% by mass of the (meth)acrylate monomer unit in 100% by mass of the copolymer, and the optical styrene resin composition contains 0.001 to 1.0 part by mass of the hindered amine light stabilizer (B) based on 100 parts by mass of the styrene resin (A).
[0017] [2] The optical styrene resin composition according to [1], wherein the hindered amine light stabilizer (B) is an NH-type hindered amine light stabilizer and / or an NR-type hindered amine light stabilizer.
[0018] [3] The optical styrene resin composition as described in [2], wherein the NH type hindered amine light stabilizer is selected from
[0019] Sebacate bis(2,2,6,6-tetramethylpiperidin-4-yl) ester,
[0020] Hexadecanoic acid 2,2,6,6-tetramethyl-4-piperidinyl ester, octadecanoic acid 2,2,6,6-tetramethyl-4-piperidinyl ester,
[0021] 1,2,3,4-Butanetetracarboxylic acid tetrakis (2,2,6,6-tetramethyl-4-piperidinyl) ester,
[0022] N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 4-morpholinyl 2,6-dichloro-1,3,5-triazine, polycondensate,
[0023] Condensation product of 2,4-dichloro-6-(1,1,3,3-tetramethylbutylamino) and 1,3,5-triazine·N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)hexamethylenediamine,
[0024] N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 2,4,6-trichloro-1,3,5-triazine and N-butyl-1-butylamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine, polycondensate,
[0025] 1,6,11-Tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidinyl)amino)symmetrical triazine-6-yl]aminoundecane,
[0026] Polycondensation of 1,2,3,4-butanetetracarboxylic acid with 2,2,6,6-tetramethyl-4-piperidinol and β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol
[0027] At least one of the following.
[0028] [4] The optical styrene resin composition as described in [2] or [3], wherein the NR type hindered amine light stabilizer is selected from
[0029] Methyl sebacate (1,2,2,6,6-pentamethylpiperidin-4-yl) ester,
[0030] Sebacate bis(1,2,2,6,6-pentamethylpiperidin-4-yl) ester,
[0031] n-Butyl 3,5-di-tert-butyl 4-hydroxybenzylmalonate bis(1,2,2,6,6-pentamethylpiperidin-4-yl) ester, polycondensate of 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol and dimethyl succinate,
[0032] 1,5,8,12-Tetrakis[4,6-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidinyl)amino)-1,3,5-triazine-2-yl]-1,5,8,12-tetraazadodecane,
[0033] 1,2,3,4-Butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol, polycondensate,
[0034] A mixture of succinic acid, polycondensate with (4-hydroxy-2,2,6,6-tetramethylpiperidin-1-yl)ethanol and N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine
[0035] At least one of the following.
[0036] [5] The optical styrene resin composition according to any one of [1] to [4], comprising 0.001 to 0.5 parts by mass of a phosphorus antioxidant (C-1) based on 100 parts by mass of the styrene resin (A).
[0037] [6] The optical styrene resin composition according to [5], wherein the phosphorus-based antioxidant (C-1) is at least one selected from tris(2,4-di-tert-butylphenyl) phosphite, 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphite, bis-(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diylbisphosphonite, and bis(2,4-di-tert-butyl-6-methylphenyl)ethyl phosphite.
[0038] [7] A light guide plate obtained by molding the optical styrene resin composition according to any one of [1] to [6].
[0039] [8] An edge-lit surface light source unit comprising the light guide plate as described in [7], and a light source that supplies LED light to an end surface of the light guide plate.
[0040] [9] A light diffusion plate obtained by molding the optical styrene resin composition according to any one of [1] to [6].
[0041]
[10] A direct-type surface light source unit comprising the light diffusion plate as described in [9] and a light source for supplying LED light to the light diffusion plate. DETAILED DESCRIPTION
[0042] Hereinafter, embodiments of the present invention will be described. Various characteristic matters illustrated in the embodiments shown below can be combined with each other. In addition, each characteristic matter independently establishes the invention.
[0043] 1. Optical styrene resin composition
[0044] The optical styrene resin composition according to one embodiment of the present invention is an optical styrene resin composition containing a styrene resin (A) and a hindered amine light stabilizer (B).
[0045] <Styrene Resin (A)>
[0046] Styrene resin (A) is a resin obtained by copolymerizing monomers containing styrene monomers and (meth) acrylate monomers. Styrene resin (A) is a copolymer containing styrene monomer units and (meth) acrylate monomer units. The copolymer contains 95-20% by mass of styrene monomer units and 5-80% by mass of (meth) acrylate monomer units in 100% by mass of the copolymer, preferably 90-25% by mass of styrene monomer units and 10-75% by mass of (meth) acrylate monomer units, more preferably 80-30% by mass of styrene monomer units and 20-70% by mass of (meth) acrylate monomer units, and further preferably 60-40% by mass of styrene monomer units and 40-60% by mass of (meth) acrylate monomer units. By setting it to such a range, transparency, hue, and dimensional stability can be satisfied at the same time. By setting the styrene monomer to 90% by mass or less, a light guide plate with excellent transparency and hue can be obtained, and by setting the styrene monomer to more than 20%, a light guide plate with excellent dimensional stability can be obtained. The content of the (meth)acrylate monomer unit in the styrene resin (A) is specifically, for example, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, or 80 mass %, and may be within the range between any two of the values exemplified here.
[0047] Examples of the styrene monomer include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, ethylstyrene, and p-tert-butylstyrene. These may be used alone or in combination of two or more. The styrene monomer is preferably styrene.
[0048] Examples of the (meth)acrylate monomer include: alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; aryl (meth)acrylates such as phenyl (meth)acrylate and benzyl (meth)acrylate; cyclohexyl (meth)acrylate, 4-tert-butylcyclohexyl (meth)acrylate, 2-norbornyl (meth)acrylate, isobornyl (meth)acrylate, adamantane-1-yl (meth)acrylate, 2-methyladamantan-2-yl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, and cycloalkyl (meth)acrylates such as tricyclodecyl (meth)acrylate; glycidyl (meth)acrylate; and dicyclopentanyl (meth)acrylate. These may be used alone or in combination of two or more. The (meth)acrylate monomer is preferably an alkyl (meth)acrylate, and more preferably methyl methacrylate.
[0049] In addition, the styrene resin (A) may be a copolymer obtained by copolymerizing a styrene monomer and a (meth)acrylate monomer with a copolymerizable monomer. Examples of copolymerizable monomers include: (meth)acrylic acids such as acrylic acid and methacrylic acid; vinyl cyanides such as acrylonitrile and methacrylonitrile; α,β-ethylene unsaturated carboxylic acids such as maleic anhydride and fumaric acid; and imides such as phenylmaleimide and cyclohexylmaleimide. These may be used alone or in combination of two or more.
[0050] The weight average molecular weight (Mw) of the styrene resin (A) is preferably 50,000 to 400,000, and more preferably 100,000 to 350,000. In addition, the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the styrene resin (A) is preferably 1.0 to 3.5, and more preferably 1.5 to 3.0. By setting it to such a range, it is possible to take into account both the moldability and the strength of the light guide plate. If the weight average molecular weight (Mw) is less than 50,000, the strength of the molded product may become insufficient, and if it exceeds 400,000, the moldability may decrease. In addition, if the ratio (Mw / Mn) of the number average molecular weight (Mn) is less than 1.0, the moldability may decrease, and if it exceeds 3.5, the strength of the molded product may decrease.
[0051] <Hindered Amine Light Stabilizer (B)>
[0052] In the optical styrene resin composition, 0.001 to 1.0 parts by mass of a hindered amine light stabilizer (B) is contained relative to 100 parts by mass of the styrene resin (A), preferably 0.01 to 0.3 parts by mass. By setting it to such a range, the transparency, hue, and light stability to the LED light source can be improved. The content of the hindered amine light stabilizer (B) is, for example, 0.001, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 parts by mass relative to the styrene resin (A), and can also be within the range between any two of the numerical values exemplified here. In addition, the hindered amine light stabilizer (B) can be used alone or in combination of two or more.
[0053] The hindered amine light stabilizer (B) is a compound having a structural unit represented by the following general formula (1).
[0054] [Chemistry 1]
[0055]
[0056] In the general formula (1), X is an organic group bonded to the 4-position of the piperidinyl group via a carbon atom, an oxygen atom, or a nitrogen atom, and examples of R include a hydrogen atom, a linear or branched alkyl group having 1 to 10 carbon atoms, a methylene group, and an alkoxy group. Here, when R is a hydrogen atom, it is an NH type hindered amine light stabilizer, when R is a linear or branched alkyl group having 1 to 10 carbon atoms, or a methylene group, it is an NR type hindered amine light stabilizer, and when R is an alkoxy group, it is an N-OR hindered amine light stabilizer.
[0057] Specific examples of the NH type hindered amine light stabilizer include: bis(2,2,6,6-tetramethylpiperidin-4-yl) sebacate (TINUVIN770DF manufactured by BASF), 2,2,6,6-tetramethyl-4-piperidinyl hexadecanoate, 2,2,6,6-tetramethyl-4-piperidinyl octadecanoate (SABOSTAB UV91 manufactured by SONGWON), tetrakis(2,2,6,6-tetramethyl-4-piperidinyl) 1,2,3,4-butanetetracarboxylate (ADK STAB LA-57 manufactured by ADEKA), polycondensate of N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 4-morpholino-2,6-dichloro-1,3,5-triazine (SABOSTAB UV91 manufactured by SONGWON), UV79), polycondensation product of 2,4-dichloro-6-(1,1,3,3-tetramethylbutylamino) and 1,3,5-triazine and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)hexamethylenediamine (Chimassorb 944FDL manufactured by BASF), polycondensation product of N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 2,4,6-trichloro-1,3,5-triazine and N-butyl-1-butylamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine (SABOSTAB manufactured by SONGWON UV40), 1,6,11-tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidinyl)amino) symmetrical triazin-6-yl]aminoundecane (Chimassorb 2020FDL manufactured by BASF), polycondensation product of 1,2,3,4-butanetetracarboxylic acid, 2,2,6,6-tetramethyl-4-piperidinol, and β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol (ADKSTAB manufactured by ADEKA) LA-68), dodecyl 3-(2,2,4,4-tetramethyl-21-oxo-7-oxa-3,20-diazadispiro(5.1.11.2)heneicosane-20-yl)propionate, tetradecyl 3-(2,2,4,4-tetramethyl-21-oxo-7-oxa-3,20-diazadispiro(5.1.11.2)heneicosane-20-yl)propionate (HOSTAVIN 3030 manufactured by CLARIANT), polycondensate of 2,2,4,4-tetramethyl-7-oxa-3,20-diazadispiro-(5.1.11.2)heneicosane-21-one and epichlorohydrin (HOSTAVIN N30P manufactured by CLARIANT).
[0058] Specific examples of NR-type hindered amine light stabilizers include: methyl sebacate (1,2,2,6,6-pentamethylpiperidin-4-yl) ester, bis (1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate (TINUVIN 292 and TINUVIN 765 manufactured by BASF), bis (1,2,2,6,6-pentamethylpiperidin-4-yl) n-butyl 3,5-di-tert-butyl 4-hydroxybenzylmalonate (TINUVIN 144 manufactured by BASF), polycondensate of 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinol and dimethyl succinate (TINUVIN 144 manufactured by BASF), TINUVIN622SF, 1,5,8,12-tetrakis[4,6-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidinyl)amino)-1,3,5-triazine-2-yl]-1,5,8,12-tetraazadodecane (Chimassorb 119 manufactured by BASF), polycondensation product of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol and β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol (ADKSTAB manufactured by ADEKA) LA-63P), a condensation product of succinic acid and (4-hydroxy-2,2,6,6-tetramethylpiperidin-1-yl)ethanol, and a mixture of N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine (TINUVIN111FDL manufactured by BASF).
[0059] Specific examples of the N-OR type hindered amine light stabilizer include bis(1-octyloxy-2,2,6,6-tetramethylpiperidinyl) sebacate (TINUVIN 123 manufactured by BASF) and bis(1-undecyloxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate (ADKSTAB LA-81 manufactured by ADEKA).
[0060] Among them, from the viewpoint of having less influence on the transparency and hue of the optical styrene resin composition, the hindered amine light stabilizer (B) is preferably an NH type hindered amine light stabilizer and / or an NR type hindered amine light stabilizer, and more preferably an NR type hindered amine light stabilizer. It is known that the hindered amine light stabilizer (B) is generally oxidized by oxygen, ultraviolet rays and peroxides to produce nitroxide free radicals. In this embodiment, although the mechanism by which the hindered amine light stabilizer (B) can improve the light stability for long-term use of the LED light source has not been clarified, the present invention has found the effectiveness of the hindered amine light stabilizer (B).
[0061] <Antioxidant (C)>
[0062] In the optical styrene resin composition, it is preferred to contain 0.001 to 0.5 parts by mass of a phosphorus antioxidant (C-1) relative to 100 parts by mass of the styrene resin (A), more preferably 0.002 to 0.4 parts by mass, and particularly preferably 0.005 to 0.3 parts by mass. By setting it to such a range, transparency and hue can be improved. The content of the phosphorus antioxidant (C-1) is specifically, for example, 0.001, 0.002, 0.003, 0.004, 0.005, 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 parts by mass relative to 100 parts by mass of the styrene resin (A), and may also be in the range between any two of the numerical values exemplified herein.
[0063] The so-called phosphorus antioxidant (C-1) is a (phosphite) ester having no phenolic hydroxyl group in the basic skeleton, and is preferably a phosphite ester as a trivalent phosphorus compound. Specific examples of the phosphorus antioxidant (C-1) include 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphite, bis-(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl)phosphite, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diylbisphosphonite, bis(2,4-di-tert-butyl-6-methylphenyl)ethylphosphite, and the like, and these can be used alone or in combination of two or more.
[0064] In addition, the optical styrene resin composition may contain 0 to 0.5 parts by mass of a phenolic antioxidant (C-2) relative to 100 parts by mass of the styrene resin (A). If the content of the phenolic antioxidant (C-2) exceeds 0.5 parts by mass, the hue will deteriorate, so it is not preferred. The content of the phenolic antioxidant (C-2) relative to 100 parts by mass of the styrene resin (A) is specifically, for example, 0, 0.001, 0.002, 0.003, 0.004, 0.005, 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 parts by mass, and may also be within the range between any two of the numerical values exemplified here.
[0065] The so-called phenolic antioxidant (C-2) is an antioxidant having a phenolic hydroxyl group in the basic skeleton and not being a (phosphite) type antioxidant. Specific examples of the phenolic antioxidant (C-2) include, for example, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, ethylenebis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl) propionate], and pentaerythritoltetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and these can be used alone or in combination of two or more.
[0066] The antioxidant is a phosphorus-phenol compound having both a phosphite structure and a phenol structure in the same molecule, such as 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphine. In the case of such a compound, the optical styrene resin composition is considered to contain both a phosphorus-based antioxidant and a phenolic antioxidant. For example, when the phosphorus-phenol compound is contained in an amount of 0.1 parts by mass relative to 100 parts by mass of the styrene resin (A), the composition is considered to contain 0.1 parts by mass of the phosphorus-phenol compound and 0.1 parts by mass of the phenolic antioxidant.
[0067] <Other ingredients>
[0068] The tert-butylcatechol (TBC) in the optical styrene resin composition is preferably 10 ppm or less, more preferably 5 ppm or less. By setting it to this range, a light guide plate with excellent hue and transmittance can be obtained. The content of TBC is specifically, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 ppm, and can also be in the range between any two of the numerical values exemplified here.
[0069] The 6-tert-butyl-2,4-xylenol (TBX) in the optical styrene resin composition is preferably 10 ppm or less, more preferably 5 ppm or less. By setting it to such a range, a light guide plate with excellent hue and transmittance can be obtained. The content of TBX is specifically, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 ppm, and can also be in the range between any two of the numerical values exemplified here.
[0070] The optical styrene resin composition may contain a sulfur-based antioxidant, a lactone-based antioxidant, an ultraviolet absorber, an antistatic agent, a hydrophilic additive, liquid paraffin (mineral oil), polyethylene wax, microcrystalline wax, a bluing agent, higher fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid, higher fatty acid amides such as stearamide, erucamide, and ethylenebisstearamide, higher fatty acid glycerides such as lauric acid monoglyceride, palmitic acid monoglyceride, stearic acid monoglyceride, and behenic acid monoglyceride, and a release agent such as a higher alcohol such as myristyl alcohol, cetyl alcohol, and stearyl alcohol, within a range not impairing the characteristics of the present invention.
[0071] The melt mass flow rate (MFR) of the optical styrene resin composition at a temperature of 200° C. and a load of 49 N is preferably 0.5 to 5.0 g / 10 min, more preferably 1.0 to 4.0 g / 10 min. If the MFR is less than 0.5 g / 10 min, molding stability decreases, and if the MFR exceeds 5.0 g / 10 min, strength becomes insufficient.
[0072] The Vickers softening temperature of the optical styrene resin composition is preferably 95 to 104° C., more preferably 100 to 104° C. If the Vickers softening temperature is lower than 95° C., heat resistance is insufficient and the light guide plate may be deformed depending on the use environment.
[0073] <Method for producing optical styrene resin composition>
[0074] As the polymerization method of the styrene resin (A), known styrene polymerization methods such as block polymerization, solution polymerization, suspension polymerization, and emulsion polymerization can be cited. In terms of quality or productivity, block polymerization and solution polymerization are preferred, and continuous polymerization is preferred. As the solvent, for example, alkylbenzenes such as benzene, toluene, ethylbenzene, and xylene, ketones such as acetone and methyl ethyl ketone, aliphatic hydrocarbons such as hexane or cyclohexane, etc. can be used.
[0075] During the polymerization of the styrene resin (A), polymerization aids such as polymerization initiators, chain transfer agents, and crosslinking agents, and other polymerization aids may be used as needed. As the polymerization initiator, a free radical polymerization initiator is preferred, and examples thereof include known and commonly used peroxyketals such as 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(tert-butylperoxy)butane, 2,2-di(4,4-di-tert-butylperoxycyclohexyl)propane, and 1,1-di(tert-amylperoxy)cyclohexane, hydroperoxides such as cumene hydroperoxide and tert-butyl hydroperoxide, alkyl peroxides such as tert-amyl peroxynonanoate, tert-butyl isopropyl peroxide, di-tert-butyl peroxide, diisopropyl peroxide, and di-tert-butyl isononanoate. Dialkyl peroxides such as hexyl peroxide, peroxyesters such as tert-butyl peroxyacetate, tert-butyl perbenzoate, and tert-butyl peroxyisopropyl monocarbonate, peroxycarbonates such as tert-butyl peroxyisopropyl carbonate and polyethertetrakis (tert-butyl peroxycarbonate), N,N'-azobis(cyclohexane-1-carbonitrile), N,N'-azobis(2-methylbutyronitrile), N,N'-azobis(2,4-dimethylvaleronitrile), and N,N'-azobis[2-(hydroxymethyl)propionitrile], etc., can be used alone or in combination of two or more. Examples of the chain transfer agent include aliphatic mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, aromatic mercaptans, thiocarboxylic acids such as thioglycolic acid and mercaptopropionic acid, polyfunctional mercaptans obtained by esterifying hydroxyl groups of polyols such as ethylene glycol, tetraethylene glycol, neopentyl glycol, trimethylolpropane, pentaerythritol, dipentaerythritol, tripentaerythritol, and sorbitol with thioglycolic acid or mercaptopropionic acid, pentaphenylethane, α-methylstyrene dimer, and terpinolene, etc. Among them, aliphatic mercaptans, aromatic mercaptans, thiocarboxylic acids, and polyfunctional mercaptans are preferred from the viewpoint of easy adjustment of molecular weight.
[0076] In the case of continuous polymerization, the styrene resin (A) can be produced by a method comprising a polymerization step, a devolatilization step, and a granulation step.
[0077] First, in the polymerization step, a known complete mixing tank type stirring tank or tower type reactor is used, and the polymerization reaction is controlled by adjusting the polymerization temperature and the like so as to achieve the target molecular weight, molecular weight distribution, and reaction conversion rate.
[0078] The polymer solution containing the polymer that has completed the polymerization step is transferred to the de-volatilization step to remove the unreacted monomer and the polymerization solvent. The de-volatilization step includes a vacuum de-volatilization tank with a heater or a de-volatilization extruder with a vent hole. The molten polymer that has completed the de-volatilization step is transferred to the granulation step. In the granulation step, the molten resin is extruded from a porous die in a linear shape and processed into a pellet shape by a cold cutting method, an in-air thermal cutting method, or an underwater thermal cutting method.
[0079] The optical styrene resin composition can be produced by adding a hindered amine light stabilizer (B), a phosphorus antioxidant (C-1), and a phenolic antioxidant (C-2) to a styrene resin (A). The hindered amine light stabilizer (B), the phosphorus antioxidant (C-1), and the phenolic antioxidant (C-2) can be added to the raw material solution before the polymerization of the styrene resin (A), or mixed by an extruder or a static mixer installed after the polymerization of the styrene resin (A) and before granulation. In addition, the granulated particles of the styrene resin (A) can be dry-blended with the hindered amine light stabilizer (B), the phosphorus antioxidant (C-1), and the phenolic antioxidant (C-2) and melt-kneaded to produce the composition. In addition, a granular masterbatch can be prepared by melt-kneading the hindered amine light stabilizer (B), the phosphorus antioxidant (C-1), and the phenolic antioxidant (C-2) together with a small amount of styrene resin in advance, and then dry-blending the styrene resin (A) with the masterbatch and melt-kneading them.
[0080] The content of tert-butylcatechol or 6-tert-butyl-2,4-xylenol in the optical styrene resin composition can be adjusted at the start of polymerization of the styrene resin (A) and in the subsequent devolatilization step or the like.
[0081] 2. Light guide plate
[0082] A light guide plate according to one embodiment of the present invention is a molded product obtained by molding the optical styrene resin composition. The light guide plate is a light guide plate that can be used in an edge-light type surface light source unit.
[0083] <Shape of light guide plate>
[0084] The light guide plate may have a concave-convex shape on the surface of the light guide plate. More specifically, the surface of the light guide plate may have a plurality of lens-shaped and / or prism-shaped convex portions. The convex portion is preferably provided on at least one side of the light guide plate, and in particular, is provided on the side that serves as the front surface (light-emitting surface) of the light guide plate. It may also be provided on other surfaces if necessary, but it is more preferably provided only on the front surface (light-emitting surface) of the light guide plate.
[0085] Here, the so-called lens-shaped convex portion is an arc-shaped convex portion, and the edge shape of the cross section is an arc-shaped convex strip. In addition, the so-called prism shape is an arc-shaped convex portion, and the edge shape of the cross section is a triangular mountain-shaped convex strip. In addition, the convex portion can be formed into a plurality of convex portions and be parallel to each other. In addition, the convex portion can be formed integrally with the light guide plate.
[0086] The thickness of the light guide plate is 0.2 to 3.0 mm, preferably 0.3 to 2.5 mm, and more preferably 0.4 to 2.4 mm. Within this range, a light guide plate having excellent moldability such as excellent extrusion stability and excellent strength can be easily produced in molding the optical styrene resin composition.
[0087] <Optical Characteristics>
[0088] The average transmittance of the light guide plate at a wavelength of 380 to 780 nm at an optical path length of 115 mm is preferably 85% or more, more preferably 86% or more.
[0089] The YI (Yellowness Index) value of the light guide plate at an optical path length of 115 mm is preferably 6.0 or less, and more preferably 4.0 or less.
[0090] <Method for Manufacturing Light Guide Plate>
[0091] The light guide plate of one embodiment of the present invention is obtained by molding the above-mentioned optical styrene resin composition. As a molding method, known methods such as sheet extrusion molding, injection molding, and compression molding can be used. From the perspective of productivity and easy large-scale molding, continuous sheet extrusion molding with a surface shape transfer mold is preferred. As an example of the sheet extrusion molding, a continuous sheet extrusion molding method can be cited, which has: an extrusion step, in which the resin is supplied to a feed block in a heated and molten state, and is continuously extruded from the mold to form a sheet; a pressing step, in which the above-mentioned resin sheet is clamped by a crimping roller and a cooling roller; and a conveying step, in which, after the pressing step, the resin sheet is conveyed while being in close contact with the cooling roller; and a transfer mold is provided on the surface of the cooling roller; by changing the shape of the transfer mold, any concave and convex shape can be transferred to the sheet surface.
[0092] In addition, the light guide plate may have a concavo-convex shape on the front surface (light-emitting surface), and a reflective process for diffusely reflecting light may be applied to the back surface. As the reflective process, for example, in addition to screen printing or inkjet printing, a method of imparting a dot-shaped concavo-convex shape by laser irradiation can be cited, and the printing of the dot pattern can use ink having microparticles that diffuse light.
[0093] 3. Edge light type surface light source unit
[0094] An edge-lit surface light source unit according to an embodiment of the present invention includes the above-mentioned light guide plate and a light source for supplying LED light to an end surface of the light guide plate. The edge-lit surface light source unit can be suitably used as a surface light source device for a liquid crystal display device.
[0095] 4. Light diffusion plate
[0096] The light diffuser plate according to one embodiment of the present invention is a molded product obtained by molding the optical styrene resin composition. The light diffuser plate is a light diffuser plate that can be used in a direct-type surface light source unit.
[0097] <Shape of light diffusion plate>
[0098] The thickness of the light diffuser plate of one embodiment of the present invention is not limited, and is, for example, 1 to 3 mm. An antistatic agent may also be coated on the surface of the light diffuser plate. By coating the antistatic agent, after the light diffuser plate is mounted on the backlight device, the adhesion of dust and the like caused by static electricity can be suppressed, so that the brightness can be used for a long time without decreasing. In addition, the light diffuser plate of the present invention may be formed with micro-concave and convex shapes such as embossing on both sides or one side, and may also be formed with lens shapes or prism shapes on both sides or one side.
[0099] In the light diffusion plate, 0.1 to 1.0 parts by weight of a light diffusing agent may be included relative to 100 parts by weight of the optical styrene resin composition. The light diffusing agent can be used as long as it is a particle having a different refractive index from the optical styrene resin composition and having the effect of diffusing incident light. For example, organic particles such as styrene polymer particles, acrylic polymer particles, and silicone polymer particles, or inorganic particles such as glass beads, silica particles, aluminum hydroxide particles, calcium carbonate particles, barium sulfate particles, titanium oxide particles, and talc can be used. Among them, at least one selected from acrylic polymer particles, styrene polymer particles, and silicone polymer particles is preferred.
[0100] <Method for Manufacturing Light Diffuser Plate>
[0101] The light diffusion plate of one embodiment of the present invention can be manufactured by molding the above-mentioned optical styrene resin composition by various methods such as extrusion molding and injection molding, preferably manufactured by extrusion molding. As an example of extrusion molding, the following method can be cited: the optical styrene resin composition is melt-kneaded using a single-axis extruder or a double-axis extruder, and after continuous extrusion from a T-die, it is cooled and solidified by a cooling roller unit. In the case where a concavo-convex shape is formed on the surface of the light diffusion plate, an arbitrary concavo-convex shape can be formed by providing a transfer mold on the surface of the cooling roller and changing the shape of the transfer mold. In addition, when the surface layer is laminated on both sides or one side of the light diffusion plate, methods such as co-extrusion, attachment, heat bonding, solvent bonding, casting, and surface coating can be used.
[0102] 5. Direct-down type surface light source unit
[0103] A direct-type surface light source unit according to one embodiment of the present invention includes the light diffusion plate and a light source for supplying LED light to the light diffusion plate. The direct-type surface light source unit can be suitably used as a surface light source device for a liquid crystal display device.
[0104] [Example]
[0105] Hereinafter, the present invention will be described in further detail by giving examples. However, these are merely illustrative and do not limit the content of the present invention.
[0106] 1. Production of optical styrene resin composition
[0107] [Example 1]
[0108] The first reactor as a complete mixing type stirring tank and the second reactor as a plug flow type reactor with a static mixer are connected in series to form a polymerization step to implement the production of styrene resin. The capacity of each reactor is: 30 liters for the first reactor and 12 liters for the second reactor. With respect to the raw material composition of 51% by mass of styrene (TBC concentration 11μg / g), 39% by mass of methyl methacrylate (TBX concentration 7μg / g), and 10% by mass of ethylbenzene, at the inlet of the first reactor, the addition concentration of tert-butyl peroxyisopropyl monocarbonate (manufactured by NOF Corporation: PERBUTYL I) as a polymerization initiator is adjusted to 150ppm, and the addition concentration of n-dodecyl mercaptan (manufactured by Arkema Co., Ltd.) as a chain transfer agent is adjusted to 500ppm (both are concentrations based on the mass of the entire monomer), and then the raw material solution is continuously supplied to the first reactor set at 128°C at 8.0kg / h. Furthermore, the obtained polymerization solution is continuously supplied to the second reactor to terminate the polymerization. The polymerization rate of the monomer at this time is 70%. Furthermore, in the second reactor, a temperature gradient was set along the flow direction and adjusted to 130°C in the middle portion and 145°C in the outlet portion.
[0109] Then, the solution containing the polymer continuously taken out from the second reactor was introduced into a vacuum de-volatilization tank with a preheater composed of two stages in series, and the temperature of the preheater was adjusted so that the resin temperature became 220°C, and the unreacted styrene and ethylbenzene were separated under a pressure of 0.8 kPa. The obtained molten polymer was continuously supplied to the extruder, and 0.1 parts by mass of a hindered amine light stabilizer (770) was added from the feed port of the additive relative to 100 parts by mass of the polymer. After mixing at a set temperature of 220°C, it was extruded from a porous die in a linear form, and the linear material was cooled and cut by cold cutting to pelletize it. The TBC concentration in the obtained optical styrene resin composition was 1.5 μg / g, and the TBX concentration was 0.2 μg / g. In addition, the weight average molecular weight (Mw) was 170,000, and the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) was 2.0.
[0110] [Examples 2 to 17 and Comparative Examples 1 to 6]
[0111] The composition of the raw material solution and the polymerization conditions were changed as shown in Table 1, and the compositions of the hindered amine light stabilizer (B), the phosphorus antioxidant (C-1), the phenolic antioxidant (C-2), and the ultraviolet absorber (D) were changed as shown in Table 2 (Table 2-1 and Table 2-2) to Table 3. An optical styrene resin composition and a light guide plate were produced in the same manner as in Example 1. Various measurement and evaluation results are shown in Table 2 (Table 2-1 and Table 2-2) to Table 3.
[0112] [Table 1]
[0113]
[0114] *1 Concentration based on mass of the total monomers. Polymerization initiator: tert-butyl peroxy isopropyl monocarbonate. Chain transfer agent: n-dodecyl mercaptan.
[0115] *2EXT: Extruder
[0116] [Table 2-1]
[0117]
[0118] [Table 2-2]
[0119]
[0120] [Table 3]
[0121]
[0122] The hindered amine light stabilizer (B), phosphorus antioxidant (C-1), phenolic antioxidant (C-2), and ultraviolet absorber (D) in Table 2 (Table 2-1 and Table 2-2) to Table 3 are as follows.
[0123] (Hindered amine light stabilizer (B))
[0124] 770: Bis(2,2,6,6-tetramethylpiperidin-4-yl) sebacate (TINUVIN770DF manufactured by BASF)
[0125] 944: Polycondensation product of 2,4-dichloro-6-(1,1,3,3-tetramethylbutylamino) and 1,3,5-triazine·N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)hexamethylenediamine (Chimassorb 944FDL manufactured by BASF)
[0126] 292: A mixture of 25% methyl (1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate and 75% bis (1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate (TINUVIN 292 manufactured by BASF)
[0127] 123: Bis(1-octyloxy-2,2,6,6-tetramethylpiperidinyl) sebacate (TINUVIN 123 manufactured by BASF)
[0128] (Phosphorus antioxidant (C-1))
[0129] 168: Tris(2,4-di-tert-butylphenyl)phosphite (Irgafos 168 manufactured by BASF)
[0130] HP-10: 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphine (ADKSTAB HP-10 manufactured by ADEKA Corporation)
[0131] 126: Bis-(2,4-di-tert-butylphenyl) pentaerythritol diphosphite (Irgafos 126 manufactured by BASF)
[0132] (Phenol antioxidant (C-2))
[0133] 1076: Octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (Irganox 1076 manufactured by BASF)
[0134] (Ultraviolet light absorber (D))
[0135] P: 2-(2-hydroxy-5-methylphenyl)benzotriazole (TINUVIN P manufactured by BASF)
[0136] 2. Evaluation
[0137] The evaluation of the optical styrene-based resin compositions described in Tables 2 (Table 2-1 and Table 2-2) to 3 was performed according to the following method.
[0138] <Melt mass flow rate (MFR)>
[0139] The melt mass flow rate was measured in accordance with JIS K 7210 under the conditions of a temperature of 200° C. and a load of 49 N.
[0140] <Vickers softening temperature>
[0141] The Vickers softening temperature was measured at a heating rate of 50° C. / hr and a test load of 50N in accordance with JIS K 7206.
[0142] <Contents of TBC and TBX in the Optical Styrene Resin Composition>
[0143] After dissolving 0.2 g of the optical styrene resin composition in a small amount of THF, 200 μL of BSTFA (M, O-bis(trimethylsilyl)trifluoroacetamide) was added to perform trimethylsilyl derivatization, and the volume was fixed to 10 mL with THF (tetrahydrofuran). The supernatant separated by centrifugation was measured by gas chromatography mass spectrometry (GC / MS) under the following conditions. The concentration was determined using a calibration curve prepared in advance.
[0144] GC device: 7890A manufactured by Agilent
[0145] Chromatographic column: DB-5ms (0.25 mm i.d. × 30 m) manufactured by Agilent, liquid phase film thickness 0.25 μm
[0146] Column temperature: 50℃ (1min) → (20℃ / min heating) → 320℃ (6.5min) for a total of 20min
[0147] Injection port: 300℃, 1.5mL / min, (split ratio 1:5)
[0148] Injection volume: 1μL
[0149] MS device: 5975C manufactured by Agilent
[0150] Interface temperature: 320℃
[0151] MS detection conditions: SIM determination of TBC (m / z 295 for quantification, m / z 310 for confirmation)
[0152] <Contents of Hindered Amine Light Stabilizer (B), Phosphorus Antioxidant (C-1), and Phenolic Antioxidant (C-2) in the Optical Styrene Resin Composition>
[0153] After 1.0 g of the optical styrene resin composition was completely dissolved in 20 mL of THF, 5 mL of methanol was added dropwise and stirred for 20 minutes. Centrifugation was performed at 4000 rpm for 10 minutes, and the separated supernatant was measured by gas chromatography (GC) under the following conditions. In addition, the concentration was determined using a pre-made calibration curve.
[0154] GC device: GC2010 Plus manufactured by Shimadzu Corporation
[0155] Chromatographic column: DB-1 (30m×0.25mmi.d., df=0.10μm)
[0156] Column temperature: 240℃(1min)→(10℃ / min heating)→320℃(15min)
[0157] Injection port: 320℃, 1.02mL / min (split ratio 1:5)
[0158] Injection volume: 1μL
[0159] <Weight average molecular weight (Mw)>
[0160] The weight average molecular weight (Mw), the Z average molecular weight (Mz), and the number average molecular weight (Mn) were measured using gel permeation chromatography (GPC) under the following conditions.
[0161] GPC model: Shodex GPC-101 manufactured by Showa Denko Co., Ltd.
[0162] Chromatographic column: PLgel 10μm MIXED-B manufactured by Polymer Laboratories
[0163] Mobile phase: tetrahydrofuran
[0164] Sample concentration: 0.2 mass%
[0165] Temperature: oven 40°C, injection port 35°C, detector 35°C
[0166] Detector: Differential refractometer
[0167] The molecular weight was calculated as a molecular weight in terms of polystyrene by calculating the molecular weight at each dissolution time based on the dissolution curve of monodisperse polystyrene.
[0168] 3. Manufacturing and evaluation of light guide plates
[0169] <Manufacturing of Light Guide Plate>
[0170] The above-mentioned optical styrene resin composition is supplied to a single-shaft extruder with a screw diameter of 90 mm and L / D=32 and a vent hole. After melt kneading at 200-235°C, it is discharged at a T-die temperature of 245-250°C using a lip width of 1000 mm and a lip opening of 3.0 mm. After being cooled and solidified using a vertical three-roll cooling roll, the end face is trimmed to obtain a light guide plate with a width of 800 mm and a thickness of 2.0 mm.
[0171] <Evaluation of Light Guide Plate>
[0172] The average transmittance, YI value, dimensional stability (moisture absorption deformation), and LED durability of the light guide plates in Tables 2 and 3 were evaluated as follows.
[0173] <Average Transmittance and YI Value of the Light Guide Plate>
[0174] The average transmittance and YI value are measured through the following steps.
[0175] Cut a test piece of 115 mm × 85 mm from the light guide plate obtained above, grind the end face by polishing to make a plate-shaped molded product with a mirror surface on the end face. For the ground plate-shaped molded product, use the ultraviolet-visible spectrophotometer V-670 manufactured by JASCO Corporation to measure the spectral transmittance at wavelengths from 350 nm to 800 nm with a light path length of 115 mm under incident light of size 20 × 1.6 mm and a diffusion angle of 0°, and calculate the YI value at a viewing angle of 2° in the C light source according to JIS K7105. The average transmittance (total light transmittance) is calculated in the form of the average of the spectral transmittances at wavelengths from 380 to 780 nm.
[0176] <Dimensional Stability (Moisture Absorption Deformation)>
[0177] Cut a test piece of 200 mm × 300 mm from the light guide plate obtained above, store the test piece under the conditions of a temperature of 60 °C and a relative humidity of 90% for 500 hours, measure the dimensional change of the long side before and after storage, and calculate the deformation rate according to the following formula.
[0178] Deformation rate = ((Length of the long side after storage) - (Length of the long side before storage)) ÷ (Length of the long side before storage) × 100 (%)
[0179] Record those with a change rate lower than 0.10% as 〇, those with a change rate of 0.10 - 0.15% as △, and those with a change rate exceeding 0.15% as ×, and evaluate the dimensional stability (moisture absorption change) of the light guide plate.
[0180] <LED Durability>
[0181] Cut a test piece of 115 mm × 85 mm from the light guide plate obtained above, use an end face grinding machine (GCPB-500 manufactured by Mikaro Technology Co., Ltd.), and grind the end face with a diamond knife rotating at a speed of 8000 rpm at a feed rate of 2.0 m / min by 0.2 mm to make a plate-shaped molded product with a mirror surface on the end face. For the ground plate-shaped molded product, configure a flat-panel blue LED light source for TV (television) (peak wavelength 445 nm) at a position 0.5 mm from the end face, and under the environment of 80 °C and 0.05 W / mm 2The LED light was irradiated for 500 hours at an input current of . For the plate-like molded products after the test, the UV-visible spectrophotometer V-670 manufactured by JASCO Corporation was used to measure the spectral transmittance of wavelengths of 350nm to 800nm at an optical path length of 115mm under incident light of size 20×1.6mm and a diffusion angle of 0°, and the YI value at a field of view of 2° in the C light source was calculated according to JISK7105. The value obtained by subtracting the YI value before the test from the YI value after the test is set to ΔYI. In addition, the LED light incident part of the plate-like molded product after the test was visually confirmed, and the one with no change was recorded as 0, and the one with carbonization was recorded as × to evaluate the LED durability.
[0182] In Examples 1 to 17, the transparency, hue, and dimensional stability were good, no carbonization occurred after LED exposure, and the hue stability was excellent.
Claims
1. An optical styrene resin composition comprising a styrene resin (A) which is a copolymer containing a styrene monomer unit and a (meth)acrylate monomer unit, and a hindered amine light stabilizer (B), The copolymer contains 95 to 20% by mass of the styrene monomer unit and 5 to 80% by mass of the (meth)acrylate monomer unit in 100% by mass of the copolymer. The optical styrene resin composition contains 0.001 to 1.0 parts by mass of the hindered amine light stabilizer (B) based on 100 parts by mass of the styrene resin (A).
2. The optical styrene resin composition according to claim 1, wherein The hindered amine light stabilizer (B) is an NH type hindered amine light stabilizer and / or an NR type hindered amine light stabilizer.
3. The optical styrene resin composition according to claim 2, wherein The NH type hindered amine light stabilizer is selected from Sebacate bis(2,2,6,6-tetramethylpiperidin-4-yl) ester, Hexadecanoic acid 2,2,6,6-tetramethyl-4-piperidinyl ester, octadecanoic acid 2,2,6,6-tetramethyl-4-piperidinyl ester, 1,2,3,4-Butanetetracarboxylic acid tetrakis (2,2,6,6-tetramethyl-4-piperidinyl) ester, N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 4-morpholinyl 2,6-dichloro-1,3,5-triazine, polycondensate, Condensation product of 2,4-dichloro-6-(1,1,3,3-tetramethylbutylamino) and 1,3,5-triazine·N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)hexamethylenediamine, N,N'-bis(2,2,6,6-tetramethylpiperidin-4-yl)hexamethylenediamine and 2,4,6-trichloro-1,3,5-triazine and N-butyl-1-butylamine and N-butyl-2,2,6,6-tetramethyl-4-piperidinamine, polycondensate, 1,6,11-Tris[2,4-bis(N-butyl-N-(2,2,6,6-tetramethyl-4-piperidinyl)amino)symmetrical triazine-6-yl]aminoundecane, Polycondensation of 1,2,3,4-butanetetracarboxylic acid with 2,2,6,6-tetramethyl-4-piperidinol and β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol At least one of the following.
4. The optical styrene resin composition according to claim 2 or 3, wherein The NR type hindered amine light stabilizer is selected from Methyl sebacate (1,2,2,6,6-pentamethylpiperidin-4-yl) ester, Sebacate bis(1,2,2,6,6-pentamethylpiperidin-4-yl) ester, n-Butyl 3,5-di-tert-butyl 4-hydroxybenzylmalonate bis(1,2,2,6,6-pentamethylpiperidin-4-yl) ester, polycondensate of 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinylethanol and dimethyl succinate, 1,5,8,12-Tetrakis[4,6-bis(N-butyl-N-(1,2,2,6,6-pentamethyl-4-piperidinyl)amino)-1,3,5-triazine-2-yl]-1,5,8,12-tetraazadodecane, 1,2,3,4-Butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, β,β,β',β'-tetramethyl-2,4,8,10-tetraoxaspiro[5,5]undecane-3,9-diethanol, polycondensate, A mixture of succinic acid, polycondensate with (4-hydroxy-2,2,6,6-tetramethylpiperidin-1-yl)ethanol and N,N',N",N"'-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine-2-yl)-4,7-diazadecane-1,10-diamine At least one of the following. The optical styrene resin composition according to any one of claims 1 to 3, comprising 0.001 to 0.5 parts by mass of a phosphorus antioxidant (C-1) based on 100 parts by mass of the styrene resin (A).
6. The optical styrene resin composition according to claim 5, wherein The phosphorus antioxidant (C-1) is at least one selected from tris(2,4-di-tert-butylphenyl) phosphite, 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphite, bis-(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5,5]undecane, tetrakis(2,4-di-tert-butylphenyl)[1,1-biphenyl]-4,4'-diylbisphosphonite, and bis(2,4-di-tert-butyl-6-methylphenyl)ethyl phosphite. 7 . A light guide plate obtained by molding the optical styrene resin composition according to claim 1 . 8 . An edge-lit surface light source unit comprising the light guide plate according to claim 7 , and a light source for supplying LED light to an end surface of the light guide plate. 9 . A light diffusion plate obtained by molding the optical styrene resin composition according to claim 1 . 10 . A direct-type surface light source unit comprising the light diffusion plate according to claim 9 and a light source for supplying LED light to the light diffusion plate.