Molded pulp product and manufacturing process thereof
Incorporating coarse fibrillated MFC into pulp compositions addresses the challenges of energy-intensive drying and structural weaknesses in molded pulp products, enhancing tensile stiffness and ductility, resulting in lighter, higher-quality three-dimensional objects with improved barrier properties and reduced drying times.
Patent Information
- Application Number
- CN202380034160.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-21
- Filing Date
- 2023-03-20
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing wet and dry moldable pulp forming processes face challenges such as energy-intensive drying, material deformation, and structural weaknesses in forming deep-drawn products, particularly when incorporating cellulose fibers, which affect the quality and efficiency of three-dimensional molded pulp products.
Incorporating coarse fibrillated microfibrillated cellulose (MFC) into pulp compositions enhances mechanical properties, allowing for reduced object weight and improved tensile stiffness without compromising integrity, and facilitates faster drainage and better coating adherence, thereby improving the formation and drying processes.
The addition of coarse fibrillated MFC significantly enhances the tensile stiffness and ductility of molded pulp products, enabling lighter, higher-quality objects with improved barrier properties and reduced drying times, thus increasing productivity and product integrity.
Smart Images

Figure CN119096018A_ABST
Abstract
Description
Technical Field
[0001] Three-dimensional molded packaging articles comprising moldable cellulose pulp and coarse-fibrillated microfibrillated cellulose and optionally inorganic particulate material, processes for their manufacture and uses of such three-dimensional molded pulp articles. Background Art
[0002] Many three-dimensional packaging objects, such as egg cartons, food trays, and cushioning supports for electronics and consumer products, are made by molding cellulose pulp. Moldable pulp products are currently made in a wet pulp molding process or a dry pulp forming process. In one aspect, the wet pulp molding process is similar to papermaking in that it involves filtering a pulp suspension in water, which is then squeezed and dried to make the final product. However, unlike filtering the suspension on a continuously moving flat net in papermaking, in the wet pulp molding process, a three-dimensional net mold is typically immersed in a pulp tank, and a vacuum is applied to the inside of the mold to form a pulp filter cake on its outside to form an object. Wet pulp molding is often used to make complex shapes that cannot be pressed from a flat sheet or cellulose blank, nor can they be easily made by folding a flat sheet or cellulose blank. Since each object requires a separate mold, it is essentially a batch process.
[0003] Packaging inserts are often made from molded pulp. Molded pulp has the advantage of being seen as a sustainable packaging material because it is made from biomaterials and can be recycled after use.
[0004] Wet pulp molded products can be formed by immersing a suction mold in a pulp suspension while applying suction. As a result, the body of the pulp is formed into the shape of the desired article by fiber deposition. The suction mold is then removed from the suspension and suction is usually continued to compact the deposited fibers while the residual liquid is discharged. Different drying techniques can be used, including oven drying, hot pressing, microwave drying and freeze drying. The disadvantage of all wet forming techniques is the need to dry the molded product, which is a time-consuming and energy-consuming step. Through this wet forming technique, the molded product forms strong fiber-to-fiber bonds, which provide strength and rigidity to the molded product.
[0005] Wet forming methods for making cellulose products having a flat or non-flat product shape by pressure molding are also known in the art. One such method is described in EP3736099A1, which is incorporated herein by reference in its entirety. In this reference, a method for making a cellulose product having a flat or non-flat product shape by a pressure molding device including a forming mold is disclosed, the forming mold having a forming surface that defines the shape of the product. The method comprises the following steps: placing a cellulose blank having a moisture content of less than 45% by weight in a forming mold; heating the cellulose blank to a forming temperature in the range of 100°C to 200°C; and pressing the cellulose blank through the forming mold, wherein a forming pressure acts on the cellulose blank across the forming surface, and the forming pressure is in the range of 1MPa to 100MPa.
[0006] An alternative method for making a 3D molded pulp product comprises dry forming a cellulose blank in a forming mold comprising a preheated non-flexible negative pressure mold part and a preheated non-flexible positive pressure forming mold part, then heating the cellulose blank to a forming temperature, typically in the range of 100° C. to 200° C., and pressing the cellulose blank in the forming mold at a forming pressure of at least 1 MPa. An example of such a method can be found in EP 3882167A1, which is incorporated herein by reference in its entirety.
[0007] A system for producing cellulose products by shaping cellulose fibers without using wet forming technology is also disclosed in WO2021156222, which is incorporated herein by reference in its entirety. Wherein, an air-formed cellulose blank structure is inserted into a forming die. During the forming process of the cellulose product, the cellulose blank is subjected to high forming pressure and high forming temperature. The problem with this forming method is that when the cellulose blank structure is inserted into the forming die, there is a risk that the cellulose blank structure may break and cause the cellulose product to deform. It should be noted that this is a common problem with traditional cellulose high-pressure forming dies, especially for deep-drawn products, which can result in low product quality. Other problems with traditional forming dies are that, especially when forming deep-drawn products, cracks, fiber separation, material breakage or other undesirable structural weakening of the cellulose blank structure may be formed during the insertion of the forming die.
[0008] WO2021156222 discloses a forming die system for forming a cellulose product from an air-formed cellulose blank structure, and a method for forming a cellulose product from an air-formed cellulose blank structure in a forming die system, wherein the aforementioned problems are allegedly avoided. This solution to the problems of cracks, fiber separation, and material weakening and separation is allegedly at least partially achieved by a forming die system for forming a cellulose product from an air-formed cellulose blank structure, wherein the forming die system comprises a first die component and a second die component, wherein the first die component and the second die component are configured to move relative to each other in a pressing direction, wherein the second die component comprises a forming cavity portion and an inlet portion, wherein the inlet portion is arranged to be connected to the forming cavity portion and is configured to facilitate displacement of the cellulose blank structure into a forming cavity of the forming cavity portion, wherein the inlet portion comprises a transition surface defining an inlet opening, wherein the inlet opening has a tapered configuration toward the forming cavity.
[0009] WO2021037946 discloses an alternative method of forming a cellulose product from an air-formed cellulose blank structure in a rotary forming die system, which document is incorporated herein by reference in its entirety. In the aforementioned system, the dry basis weight of the air-formed cellulose blank structure ranges from 200 to 3000 g / m 2 , preferably 300-3000g / m 2 , and more preferably 400-3000g / m 2 The air-formed cellulose blank structure having these properties is considered suitable for the formation of three-dimensional cellulose products. The cellulose blank structure is described as a relatively thick and fluffy structure compared to conventional wet laid laid paper or tissue paper structures. The loose cellulose blank structure is compacted during the forming process, and the cellulose fibers in the three-dimensional cellulose product are firmly bonded to each other by hydrogen bonds, thereby providing a hard compacted three-dimensional product structure.
[0010] WO2021001276 discloses a similar method in which an air-formed cellulose blank structure is formed from cellulose fibers, and the document is incorporated herein by reference in its entirety, wherein an alkyl ketene dimer (AKD) dispersion is applied to the cellulose blank structure, and in a second coating step after the first coating step, a latex dispersion is applied to the cellulose blank structure together with the coated alkyl ketene dimer (AKD) dispersion; then, the cellulose blank structure coated with the alkyl ketene dimer (AKD) dispersion and the latex dispersion is introduced into a forming mold and heated to a forming temperature in the range of 100°C to 300°C, and a cellulose product is formed by pressing the heated cellulose blank structure at a forming pressure of at least 1 MPa, preferably 4-20 MPa.
[0011] WO2020229608 discloses another method for producing discrete three-dimensional cellulose products from an air-formed cellulose blank structure in a rotary forming die system, which is incorporated herein by reference in its entirety. The rotary forming die system provides an air-formed cellulose blank structure that is conveyed and fed to a position between a first die part and a second die part, and is heated to a forming temperature in the range of 100°C to 300°C; and thereafter, the heated air-formed cellulose blank structure is pressed between the first die part and the second die part at a forming pressure of at least 1 MPa, preferably 4-20 MPa, to form a three-dimensional cellulose, wherein during forming, the first die part rotates around a first rotation axis, and the second die part rotates around a second rotation axis.
[0012] Both the aforementioned wet and dry moldable pulp forming processes utilize cellulose fibers, but do not mention the inclusion of microfibrillated cellulose as an additive.
[0013] In the context of the aforementioned process, microfibrillated cellulose (MFC) or so-called cellulose microfibrils (CMF) are defined as micrometer-sized cellulose particle fibers or fibrils, at least one of whose average dimensions is less than 1000 nm. MFC comprises partially or fully fibrillated cellulose or lignocellulosic fibers. The cellulose fibers are preferably fibrillated to such an extent that the final specific surface area of the formed MFC is from about 1 to about 500 m2, when determined by the BET method on solvent exchanged and freeze-dried material. 2 / g, such as 10 to 400 m 2 / g, or more preferably 50 to 300 m 2 / g. An advantage of comprising microfibrillated cellulose and a metal salt is said to be that the combination of the metal salt and microfibrillation is said to enhance printing properties, ie the combination of MFC and the metal salt is believed to make the surface of the molded object more receptive to printing inks.
[0014] An overview of the wet forming process of moldable pulp products can be found in Didone, Mattia et al., "Moulded Pulp Manufacturing: Overview and Prospects for the Process Technology, Packaging Technology and Science 92017): 30: 231-249 (2017), which is incorporated herein by reference in its entirety.
[0015] The production of 3D molded articles solely from cellulose nanofibers is described in Rol, Fleur et al., "Production of 100% Cellulose Nanofibril Objects Using the Molded Cellulose Process: A Feasibility Study," Ind. Eng. Chem. Res. (2020), 59, 16, 7670-7679, which is incorporated herein by reference in its entirety.
[0016] In the aforementioned study, the authors reported the preparation of 100% CNF 3D molded objects. Cellulose fibers were hydrolyzed using enzymatic hydrolysis (using 300 ECU / g cellulase Fiber Care from Novozymes) TM ), CNF was produced by the twin-screw refining process described. Two types of CNF were used in this work: (i) a commercial CNF grade produced at 2 wt% solids by enzyme pretreatment and using a homogenizer, and (ii) a high solids content CNF (20 wt% solids content) produced by enzymatic hydrolysis of cellulose fibers and twin-screw extrusion. The two CNF suspensions were then characterized using several techniques. The CNF suspension was diluted and then filtered through a standard sheet former (Fast Klothen former, ISO 5269-2 standard) to form a 60 g / m 2 Nanopaper. The molded nanostructured objects were produced following different steps: (i) forming a cellulose mat by filtration or extrusion, and (ii) drying. Different drying techniques were used, including oven drying, hot pressing, microwave drying and freeze drying. The authors note that after optimizing the mold porosity, different methods were tried to form the nanocellulose mat. Because the amount of bound water in CNF is much higher than that in the cellulose fiber suspension, the maximum dry content reached after pressing is only 30 wt%. The nanocellulose mat was formed by pressing at 4 tons for 1 minute, and this was possible because of the high solid content of CNF. In fact, due to its gel-like behavior, several hours were required to filter 2 wt% of classical CNF until this solid content was reached. The authors concluded that none of the drying methods could produce 3D transparent objects due to shrinkage and failure, especially in the area between the flat and curved areas of the mold. 2D objects were produced using a combination of drying methods and are said to present interesting properties such as grease barrier properties and good mechanical properties.
[0017] Molded pulp has traditionally been associated with objects where appearance and surface properties are not important.
[0018] With the recent renewed interest in replacing conventional plastics with bio-sourced, recyclable and biodegradable materials, the molded pulp industry is experiencing significant growth and development. Molded pulp objects can be made with high surface quality and stiffness, so they are beginning to be used for primary packaging of higher value goods, such as electronics and cosmetics.
[0019] For most applications (about 85%), recycled fibers are used.
[0020] Mineral fillers are not usually used, but molded pulp products may contain significant amounts of ash from the recycled pulp used.
[0021] Although wet pulp molded objects are formed on a wire mesh mold immersed in a pulp suspension, variations in the subsequent pressing and drying processes have led the International Molding Fiber Association (IMFA) to classify them into four major categories.
[0022] "Thick Wall": Made using an open mold and then oven dried. Typical wall thickness ranges from 5mm to 10mm. The side in contact with the mold is relatively smooth, while the other side is rough. The raw material is usually kraft paper mixed with recycled paper. Thick wall parts are often used as support packaging for non-fragile, heavy items such as furniture and vehicle parts.
[0023] "Transfer molded" products in this category have thinner walls, about 3mm to 5mm. They are manufactured using a forming die and a transfer or demoulding die. The result is a product with relatively smooth surfaces on both sides and greater dimensional accuracy. The wet product is ejected from the transfer mold and dried in a heated oven. A common raw material is recycled newspaper. Typical examples are egg trays and packaging for electronic devices.
[0024] "Thermoforming" ("thin-wall") is the most recent method. The initially formed product is collected in a heated mould where it is pressed, densified and dried. No oven curing is required. This process produces high-quality thin-walled articles (from 2 to 4 mm) with good dimensional accuracy and a smooth, rigid surface. The result is similar to the appearance of thermoformed plastic articles.
[0025] "Processed" refers to molded pulp products that require some further or special treatment, such as additional printing, coatings or additives.
[0026] Recycled fibers are used for most applications, but virgin fibers are sometimes available for higher quality thermoforming. Refining of pulp is not common, but is possible with some manufacturers. There is a growing interest in enhanced properties, such as oil, grease or moisture resistance for food packaging, or improving the feel and appearance of consumer products.
[0027] Molded pulp products are not classified by basis weight (g / m 2or GSM) definition and sales; only the performance of concern is important.
[0028] The use of increased contents of microfibrillated cellulose (MFC) increases the time required to form the object and establish a constant basis weight when the mold is immersed in the pulp tank (forming or molding time). However, the use of MFC brings enhanced performance, which makes it possible to reduce the necessary basis weight of the product very significantly for a given application. The reduction in basis weight can compensate for the reduction in drainage rate, so that the forming time is not increased to an unacceptable extent. Any increase in forming time can also be compensated by the reduction in drying time and energy consumption caused by the reduction in product weight. In fact, if the rate-determining step of the process is drying rather than forming, the reduction in basis weight achieved by using MFC can even contribute to an increase in productivity.
[0029] Therefore, there is a need for a moldable pulp composition having enhanced properties due to the incorporation of coarse fibrillated MFC in the moldable pulp composition imparting better mechanical properties to the molded article. Summary of the invention
[0030] The addition of coarsely fibrillated MFC to compositions for wet or dry molding of pulp allows the weight of formed objects to be greatly reduced without compromising their quality or integrity. In particular, the tensile stiffness of moldable pulp products can be greatly improved, allowing lighter objects to be manufactured with the same stiffness. As a first approximation, the stiffness of simple three-dimensional molded objects (such as pallets) depends on the tensile stiffness of their walls. The tensile stiffness of a sheet is defined as the force per unit width required to stretch the sheet per unit strain. The tensile stiffness index of a sheet is defined as the tensile stiffness divided by the mass of the material per unit area (g / m 2 Adding coarse fibrillated MFC to a pulp composition increases its tensile stiffness index, making it possible to produce sheets with the same tensile stiffness at a lower gsm.
[0031] Likewise, by adding coarse fibrillated MFC to the composition, molded objects of equal rigidity can be made at lower weights. Adding coarse fibrillated MFC to a moldable pulp composition also makes the wet-laid pulp more ductile so that, surprisingly, it can be molded in thinner layers around corners without tearing. While the use of coarse fibrillated MFC will reduce the rate of formation of the object in the mold, this is generally not the rate determining step and can be offset by the reduction in weight required. Another advantage of adding coarse fibrillated MFC to a composition comprising pulp for molding is that the Bendtsen porosity it causes in the dry molded article will be greatly reduced, which will improve the integrity of any barrier coating subsequently sprayed onto the molded object.
[0032] At high levels, the use of coarse fibrillated MFC can produce excellent oil and grease resistance even without a coating. By adding about 0.5% by weight to about 50% by weight of coarse fibrillated microfibrillated cellulose based on the total dry weight of the pulp composition to a pulp composition to be wet or dry molded, the above-mentioned problems in the field of wet or dry molding cellulose fibers to produce three-dimensional molded pulp products are overcome. As measured by a fiber image analyzer, such coarse fibrillated microfibrillated cellulose includes less than about 90% by weight of fine particles and / or less than 75% fine particles A, and has a length-weighted median length Lc (w) greater than 0.3 mm. Coarse fibrillated microfibrillated cellulose is introduced into a pulp composition to be wet or dry molded. The inventors were surprised to find that coarse fibrillated MFC also drains faster and therefore provides better overall performance than more finely fibrillated MFC forms. Coarse fibrillated MFC materials provide a better compromise between strength and drainage compared to more fibrillated MFC forms. Drainage has been significantly improved, but tensile stiffness has also increased. Figure 2 , which shows the calculated grammage required for 1000 N / m tensile stiffness for each blend, plotted against that grammage and the calculated drainage time for the blend. For blends up to 50% MFC, the coarser material achieves any given grammage reduction at lower MFC content and significantly shorter drainage times.
[0033] According to the description, drawings, embodiments and claims of this specification, the inventors have invented a method for manufacturing a three-dimensional molded object sheet, which comprises cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials (or is mainly composed of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials, or is composed of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials), and the sheet has improved mechanical properties, and invented a three-dimensional molded object manufactured by such a method and the use of such a three-dimensional molded object as a packaging container, blister packaging, egg box, bottle, container or food tray. The three-dimensional molded object comprises about 0.5 wt. % to about 50 wt. % coarse fibrillated microfibrillated cellulose on a dry weight basis of the total dry mass of a mixture of cellulose fibers and microfibrillated cellulose and optionally one or more inorganic particulate materials; wherein the coarse microfibrillated cellulose comprises less than about 90 wt. % fines and / or less than 75 % fines A as measured by a fiber image analyzer and has a length-weighted median length Lc(w) greater than 0.3 mm, and wherein the coarse fibrillated microfibrillated cellulose optionally has a fiber steepness of about 20 to about 50 as measured by a Malvern Mastersizer. In a first aspect of the invention, the inventors have invented a three-dimensional molded object comprising a mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials, wherein the coarse microfibrillated cellulose comprises less than about 90 wt. % fines and / or less than 75 % fines A as measured by a fiber image analyzer and has a length-weighted median length Lc(w) greater than 0.3 mm, and wherein the coarse fibrillated microfibrillated cellulose optionally has a fiber steepness of about 20 to about 50 as measured by a Malvern Mastersizer.
[0034] In an embodiment of the first aspect of the present invention, the fiber steepness of the coarse fibrillated microfibrillated cellulose is from about 20 to about 50.
[0035] In a further embodiment of the first aspect of the invention, the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt % to about 50 wt %, or 0.5 wt % to about 25 wt %, or about 0.5 wt % to about 20 wt %, or about 0.5 wt % to about 15 wt %, or about 0.5 wt % to about 10 wt %, or about 0.5 wt % to about 5 wt %.
[0036] In an additional embodiment of the first aspect of the invention the coarse fibrillated microfibrillated cellulose is obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
[0037] In other embodiments of the first aspect of the present invention, the coarse fibrillated microfibrillated cellulose is obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
[0038] In other embodiments of the first aspect of the present invention, the cellulosic fibers are obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills, and combinations thereof.
[0039] In a further embodiment of the first aspect of the invention the cellulosic fibres are obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
[0040] In a further embodiment of the first aspect of the present invention both cellulose fibres and coarse-fibrillated microfibrillated cellulose are obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
[0041] In additional embodiments of the first aspect of the invention, the molded object comprises one or more inorganic particulate materials.
[0042] In a further embodiment of the first aspect of the present invention, the one or more inorganic particulate materials are calcium carbonate or kaolin or a mixture thereof, or comprise platy minerals, kaolin and / or talc.
[0043] In an embodiment of the first aspect of the present invention, the calcium carbonate is ground calcium carbonate, precipitated calcium carbonate or a mixture thereof, or the calcium carbonate is precipitated calcium carbonate.
[0044] In a further embodiment of the first aspect of the present invention, the calcium carbonate is ground calcium carbonate, or the ground calcium carbonate is marble, chalk, limestone and mixtures thereof.
[0045] In other embodiments of the first aspect of the present invention, the inorganic particulate material is ground calcium carbonate and precipitated calcium carbonate.
[0046] In additional embodiments of the first aspect of the invention, the inorganic particulate material is selected from the group consisting of alkaline earth metal carbonates or sulfates, calcium carbonate, magnesium carbonate, dolomite, gypsum, bentonite, hydrous kandite clay, kaolin, halloysite, ball clay, anhydrous (calcined) kandite clay, metakaolin, fully calcined kaolin, talc, mica, perlite, sepiolite, huntite, diatomaceous earth, magnesite, silicates, diatomaceous earth, brucite, aluminum trihydrate, and combinations thereof.
[0047] In a second aspect of the present invention, there is provided a method for producing a three-dimensional molded object comprising cellulose fibers and coarse fibrillated microfibrillated cellulose, comprising the following steps: providing a mixture comprising cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials, wherein the mixture comprises about 0.5 wt.% to about 50 wt.% coarse fibrillated microfibrillated cellulose on a dry weight basis of the total dry mass of the mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; wherein the coarse microfibrillated cellulose comprises less than about 90 wt.% fine particles and / or less than 75% fine particles A as measured by a fiber image analyzer, and its length-weighted median length Lc(w) is greater than 0.3 mm, and wherein the coarse fibrillated microfibrillated cellulose optionally has a fiber steepness of about 20 to about 50 as measured by a Malvern Mastersizer.
[0048] In an embodiment of the second aspect of the invention the coarse fibrillated microfibrillated cellulose has a fibre steepness of about 20 to about 50 as measured by a Malvern Mastersizer.
[0049] In other embodiments of the second aspect of the invention, the forming step is a wet forming step, or the forming step is a dry forming step.
[0050] In a further embodiment of the second aspect of the invention, the method further comprises the steps of: providing a porous mould having a three-dimensional shape, the mould comprising a forming part having an inner part and an outer part; contacting the forming part with a mixture comprising cellulose fibres and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; applying a vacuum to the inner part of the forming part to form a wet layer of cellulose fibres and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials on the outer part of the forming part, thereby forming a three-dimensional moulded object, wherein the fibres The wet layer of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials is about 100 to 3,000 gsm (or 200 to 2,000 gsm, or 250 to 1,000 gsm) on a dry weight basis of the total dry mass of the mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; transferring the molded object to a drying conveyor and drying the three-dimensional molded object; optionally, transferring the three-dimensional molded object to a second reverse forming mold and pressing the three-dimensional molded object before oven drying.
[0051] In embodiments of the invention and of the second aspect, the cellulose fibers are obtained from virgin pulp, recycled paper or old corrugated cardboard or a combination thereof.
[0052] In additional embodiments of the invention and of the second aspect, the cellulose fibers are obtained from virgin pulp, or from recycled pulp, or from old corrugated cardboard.
[0053] In embodiments of the invention and embodiments of the second aspect, the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt % to about 50 wt %, or 0.5 wt % to about 25 wt %, or about 0.5 wt % to about 20 wt %, or about 0.5 wt % to about 15 wt %, or about 0.5 wt % to about 10 wt %, or about 0.5 wt % to about 5 wt %.
[0054] In an embodiment of the invention and of the second aspect, the coarse fibrillated microfibrillated cellulose is obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
[0055] In an embodiment of the invention and of the second aspect, the coarse fibrillated microfibrillated cellulose is obtained from a pulp selected from the group consisting of recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
[0056] In an embodiment of the invention and an embodiment of the second aspect, the cellulose fibers are obtained from recycled pulp, broke pulp, paper mill waste stream, waste from paper mills and combinations thereof, or from a pulp selected from chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste stream, waste from paper mills and combinations thereof.
[0057] In embodiments of the invention and of the second aspect, the molded object comprises one or more inorganic particulate materials.
[0058] In a further embodiment of the second aspect of the invention, the one or more inorganic particulate materials are calcium carbonate or kaolin or a mixture thereof, or the one or more inorganic particulate materials comprise platy minerals, kaolin and / or talc.
[0059] In other embodiments of the second aspect and embodiments thereof, the calcium carbonate is ground calcium carbonate, precipitated calcium carbonate or a mixture thereof; or the calcium carbonate is precipitated calcium carbonate; or the calcium carbonate is ground calcium carbonate.
[0060] In other embodiments of the second aspect and embodiments thereof, the ground calcium carbonate is marble, chalk, limestone and mixtures thereof.
[0061] In further embodiments of the second aspect and embodiments thereof, the inorganic particulate material is ground calcium carbonate and precipitated calcium carbonate.
[0062] In additional embodiments of the second aspect and embodiments thereof, the inorganic particulate material is selected from the group consisting of alkaline earth metal carbonates or sulfates, calcium carbonate, magnesium carbonate, dolomite, gypsum, bentonite, hydrous kandite clay, kaolin, halloysite, ball clay, anhydrous (calcined) kandite clay, metakaolin, fully calcined kaolin, talc, mica, perlite, sepiolite, magnesite, diatomaceous earth, magnesite, silicates, diatomaceous earth, brucite, aluminum trihydrate, and combinations thereof.
[0063] In a third aspect of the invention there is provided a three-dimensional packaging container, blister pack, egg box, bottle, container or food tray comprising the three-dimensional article according to the first aspect.
[0064] In a fourth aspect of the invention there is provided a three-dimensional packaging container, blister pack, egg box, bottle, container or food tray comprising a three-dimensional article produced according to the second aspect.
[0065] In a fifth aspect of the present invention there is provided the use of a three-dimensional article obtained by the process according to the first or second aspect as a blister pack, egg box, bottle, container or food tray. BRIEF DESCRIPTION OF THE DRAWINGS
[0066] For a more complete understanding of the principles and advantages disclosed herein, reference is made to the following description in conjunction with the accompanying drawings, in which:
[0067] Figure 1 is a schematic diagram of the layout of a test molding machine, which depicts the standard sequence of thermoforming to make one product at a time. Commercially available machines are more compact and contain multiple molds that make products simultaneously but use the same basic steps.
[0068] Figure 2 is a graph of the calculated gsm required to achieve a tensile stiffness of 1000 n / m versus the calculated drainage time for different MFC / pulp blends. DETAILED DESCRIPTION
[0069] The titles, subheadings and subheadings provided herein should not be construed as limiting the various aspects of the present disclosure. Therefore, the terms defined below are more fully defined by citing the entire contents of the specification. All references cited herein are incorporated herein by reference in their entirety.
[0070] The foregoing has fairly broadly outlined the features and technical advantages of various aspects of the present invention so that the detailed description of the present invention below can be better understood. Additional features and advantages of the present invention will be described herein, which may form the subject matter of the claims of the present invention. It should be understood by those skilled in the art that any concepts and specific embodiments disclosed herein can be easily used as the basis for modifying or designing other devices for achieving the same purpose of the present invention. It should also be recognized by those skilled in the art that such equivalent devices do not deviate from the spirit and scope of the present invention as set forth in the appended claims. When considered in conjunction with the accompanying drawings, the novel features (including their organization and method of operation) that are considered to be features of the present invention and further objects and advantages will be better understood from the following description. However, it should be clearly understood that any description, drawings, examples, etc. are provided only for the purpose of illustration and description, and are by no means intended to limit the scope of the present invention.
[0071] Unless otherwise defined, scientific and technical terms used herein shall have the meanings commonly understood by those of ordinary skill in the art. In addition, unless otherwise required by context, singular terms shall include pluralities and plural terms shall include the singular.
[0072] When used in conjunction with the term "comprising," the use of the word "a" or "an" may mean "one," but is also consistent with the meaning of "one or more," "at least one," and "one or more than one."
[0073] Use of the term "or" is intended to mean "and / or" unless explicitly stated to refer to alternatives only when the alternatives are mutually exclusive, but the present disclosure supports a definition referring only to the alternatives and "and / or."
[0074] In this application, the term "about" is used to indicate that a value includes the inherent error variation of the quantitative device, the method used to determine the value, or the variation present in the subject of study. For example, but not as a limitation, when the term "about" is used, the specified value can vary plus or minus 12%, or 11%, or 10%, or 9%, or 8%, or 7%, or 6%, or 5%, or 4%, or 3%, or 2%, or 1%.
[0075] The use of the term "at least one" should be understood to include one and any number more than one, including but not limited to 1, 2, 3, 4, 5, 10, 15, 20, 30, 40, 50, 100, etc. The term "at least one" can extend to 100 or 1000 or more, depending on the term to which it is attached. In addition, the number of 100 / 1000 should not be considered restrictive, as lower or higher limits can also produce satisfactory results. In addition, the use of the term "at least one of X, Y, and Z" will be understood to include only X, only Y, and only Z, as well as any combination of X, Y, and Z.
[0076] As used herein, the term "biodegradable" refers to a composition that can be degraded over time by water and / or enzymes found in nature without any harmful effects on the environment. The compositions of the present disclosure exhibit properties that meet the requirements of ASTM D6868-11 "Standard Specification for Labeling of End Items that Incorporate Plastics and Polymers as Coatings or Additives" (ASTM International, West Conshohocken, PA.). Alternatively, the compositions of the present disclosure exhibit properties that meet the requirements of ASTM D6400-04--"Specification for Compostable Plastics" (ASTM International, West Conshohocken, PA.).
[0077] The use of ordinal terms (i.e., "first," "second," "third," "fourth," etc.) is solely for the purpose of distinguishing between two or more items and, unless otherwise stated, is not meant to imply any order or sequence or importance of one item relative to another or any order of addition.
[0078] As used herein, the term "coarse fibrillated microfibrillated cellulose" refers to MFC, wherein the coarse microfibrillated cellulose comprises less than about 90 wt. % fines and / or less than 75 % fines A, as measured by a fiber image analyzer, and its length weighted median length Lc(w) is greater than 0.3, and wherein the microfibrillated cellulose optionally has a fiber steepness of about 20 to about 50, as measured by a Malvern Mastersizer. As used herein, the terms "comprising" (and any form of comprising, such as "comprise", "comprises", and "comprised"), "having" (and any form of having, such as "have" and "has"), "including" (and any form of including, such as "includes" and "include"), or "containing" (and any form of containing, such as "contains" and "contain"), are inclusive or open-ended, and do not exclude additional, unrecited elements or method steps. Furthermore, terms used in conjunction with the term "comprising" are also understood to be capable of being used in conjunction with the terms "including" or "substantially comprising."
[0079] As used herein, the term "include" and its grammatical variations are non-limiting, such that recitation of items in a list is not to the exclusion of other like items that can be substituted or added to the listed items.
[0080] The fibrous substrate comprising cellulose (variously referred to herein as "fibrous substrate comprising cellulose", "cellulose fibers", "fibrous cellulose raw material", "cellulose raw material" and "cellulose-containing fibers (or fibers), etc.)" can be derived from virgin or recycled pulp or paper mill broke and / or industrial waste, or from paper streams rich in mineral fillers and cellulose materials from paper mills.
[0081] As used herein, the term "substantially" means that the subsequently described event or circumstance occurs completely, or that the subsequently described event or circumstance occurs to a large extent. For example, when related to a specific event or circumstance, the term "substantially" means that the subsequently described event or circumstance occurs at least 80% of the time, or at least 85% of the time, or at least 90% of the time, or at least 95% of the time.
[0082] As used herein, the phrase "an integer from X to Y" refers to any integer including the endpoints. For example, the phrase "an integer from 1 to 5" refers to 1, 2, 3, 4 or 5.
[0083] Unless otherwise stated, the particle size properties of inorganic particulate materials referred to herein can be measured in a well-known manner by using a Sedigraph 5100 machine (referred to herein as the "Micromeritics Sedigraph 5100 unit") supplied by Micromeritics Instruments Corporation, Norcross, Georgia, USA (Tel: +1 7706623620; website: www.micromeritics.com) to measure the sedimentation of particulate materials under conditions of complete dispersion in an aqueous medium. Such a machine provides a measurement and plot of the cumulative weight percentage of particles having a size, known in the art as the "equivalent spherical diameter" (esd), less than a given esd value. The average particle size d 50 is the value of the esd of the particles determined in this way at which 50% by weight of the particles have an esd smaller than this esd 50 The equivalent spherical diameter of the value.
[0084] Alternatively, as described, the particle size properties of the inorganic particulate materials referred to herein are measured using a Malvern Mastersizer 3000 or Malvern Insitec provided by Malvern Instruments Ltd, using conventional methods well known in the art of laser scattering (or equivalent laser scattering equipment or by other methods that give substantially the same results). In the laser scattering technique, the diffraction of a laser beam can be used to measure the size of particles in powders, suspensions and emulsions, based on the application of the Mie theory. Such machines provide measurements and plots of the cumulative volume percentage of particles whose size, referred to in the art as the "equivalent spherical diameter" (esd), is less than a given esd value. The average particle size d 50 is the value of the esd of the particles determined in this way at which 50% by volume of the particles have an esd smaller than this esd 50 The equivalent spherical diameter of the value.
[0085] Unless otherwise stated, particle size properties of coarse fibrillated microfibrillated cellulosic material are measured using a Malvern Insitec machine supplied by Malvern Instruments Ltd using conventional methods well known in the art of laser light scattering (or by other methods giving essentially the same results).
[0086] Details of the procedure for characterising the particle size distribution of a mixture of inorganic particulate material and microfibrillated cellulose using a Malvern Insitec machine are provided in Example 7.
[0087] Microfibrillated cellulose may be derived from any suitable source.
[0088] "Microfibrillated cellulose (MFC)" refers to a cellulose composition in which the microfibrils of cellulose are released or partially released as single species or smaller aggregates compared to the fibers of pre-microfibrillated cellulose. Microfibrillated cellulose can be obtained by microfibrillating cellulose (including but not limited to the processes described herein). Typical cellulose fibers suitable for papermaking (i.e., pre-microfibrillated pulp or pulp that has not yet been fibrillated) include larger aggregates of hundreds or thousands of individual cellulose microfibrils. By microfibrillating cellulose, specific characteristics and properties are imparted to microfibrillated cellulose and compositions comprising microfibrillated cellulose, including but not limited to the characteristics and properties described herein.
[0089] Although microfibrillated cellulose (MFC) is well known and described in the art, for the purposes of the presently disclosed and / or claimed inventive concepts, microfibrillated cellulose is defined as cellulose consisting of microfibrils in the form of isolated cellulose microfibrils and / or microfibril bundles of cellulose, both of which are derived from cellulose raw materials. Thus, microfibrillated cellulose is understood to include partially or fully fibrillated cellulose or lignocellulosic fibers, which can be achieved by various processes known in the art.
[0090] As used herein, "microfibrillated cellulose" may be used interchangeably with "microfibrillated cellulose", "nanofibrillar cellulose", "nanofibrillar cellulose", "cellulose nanofibers", "nanoscale fibrillated cellulose", "cellulose microfibrils", and / or simply "MFC". Furthermore, as used herein, the above listed terms that may be interchangeable with "microfibrillated cellulose" may refer to cellulose that has been fully microfibrillated or cellulose that has been substantially microfibrillated but still contains a certain amount of non-microfibrillated cellulose in an amount that does not interfere with the benefits of microfibrillated cellulose described and / or claimed herein.
[0091] Microfibrillated cellulose (MFC) in the context of this patent application refers to nanoscale cellulose particle fibers or fibrils having at least one dimension less than 100 nm. MFC comprises partially or fully fibrillated cellulose or lignocellulose fibers. The diameter of the released fibrils is less than 100 nm, while the actual fibril diameter or particle size distribution and / or aspect ratio (length / width) depends on the source and manufacturing method.
[0092] The smallest fibrils are called elementary fibrils and have a diameter of about 2 to 4 nm (see, for example, Chinga-Carrasco, G., Cellulose fibres, nanofibrils and microfibrils: The morphological sequence of MFC components from a plant physiology and fibre technology point of view, Nanoscale research letters 2011, 6: 417), while the aggregated form of the elementary fibrils is usually also defined as microfibrils (Fengel, D., Ultrastructural behavior of cell wall polysaccharides, Tappi J., March 1970, Vol 53, No. 3.), which is the main product obtained when manufacturing MFC, for example, by using an extended refining process or a pressure drop decomposition process. Depending on the source and the manufacturing process, the length of the fibrils can vary from about 1 μm to more than 10 μm. The crude MFC fraction may contain a considerable portion of fibrillated fibers, ie fibrils (cellulose fibers) protruding from the tracheids, as well as a certain amount of fibrils (cellulose fibers) released from the tracheids.
[0093] MFC has various abbreviations such as cellulose microfibrils, fibrillated cellulose, nanofibrillated cellulose, fibril aggregates, nanoscale cellulose fibrils, cellulose nanofibrils, cellulose nanofibrils, cellulose microfibrils, cellulose fibrils, microfibrous cellulose, microfibril aggregates and cellulose microfibril aggregates. MFC can also be characterized by various physical or physicochemical properties, such as large surface area or its ability to form a gel-like material at low solids content (1 to 5 wt %) when dispersed in water. The cellulose fibers are preferably fibrillated to such an extent that the final specific surface area of the formed MFC is from about 1 to about 300 m2 when measured by the BET method on freeze-dried material. 2 / g, such as 1 to 200 m 2 / g, or more preferably 50 to 200 m 2 / g.
[0094] Nanofibrous cellulose may contain some hemicellulose; the amount depends on the plant source. Pretreated fibers, such as mechanical decomposition of hydrolyzed, pre-swollen or oxidized cellulose raw materials, are carried out with suitable equipment, such as refiners, grinders, homogenizers, gelatinizers, friction grinders, ultrasonic generators, fluidizers such as microfluidizers, macrofluidizers or fluidizer-type homogenizers. Depending on the manufacturing method of MFC, the product may also contain fine particles, or nano-microcrystalline cellulose or other chemicals present in, for example, wood fibers or papermaking processes. The product may also contain various numbers of micron-sized fiber particles that are not effectively fibrillated. MFC is made of wood cellulose fibers from hardwood or softwood fibers. MFC can also be made from microbial sources, agricultural fibers such as wheat straw pulp, bamboo, bagasse or other non-wood fiber sources. MFC is preferably made of pulp, and the pulp includes pulp from virgin fiber, such as mechanical, chemical and / or thermomechanical pulp. MFC can also be made of broken paper or recycled paper.
[0095] In one embodiment of the present invention, the microfibrillated cellulose has a Schopper Riegler value (°SR) of greater than 85°SR, or greater than 90°SR, or greater than 92°SR. The Schopper Riegler value can be determined by the EN ISO 526 standard method.
[0096] The microfibrillated cellulose preferably has a water retention value of at least 200%, more preferably at least 250%, most preferably at least 300%.The addition of certain chemicals may affect the water retention value.
[0097] The above definition of MFC includes, but is not limited to, the newly proposed TAPPI standard W13021 on cellulose nanofibrils (CNF), which defines a cellulose nanofiber material comprising a plurality of elementary fibrils having crystalline and amorphous regions.
[0098] In an embodiment of any of the foregoing aspects and embodiments, the microfibrillated cellulose is obtained from a chemical pulp, or a chemithermomechanical pulp, or a mechanical pulp, or a thermomechanical pulp, including, for example, northern bleached softwood kraft pulp ("NBSK"), bleached chemithermomechanical pulp ("BCTMP"), or recycled pulp, or broke pulp, or a paper mill waste stream, or waste from a paper mill, or a combination thereof.
[0099] In an embodiment of any of the foregoing aspects and embodiments, the pulp source is kraft pulp or bleached long fiber kraft pulp.
[0100] In an embodiment of any of the foregoing aspects and embodiments, the pulp source is a softwood pulp selected from spruce, pine, fir, larch and hemlock, or a mixed softwood pulp.
[0101] In an embodiment of any of the foregoing aspects and embodiments, the pulp source is a hardwood pulp selected from eucalyptus, poplar and birch, or a mixed hardwood pulp.
[0102] In an embodiment of any of the foregoing aspects and embodiments, the pulp source is eucalyptus pulp, spruce pulp, pine pulp, beech pulp, hemp pulp, acacia cotton pulp and mixtures thereof.
[0103] "Microfibrillation" refers to a process in which the microfibrils of cellulose are released or partially released as individual species or small aggregates compared to the fibers of a pre-microfibrillated pulp. Typical cellulose fibers suitable for papermaking (i.e. pre-microfibrillated pulp) include larger aggregates of hundreds or thousands of individual cellulose fibrils.
[0104] Microfibrillated cellulose comprises cellulose, which is a natural polymer comprising repeating glucose units. The term "microfibrillated cellulose", also referred to as MFC, as used in this specification includes microfibrillated / microfibrous cellulose and nanofibrillated / nanofibrillar cellulose (NFC), these materials also referred to as nanocellulose.
[0105] Many methods for preparing microfibrillated cellulose are known in the prior art.
[0106] WO-A-2010 / 131016 discloses a process for preparing microfibrillated cellulose, which comprises microfibrillating, for example, by grinding a fibrous material comprising cellulose, optionally in the presence of grinding media and inorganic particulate material. When used as a filler in paper, for example as a substitute or partial substitute for conventional mineral fillers, the microfibrillated cellulose obtained by the process, optionally in combination with inorganic particulate material, improves the bursting properties of the paper. That is, paper filled with microfibrillated cellulose was found to have improved bursting strength relative to paper filled with mineral fillers alone. In other words, the microfibrillated cellulose filler was found to have the property of strengthening the bursting strength of paper. In a particularly advantageous embodiment of the present invention, the fibrous material comprising cellulose is ground in the presence of grinding media and optionally in combination with inorganic particulate material to obtain microfibrillated cellulose having a fiber steepness of 20 to about 50.
[0107] The method described in WO-A-2010 / 131016 comprises the step of microfibrillating a fibrous substrate comprising cellulose by grinding in the presence of a particulate grinding medium which is removed after grinding is complete. "Microfibrillation" refers to a process in which the microfibrils of cellulose are released or partially released as individual species or small aggregates compared to the fibers of a pre-microfibrillated pulp. Typical cellulose fibers suitable for papermaking (i.e. pre-microfibrillated pulp) comprise larger aggregates of hundreds or thousands of individual cellulose fibrils. By microfibrillating the cellulose, specific characteristics and properties are imparted to the microfibrillated cellulose and compositions comprising the microfibrillated cellulose, including those described herein.
[0108] The cellulose-containing fibrous substrate (variously referred to herein as "cellulose-containing fibrous substrate", "cellulose fibers", "fibrous cellulose raw material", "cellulose raw material" and "cellulose-containing fibers (or fibrous) etc.)" can be derived from recycled pulp or paper mill broke and / or industrial waste, or from paper streams rich in mineral fillers and cellulose materials from paper mills.
[0109] Regenerated cellulose pulp may be beaten (e.g., in a Valley beater) and / or otherwise refined (e.g., processed in a cone or plate refiner) to any predetermined freeness, reported in the art as % freeness in cm. 3 The freeness of a cellulose pulp is measured by the Canadian standard freeness (CSF). CSF refers to the value of the freeness or drainage rate of a pulp measured by the drainage rate of a pulp suspension, and the test is performed according to the T227cm-09 TAPPI standard. For example, before microfibrillation, a cellulose pulp may have a freeness of about 10 cm 3 or greater Canadian Standard Freeness. Regenerated cellulose pulp may have a freeness of about 700 cm 3 or smaller CSF, e.g., equal to or less than about 650 cm 3 , or equal to or less than about 600cm 3 , or equal to or less than about 550cm 3 , or equal to or less than about 500cm 3 , or equal to or less than about 450cm 3 , or equal to or less than about 400cm 3 , or equal to or less than about 350cm 3 , or equal to or less than about 300cm 3 , or equal to or less than about 250cm 3 , or equal to or less than about 200cm 3 , or equal to or less than about 150cm 3 , or equal to or less than about 100cm 3, or equal to or less than about 50cm 3 The regenerated cellulose pulp may have a CSF of about 20 to about 700. The regenerated cellulose pulp may then be dewatered by methods known in the art, for example, the pulp may be filtered through a screen to obtain a wet sheet containing at least about 10% solids, such as at least about 15% solids, or at least about 20% solids, or at least about 30% solids, or at least about 40% solids. The regenerated pulp may be used in an unrefined state without beating or dewatering, or refined in other ways.
[0110] The fibrous substrate comprising cellulose can be added to the grinding vessel in a dry state. For example, dry broke can be added directly to the grinder vessel. The water environment in the grinder vessel will promote the formation of pulp.
[0111] The inorganic particulate material, if any, may be, for example, an alkaline earth metal carbonate or sulfate (such as calcium carbonate), magnesium carbonate, dolomite, gypsum, hydrous kandite clay (such as kaolin, halloysite or ball clay), anhydrous (calcined) kandite clay (such as metakaolin or fully calcined kaolin), talc, mica, perlite or diatomaceous earth, or brucite, or aluminum trihydrate or a combination thereof.
[0112] The preferred inorganic particulate material for the method is calcium carbonate. Hereinafter, the present invention may tend to be discussed in terms of calcium carbonate and aspects relating to which calcium carbonate is processed and / or treated. The present invention should not be construed as being limited to such embodiments.
[0113] The granular calcium carbonate used in the present invention can be obtained from natural sources by grinding. Ground calcium carbonate (GCC) is usually obtained by pulverizing and then grinding a mineral source such as chalk, marble or limestone, and a particle size classification step can be performed subsequently to obtain a product with the desired fineness. Other technologies such as bleaching, flotation and magnetic separation can also be used to obtain a product with the desired fineness and / or color. The granular solid material can be ground by itself, i.e. ground by friction between the solid material particles themselves, or ground in the presence of a granular grinding medium containing particles of the material to be ground that are different from calcium carbonate. These processes can be carried out with or without a dispersant and a bactericide, which can be added at any stage of the process.
[0114] Precipitated calcium carbonate (PCC) can be used as the source of particulate calcium carbonate in the present invention, and can be produced by any method in the known methods available in the art. TAPPI Monograph Series No. 30, "Paper Coating Pigments", pages 34-35 describe three main commercial processes for preparing precipitated calcium carbonate, which are suitable for preparing products used in the paper industry, but can also be used in the practice of the present invention. In all three processes, calcium carbonate raw materials, such as limestone, are first calcined to produce quicklime, and then the quicklime is slaked in water to produce calcium hydroxide or milk of lime. In the first process, the milk of lime is directly carbonized with carbon dioxide gas. The advantage of this process is that no by-product is formed, and it is relatively easy to control the performance and purity of the calcium carbonate product. In the second process, the milk of lime contacts with soda ash to produce calcium carbonate precipitation and sodium hydroxide solution by double decomposition. If this process is used commercially, sodium hydroxide can be separated from calcium carbonate completely. In the third main commercial process, the milk of lime first contacts with ammonium chloride to obtain calcium chloride solution and ammonia. Calcium chloride solution contacts with soda ash then, produces precipitated calcium carbonate and sodium chloride solution by double decomposition.According to used specific reaction process, crystal can be made into various shapes and sizes.Three kinds of main forms of PCC crystal are aragonite, rhombohedron and trigonal body, they are all suitable for the present invention, and comprise that their mixture is also suitable for.
[0115] Wet grinding of calcium carbonate includes forming an aqueous suspension of calcium carbonate, which can then be ground optionally in the presence of a suitable dispersant. For more information on wet grinding of calcium carbonate, reference can be made, for example, to EP-A-614948 (the entire contents of which are incorporated herein by reference).
[0116] In some cases, other minerals may be included in small amounts, for example, one or more of kaolin, calcined kaolin, wollastonite, bauxite, talc, or mica may also be present.
[0117] When the inorganic particulate material of the present invention is obtained from a natural source, it is possible that some mineral impurities will contaminate the grinding material. For example, naturally occurring calcium carbonate can exist in conjunction with other minerals. Therefore, in some embodiments, the inorganic particulate material includes a certain amount of impurities. However, in general, the inorganic particulate material used for the present invention will contain less than about 5% by weight, preferably less than about 1% by weight of other mineral impurities. The inorganic particulate material used in the microfibrillation step of the method of the present invention will preferably have a particle size distribution in which at least about 10% by weight of the particles have an equivalent spherical diameter (esd) less than 2 μm, for example, at least about 20% by weight, or at least about 30% by weight, or at least about 40% by weight, or at least about 50% by weight, or at least about 60% by weight, or at least about 70% by weight, or at least about 80% by weight, or at least about 90% by weight, or at least about 95% by weight, or about 100% of the particles have an esd less than 2 μm.
[0118] Unless otherwise stated, the particle size properties of the microfibrillated cellulose material are measured using conventional methods well known in the art of laser light scattering (or by other methods giving essentially the same results) using a Malvern Insitec machine supplied by Malvern Instruments Ltd. Details of the procedure for characterising the particle size distribution of a mixture of inorganic particulate material and microfibrillated cellulose using a Malvern Mastersizer S machine are provided below.
[0119] A fibrous substrate comprising cellulose can be microfibrillated in the presence of an inorganic particulate material to obtain a d 50 Microfibrillated cellulose having a size of about 5 μm to about 500 μm. A fibrous substrate comprising cellulose may be microfibrillated in the presence of an inorganic particulate material to obtain a microfibrillated cellulose having a size of about 5 μm to about 500 μm. 50 Microfibrillated cellulose of about 400 μm or less, for example, about 300 μm or less, or about 200 μm or less, or about 150 μm or less, or about 125 μm or less, or about 100 μm or less, or about 90 μm or less, or about 80 μm or less, or about 70 μm or less, or about 60 μm or less, or about 50 μm or less, or about 40 μm or less, or about 30 μm or less, or about 20 μm or less, or about 10 μm or less.
[0120] A fibrous substrate comprising cellulose may be microfibrillated in the presence of an inorganic particulate material to obtain microfibrillated cellulose having a modal fiber particle size of about 0.1 to 500 μm and a modal inorganic particulate material particle size of 0.25 to 20 μm. A fibrous substrate comprising cellulose may be microfibrillated in the presence of an inorganic particulate material to obtain microfibrillated cellulose having a modal fiber particle size of at least about 0.5 μm, such as at least about 10 μm, or at least about 50 μm, or at least about 100 μm, or at least about 150 μm, or at least about 200 μm, or at least about 300 μm, or at least about 400 μm.
[0121] The fibrous substrate comprising cellulose may be microfibrillated in the presence of an inorganic particulate material to obtain microfibrillated cellulose having a fiber steepness equal to or greater than about 10 as measured by Malvern. The fiber steepness (i.e., the steepness of the fiber size distribution) is determined by the following formula:
[0122] Steepness = 100 × (d 30 / d 70 )
[0123] The fiber steepness of the microfibrillated cellulose may be equal to or less than about 100. The fiber steepness of the microfibrillated cellulose may be equal to or less than about 75, or equal to or less than about 50, or equal to or less than about 40, or equal to or less than about 30. The microfibrillated cellulose may have a fiber steepness of about 20 to about 50, or about 25 to about 40, or about 25 to about 35, or about 30 to about 40.
[0124] The finer mineral peak can be fitted to the measured data points and mathematically subtracted from the distribution to leave the fiber peak, which can then be converted to a cumulative distribution. Similarly, the fiber peak can be mathematically subtracted from the original distribution to leave the mineral peak, which can then also be converted to a cumulative distribution. Both cumulative curves can then be used to calculate the average particle size (d 50 ) and distribution steepness (d 30 / d 70 × 100). The differential curve can then be used to find the modal grain size of both the mineral and fiber fractions.
[0125] Another preferred inorganic particulate material is kaolin. The present invention should not be construed as being limited to such embodiments. Therefore, in some embodiments, kaolin is used in an unprocessed form.
[0126] The kaolin used in the present invention can be a processed material derived from a natural source, i.e., a natural kaolin mineral. The processed kaolin can typically contain at least about 50% by weight kaolinite. For example, most commercially processed kaolin contains greater than about 75% by weight kaolinite, and can contain greater than about 90% by weight, in some cases greater than about 95% by weight kaolinite.
[0127] The kaolin used in the present invention may be prepared from natural kaolin minerals by one or more other processes well known to those skilled in the art, such as by known refining or beneficiation steps.
[0128] For example, the clay mineral can be bleached with a reducing bleach, such as sodium dithionite. If sodium dithionite is used, after the sodium dithionite bleaching step, the bleached clay mineral can be optionally dehydrated, and optionally washed, and optionally dehydrated again.
[0129] The clay mineral may be treated to remove impurities, for example by flocculation, flotation or magnetic separation techniques well known in the art. Alternatively, the clay mineral used in the first aspect of the invention may be in untreated solid form or in the form of an aqueous suspension.
[0130] The method for preparing the particulate kaolin of the present invention may also include one or more comminution steps, such as grinding or milling. Slight comminution of the crude kaolin is used to produce suitable delamination thereof. Comminution may be performed using plastic (e.g., nylon) beads or particles, sand, or ceramic grinding or milling aids. The crude kaolin may be refined using well-known procedures to remove impurities and improve physical properties. The kaolin may be treated by known particle size classification procedures, such as screening and centrifugation (or both), to obtain particles having the desired d 50 value or particle size distribution of particles.
[0131] In a non-limiting example, the term microfibrillated cellulose is used to describe fibrillated cellulose, which comprises nanoscale cellulose particle fibers or fibrils, typically having at least one dimension less than 100 nm. When released from cellulose fibers, the diameter of the fibrils is typically less than 100 nm. The actual diameter of the cellulose fibrils depends on the source and measurement method of such fibrils and the manufacturing method used.
[0132] The particle size distribution and / or aspect ratio (length / width) of the cellulose microfibrils attached to the fibrillated cellulose fibers or as released microfibrils depends on the source and the manufacturing method used in the microfibrillation process.
[0133] In a non-limiting example, the aspect ratio of microfibrils is generally high, and the length of a single microfibril may be greater than 1 μm, and the diameter may be in the range of about 5 to 60 nm, with the number average diameter being generally less than 20 nm. The diameter of a microfibril bundle may be greater than 1 μm.
[0134] In a non-limiting example, the smallest fibrils are often referred to as elementary fibrils, which typically have a diameter of about 2 to 4 nm. Aggregates of elementary fibrils are also common, which can also be considered microfibrils.
[0135] In a non-limiting example, microfibrillated cellulose may at least partially comprise nanocellulose. Nanocellulose may primarily comprise nano-sized fibrils, whose diameter is less than 100 nm and whose length may be in the micrometer range or lower. The smallest microfibrils are similar to so-called elementary fibrils, whose diameter is typically 2 to 4 nm. Of course, in addition to the method for producing microfibrillated cellulose, the size and structure of microfibrils and microfibril bundles also depend on the raw materials used. Nevertheless, it is expected that those of ordinary skill in the art will understand the meaning of "microfibrillated cellulose" in the context of the inventive concept currently disclosed and / or claimed.
[0136] Depending on the source of the cellulose fibers and the manufacturing process used to microfibrillate the cellulose fibers, the length of the fibrils can vary, typically ranging from about 1 to greater than 10 μm.
[0137] The crude MFC fraction may contain a considerable portion of fibrillated fibers, ie, fibrils (cellulose fibers) protruding from the tracheids, as well as a certain amount of fibrils (cellulose fibers) released from the tracheids.
[0138] Manufacturing microfibrillated cellulose
[0139] In embodiments, microfibrillated cellulose may also be produced from recycled pulp or paper mill broke and / or industrial waste, or paper streams from paper mills rich in mineral fillers and cellulosic material.
[0140] The fibrous substrate comprising cellulose can be added to the grinding vessel in a dry state. For example, dry broke can be added directly to the grinder vessel. The water environment in the grinder vessel will promote the formation of pulp.
[0141] In some embodiments, the microfibrillated cellulose has a d value of about 5 μm to about 500 μm as measured by laser light scattering. 50 In some embodiments, the microfibrillated cellulose has a 50Equal to or less than about 400μm, for example, equal to or less than about 300μm, or equal to or less than about 200μm, or equal to or less than about 150μm, or equal to or less than about 125μm, or equal to or less than about 100μm, or equal to or less than about 90μm, or equal to or less than about 80μm, or equal to or less than about 70μm, or equal to or less than about 60μm, or equal to or less than about 50μm, or equal to or less than about 40μm, or equal to or less than about 30μm, or equal to or less than about 20μm, or equal to or less than about 10μm.
[0142] In some embodiments, the microfibrillated cellulose has a modal fiber particle size of about 0.1 to 500 μm. In some embodiments, the microfibrillated cellulose has a modal fiber particle size of at least about 0.5 μm, such as at least about 10 μm, or at least about 50 μm, or at least about 100 μm, or at least about 150 μm, or at least about 200 μm, or at least about 300 μm, or at least about 400 μm.
[0143] Additionally or alternatively, the microfibrillated cellulose may have a fiber steepness, as measured by Malvern, equal to or greater than about 10. The fiber steepness (i.e., the steepness of the fiber size distribution) is determined by the following formula, where "d" represents the median diameter as measured by Malvern:
[0144] Steepness = 100 × (d 30 / d 70 )
[0145] The fiber steepness of the microfibrillated cellulose may be equal to or less than about 100. The fiber steepness of the microfibrillated cellulose may be equal to or less than about 75, or equal to or less than about 50, or equal to or less than about 40, or equal to or less than about 30. The microfibrillated cellulose may have a fiber steepness of about 20 to about 50, or about 25 to about 40, or about 25 to about 35, or about 30 to about 40.
[0146] Inorganic particle materials
[0147] The inorganic particulate material may be, for example, an alkaline earth metal carbonate or sulfate (such as calcium carbonate, magnesium carbonate), dolomite, gypsum, hydrous kandite clay (such as kaolin, halloysite or ball clay), anhydrous (calcined) kandite clay (such as metakaolin or fully calcined kaolin), talc, mica, magnesite, hydromagnesite, ground glass, perlite or diatomaceous earth, or wollastonite, or titanium dioxide, or brucite, or aluminum trihydrate, lime, graphite or a combination thereof.
[0148] In some embodiments, the inorganic particulate material includes or is calcium carbonate, magnesium carbonate, dolomite, gypsum, anhydrous kandite clay, perlite, diatomaceous earth, wollastonite, brucite, or aluminum trihydrate, titanium dioxide, or a combination thereof.
[0149] In some embodiments, the inorganic particulate material is selected from the group consisting of alkaline earth metal carbonates or sulfates, calcium carbonate, magnesium carbonate, dolomite, gypsum, bentonite, hydrous kandite clay, kaolin, halloysite, ball clay, anhydrous (calcined) kandite clay, metakaolin or fully calcined kaolin, talc, mica, perlite, sepiolite, magnesite, diatomaceous earth, magnesite, silicates, or diatomaceous earth, brucite, aluminum trihydrate, and combinations thereof.
[0150] In some embodiments of aspects of the invention, the inorganic particulate material is selected from the group consisting of alkaline earth metal carbonates or sulfates, calcium carbonate, magnesium carbonate, dolomite, gypsum, bentonite, hydrous kandite clay, kaolin, halloysite, ball clay, anhydrous (calcined) kandite clay, metakaolin or fully calcined kaolin, talc, mica, perlite, sepiolite, magnesite, diatomaceous earth, magnesite, silicates, or diatomaceous earth, brucite, aluminum trihydrate, and combinations thereof.
[0151] An exemplary inorganic particulate material for use in the present invention is calcium carbonate. Hereinafter, the present invention may tend to be discussed in terms of calcium carbonate and aspects involving the processing and / or treatment of calcium carbonate. The present invention should not be construed as being limited to such embodiments.
[0152] The granular calcium carbonate used in the present invention can be obtained from natural sources by grinding. Ground calcium carbonate (GCC) is usually obtained by pulverizing and then grinding a mineral source such as chalk, marble or limestone, and a particle size classification step can be performed subsequently to obtain a product with the desired fineness. Other technologies such as bleaching, flotation and magnetic separation can also be used to obtain a product with the desired fineness and / or color. The granular solid material can be ground autogenously, i.e., by friction between the solid material particles themselves, or, in the presence of a granular grinding medium containing particles that are different from the calcium carbonate material to be ground, ground. These processes can be carried out with or without a dispersant and a bactericide, which can be added at any stage of the process.
[0153] Precipitated calcium carbonate (PCC) can be used as the source of particulate calcium carbonate in the present invention, and can be produced by any method in the known methods available in the art. TAPPI Monograph Series No. 30, "Paper Coating Pigments", pages 34-35 describe three main commercial processes for preparing precipitated calcium carbonate, which are suitable for preparing products used in the paper industry, but can also be used in the practice of the present invention. In all three processes, calcium carbonate raw materials, such as limestone, are first calcined to produce quicklime, and then the quicklime is slaked in water to produce calcium hydroxide or milk of lime. In the first process, the milk of lime is directly carbonized with carbon dioxide gas. The advantage of this process is that no by-product is formed, and it is relatively easy to control the performance and purity of the calcium carbonate product. In the second process, the milk of lime contacts with soda ash to produce calcium carbonate precipitation and sodium hydroxide solution by double decomposition. If this process is used commercially, sodium hydroxide can be separated from calcium carbonate completely. In the third main commercial process, the milk of lime first contacts with ammonium chloride to obtain calcium chloride solution and ammonia. Calcium chloride solution is then contacted with soda ash to produce precipitated calcium carbonate and sodium chloride solution by double decomposition. According to the specific reaction process used, crystal can be made into various shapes and sizes. Three main forms of PCC crystals are aragonite, rhombohedron and trigonal body (for example calcite), which are all suitable for the present invention, including that their mixture is also suitable.
[0154] In some embodiments of aspects of the invention, PCC may be formed during the production of microfibrillated cellulose.
[0155] Wet grinding of calcium carbonate comprises forming an aqueous suspension of calcium carbonate and then grinding the aqueous suspension optionally in the presence of a suitable dispersant. For more information on wet grinding of calcium carbonate, reference may be made, for example, to EP-A-614948 (the entire contents of which are incorporated herein by reference).
[0156] When the inorganic particulate material of the present invention is obtained from a natural source, it is possible that some mineral impurities will contaminate the abrasive material. For example, naturally occurring calcium carbonate may coexist with other minerals. Therefore, in some embodiments, the inorganic particulate material includes a certain amount of impurities. However, in general, the inorganic particulate material used in the present invention will contain less than about 5% by weight, or less than about 1% by weight of other mineral impurities.
[0157] The inorganic particulate material can have a particle size distribution wherein at least about 10 wt % of the particles have an esd less than 2 μm, for example, at least about 20 wt %, or at least about 30 wt %, or at least about 40 wt %, or at least about 50 wt %, or at least about 60 wt %, or at least about 70 wt %, or at least about 80 wt %, or at least about 90 wt %, or at least about 95 wt %, or about 100 % of the particles have an esd less than 2 μm.
[0158] In another embodiment of aspects of the invention, the inorganic particulate material has a particle size distribution in which at least about 10% by volume of the particles have an esd less than 2 μm, for example, at least about 20% by volume, or at least about 30% by volume, or at least about 40% by volume, or at least about 50% by volume, or at least about 60% by volume, or at least about 70% by volume, or at least about 80% by volume, or at least about 90% by volume, or at least about 95% by volume, or about 100% by volume of the particles have an esd less than 2 μm, as measured using a Malvern Insitec or 3000 machine.
[0159] Details of the procedure for characterising the particle size distribution of a mixture of inorganic particulate material and microfibrillated cellulose using a Malvern Insitec OR 3000 machine are provided in Example 7.
[0160] Method for producing microfibrillated cellulose and inorganic particulate material
[0161] In some embodiments of aspects of the present invention, coarse fibrillated microfibrillated cellulose may be prepared in the presence or absence of inorganic particulate material.
[0162] Microfibrillated cellulose is derived from a fiber substrate comprising cellulose. The fiber substrate comprising cellulose can be derived from any suitable source, such as wood, grass (e.g., sugar cane, bamboo) or rags (e.g., textile waste, cotton, hemp or flax). The fiber substrate comprising cellulose can be in the form of pulp (i.e., a suspension of cellulose fibers in water), which can be prepared by any suitable chemical or mechanical treatment or combination thereof. For example, the pulp can be chemical pulp, or chemical thermomechanical pulp, or mechanical pulp, or recycled pulp, or paper mill broke, or paper mill waste stream, or waste from a paper mill, or dissolving pulp, kenaf pulp, market pulp, partially carboxymethylated pulp, abaca pulp, birch pulp, grass pulp, bamboo pulp, palm pulp, peanut shells or a combination thereof. The cellulose pulp can be beaten (e.g., in a Valley beater) and / or otherwise refined (e.g., processed in a cone or plate refiner) to any predetermined freeness, reported in the art as cm 3The Canadian Standard Freeness (CSF) is measured by the CSF. CSF refers to the value of the freeness or drainage rate of the pulp measured by the rate at which the pulp suspension drains. For example, before microfibrillation, a cellulose pulp may have a freeness of about 10 cm 3 or greater Canadian Standard Freeness. Cellulose pulp may have a freeness of about 700 cm 3 or smaller CSF, e.g., equal to or less than about 650 cm 3 , or equal to or less than about 600cm 3 , or equal to or less than about 550cm 3 , or equal to or less than about 500cm 3 , or equal to or less than about 450cm 3 , or equal to or less than about 400cm 3 , or equal to or less than about 350cm 3 , or equal to or less than about 300cm 3 , or equal to or less than about 250cm 3 , or equal to or less than about 200cm 3 , or equal to or less than about 150cm 3 , or equal to or less than about 100cm 3 , or equal to or less than about 50cm 3 .
[0163] In some embodiments of aspects of the invention, the pulp is obtained from a chemical pulp, or a chemithermomechanical pulp, or a mechanical pulp, or a thermomechanical pulp, including, for example, northern bleached softwood kraft pulp ("NBSK"), bleached hardwood pulp, bleached chemithermomechanical pulp ("BCTMP"), or recycled pulp, or broke pulp, or a paper mill waste stream, or waste from a paper mill, or a combination thereof.
[0164] The cellulose pulp can then be dewatered by methods known in the art, for example, the pulp can be filtered through a screen to obtain a wet sheet containing at least about 10% solids, such as at least about 15% solids, or at least about 20% solids, or at least about 30% solids, or at least about 40% solids. The pulp can be used in an unrefined state, that is, without being beaten or dewatered, or refined in other ways.
[0165] In some embodiments of aspects of the present invention, slurrying may be performed in the presence of an inorganic particulate material, such as calcium carbonate.
[0166] Co-grinding process of microfibrillated cellulose and inorganic particulate materials
[0167] In embodiments of aspects of the present invention, the invention relates to modifications, such as improvements, to the methods and compositions described in WO-A-2010 / 131016, the entire contents of which are incorporated herein by reference.
[0168] WO-A-2010 / 131016 discloses a process for preparing microfibrillated cellulose, which comprises microfibrillating, for example, by grinding a fibrous material comprising cellulose, optionally in the presence of grinding media and / or inorganic particulate material. When used as a filler in paper, for example as a substitute or partial substitute for conventional mineral fillers, it was unexpectedly found that the microfibrillated cellulose obtained by the process, optionally in combination with inorganic particulate material, improves the bursting properties of the paper. That is, relative to paper filled with mineral fillers alone, it was found that paper filled with microfibrillated cellulose has improved bursting strength. In other words, it was found that the microfibrillated cellulose filler has the property of strengthening the bursting strength of paper. In a particularly advantageous embodiment of the present invention, the fibrous material comprising cellulose is ground in the presence of grinding media and optionally in combination with inorganic particulate material to obtain microfibrillated cellulose having a fiber steepness of 20 to about 50.
[0169] To prepare microfibrillated cellulose, the fiber substrate comprising cellulose can be added to a grinding container or a homogenizer in a dry state. For example, dry broke paper can be added directly to a grinder container. The water environment in the grinder container will promote the formation of pulp.
[0170] The microfibrillation step can be performed in any suitable equipment, including but not limited to a refiner. In one embodiment, the microfibrillation step is performed in a grinding vessel under wet grinding conditions. In another embodiment, the microfibrillation step is performed in a homogenizer. Each of these embodiments is described in more detail below.
[0171] Wet grinding
[0172] Grinding is suitably performed in a conventional manner. Grinding may be a friction grinding process in the presence of particulate grinding media, or may be an autogenous grinding process, i.e., a grinding process without grinding media. Grinding media refers to media other than inorganic particulate material, which in some embodiments may be co-grinded with the fibrous substrate comprising cellulose.
[0173] The particulate grinding media, if any, may be natural or synthetic materials. The grinding media may, for example, include balls, beads or particles made of any hard mineral, ceramic or metallic material. Such materials may include, for example, aluminum oxide, zirconium oxide, zirconium silicate, aluminum silicate or a fusate material produced by calcining kaolinite clay at a temperature ranging from about 1300° C. to about 1800° C. For example, in some embodiments, the use of Abrasive Media. Alternatively, natural sand particles of a suitable particle size may be used.
[0174] In other embodiments, hardwood grinding media (eg, wood flour) may be used.
[0175] Typically, the type and particle size of the grinding media selected for the present invention can depend on performance, for example, the particle size and chemical composition of the feed suspension of the material to be ground. In some embodiments, the particulate grinding media includes particles with an average diameter in the range of about 0.1 mm to about 6.0 mm, for example, in the range of about 0.2 mm to about 4.0 mm. The amount of the grinding media (or media) can be up to about 70% of the charge volume. The amount of the grinding media can be at least about 10% of the charge volume, for example at least about 20% of the charge volume, or at least about 30% of the charge volume, or at least about 40% of the charge volume, or at least about 50% of the charge volume, or at least about 60% of the charge volume.
[0176] Grinding may be performed in one or more stages. For example, a coarse inorganic particulate material may be ground to a predetermined particle size distribution in a grinding vessel, followed by addition of cellulose-containing fibrous material and continued grinding until the desired microfibrillation level is achieved and coarse fibrillated microfibrillated cellulose is produced.
[0177] The inorganic particulate material can be wet or dry ground in the presence or absence of grinding media. In the case of the wet grinding stage, the coarse inorganic particulate material is ground in an aqueous suspension in the presence of grinding media.
[0178] In an embodiment of aspects of the present invention, the median particle size (d 50 For example, the inorganic particulate material 50 The d of the inorganic particulate material may be reduced by at least about 10% (as measured by a Malvern Insitec or 3000 machine), for example. 50 It can be reduced by at least about 20%, or by at least about 30%, or by at least about 50%, or by at least about 50%, or by at least about 60%, or by at least about 70%, or by at least about 80%, or by at least about 90%. For example, before co-grinding, d 50 2.5 μm and after co-grinding 50 An inorganic particulate material of 1.5 μm will experience a 40% particle size reduction.
[0179] In some embodiments of aspects of the present invention, the median particle size of the inorganic particulate material is not significantly reduced during the co-grinding process. "Not significantly reduced" means that the median particle size of the inorganic particulate material is not significantly reduced. 50 Reduce by less than about 10%, for example, the d 50 The reduction was less than about 5%.
[0180] The fibrous substrate comprising cellulose may be microfibrillated, optionally in the presence of an inorganic particulate material, to obtain a d50 The fibrous substrate comprising cellulose may be microfibrillated, optionally in the presence of an inorganic particulate material, to obtain a microfibrillated cellulose having a diameter of about 5 μm to about 500 μm. 50 Microfibrillated cellulose of about 400 μm or less, for example, about 300 μm or less, or about 200 μm or less, or about 150 μm or less, or about 125 μm or less, or about 100 μm or less, or about 90 μm or less, or about 80 μm or less, or about 70 μm or less, or about 60 μm or less, or about 50 μm or less, or about 40 μm or less, or about 30 μm or less, or about 20 μm or less, or about 10 μm or less.
[0181] The fibrous substrate comprising cellulose may be microfibrillated, optionally in the presence of an inorganic particulate material, to obtain microfibrillated cellulose having a modal fiber particle size of about 0.1 to 500 μm and a modal inorganic particulate material particle size of 0.25 to 20 μm. The fibrous substrate comprising cellulose may be microfibrillated, optionally in the presence of an inorganic particulate material, to obtain microfibrillated cellulose having a modal fiber particle size of at least about 0.5 μm, such as at least about 10 μm, or at least about 50 μm, or at least about 100 μm, or at least about 150 μm, or at least about 200 μm, or at least about 300 μm, or at least about 400 μm.
[0182] As mentioned above, the fibrous substrate comprising cellulose may be microfibrillated, optionally in the presence of an inorganic particulate material, to obtain microfibrillated cellulose having fiber steepness.
[0183] The grinding can be carried out in a grinding vessel, such as a tumble mill (e.g., rod mill, ball mill and autogenous mill), a stirred mill (e.g., SAM mill or Isa mill), a tower mill, a stirred media mill (SMD) or a grinding vessel comprising rotating parallel grinding plates between which the feed to be ground is fed.
[0184] In embodiments of aspects of the invention, grinding is performed in a screen grinder, such as a stirred media pulverizer. The screen grinder may include one or more screens having a nominal aperture of at least about 250 μm, for example, one or more screens may have a nominal aperture of at least about 300 μm, or at least about 350 μm, or at least about 400 μm, or at least about 450 μm, or at least about 500 μm, or at least about 550 μm, or at least about 600 μm, or at least about 650 μm, or at least about 700 μm, or at least about 750 μm, or at least about 800 μm, or at least about 850 μm, or at least about 900 μm, or at least about 1000 μm.
[0185] The screen sizes mentioned above apply to the tower mill embodiment described above.
[0186] As described above, grinding can be performed in the presence of a grinding medium. In embodiments of aspects of the invention, the grinding medium is a coarse medium comprising particles having an average diameter in the range of about 1 mm to about 6 mm, such as about 2 mm, or about 3 mm, or about 4 mm, or about 5 mm.
[0187] In another embodiment of aspects of the invention, the specific gravity of the grinding media is at least about 2.5, e.g., at least about 3, or at least about 3.5, or at least about 4.0, or at least about 4.5, or at least about 5.0, or at least about 5.5, or at least about 6.0.
[0188] In yet another embodiment of aspects of the present invention, the grinding media comprises particles having an average diameter in the range of about 1 mm to about 6 mm and a specific gravity of at least about 2.5.
[0189] In another embodiment of aspects of the present invention, the grinding media comprises particles having an average diameter of about 3 mm and a specific gravity of about 2.7.
[0190] As described above, the grinding media (or media) may be present in an amount up to about 70% of the charge volume. The grinding media may be present in an amount of at least about 10% of the charge volume, such as at least about 20% of the charge volume, or at least about 30% of the charge volume, or at least about 40% of the charge volume, or at least about 50% of the charge volume, or at least about 60% of the charge volume.
[0191] In an embodiment of aspects of the present invention, the grinding media is present in an amount of about 50% by volume of the charge.
[0192] The term "charge" refers to the composition delivered as feed to the mill vessel. The charge includes water, grinding media, a fibrous substrate comprising cellulose and optional inorganic particulate material, and any other optional additives described herein.
[0193] Using relatively coarse and / or dense media has the advantage of increasing settling rates (ie, faster) and reducing media carryover through quiescent zones and / or classifiers and / or screens.
[0194] Another advantage of using relatively coarse grinding media is that during the grinding process, the average particle size (d 50 ) will not be significantly reduced, so that the energy imparted to the grinding system is mainly consumed in the microfibrillation of the cellulose-containing fiber substrate.
[0195] Another advantage of using a relatively coarse screen is that relatively coarse or dense grinding media can be used in the microfibrillation step. In addition, the use of a relatively coarse screen (i.e., having a nominal aperture of at least about 250 μm) allows a relatively high solids content product to be processed and removed from the grinder, which allows a relatively high solids content feed (including a fibrous substrate comprising cellulose and an inorganic particulate material) to be processed in an economically viable process. As described below, it has been found that, in terms of energy sufficiency, it is desirable to have a feed with a high initial solids content. In addition, it has also been found that products produced (at a given energy) at a lower solids content have a coarser particle size distribution.
[0196] Grinding can be carried out in a cascade of grinding containers, wherein one or more grinding containers can include one or more grinding zones. For example, a fibrous substrate comprising cellulose and an inorganic particulate material can be ground in a cascade of two or more grinding containers, such as a cascade of three or more grinding containers, or a cascade of four or more grinding containers, or a cascade of five or more grinding containers, or a cascade of six or more grinding containers, or a cascade of seven or more grinding containers, or a cascade of eight or more grinding containers, or a cascade of nine or more grinding containers in series, or a cascade comprising up to ten grinding containers. The cascade of grinding containers can be operably connected in series or in parallel or in a combination of series and parallel. The output and / or input of one or more grinding containers in the cascade can be subjected to one or more screening steps and / or one or more classification steps.
[0197] The circuit may comprise one or more grinding vessels and homogenizer combinations.
[0198] In an embodiment, the grinding is performed in a closed loop. In another embodiment, the grinding is performed in an open loop. The grinding can be performed in a batch mode. The grinding can be performed in a recirculating batch mode.
[0199] As mentioned above, the grinding circuit may include a pre-grinding step, wherein the coarse inorganic particles are ground to a predetermined particle size distribution in a grinding vessel, after which the cellulose-containing fibrous material is mixed with the pre-ground inorganic particulate material and further ground in the same or a different grinding vessel until the desired microfibrillation level is obtained.
[0200] Since the suspension of the material to be ground may have a relatively high viscosity, a suitable dispersant may be added to the suspension prior to grinding. The dispersant may be, for example, a water-soluble condensed phosphate, polysilicic acid or a salt thereof, or a polyelectrolyte, such as a water-soluble salt of poly(acrylic acid) or poly(methacrylic acid) having a number average molecular weight of not more than 80,000. The amount of dispersant used is generally in the range of 0.1 to 2.0 wt % based on the weight of the dry inorganic solid particulate material. The suspension may be ground at a temperature in the range of 4°C to 100°C.
[0201] Other additives that may be included in the microfibrillation step include: carboxymethyl cellulose, amphoteric carboxymethyl cellulose, oxidizing agents, 2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPO), TEMPO derivatives, and wood degrading enzymes.
[0202] The pH of the suspension of the material to be ground can be about 7 or greater than about 7 (i.e., alkaline), for example, the pH of the suspension can be about 8, or about 9, or about 10, or about 11. The pH of the suspension of the material to be ground can be less than about 7 (i.e., acidic), for example, the pH of the suspension can be about 6, or about 5, or about 4, or about 3. The pH of the suspension of the material to be ground can be adjusted by adding an appropriate amount of acid or base. Suitable bases include alkali metal hydroxides, such as NaOH. Other suitable bases are sodium carbonate and ammonia. Suitable acids include inorganic acids, such as hydrochloric acid and sulfuric acid, or organic acids. An exemplary acid is orthophosphoric acid.
[0203] The amounts of inorganic particulate material (if any) and cellulosic pulp in the mixture to be co-ground can be varied to produce a pulp suitable for use as a top ply or layer pulp, or it can be further modified, for example with the addition of other inorganic particulate material, to produce a pulp suitable for use as a top ply or layer pulp.
[0204] Homogenize
[0205] Can be under wet conditions, optionally, in the presence of inorganic particulate material, by wherein pressurizing the mixture of cellulose pulp and optional inorganic particulate material (for example, to a pressure of about 500 bar), then by the method of lower pressure zone to realize the microfibrillation of the fiber substrate containing cellulose. The speed of the mixture through the low pressure zone is high enough, and the pressure of the low pressure zone is low enough to cause the microfibrillation of cellulose fiber. For example, the pressure drop can be realized by forcing the mixture to pass through an annular opening, and the annular opening has a narrow inlet orifice and a much larger outlet orifice. When the mixture is accelerated to enter a larger volume (i.e., a lower pressure zone), the sharp drop in pressure causes cavitation, which leads to microfibrillation. In an embodiment, can be under wet conditions, optionally, in the presence of inorganic particulate material, realize the microfibrillation of the fiber substrate containing cellulose in a homogenizer. In the homogenizer, cellulose pulp and optional inorganic particulate material are pressurized (for example, to a pressure of about 500 bar), and are forced through a small nozzle or orifice. The mixture can be pressurized to a pressure of about 100 to about 1000 bar, for example, to a pressure equal to or greater than 300 bar, or equal to or greater than about 500 bar, or equal to or greater than about 200 bar, or equal to or greater than about 700 bar. Homogenization subjects the fibers to high shear forces so that when the pressurized cellulose pulp leaves the nozzle or orifice, cavitation causes the cellulose fibers in the pulp to be microfibrillated. Additional water can be added to improve the mobility of the suspension through the homogenizer. The resulting aqueous suspension comprising microfibrillated cellulose and optional inorganic particulate material can be fed back to the inlet of the homogenizer to pass through the homogenizer multiple times. When there is inorganic particulate material, and when the inorganic particulate material is a natural plate-like mineral, such as kaolin, homogenization not only promotes the microfibrillation of cellulose pulp, but also promotes the delamination of the plate-like particulate material.
[0206] An exemplary homogenizer is a Manton Gaulin (APV) homogenizer.
[0207] After the microfibrillation step is carried out, the aqueous suspension containing microfibrillated cellulose and optional inorganic particulate material can be sieved to remove fibers above a certain size and to remove any grinding media. For example, a sieve with a selected nominal aperture size can be used to screen the suspension to remove fibers that do not pass through the sieve. The nominal aperture size refers to the nominal center spacing of the opposite sides of the square aperture or the nominal diameter of the circular aperture. The sieve can be a BSS sieve (according to BS1796) with a nominal aperture of 150 μm, for example, a nominal aperture of 125 μm, or 106 μm, or 90 μm, or 74 μm, or 63 μm, or 53 μm, or 45 μm or 38 μm. In one embodiment, the BSS sieve with a nominal aperture of 125 μm is used to screen the aqueous suspension. The aqueous suspension can then be optionally dehydrated.
[0208] It will therefore be appreciated that the amount of microfibrillated cellulose (i.e., weight %) in the aqueous suspension after grinding or homogenization may be less than the amount of dry fibers in the pulp if the ground or homogenized suspension is treated to remove fibers above a selected size. The relative amounts of pulp and optional inorganic particulate material fed to the grinder or homogenizer may therefore be adjusted depending on the amount of microfibrillated cellulose desired in the aqueous suspension after removal of fibers above a selected size.
[0209] In some embodiments of aspects of the invention, microfibrillated cellulose can be prepared by a method comprising the step of microfibrillating a fibrous substrate comprising cellulose in an aqueous environment by grinding in the presence of a grinding medium (as described herein), wherein the grinding is performed in the absence of an inorganic particulate material. In some embodiments, an inorganic particulate material can be added after grinding to produce a top slurry or layer slurry.
[0210] Microfibrillation in the absence of grindable inorganic particulate material
[0211] In another aspect, microfibrillation of cellulose fibers can be performed in a process comprising microfibrillating a fibrous substrate comprising cellulose in an aqueous environment by grinding in the presence of grinding media, the grinding media being removed after the grinding is complete, wherein the grinding is performed in a tower mill or a screen mill (including a stirred media mill), and wherein the grinding is performed in the absence of grindable inorganic particulate material. Grindable inorganic particulate material is material that will be ground in the presence of grinding media.
[0212] The particulate grinding media may be natural or synthetic materials. The grinding media may, for example, include balls, beads or particles made of any hard mineral, ceramic or metallic material. Such materials may include, for example, aluminum oxide, zirconium oxide, zirconium silicate, aluminum silicate or a fumulite material produced by calcining kaolinite clay at a temperature in the range of about 1300° C. to about 1800° C. For example, in some embodiments, it is preferred Abrasive Media. Alternatively, natural sand particles of a suitable particle size may be used.
[0213] Generally, the type and particle size of the grinding media selected for use in the present invention can depend on the properties, for example, the particle size and chemical composition of the feed suspension of the material to be ground. Preferably, the particulate grinding media comprises particles having an average diameter in the range of about 0.5 mm to about 6 mm. In one embodiment, the average diameter of the particles is at least about 3 mm. In other embodiments, the average diameter range can be 6 mm to 15 mm.
[0214] The grinding media may include particles having a specific gravity of at least about 2.5. The grinding media may include particles having a specific gravity of at least about 3, or at least about 4, or at least about 5, or at least about 6.
[0215] The grinding media (or media) may be present in an amount up to about 70% of the charge volume. The grinding media may be present in an amount of at least about 10% of the charge volume, such as at least about 20% of the charge volume, or at least about 30% of the charge volume, or at least about 40% of the charge volume, or at least about 50% of the charge volume, or at least about 60% of the charge volume.
[0216] A fibrous substrate comprising cellulose can be microfibrillated in the presence of an inorganic particulate material to obtain a d 50 The fibrous substrate comprising cellulose may be microfibrillated in the presence of an inorganic particulate material to obtain microfibrillated cellulose having a size of about 5 μm to about 500 μm. 50 Microfibrillated cellulose of about 400 μm or less, for example, about 300 μm or less, or about 200 μm or less, or about 150 μm or less, or about 125 μm or less, or about 100 μm or less, or about 90 μm or less, or about 80 μm or less, or about 70 μm or less, or about 60 μm or less, or about 50 μm or less, or about 40 μm or less, or about 30 μm or less, or about 20 μm or less, or about 10 μm or less.
[0217] The fibrous substrate comprising cellulose may be microfibrillated to obtain microfibrillated cellulose having a modal fiber particle size of about 0.1 to 500 μm. The fibrous substrate comprising cellulose may be microfibrillated, when present, to obtain microfibrillated cellulose having a modal fiber particle size of at least about 0.5 μm, such as at least about 10 μm, or at least about 50 μm, or at least about 100 μm, or at least about 150 μm, or at least about 200 μm, or at least about 300 μm, or at least about 400 μm.
[0218] The fibrous substrate comprising cellulose may be microfibrillated in the presence of an inorganic particulate material to obtain microfibrillated cellulose having a fiber steepness equal to or greater than about 10 as measured by Malvern. The fiber steepness (i.e., the steepness of the fiber size distribution) is determined by the following formula:
[0219] Steepness = 100 × (d 30 / d 70 )
[0220] The fiber steepness of the microfibrillated cellulose may be equal to or less than about 100. The fiber steepness of the microfibrillated cellulose may be equal to or less than about 75, or equal to or less than about 50, or equal to or less than about 40, or equal to or less than about 30. The microfibrillated cellulose may have a fiber steepness of about 20 to about 50, or about 25 to about 40, or about 25 to about 35, or about 30 to about 40.
[0221] The particle size distribution can be calculated using Mie theory and gives an output value as a differential volume distribution.
[0222] When three minerals are present, the presence of two distinct peaks can be explained as coming from the groups of minerals (the finer peak) and fibers (the coarser peak).
[0223] The finer mineral peak can be fitted to the measured data points and mathematically subtracted from the distribution to leave the fiber peak, which can then be converted to a cumulative distribution. Similarly, the fiber peak can be mathematically subtracted from the original distribution to leave the mineral peak, which can then also be converted to a cumulative distribution. Both cumulative curves can then be used to calculate the average particle size (d 50 ) and distribution steepness (d 30 / d 70 ×100). The differential curve can be used to find the modal grain size of both the mineral and fiber fractions.
[0224] When the process does not include grinding the fibrous substrate comprising cellulose in the presence of an inorganic particulate material, the particle size distribution of the microfibrillated cellulose can be calculated by Mie theory and output as a differential volume distribution.
[0225] In one embodiment, the grinding vessel is a tower mill. In another embodiment, the grinding is carried out in a screen mill, preferably a stirred media pulverizer. The screen mill can include one or more screens with a nominal aperture of at least about 250 μm, for example, one or more screens can have a nominal aperture of at least about 300 μm, or at least about 350 μm, or at least about 400 μm, or at least about 450 μm, or at least about 500 μm, or at least about 550 μm, or at least about 600 μm, or at least about 650 μm, or at least about 700 μm, or at least about 750 μm, or at least about 800 μm, or at least about 850 μm, or at least about 900 μm, or at least about 1000 μm, or at least 1250 μm or 1500 μm. The screen sizes just mentioned above also apply to the use of the tower mill embodiment.
[0226] As described above, grinding is performed in the presence of a grinding medium. In embodiments, the grinding medium is a coarse medium comprising particles having an average diameter in the range of about 1 mm to about 6 mm, such as about 2 mm, or about 3 mm, or about 4 mm, or about 5 mm.
[0227] In another embodiment, the specific gravity of the grinding media is at least about 2.5, e.g., at least about 3, or at least about 3.5, or at least about 4.0, or at least about 4.5, or at least about 5.0, or at least about 5.5, or at least about 6.0.
[0228] As described above, the amount of grinding media (or media) can be up to about 70% of the charge volume. The grinding media can be present in an amount of at least about 10% of the charge volume, such as at least about 20% of the charge volume, or at least about 30% of the charge volume, or at least about 40% of the charge volume, or at least about 50% of the charge volume, or at least about 60% of the charge volume.
[0229] In one embodiment, the amount of grinding media present is about 50% of the charge volume. "Charge" refers to the composition delivered to the grinder container as a feed. Charge includes water, grinding media, cellulose-containing fiber substrate and any other optional additives (except as described herein). Using relatively rough and / or dense media has the advantages of improving deposition rate (i.e. faster) and reducing media carrying through the static zone and / or classifier and / or screen. Another advantage of using a relatively coarse screen is that relatively coarse or dense grinding media can be used in the microfibrillation step. In addition, using a relatively coarse screen (i.e., having a nominal aperture of at least about 250 μm) allows the product of relatively high solid content to be processed and removed from the grinder, which allows the feed (including fiber substrate, which includes cellulose and inorganic particulate material) of relatively high solid content to be processed with an economically feasible process. As described below, it has been found that, with respect to energy efficiency, it is desirable to have a feed with high initial solid content. In addition, it is also found that the product produced (at a given energy) at a lower solid content has a coarser particle size distribution.
[0230] According to one embodiment, the fibrous substrate comprising cellulose is present in the aqueous environment at an initial solid content of at least about 1% by weight. The fibrous substrate comprising cellulose may be present in the aqueous environment at an initial solid content of at least about 0.25% by weight, or at least about 0.5% by weight, or at least about 1.5% by weight, or at least about 2% by weight, or for example at least about 3% by weight or at least about 4% by weight. Typically, the initial solid content does not exceed about 10% by weight.
[0231] In another embodiment, grinding is carried out in a cascade of grinding containers, wherein one or more grinding containers may comprise one or more grinding zones. For example, a cellulose-containing fiber substrate may be ground in a cascade of two or more grinding containers, such as a cascade of three or more grinding containers, or a cascade of four or more grinding containers, or a cascade of five or more grinding containers, or a cascade of six or more grinding containers, or a cascade of seven or more grinding containers, or a cascade of eight or more grinding containers, or a cascade of nine or more grinding containers in series, or a cascade comprising up to ten grinding containers. The cascade of grinding containers may be operably connected in series or in parallel or in a combination of series and parallel. The output and / or input of one or more grinding containers in the cascade may be subjected to one or more screening steps and / or one or more classification steps.
[0232] The total energy consumed in the microfibrillation process may be distributed equally among each of the grinding containers in the cascade. Alternatively, the energy input may be varied between some or all of the grinding containers in the cascade.
[0233] A person skilled in the art will appreciate that the energy consumed per container may vary between containers in a cascade, depending on the amount of fibrous substrate being microfibrillated in each container, and optionally the speed of grinding in each container, the duration of grinding in each container and the type of grinding media in each container. In order to control the particle size distribution of the microfibrillated cellulose, the grinding conditions may be varied in each container of the cascade.
[0234] In an embodiment, the grinding is performed in a closed circuit. In another embodiment, the grinding is performed in an open circuit.
[0235] Since the suspension of the material to be ground may have a relatively high viscosity, a suitable dispersant may optionally be added to the suspension prior to grinding. The dispersant may be, for example, a water-soluble condensed phosphate, polysilicic acid or a salt thereof, or a polyelectrolyte, such as a water-soluble salt of poly(acrylic acid) or poly(methacrylic acid) having a number average molecular weight of not more than 80,000. The amount of dispersant is typically in the range of 0.1 to 2.0 wt % based on the weight of the dry inorganic solid particulate material. The suspension may be suitably ground at a temperature in the range of 4° C. to 100° C.
[0236] Other additives that may be included in the microfibrillation step include: carboxymethyl cellulose, amphoteric carboxymethyl cellulose, oxidizing agents, 2,2,6,6-tetramethylpiperidin-1-oxyl (TEMPO), TEMPO derivatives, and wood degrading enzymes.
[0237] The pH of the suspension of the material to be ground can be about 7 or greater than about 7 (i.e., alkaline), for example, the pH of the suspension can be about 8, or about 9, or about 10, or about 11. The pH of the suspension of the material to be ground can be less than about 7 (i.e., acidic), for example, the pH of the suspension can be about 6, or about 5, or about 4, or about 3. The pH of the suspension of the material to be ground can be adjusted by adding an appropriate amount of acid or base. Suitable bases include alkali metal hydroxides, such as NaOH. Other suitable bases are sodium carbonate and ammonia. Suitable acids include inorganic acids, such as hydrochloric acid and sulfuric acid, or organic acids. An exemplary acid is orthophosphoric acid.
[0238] The total energy input during a typical milling process to obtain the desired aqueous suspension composition may generally be in the range of about 100 to 1500 kWht based on the total dry weight of the inorganic particulate filler. -1 The total energy input can be less than about 1000 kWht -1 , for example, less than about 800 kWht -1 , less than about 600kWht -1 , less than about 500kWht -1 , less than about 400kWht -1 , less than about 300kWht -1 , or less than about 200kWht -1 .
[0239] When co-grinded in the presence of inorganic particulate material, cellulose pulp can be microfibrillated at relatively low energy input. The total energy input per metric ton of dry fiber in the fibrous substrate comprising cellulose will be less than about 10,000 kWht -1 , for example less than about 9000 kWht -1 , or less than about 8000kWht -1 , or less than about 7000kWht -1 , or less than about 6000kWht -1 , or less than about 5000kWht -1 , for example less than about 4000 kWht -1 , less than about 3000kWht -1 , less than about 2000kWht -1 , less than about 1500kWht -1 , less than about 1200kWht -1 , less than about 1000kWht -1 or less than about 800kWht -1 The total energy input varies depending on the amount of dry fibers in the fiber substrate to be microfibrillated and, optionally, the grinding speed and grinding duration.
[0240] Wet molding process for 3D formable objects comprising pulp and macrofibrillated and microfibrillated cellulose
[0241] Various wet pulp molding methods are known in the prior art. They usually start with a porous mold. In the simplest process (usually called thick wall molding), when a sufficient amount of solids has been deposited, the mold is removed from the pulp and coarse fibrillated microfibrillated cellulose suspension (optionally containing one or more inorganic particulate materials) and then discharged from the mold (usually with compressed air) onto a conveyor belt, which then transports the molded pulp and coarse fibrillated microfibrillated cellulose (and optional inorganic particulate material) to an oven for drying.
[0242] In transfer molding, after the object is removed from the mold, it is transferred to a second, oppositely shaped mold (which is not porous but has some venting holes to apply vacuum or compressed air). The second mold delivers the object to a conveyor, where it is then discharged onto a conveyor for transport to a drying oven.
[0243] The third production method is thermoforming. In thermoforming, the object is heated and dried while it is held between a second mold and a third mold (the same shape as the first porous mold, but mostly solid, with vent holes for steam to escape). Thus, in thermoforming, there are no conveyors or ovens.
[0244] Therefore, wet molded pulp products are usually made by a process that uses two main steps. These steps include forming the pulp mixture into the desired shape (usually by applying a vacuum) and then drying the pulp to remove water.
[0245] When forming the three-dimensional article, water is usually removed by vacuum until the total solids content of the formed product is in the range of 40% to 55%. The remaining water is then removed in a drying step. Thus, after the drying step, the three-dimensional molded article typically contains 4% to 8% water, which roughly corresponds to the water vapor content of paper under humidity conditions typically suitable for storing paper products.
[0246] The tool design of the three-dimensional molded article is determined by its intended geometry and surface characteristics, for example, a smooth surface may exist on the inner or outer surface. Therefore, the mold is designed to produce the intended geometry of the three-dimensional product and to produce the desired finish of the inner and outer surfaces of the three-dimensional molded pulp product. In a preferred embodiment of the manufacturing apparatus of a three-dimensional molded pulp product comprising coarse fibrillated microfibrillated cellulose (and optional inorganic particulate material), the process includes providing a porous mold having a three-dimensional shape, the mold comprising a forming part having an inner and outer part; contacting the forming part with an aqueous pulp and coarse fibrillated microfibrillated cellulose suspension and optional inorganic particulate material; applying a vacuum to the inner part of the forming part to form a wet layer of cellulose fibers and coarse fibrillated microfibrillated cellulose on the outer part of the forming part, thereby forming a three-dimensional molded object.
[0247] The aqueous pulp and coarse fibrillated microfibrillated cellulose suspension comprises about 0.5 wt. % to about 50 wt. % coarse fibrillated microfibrillated cellulose.
[0248] In the case of wet molded pulp products, the total solids content of the aqueous composition comprising pulp and coarse fibrillated microfibrillated cellulose is generally in the range of about 0.05 wt% to about 10 wt%.
[0249] The pulp layer present on the forming mold in the thermoforming process can be press dried at a pressure of 0.2 to 50 bar, preferably 0.5 to 15 bar, more preferably 1 to 10 bar. The three-dimensional molded pulp product can be produced in the range of 100 to 2,000 grams per square meter ("gsm").
[0250] Drying of the pulp present on the forming mould may be achieved by applying elevated temperatures, typically in the range of about 100 to 350°C, preferably 120 to 250°C, more preferably 150 to 220°C.
[0251] Dry molding process for 3-D formable objects comprising pulp and macrofibrillated and microfibrillated cellulose
[0252] An alternative manufacturing process for producing 3-D formable pulp molded articles is a dry forming process using a cellulose blank. In the present invention, the cellulose blank is formed from pulp and coarse fibrillated microfibrillated cellulose (and optionally inorganic particulate material), and the cellulose blank is conveyed into a forming mold, wherein the blank is heated to a forming temperature of about 100° C. to 200° C., wherein the blank is pressed at a forming pressure of at least 1 MPa and in the range of 1 MPa to about 100 MPa, depending on the article to be formed.
[0253] The cellulose blank containing cellulose fibers is manufactured by a process in which the cellulose fibers (and optional inorganic particulate material) are air laid or air formed to form the cellulose blank. When the cellulose blank is formed in an air laid or air formed process, the cellulose fibers are carried by air as a carrying medium and formed into a blank structure.
[0254] Aqueous adhesives can be applied to air-formed blanks. This will include applying a coarse fibrillated MFC suspension in this way. Coarse fibrillated MFC suspensions can be applied to the blank in a manner such as an additive, such as latex or AKD. Therefore, coarse fibrillated microfibrillated cellulose suspensions, as well as AKD and latex suspensions, can be sprayed onto the surface of the blank before pressing the air-formed blank. Therefore, the sprayed suspension forms a coating on the object after molding. Alternatively, coarse fibrillated MFC suspensions can be sprayed onto the fibers before the fibers are air-laid into the blank. This will help to bond the fibers together, thereby increasing the strength of the pressed object and reducing its porosity.
[0255] This differs from the above-mentioned wet molding process similar to the papermaking process in which water is used as a supporting medium for the cellulose fibers when forming the paper structure.
[0256] In the air laying or air forming process, water and / or other additives, including a suspension of coarse fibrillated cellulose, can be added, for example by spraying other additives, including coarse fibrillated MFC, into the cellulose-containing pulp fibers to change the properties of the cellulose blank, but air is still used as the carrying medium in the forming process.
[0257] The advantage of the dry molding process is that, when heated and pressed, 3-D moldable pulp and coarse fibrillated microfibrillated cellulose (and optional inorganic particulate material) produce 3-D objects with good material properties. Higher forming temperatures lead to increased fibril aggregation, water resistance, Young's modulus and mechanical properties of the final cellulose product. High pressure increases fibril aggregation, thereby giving improved mechanical properties to the 3-D formed products formed from cellulose-containing pulp fibers and coarse fibrillated microfibrillated cellulose. The 2-D cellulose blank of the process is formed into a 3-D shaped product by a forming process.
[0258] In an embodiment of the dry forming process, a sizing agent is applied to the cellulose fibers of the pulp and the fibrils of the coarse fibrillated microfibrillated cellulose (and optional inorganic particulate material) to increase the hydrophobicity and / or mechanical strength of the cellulose blank. Different types of sizing agents can be used to increase the hydrophobicity and / or mechanical strength of the cellulose product produced by the cellulose blank, depending on the type of product produced. For example, the sizing agent can be a fluorinated compound, an alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), rosin (acid sizing), wax, lignin and water glass (sodium silicate). The sizing agent or other substances are applied to the cellulose fibers by an application unit, such as a nozzle or a similar device.
[0259] In an embodiment, the cellulose blank is formed into a continuous cellulose web in a drying forming unit. The continuous cellulose web can then be used in a continuous manufacturing process, wherein the continuous cellulose web is dry-formed from cellulose fibers in a drying forming unit and then transported to a forming die. In another embodiment, the cellulose web can be intermittently fed into the forming die.
[0260] The three-dimensional objects formed by the above dry molding process can be hollow bowls, cups and bottles with uniform wall thickness. In various embodiments, the three-dimensional objects are not hollow and can have different thicknesses and shapes.
[0261] The dry-laid process may use cellulose blanks in the form of rolled webs or stacked sheets.The cellulose fibres and coarse-fibrillated microfibrillated cellulose (and optionally inorganic particulate material) may be pressed or calendered in a pressing unit with calender rolls, which may be heated in other embodiments of the process.
[0262] An alternative method for producing a cellulose blank comprising coarse fibrillated microfibrillated cellulose (and optional inorganic particulate material) is to produce a nonwoven material, such as described in WO2017182877, which is incorporated herein by reference in its entirety. In this method, fibers comprising coarse fibrillated cellulose (and optional inorganic particulate material) are prepared by grinding a fibrous substrate comprising cellulose in a grinding container in the presence of an inorganic particulate material, wherein the grinding is performed in an aqueous environment in the presence or absence of a grinding medium; wherein the term "grinding medium" refers to a medium other than an inorganic particulate material, and wherein the size of the grinding medium is 0.5 mm or greater; the microfibrillated cellulose (and optional inorganic particulate material) is then extruded through an extruder; the extruded microfibrillated cellulose (and optional inorganic particulate material) is subjected to a decaying treatment with an attenuating gas; and (4) the extruded fibers are collected on a porous surface to form a nonwoven fabric. The porous surface is a moving screen or mesh. The nonwoven fabric is then bonded by hydroentangling or through air thermal bonding, or the nonwoven fabric is mechanically bonded.
[0263] Example
[0264] Flat sheets of MFC or blends of MFC with inorganic particulate material composites and kraft pulp are made in a simple vacuum-assisted hand sheet former. After the wet sheet is formed, blotter is applied and the sheet is transferred to a fast Kothen dryer, pressurized and heated until dry. After conditioning at 23°C and 50%RH, the grammage, thickness (Caliper), tensile stiffness and Bendtsen porosity (air permeability) of the test sheet are tested. The tensile stiffness is calculated by dividing the gradient of the force / extension curve by the width of the sample, and the tensile stiffness index is calculated by dividing the tensile stiffness by the grammage. The grammage required for the tensile stiffness of 1000N / m to meet any target is calculated by the tensile stiffness index of each sample. Assuming that three-dimensional wall-made objects with the same tensile stiffness will have the same stiffness, the increase in the tensile stiffness index will allow the weight of the object to be reduced while maintaining stiffness. The Bentsen porosity at this gram weight is estimated according to Darcy's law, which states that the flow rate of fluid at a fixed pressure drop through a constant permeability material is inversely proportional to its thickness. Therefore, the Bentsen porosity (air flow rate per unit cross-sectional area of the sample) is estimated by multiplying the measured Bentsen porosity value (in ml / min) by the ratio of the measured gram weight to the required gram weight. Oil resistance is measured using a test kit (TAPPI T559), which consists of a series of 16 numbered solutions made from a mixture of castor oil, toluene and n-heptane, where solution 1 is pure castor oil and solution 16 is pure heptane. Each solution is dripped onto the sheet and wiped off after 15 seconds. If a stain is observed, the test is considered to have failed. The kit grade of the sample represents the highest solution number that passed the test; if even solution 1 leaves a stain, the kit grade is zero.
[0265] The MFC was prepared by grinding bleached softwood kraft pulp in a stirred media mill as described above in the specification. The inorganic particulate material used, if present, was Intracarb 60 available from Imerys Minerals Limited (Cornwall, UK).
[0266] Example 1: MFC / softwood pulp flat sheet
[0267] Sheets were made using the above procedure using different combinations of unrefined softwood kraft pulp and MFC. The tensile stiffness index of the sheets increased significantly with increasing MFC content. The grammage required to achieve a target tensile stiffness of 1000 N / m was calculated from the measured values for each sheet, showing that the weight of the pallet could be reduced by almost 50% using only 17% MFC. In addition, the porosity of such a pallet would be reduced by nearly two orders of magnitude. At 50% MFC, the weight was reduced by almost 2 / 3 and the sheets had the highest oil resistance measurable with standard tests. Table 1 shows the properties of the produced sheets.
[0268] Table 1: Properties of dry sheets made from blends of unrefined bleached softwood kraft pulp and MFC% MFC
[0269]
[0270] Example 2: Wet tensile properties of flat sheets
[0271] The tensile properties of the sheets were also measured after pressing but before drying. After forming, the sheets were laid flat and then pressed in a tablet press according to TAPPI T205. The solids content was controlled by the number of blotters used in the tablet press (1 or 4), with two different options targeting approximately 30% and 40% solids. The wet sheets were weighed, then carefully cut into strips and fixed in a tensiometer for measuring tensile strength and elongation. For each sheet, the solids content and grammage were determined from the wet and dry weights of the sheet trim.
[0272] Although the sheets containing MFC have a higher moisture content after pressing, the tensile elongation at break and strength increase significantly with increasing MFC content. This increased ductility greatly improves the performance during thermoforming, allowing lighter objects or deeper shapes to be easily pressed without damage. Tables 2 and 3 show the tensile properties of the wet sheets under two corresponding pressing conditions.
[0273] Table 2: Wet tensile properties of sheets pressed with a single blotting paper
[0274]
[0275] Table 3: Wet tensile properties of sheets pressed with 4 sheets of blotting paper
[0276]
[0277] Example 3: MFC / cork pulp molded pallet
[0278] Moulded trays were manufactured on a pilot moulding machine at the Bangor Biocomposites Centre. Similar blends of softwood kraft pulp and MFC were used for flat sheets. After forming, the trays were cut and the properties of the tray walls were assessed in the same way as for the flat sheets. It should be noted that the pressing and drying conditions for the moulded trays were very different, but the conclusions were similar; using MFC, the weight of a tray for a given stiffness can be almost halved, which will result in a reduction in porosity of several orders of magnitude. Despite a reduction in tray weight of over 50% at 25% MFC, all trays formed well without defects. Table 4 shows the properties of strips cut from the trays.
[0279] Table 4: Properties of strips cut from pallets made from bleached kraft pulp and MFC
[0280]
[0281] Example 4: Flat sheet of co-ground MFC / CaCO3 and pulp
[0282] Sheets were made using the above procedure using different combinations of unrefined softwood kraft pulp and 50 / 50 MFC / CaCO3 composite.
[0283] With the same amount of calcium carbonate added as MFC, the tensile properties still improve and the porosity decreases. The weight reduction for the target object stiffness is still possible and the introduction of the mineral filler reduces the raw material cost of the product. Table 5 shows the properties of the sheet.
[0284] Table 5: Properties of sheets made from bleached kraft pulp and 50 / 50 MFC / CaCO3 blend
[0285]
[0286]
[0287] Example 5: Moulded trays of co-ground MFC / CaCO3 and pulp
[0288] Molded pallets were made as described in Example 3, this time using a mixture of unrefined bleached softwood kraft pulp and a 50 / 50 co-grinded composite of MFC / CaCO3. Again, all pallets were formed without defects and cut into strips for testing after drying. Table 6 shows the properties of the strips cut from the pallets.
[0289] Table 6: Properties of strips cut from pallets made from bleached kraft pulp and 50 / 50 MFC / CaCO3 blend
[0290]
[0291] Example 6: Flat sheets of microfibrillated cellulose with different pulp types
[0292] Microfibrillated cellulose products were prepared by grinding different types of pulp in the manner described in this specification to obtain different MFC properties and mixed with the unrefined softwood kraft pulp of the above examples.
[0293] MFC A was made from northern softwood bleached kraft pulp (Botnia RMA, Metsa) which is a mixture of approximately 50% pine and 50% spruce. MFC B was made from northern hardwood (birch) bleached kraft pulp (Sodra Gold) and MFC C was made from bleached acacia kraft pulp.
[0294] Each product was analysed using a Valmet Fibre Analyser as described in the specification and examples giving the results shown in Table 7a.
[0295] Table 7(a): Analysis of MFC products using Valmet fiber analyzer
[0296]
[0297]
[0298] Figure 7(b): Malvern particle size and fiber steepness data
[0299]
[0300] Fines A is a measure of fine fibers and fragments that are not highly fibrillated, and Fines B is a measure of highly fibrillated fragments. Fines A are low aspect ratio fibers and fragments less than 200μm in length. Fines B are fibrillated fragments greater than 200μm in length but less than 10μm in width. MFC made from northern softwood has longer fibers and higher levels of fines B while maintaining high fibrillation and low overall levels of fines. This is beneficial because the impact of the MFC on sheet drainage is limited. In contrast, the MFC made from birch in this case has a high degree of fiberization, resulting in a product with high strength potential but a significantly greater adverse impact on drainage rate.
[0301] The sheets were made from blends of unrefined softwood kraft paper and the MFC products shown in Table 7. In addition, to be able to predict drainage times for different sheet weights, the drainage rates of the blends were measured and the permeability of wet sheets made from the blends was calculated accordingly using Darcy's law. The results are reported in Table 8.
[0302] Table 8: Properties of sheets made from blends of unrefined softwood pulp and MFC products made from different sources
[0303]
[0304]
[0305] Table 8 shows the properties of the sheets produced. It should be noted that those sheets produced from northern softwoods were selected from Table 1 to be in the 200-250 gsm range or as close to that range as possible. It is noteworthy that although the stiffness was highest for the finer MFC made from birch, at lower MFC levels the tensile stiffness index for the coarser MFC from northern softwood developed more rapidly than for either of the other products. The coarser MFC also drained faster and therefore provided a better combination of properties than the finer MFC. This was Figure 2 , which shows the calculated grammage required for 100 N / m tensile stiffness for each blend, plotted against that grammage and the calculated drainage time for the blend. For blends up to 50% MFC, the coarser material achieves any given grammage reduction at lower MFC content and significantly shorter drainage times.
[0306] Example 7: Particle size distribution measured by Malvern Insitec laser scattering apparatus
[0307] Ensure that the MFC slurry is homogeneous by shaking the container contents vigorously. If grinding media is present in the sample, remove it using an 850μm screen before proceeding with the Malvern analysis. If grinding media is not present, pipette the slurry from the sample. Turn on the Malvern Insitec unit and start the pump by pressing the pump speed switch button on the top of the Malvern unit. Set the speed to 2500rpm and turn off the ultrasonics. Rinse the Malvern Insitec 2 to 3 times with clean water at room temperature ±5°C to ensure the unit is clean. Raise the stirrer to the marked discharge position and remove the outlet hose to draw solution from the system, making sure to lift the inlet hose to drain any trapped solution. Replace the water with clean tap water at room temperature ±5°C (800ml to 900ml). Press the Malvern stirrer fully and the pump will start automatically. If the water is very turbulent, turn the pump off and then back on again to help the water settle. Raise the outlet hose to expel any trapped air.
[0308] Example 8
[0309] The molded fiber trays were formed on a Nature Former KPT Lab Unit 3.1 machine. The furnish consisted of 70:30 hardwood (birch) to softwood (pine / spruce unbleached kraft), different dosages of eucalyptus based fiber MFC and 1% sizing agent (AKD).
[0310] The mould was dipped into the tank containing the furnish and the drainage time was adjusted according to the desired final article weight. Chamber vacuum was used at -0.5 bar. The samples were pressed with 9500 N (cold press) for 10 seconds and then dried using a hot press at 11000 N and 240°C. Due to the different basis weights, the drying time was adjusted for each test point. The article was dried until it was dry / warm to the touch. The pulp was unrefined and had a Schober freeness of 18.
[0311] The trays were conditioned in a paper testing laboratory at 23°C and 50% RH and then weighed. A tray was then selected from each test point and cut for testing. The substrates of the objects were tested for tear, porosity, Scott Bond, and tensile testing. The trays were cut using a scalpel and guillotine.
[0312] Table 9: Tear index results for molded objects with different basis weights and MFC contents
[0313]
[0314] Table 10: Bendtsen porosity results for molded objects of varying basis weight and MFC content.
[0315]
[0316] Table 11: Scott internal bond strength of molded objects with different basis weights and MFC contents
[0317]
[0318] Table 12: Tensile index results for molded objects of varying basis weight and MFC content
[0319]
[0320]
[0321] Table 13: Malvern Insitec data for eucalyptus based MFC added to moulded objects
[0322]
[0323] Table 14: Valmet Fiber Image Analyzer data for eucalyptus based MFC added to molded objects
[0324]
[0325] Example 10
[0326] Many attempts were made to form moulded fibre objects with MFC contents > 50%, but all failed because the MFC / pulp furnish would not remain on the forming mould. It was therefore not possible to test any moulded fibre objects with > 50% MFC contents.
[0327] The foregoing embodiments and advantages are merely exemplary and should not be construed as limiting the present disclosure. In addition, the description of the embodiments of the present invention is intended to be illustrative and not to limit the scope of the claims. Many substitutions, modifications and variations are apparent to those skilled in the art.
[0328] It should be understood that although the invention has been described in conjunction with the detailed description thereof, the foregoing description is intended to illustrate and not limit the scope of the invention, which is defined by the scope of the appended claims. Other aspects, advantages and modifications are within the scope of the following claims.
[0329] The various embodiments described in this specification can be combined to provide further embodiments. Aspects of the embodiments can be modified, if necessary, to employ the concepts of various patents, applications and publications to provide yet other embodiments.
[0330] The disclosures of each patent, patent application, publication, and registration number cited herein are incorporated by reference in their entirety.
[0331] Although the present invention has been disclosed with reference to various embodiments, it is apparent that other skilled in the art may design other embodiments and variations without departing from the true spirit and scope of the present invention. The appended claims are intended to be interpreted as including all such embodiments and equivalent variations. Generally, in the following claims, the terms used should not be interpreted as limiting the claims to the specific embodiments disclosed in the specification and claims, but should be interpreted as including all possible embodiments and the full range of equivalents to which such claims are granted. Therefore, the claims are not limited by the disclosure.
[0332] The foregoing written description is sufficient to enable those skilled in the art to implement these embodiments. The foregoing description and examples describe some embodiments in detail and describe the best mode contemplated by the inventor. However, it should be understood that no matter how detailed the above content is presented in text, the embodiments can be implemented in many ways and should be interpreted according to the attached claims and any equivalents thereof.
[0333] References discussed in this application are all incorporated by reference in their entirety for the purposes for which they are intended, as is clear from their context.
Claims
1. A three-dimensional molded object comprising a mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt. % to about 50 wt. % on a dry weight basis of the total dry mass of the mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; wherein the coarse microfibrillated cellulose comprises less than about 90 wt. % fines and / or less than 75 % fines A as measured by a Valmet Fiber Image Analyzer and has a length-weighted median length Lc(w) greater than 0.3 mm, and wherein the coarse fibrillated microfibrillated cellulose optionally has a fiber steepness of about 20 to about 50 as measured by a Malvern Mastersizer. 2 . The three-dimensional molded object according to claim 1 , wherein the coarse fibrillated microfibrillated cellulose has a fiber steepness of about 20 to about 50. 3 .
3. The molded object according to claim 1, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 25 wt%.
4. The molded object according to claim 1, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 15 wt%.
5. The molded object according to claim 1, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 10 wt%.
6. The molded object according to claim 1, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 5 wt%.
7. The molded object according to claim 1, wherein the coarse fibrillated microfibrillated cellulose is obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste stream, waste from paper mills and combinations thereof.
8. The molded object according to claim 1, wherein the coarse fibrillated microfibrillated cellulose is obtained from recycled pulp, broke pulp, paper mill waste stream, waste from paper mills and combinations thereof.
9. The molded object according to claim 1, wherein the cellulosic fibers are obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills, and combinations thereof.
10. The molded object according to claim 1, wherein the cellulose fibers are obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste stream, waste from paper mills, and combinations thereof.
11. The molded object according to claim 1, wherein both the cellulose fibers and the microfibrillated cellulose are obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills, and combinations thereof.
12. The molded object of claim 1, wherein the molded object comprises one or more inorganic particulate materials.
13. The molded object of claim 1, wherein the one or more inorganic particulate materials are calcium carbonate or kaolin or a mixture thereof.
14. The molded object of claim 1, wherein the one or more inorganic particulate materials comprise platy minerals, kaolin, and / or talc.
15. The molded object according to claim 13, wherein the calcium carbonate is ground calcium carbonate, precipitated calcium carbonate or a mixture thereof.
16. The molded object according to claim 13, wherein the calcium carbonate is precipitated calcium carbonate.
17. The molded object according to claim 13, wherein the calcium carbonate is ground calcium carbonate.
18. The molded object according to claim 17, wherein the ground calcium carbonate is marble, chalk, limestone and mixtures thereof.
19. The molded object according to claim 12, wherein the inorganic particulate material is ground calcium carbonate and precipitated calcium carbonate.
20. The molded object of claim 12, wherein the inorganic particulate material is selected from the group consisting of alkaline earth metal carbonates or sulfates, calcium carbonate, magnesium carbonate, dolomite, gypsum, bentonite, hydrous kandite clay, kaolin, halloysite, ball clay, anhydrous (calcined) kandite clay, metakaolin, fully calcined kaolin, talc, mica, perlite, sepiolite, calcite, diatomaceous earth, magnesite, silicates, diatomaceous earth, brucite, aluminum trihydrate, and combinations thereof.
21. A method for producing a three-dimensional molded object comprising cellulose fibers and coarse-fibrillated microfibrillated cellulose, the method comprising the following steps: A mixture comprising cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials is provided, wherein the mixture comprises about 0.5 wt. % to about 50 wt. % microfibrillated cellulose on a dry weight basis of the total dry mass of the mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; wherein the coarse microfibrillated cellulose comprises less than about 90 wt. % fines and / or less than 75 % fines A as measured by a Valmet Fiber Image Analyzer and has a length weighted median length Lc(w) greater than 0.3 mm, and wherein the coarse fibrillated microfibrillated cellulose optionally has a fiber steepness of about 20 to about 50 as measured by a Malvern Mastersizer; forming a three-dimensional molded object from the mixture; and The three-dimensional molded object is dried.
22. The method of claim 21, wherein the coarse fibrillated microfibrillated cellulose has a fiber steepness of about 20 to about 50.
23. The method of claim 21, wherein the step of forming is a wet forming step.
24. The method of claim 21, wherein the step of forming is a dry forming step.
25. The method according to claim 21, further comprising the steps of: providing a porous mold having a three-dimensional shape, the mold comprising a shaped portion, the shaped portion having an inner portion and an outer portion; contacting said forming part with said mixture comprising cellulose fibres and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; applying a vacuum to the inner portion of the forming section to form a wet layer of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials in the outer portion of the forming section to form a three-dimensional molded object, wherein the wet layer of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials is about 100 to 5,000 gsm on a dry weight basis of the total dry mass of the mixture of cellulose fibers and coarse fibrillated microfibrillated cellulose and optionally one or more inorganic particulate materials; The molded object is transferred to a drying conveyor and the three-dimensional molded object is dried; optionally, the three-dimensional molded object is transferred to a second reverse forming mold and the three-dimensional molded object is pressed before oven drying.
26. The method according to any one of claims 21 to 25, wherein the cellulose fibers are obtained from virgin pulp, recycled paper or old corrugated cardboard or a combination thereof.
27. The method according to any one of claims 21 to 25, wherein the cellulose fibers are obtained from virgin pulp.
28. The method according to any one of claims 21 to 25, wherein the cellulose fibers are obtained from recycled pulp.
29. The method according to claim 28, wherein the recycled pulp is obtained from old corrugated cardboard.
30. The method of any one of claims 21 to 25, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 25 wt%.
31. The method of any one of claims 21 to 25, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 15 wt%.
32. The method of any one of claims 21 to 25, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 10 wt%.
33. The method of any one of claims 21 to 25, wherein the coarse fibrillated microfibrillated cellulose is present in an amount of about 0.5 wt% to about 5 wt%.
34. The method according to any one of claims 21 to 25, wherein the coarse fibrillated microfibrillated cellulose is obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
35. The method according to any one of claims 21 to 25, wherein the coarse fibrillated microfibrillated cellulose is obtained from a pulp selected from the group consisting of recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
36. The method according to any one of claims 21 to 25, wherein the cellulosic fibers are obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills, and combinations thereof.
37. The method according to any one of claims 21 to 25, wherein the cellulose fibers are obtained from a pulp selected from the group consisting of chemical pulp, chemithermomechanical pulp, mechanical pulp, thermomechanical pulp, recycled pulp, broke pulp, paper mill waste streams, waste from paper mills, and combinations thereof.
38. The method according to any one of claims 21 to 25, wherein both the cellulose fibres and the coarse fibrillated microfibrillated cellulose are obtained from recycled pulp, broke pulp, paper mill waste streams, waste from paper mills and combinations thereof.
39. A method according to any one of claims 21 to 25, wherein the moulded object comprises one or more inorganic particulate materials.
40. The method of claim 39, wherein the one or more inorganic particulate materials is calcium carbonate or kaolin or a mixture thereof.
41. The method of claim 39, wherein the one or more inorganic particulate materials comprise platy minerals, kaolin, and / or talc.
42. The method of claim 40, wherein the calcium carbonate is ground calcium carbonate, precipitated calcium carbonate, or a mixture thereof.
43. The method of claim 40, wherein the calcium carbonate is precipitated calcium carbonate.
44. The method of claim 40, wherein the calcium carbonate is ground calcium carbonate.
45. The method of claim 44, wherein the ground calcium carbonate is marble, chalk, limestone, and mixtures thereof.
46. The method of claim 39, wherein the inorganic particulate material is ground calcium carbonate and precipitated calcium carbonate.
47. The method of claim 39, wherein the inorganic particulate material is selected from the group consisting of alkaline earth carbonates or sulfates, calcium carbonate, magnesium carbonate, dolomite, gypsum, bentonite, hydrous kandite clay, kaolin, halloysite, ball clay, anhydrous calcined kandite clay, metakaolin, fully calcined kaolin, talc, mica, perlite, sepiolite, calcite, diatomaceous earth, magnesite, silicates, diatomaceous earth, brucite, aluminum trihydrate, and combinations thereof.
48. A three-dimensional packaging container, blister pack, egg box, bottle, container or food tray comprising the three-dimensional article according to any one of claims 1 to 20.
49. A three-dimensional packaging container, blister pack, egg box, bottle, container or food tray obtainable by the method according to any one of claims 21 to 47.
50. Use of a three-dimensional article obtained by the method according to any one of claims 21 to 47 as a blister pack, egg box, bottle, container or food tray.