Surface layer, optical member, glasses, and material for forming surface layer
By using the combination of components A and B on the surface of the optical component, the processing stability and stain resistance are improved, and the sliding properties of the optical component in processing and use are solved. Anti-fouling problem, achieving a surface layer that takes into account both stability and anti-fouling effect.
Patent Information
- Application Number
- CN202380036931.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-07-22
- Filing Date
- 2023-01-31
- Publication Date
- 2024-12-06
AI Technical Summary
The existing optical components are difficult to stabilize and fix during processing, and the surface with antifouling properties is highly slippery when rubbed, resulting in unstable processing.
Using a surface layer containing at least component A and component B, component A has a siloxane bond and component B has an organic group, including a selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond and a carbon-nitrogen bond Double bonds increase friction and maintain antifouling characteristics by adjusting the composition ratio of component B to component A.
It achieves both stability and anti-fouling during processing, ensuring the anti-fouling effect of optical components during use, while maintaining high friction under low loads to avoid slippage problems.
Smart Images

Figure CN119096169A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a surface layer excellent in processability and antifouling property, an optical component having the surface layer, and glasses having the optical component.
[0002] The present disclosure also relates to a surface layer forming material for forming a surface layer excellent in processability and antifouling properties, a surface layer formed using the surface layer forming material, an optical component having the surface layer, and glasses having the optical component. Background Art
[0003] Optical parts such as anti-reflection films, optical filters, optical lenses, and eyeglass lenses are generally formed of inorganic materials to suppress the reflection of light. The surface free energy of anti-reflection films formed of inorganic materials is high. Due to the high surface free energy, fingerprints, sebum, sweat, cosmetics and other dirt are often attached through human use. In addition, the attached dirt is difficult to remove. As a solution to the problem of dirt attachment and removal, patent documents 1 and 2 propose a technology that gives the surface of optical parts the performance of not easy to adhere to dirt, but easy to remove even if attached.
[0004] However, optical components having a surface that is difficult for dirt to adhere to but easy to remove even if it adheres (hereinafter such a property is also referred to as "anti-fouling property" or "anti-fouling characteristics") have low friction and a slippery surface. Therefore, when the shape of the optical components is processed, it is difficult to fix them stably and thus difficult to process.
[0005] In response to the above-mentioned problems, patent document 3 discloses an eyeglass lens, which is formed by forming a protective film on an oleophobic coating film, which is formed by a coating liquid containing a resin composed of an organic compound, inorganic oxide particles, and an organosilicon compound represented by a prescribed general formula or its hydrolyzate as active ingredients, and the composition ratio of the resin composed of an organic compound and the inorganic oxide particles and the content of the organosilicon compound represented by a prescribed general formula or its hydrolyzate are set within a prescribed range, so that even if an oleophobic coating film is provided, it can be polished by the same holding method as conventional eyeglass lenses.
[0006] In addition, Patent Document 4 discloses a spectacle lens having an anti-fouling layer formed on the surface by two or more silane compounds, at least one of which is a fluorine-containing silane compound, and wherein the highest dynamic friction coefficient value among the dynamic friction coefficients of the lens surface formed by the two or more silane compounds as separate components is made at least 1.4 times the lowest dynamic friction coefficient value, thereby reducing the smoothness of the lens surface to the extent that the lens shape processing can be performed without reducing the excellent anti-fouling effect of the anti-fouling layer.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2000-144097
[0010] Patent Document 2: Japanese Patent Application Publication No. 2003-238577
[0011] Patent Document 3: Japanese Patent Application Publication No. 2013-050652
[0012] Patent Document 4: Japanese Patent Application Publication No. 2005-003817
[0013] Non-patent literature
[0014] Non-patent literature 1: Technology Encyclopedia Series Silicon Encyclopedia Pages 10-11 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, the solutions described in Patent Documents 3 and 4 are not sufficient in terms of fixation during processing, and an antifouling surface that achieves both processing stability and antifouling properties is desired.
[0017] The present invention provides a surface layer that has both stability of fixation during processing and antifouling properties, an optical component having the surface layer, and glasses. In addition, the present invention also provides a surface layer forming material that forms a surface layer that has both stability of fixation during processing and antifouling properties.
[0018] Technical solutions to solve problems
[0019] The surface layer disclosed in the present invention is a surface layer comprising at least component A and component B, characterized in that:
[0020] The component A has a siloxane group containing a siloxane bond,
[0021] The component B is an alkyl compound having an organic group and having a structure represented by the following general formula (3), wherein the organic group has at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond,
[0022] R3-Y-R4(3)
[0023] The group represented by Y contains one or more selected from [C i H 2i-2 ] j1 , [C i H 2i ] j2 , [C6H4] j3、 [Ci+1 H 2i- 1Cl] j4 , [C i H i Cl] j5 、[C5H4O3] j6 、[C3H6N] j7 and [C4H6O2N] j8 A group consisting of at least one bond in the group,
[0024] i, j1, j2, j3, j4, j5, j6, j7 and j8 satisfy 32≤i×(j1+j2+j3+j4+j5+j6+j7+j8)≤750,
[0025] The j1, j2, j3, j4, j5, j6, j7 and j8 are each independently an integer greater than 0,
[0026] The i in each group is independently an integer greater than 1,
[0027] The R3 and the R4 are independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom,
[0028] The composition ratio of component B to component A in the surface layer is 0.04 to 3.00.
[0029] Furthermore, the optical component of the present disclosure is an optical component having the above-mentioned surface layer.
[0030] Furthermore, the glasses of the present disclosure are glasses having the above-mentioned optical components.
[0031] Furthermore, the surface layer forming material of the present disclosure is a surface layer forming material comprising at least component A and component B, characterized in that:
[0032] The component A has a siloxane group containing at least a siloxane bond,
[0033] The component B is an alkyl compound having an organic group and having a structure represented by the following general formula (3), wherein the organic group has at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond,
[0034] R3-Y-R4(3)
[0035] The group represented by Y contains one or more selected from [C i H 2i-2 ] j1 , [C i H 2i ]j2 , [C6H4] j3、 [C i+1 H 2i- 1Cl] j4 , [C i H i Cl] j5、 [C5H4O3] j6 、[C3H6N] j7 and [C4H6O2N] j8 A group consisting of at least one bond in the group,
[0036] i, j1, j2, j3, j4, j5, j6, j7 and j8 satisfy 32≤i×(j1+j2+j3+j4+j5+j6+j7+j8)≤750,
[0037] The j1, j2, j3, j4, j5, j6, j7 and j8 are each independently an integer greater than 0,
[0038] The i in each group is independently an integer greater than 1,
[0039] The R3 and the R4 are independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom,
[0040] The mass ratio of component B to component A in the surface layer forming material is 0.04 to 3.00.
[0041] Effects of the Invention
[0042] According to the present disclosure, a surface layer having both fixed stability and antifouling properties during processing, an optical component having the surface layer, and glasses can be provided. In addition, the present disclosure can also provide a surface layer forming material for forming a surface layer having both fixed stability and antifouling properties during processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic diagram showing the structure of the surface layer in the first embodiment.
[0044] Figure 2 It is a schematic diagram showing the structure of the surface layer in the second embodiment.
[0045] Figure 3 It is a schematic diagram showing the structure of the optical component in the first embodiment.
[0046] Figure 4 It is a schematic diagram showing the structure of a second embodiment of an optical component.
[0047] Figure 5 This is a schematic diagram showing the structure of one embodiment of glasses using the optical component. DETAILED DESCRIPTION
[0048] Hereinafter, preferred embodiments are given to explain the surface layer, the optical component having the surface layer, the glasses having the optical component, and the surface layer forming material according to the present disclosure. In addition, the present disclosure is not limited to the following embodiments.
[0049] In addition, in the present disclosure, the description of "XX or more and YY or less" or "XX to YY" indicating a numerical range, unless otherwise specified, means a numerical range including the lower limit and the upper limit as endpoints. Moreover, when the numerical range is described step by step, the upper limit and the lower limit of each numerical range can be arbitrarily combined.
[0050] According to the present disclosure, by keeping the friction force when applying high load to the surface layer of the base material or optical component high, the sliding property is suppressed, and the base material or optical component can be stably fixed during the processing of the base material or optical component. In addition, when the user uses the base material or optical component in daily life, the friction force becomes low within the range of the load applied to the surface layer of the base material or optical part, and the anti-fouling property can be exhibited. These results can provide a surface layer that takes into account both processability and anti-fouling properties, an optical component having the surface layer, and glasses having the optical component. In addition, a surface layer forming material that imparts the above-mentioned properties to the surface layer can also be provided.
[0051] The inventors have studied the mechanism by which the surface layer and the optical component having the surface layer according to the present disclosure achieve both stability during processing and antifouling properties as follows.
[0052] As component A contained in the surface layer, a compound having a siloxane group containing a siloxane bond is selected. In addition, as component B, a compound having an organic group is selected, and the organic group has at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon oxygen double bond, and a carbon nitrogen double bond.
[0053] Although component A having a siloxane group containing a siloxane bond exhibits antifouling properties, it tends to have low friction when a load is applied. The inventors consider the following as the reason. According to non-patent document 1, a siloxane bond is a bond composed of a silicon atom and an oxygen atom, and the chemical formula is shown in the following formula (1).
[0054] Si-O-Si···(1)
[0055] The rotational energy of the silicon-oxygen bond in the above formula (1) is as small as 0.8 kJ / mol or less, so the silicon-oxygen bond has the characteristic of being easy to rotate. Based on this characteristic, it is believed that when a load is applied to a surface having a siloxane group having a siloxane bond to fix it, the siloxane group having a siloxane bond will deform and release the force, so the friction force becomes low.
[0056] On the other hand, since component B has an organic group having at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond, it is less likely to deform even when a load is applied than component A and tends to have a higher friction force.
[0057] Therefore, when the surface layer that at least comprises component A and component B contacts with an object, when applying high load, component A is out of shape and component B is not easily out of shape.As a result, with respect to the object that contacts with the surface layer, the ratio that component B contacts raises, thereby can obtain high friction.And when component B has the organic group with at least one key in the group that is selected from by unsaturated hydrocarbon bond, carbon oxygen double bond and carbon nitrogen double bond composition, when applying load, more not easily out of shape, frictional force raises, so preferred.
[0058] On this basis, by adjusting the composition ratio of component B to component A in the surface layer within a predetermined range, a high antifouling property can be obtained when the surface layer contacts an object under a low load.
[0059] The "surface layer" refers to an interface that is in contact with a base material and is in contact with a solid, liquid, or gas. That is, in this specification, the "surface layer" is the surface of the base material, and this specification also discloses a base material having such a surface.
[0060] As the base material, any material can be used as long as it is solid and can form the base layer 12, surface layer 13, intermediate layer 14 or hard coating layer 15 described later, but preferably it is a film made of glass, ceramic, resin or metal or glass, resin or the like.
[0061] The optical component is an optical component having a base material having the above-mentioned surface layer. Examples of the optical component include optical filters, optical lenses, eyeglass lenses, photographic lenses, cover glasses for displays, touch panels for displays, and various films.
[0062] Glasses are glasses with the above optical components. The glasses include all the devices mounted around the eyes, and are not limited to ordinary glasses for vision correction, including decorative glasses, goggles, head-mounted displays, sunglasses, smart glasses, etc.
[0063] Component A involved in the present disclosure is described.
[0064] Component A has a siloxane group containing a siloxane bond. The siloxane group containing the siloxane bond is preferably at least one group selected from the group consisting of a dimethylsiloxane group, a diphenylsiloxane group, a methylphenylsiloxane group, a methylhydrogensiloxane group and a phenylhydrogensiloxane group, and more preferably at least one group selected from the group consisting of a dimethylsiloxane group, a diphenylsiloxane group and a methylphenylsiloxane group.
[0065] Specifically, for example, component A is a compound having a structure represented by the following general formula (2):
[0066] R1-X-R2(2)
[0067] It is preferably at least one selected from the group consisting of dimethylsiloxane compounds, diphenylsiloxane compounds, methylphenylsiloxane compounds, methylhydrogensiloxane compounds and phenylhydrogensiloxane compounds, and more preferably at least one selected from the group consisting of dimethylsiloxane compounds, diphenylsiloxane compounds and methylphenylsiloxane compounds.
[0068] It is a preferred embodiment that the group represented by X in formula (2) is composed of any combination of at least one group selected from the groups shown in Table 1 below.
[0069] [Table 1]
[0070] Table 1
[0071] <![CDATA[[SiC2H6-O] m1 ]]> <![CDATA[[SiC 12 H 10 -O] m2 ]]> <![CDATA[[SiC7H8-O] m3 ]]> <![CDATA[[SiCH4-O] m4 ]]> <![CDATA[[SiC6H6-O] m5 ]]>
[0072] In the table, SiC2H6 represents -Si(CH3)2-, SiC7H8 represents -Si(CH3)Ph-, SiC6H6 represents -SiHPh-, and SiC 12 H 10 represents -Si(Ph)2-, SiCH4 represents -Si(CH3)H-, and Ph represents phenyl.
[0073] m1, m2, m3, m4 and m5 in Table 1 preferably satisfy 2≤m1+m2+m3+m4+m5≤150. A more preferred range of m1+m2+m3+m4+m5 is 5≤m1+m2+m3+m4+m5≤120, and a more preferred range is 10≤m1+m2+m3+m4+m5≤50.
[0074] m1, m2, m3, m4 and m5 in Table 1 are each independently an integer greater than or equal to 0. That is, m1, m2, m3, m4 and m5 in Table 1 may have different values for each group.
[0075] Here, m1, m2, m3, m4, and m5 are 0, which means that each group described in Table 1 is not included in the group represented by X in formula (2). In addition, O in Table 1 represents oxygen constituting a siloxane bond.
[0076] Furthermore, the group represented by X may be substituted as a part of the side chain with an organic group such as an amino group, an epoxy group, a mercapto group, a carboxyl group, a polyether group, a long-chain alkyl group, or a fluoroalkyl group.
[0077] R1 and R2 in the general formula (2) are each independently preferably a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom. Examples of the hydrolyzable group include alkoxy groups having 1 to 10 carbon atoms such as methoxy, ethoxy, propoxy, butoxy, alkoxyalkoxy groups having 2 to 10 carbon atoms such as methoxymethoxy, methoxyethoxy, acyloxy groups having 1 to 10 carbon atoms such as acetoxy, alkenyloxy groups having 2 to 10 carbon atoms such as isopropenoxy, halogen groups such as chloro, bromo, iodo, and amino groups. Among them, methoxy, ethoxy, isopropenoxy, and chloro are preferred. Examples of the reactive organic group include methacryloyl, carboxyl, epoxy, and mercapto groups. Among them, methacryloyl and carboxyl are preferred.
[0078] The organic group containing a silyl group containing a hydrolyzable group is, for example, an organic group in which a hydrolyzable group is directly or indirectly bonded to a silicon atom. Examples of the hydrolyzable group include alkoxy groups having 1 to 10 carbon atoms such as methoxy, ethoxy, propoxy, butoxy, alkoxyalkoxy groups having 2 to 10 carbon atoms such as methoxymethoxy, methoxyethoxy, acyloxy groups having 1 to 10 carbon atoms such as acetoxy, alkenyloxy groups having 2 to 10 carbon atoms such as isopropenyloxy, halogen groups such as chloro, bromo, iodo, and amino groups, etc. The number of hydrolyzable groups in the organic group containing a silyl group containing a hydrolyzable group is preferably 1 to 3, more preferably 2 to 3, and even more preferably 3. The organic group containing a silyl group containing a hydrolyzable group may also have an alkylsilyl group described later. That is, examples of the organic group containing a silyl group containing a hydrolyzable group include a trimethoxysilyl group, a dimethoxymethylsilyl group, an ethyldimethoxysilyl group, a methoxydimethylsilyl group, a diethylmethoxysilyl group, an ethylmethoxymethylsilyl group, a triethoxysilyl group, a diethoxyethylsilyl group, a diethoxymethylsilyl group, an ethoxydiethylsilyl group, and an ethoxyethylmethylsilyl group.
[0079] Examples of the alkylsilyl group include alkylsilyl groups having 1 to 10 carbon atoms, and the number of carbon atoms in the alkylsilyl group is preferably 1 to 5, more preferably 1 to 3, and particularly preferably 1. The number of alkyl groups is preferably 1 to 3, more preferably 2 to 3, and further preferably 3. Specifically, examples of the alkylsilyl group include trimethylsilyl, triethylsilyl, ethyldimethylsilyl, and diethylmethylsilyl.
[0080] Specific examples of component A include the compounds shown in Table 2-1 and Table 2-2, but are not limited to these compounds.
[0081] Furthermore, as component A, a compound having a siloxane group having a siloxane bond may be used alone or in combination of two or more.
[0082] [Table 2-1]
[0083] Table 2-1
[0084] No. Structure of Component A No. Structure of Component A A-1 <![CDATA[(MeO)3-Si-O-[SiC2H6-O]2-Si-(CH3)3]]> A-11 <![CDATA[HO-[SiC2H6-O] 18 -Si-(CH3)3]]> A-2 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 10 -Si-(CH3)3]]> A-12 <![CDATA[HO-[SiC2H6-O] 120 -Si-(CH3)3]]> A-3 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 18 -Si-(CH3)3]]> A-13 <![CDATA[H-[SiC2H6-O] 30 -Si-(CH3)3]]> A-4 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 30 -Si-(CH3)3]]> A-14 <![CDATA[C4H5O2-[SiC2H6-O] 30 -Yes-(CH3)3<!-- 5 --> ]]> A-5 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 50 -Si-(CH3)3]]> A-15 <![CDATA[C4H5O2-[SiC2H6-O] 150 -Si-(CH3)3]]> A-6 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 150 -Si-(CH3)3]]> A-16 <![CDATA[(MeO)3-Si-O-[SiC2H6-O]2-Si-(MeO)3]]> A-7 <![CDATA[(EtO)3-Si-O-[SiC2H6-O]5-Si-(CH3)3]]> A-17 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 10 -Si-(MeO)3]]> A-8 <![CDATA[(EtO)3-Si-O-[SiC2H6-O] 18 -Si-(CH3)3]]> A-18 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 30 -Si-(MeO)3]]> A-9 <![CDATA[(EtO)3-Si-O-[SiC2H6-O] 30 -Si-(CH3)3]]> A-19 <![CDATA[(MeO)3-Si-O-[SiC2H6-O] 120 -Si-(MeO)3]]> A-10 <![CDATA[(EtO)3-Si-O-[SiC2H6-O] 120 -Si-(CH3)3]]> A-20 <![CDATA[HO-[SiC2H6-O] 30 -Si-OH]]>
[0085] [Table 2-2]
[0086] Table 2-2
[0087]
[0088] In Table 2-1 and Table 2-2, SiC2H6 represents -Si(CH3)2-, SiC7H8 represents -Si(CH3)Ph-, SiC6H6 represents -SiHPh-, and SiC 12 H 10 represents -Si(Ph)2-, SiCH4 represents -Si(CH3)H-, C4H5O2 represents methacryloyl, Me represents methyl, Et represents ethyl, and Ph represents phenyl.
[0089] Component B involved in the present disclosure is described.
[0090] Component B has an organic group having at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond.
[0091] Preferably, component B has an organic group having an unsaturated hydrocarbon bond, and the unsaturated hydrocarbon bond is derived from at least one compound selected from the group consisting of 1,2-polybutadiene, 1,4-polybutadiene, 1,2-polyisoprene, 1,4-polyisoprene, 1,2-polychloroprene and 1,4-polychloroprene. More preferably, the unsaturated hydrocarbon bond is derived from at least one compound selected from the group consisting of 1,2-polybutadiene and 1,2-polyisoprene.
[0092] Here, the unsaturated hydrocarbon bond derived from the at least one compound means that the unsaturated hydrocarbon bond of the organic group corresponds to the unsaturated hydrocarbon bond contained in the at least one compound.
[0093] Furthermore, it is preferred that component B has a polyolefin having an organic group having at least one bond selected from the group consisting of an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond in a side chain.
[0094] Specifically, component B is, for example, an alkyl compound having a structure represented by the following general formula (3).
[0095] R3―Y―R4(3)
[0096] Here, “an organic group having at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond and a carbon-nitrogen double bond” refers to a group represented by Y in the above general formula (3) when component B is a compound having a structure represented by the above general formula (3).
[0097] The group represented by Y in the general formula (3) includes one or more groups containing at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond shown in Table 3. In addition, as the saturated hydrocarbon bond, the unsaturated hydrocarbon bond, the carbon-oxygen double bond, and the carbon-nitrogen double bond, there may be one or more bonds of any one type, or two or more bonds may be combined.
[0098] [Table 3]
[0099] Table 3
[0100] <![CDATA[[C i H 2i-2 ] j1 ]]> <![CDATA[[C i+1 H 2i-1 Cl] j4 ]]> <![CDATA[[C3H6N] j7 ]]> <![CDATA[[C1H 2i ] j2 ]]> <![CDATA[[C i H i Cl] j5 ]]> <![CDATA[[C4H6O2N] j8 ]]> <![CDATA[[C6H4] j3 ]]> <![CDATA[[C5H4O3] j6 ]]>
[0101] C6H4 in the table represents a phenylene group.
[0102] i and j1, j2, j3, j4, j5, j6, j7 and j8 in Table 3 preferably satisfy 32≤i×(j1+j2+j3+j4+j5+j6+j7+j8)≤750, and more preferably satisfy 40≤i×(j1+j2+j3+j4+j5+j6+j7+j8)≤180.
[0103] i in Table 3 is each independently an integer greater than or equal to 1, and may have a different value for each group.
[0104] j1, j2, j in Table 3 3、 j4, j 5、 j 6、 j7 and j8 are each independently an integer greater than 0. That is, j1, j2, j 3、 j4, j 5、 j6、 j7 and j8 may have different values in each group.
[0105] Here, j1, j2, j 3、 j4, j 5、 j 6、 The fact that j7 and j8 are 0 means that each group described in Table 3 is not included in the group represented by Y in formula (3).
[0106] As long as it is within the desirable range of the above-mentioned i×(j1+j2+j3+j4+j5+j6+j7+j8), a side chain branched in the middle of the molecular chain and composed of a group having at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond and a carbon-nitrogen double bond may also exist in the group represented by Y.
[0107] C5H4O3 in Table 3 refers to a bond formed by grafting maleic anhydride onto a part of the side chain of a polyolefin such as polyethylene or polypropylene.
[0108] In addition, C3H6N in Table 3 refers to a bond in which a part of the side chain of a polyolefin such as polyethylene or polypropylene is substituted with an amino group.
[0109] In addition, C4H6O2N in Table 3 refers to a bond in which a part of the side chain of a polyolefin such as polyethylene or polypropylene is substituted with an isocyanate group.
[0110] The group represented by Y in the general formula (3) is preferably a group containing one or more bonds selected from the group consisting of saturated hydrocarbon bonds, unsaturated hydrocarbon bonds, carbon-oxygen double bonds, and carbon-nitrogen double bonds shown in Table 4.
[0111] [Table 4]
[0112] Table 4
[0113]
[0114] k1, k2, k3, k4, k5, k6, k7, k8, k9 and k in Table 4 10 It is preferred to satisfy 8≤k1+k2+k3+k4+k6+k7+k8+k 9+ k 10 ≤180, more preferably 40≤k1+k2+k3+k4+k6+k7+k8+k 9+ k 10 ≤120.
[0115] k1, k2, k3, k4, k5, k6, k7, k8, k9 and k in Table 4 10Each independently represents an integer greater than 0. That is, k1, k2, k3, k4, k5, k6, k7, k8, k9 and k 10 Different values may be used in each group.
[0116] Here, k1, k2, k 3、 k4, k5, k6, k7, k8, k9 and k 10 The term 0 means that each group described in Table 4 is not included in the group represented by Y in formula (3).
[0117] As long as in the above k1+k2+k3+k4+k6+k7+k8+k 9+ k 10 Within the desirable range, a side chain branched in the middle of the molecular chain and composed of a group having at least one bond selected from the group consisting of an unsaturated hydrocarbon bond, a carbon-oxygen double bond and a carbon-nitrogen double bond may also be present in the group represented by Y.
[0118] As a preferred structure of component B, it is preferred that any one of an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond or any combination thereof is present on the side chain side. More preferably, it is desired that any one of an unsaturated hydrocarbon bond, a carbon-oxygen double bond or any combination thereof is present on the side chain side.
[0119] R3 and R4 in the above general formula (3) can be independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group, or a hydrogen atom. Preferably, an organic group containing a silyl group containing a hydrolyzable group, a hydroxyl group, and a hydrogen atom are suitable. More preferably, it is a hydroxyl group or a hydrogen atom. As the hydrolyzable group, alkoxy groups with 1 to 10 carbon atoms such as methoxy, ethoxy, propoxy, butoxy, alkoxyalkoxy groups with 2 to 10 carbon atoms such as methoxymethoxy, methoxyethoxy, acyloxy groups with 1 to 10 carbon atoms such as acetoxy, alkenyloxy groups with 2 to 10 carbon atoms such as isopropenyloxy, halogen groups such as chloro, bromo, and iodo, and amino groups can be listed. Among them, methoxy, ethoxy, isopropenyloxy, and chloro are preferred. As the reactive organic group, methacryloyl, carboxyl, epoxy, and mercapto groups can be listed. Among them, methacryloyl and carboxyl are preferred.
[0120] The organic group containing a silyl group containing a hydrolyzable group is, for example, an organic group in which a hydrolyzable group is directly or indirectly bonded to a silicon atom. Examples of the hydrolyzable group include alkoxy groups having 1 to 10 carbon atoms such as methoxy, ethoxy, propoxy, butoxy, alkoxyalkoxy groups having 2 to 10 carbon atoms such as methoxymethoxy, methoxyethoxy, acyloxy groups having 1 to 10 carbon atoms such as acetoxy, alkenyloxy groups having 2 to 10 carbon atoms such as isopropenyloxy, halogen groups such as chloro, bromo, iodo, and amino groups, etc. The number of hydrolyzable groups in the organic group containing a silyl group containing a hydrolyzable group is preferably 1 to 3, more preferably 2 to 3, and even more preferably 3. The organic group containing a silyl group containing a hydrolyzable group may also have an alkylsilyl group described later. That is, examples of the organic group containing a silyl group containing a hydrolyzable group include a trimethoxysilyl group, a dimethoxymethylsilyl group, an ethyldimethoxysilyl group, a methoxydimethylsilyl group, a diethylmethoxysilyl group, an ethylmethoxymethylsilyl group, a triethoxysilyl group, a diethoxyethylsilyl group, a diethoxymethylsilyl group, an ethoxydiethylsilyl group, and an ethoxyethylmethylsilyl group.
[0121] Examples of the alkylsilyl group include alkylsilyl groups having 1 to 10 carbon atoms, and the number of carbon atoms in the alkylsilyl group is preferably 1 to 5, more preferably 1 to 3, and particularly preferably 1. The number of alkyl groups is preferably 1 to 3, more preferably 2 to 3, and further preferably 3. Specifically, examples of the alkylsilyl group include trimethylsilyl, triethylsilyl, ethyldimethylsilyl, and diethylmethylsilyl.
[0122] As specific examples of component B, the compounds shown in Table 5 can be cited, but are not limited to these compounds. In addition, as component B, a compound containing one or more groups containing at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond can be used alone, or two or more compounds can be used in combination.
[0123] [Table 5]
[0124] Table 5
[0125]
[0126] In addition, specific examples of component B include the compounds shown in Table 6, but are not limited to these compounds.
[0127] [Table 6]
[0128] Table 6
[0129]
[0130] The compounds shown in Table 6 are alkyl compounds having any one of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond, and d-1 to d-4 are modified polyolefins in which a part of the side chain is converted into a different group. Examples of the replacement group include an imino group, a vinyl group, a carboxylic acid group, a carboxylic anhydride group, a ketone group, an isocyanate group, and the like.
[0131] The composition ratio of component B to component A in the surface layer of the present invention is determined by measuring the peak intensity of component A when the surface layer is measured by a micro Raman spectrometer as P A , the peak intensity originating from component B is P B P B / P A It can be expressed in the range of 0.04 to 3.00. In addition, the composition ratio of component B to component A in the surface layer of the present disclosure can be adjusted by the mass ratio of component B to component A in the surface layer forming material of the present disclosure. The composition ratio is preferably 0.10 to 1.00, and more preferably 0.20 to 0.60.
[0132] Although the antifouling property is exhibited when the composition ratio of component B to component A is less than 0.04, the friction force does not increase when a high load is applied during processing, and the sliding property is not suppressed, so the processing of the base material becomes difficult. In addition, when the composition ratio of component B to component A is greater than 3.00, not only the antifouling property is reduced, but also the friction force is high even within the range of loads used by users on a daily basis, causing difficulties in the use feeling such as the cloth getting stuck when wiping dirt.
[0133] The composition ratio of component B to component A can be obtained by the following method.
[0134] First, determine the area in the surface layer that is to be measured by the micro-Raman spectrometer. This area is determined by the magnification of the objective lens attached to the device and the wavelength and aperture of the excitation laser. Hereinafter, the determined area is also referred to as the "measurement area".
[0135] Next, the scattered light generated by irradiating the measurement area with the excitation laser light is measured to obtain a Raman spectrum. The measurement conditions are as follows.
[0136] ·Measurement device: Micro-Raman spectrometer manufactured by Thermo Fisher Scientific
[0137] Objective lens magnification: 10 times
[0138] Excitation laser wavelength: 532nm
[0139] Pore size: 25 μm
[0140] ·Measurement area: 2μm
[0141] Among the peaks in the obtained Raman spectrum, the peak derived from the siloxane bond is defined as the peak derived from component A, and the peak intensity of the peak is defined as P. A In addition, when a peak derived from a C=C bond, a C=O bond, or a C=N bond is obtained among the peaks in the obtained Raman spectrum, the peak derived from the C=C bond, the C=O bond, or the C=N bond is regarded as a peak derived from component B, and the peak intensity of the peak is regarded as P. B .
[0142] When the peaks in the obtained Raman spectrum do not contain a peak derived from a C=C bond, a C=O bond, or a C=N bond, the peak derived from a C=C bond is regarded as a peak derived from component B, and the peak intensity of the peak is regarded as P. B .
[0143] The friction force measured at a load of 14 kgf and a friction speed of 2.5 mm / sec applied to the surface layer is defined as X.
[0144] When the friction force measured at a load of 70 kgf and a friction speed of 2.5 mm / sec applied to the surface layer is defined as Y,
[0145] The change ratio of the friction force represented by (YX) / X×100 is preferably 50% to 200%, more preferably 80% to 140%.
[0146] The change ratio can be controlled by the type of component A, the type of component B, and the composition ratio of component B to component A.
[0147] The surface layer of the present disclosure may contain any compound other than component A and component B within a range not impairing the effects of the present disclosure.
[0148] <<First Implementation Method>>
[0149] Figure 1 This is a schematic diagram showing the structure of the surface layer in the first embodiment, and shows a structural example in which a base layer is formed on a base material and a surface layer is provided on the base layer.
[0150] exist Figure 1 In the embodiment, a base layer 12 is present on a base material 11 , and a surface layer 13 is formed on the base layer 12 .
[0151] also, Figure 1 The diagram schematically shows a structure having a surface layer, and does not show the actual thicknesses of the base material 11 , the base layer 12 , and the surface layer 13 in a correct ratio.
[0152] (Base material 11)
[0153] As long as the base material 11 is solid and can form the base layer 12, the surface layer 13 or the intermediate layer 14 or the hard coating layer 15 described later, for example, a film made of glass, ceramics, resin or metal or glass, resin, etc. can be listed. When the above-mentioned material is used as the base material of the optical component having the surface layer of the present disclosure, the base material is preferably a material that can transmit visible light or light of a specific wavelength.
[0154] The thickness of the base material is not particularly limited and can be appropriately set depending on the intended use.
[0155] (Base layer 12)
[0156] The base layer 12 is also formed as needed. The base layer 12 is a layer that serves as a base for forming the surface layer 13 and makes the adhesion between the base material 11 and the surface layer 13 good.
[0157] In this embodiment, in order to further improve the adhesion between the base material 11 and the surface layer 13, the base layer 12 is formed on the base material 11, and the surface layer 13 is formed on the base layer 12. In addition, there is no particular limitation on the method for forming the base layer, but evaporation, dipping, coating, spraying, spin coating, etc. can be listed.
[0158] The thickness of the base layer 12 is not particularly limited, but is 2 nm to 150 nm, preferably 5 nm to 125 nm.
[0159] The material forming the base layer 12 is preferably a material having hydroxyl groups on the surface. Examples thereof include metal oxides such as SiO2 and Al2O3 having hydroxyl groups on the surface, and alkyl compounds having hydroxyl groups.
[0160] (Surface layer 13)
[0161] The surface layer 13 is a surface layer of the component A and the component B of the present disclosure described above.
[0162] The thickness of the surface layer 13 is not particularly limited, but preferably 4nm to 20nm. When the thickness is 4nm or more, sufficient antifouling properties can be obtained, and when the thickness is 20nm or less, the transparency is good. In addition, as the formation method of the surface layer, there is no particular limitation, but a vapor deposition method, a coating method, etc. can be listed. In addition, as the coating method, spin coating, dip coating, rod coating, spray coating, etc. can be listed. By using component A and component B in the formation method of the surface layer, the surface layer of component A and component B can be formed. For example, the surface layer is a vapor deposition layer. In addition, for example, the surface layer is a coating layer.
[0163] Second Implementation Method
[0164] Figure 2 This is a schematic diagram showing the structure of the surface layer in the second embodiment, showing a structural example in which an intermediate layer is formed on a base material, a base layer is formed on the intermediate layer, and a surface layer is formed on the base layer.
[0165] exist Figure 2 In the embodiment, an intermediate layer 14 is formed on a base material 11. The intermediate layers 14a and 14c are alternately stacked with the intermediate layers 14b and 14d are alternately stacked with the intermediate layers 14a and 14c. The surface layer 13 is formed on the base layer 12 provided on the intermediate layer 14.
[0166] also, Figure 2 The diagram schematically shows the structure of the surface layer, and does not show the actual thicknesses of the base material 11 , the intermediate layer 14 , the base layer 12 , and the surface layer 13 in a correct ratio.
[0167] (Middle layer 14)
[0168] like Figure 2 As shown, the odd-numbered intermediate layers 14a and 14c stacked from the base material 11 side are made of a low refractive index material, and the even-numbered intermediate layers 14b and 14d stacked are made of a high refractive index material.
[0169] In addition, in the present embodiment, the base layer 12 is also composed of a low refractive index material, is stacked on the intermediate layer 14, and performs an anti-reflection function together with the intermediate layer 14. In the present embodiment, as an example, the intermediate layer 14 has four layers, and the base layer 12 is formed on the intermediate layer 14d having a high refractive index material, so the base layer 12 is preferably a low refractive index material. In addition, for example, when the intermediate layer 14 has three layers and the base layer 12 is formed on the intermediate layer 14b having a high refractive index material, the base layer 12 is preferably a low refractive index material.
[0170] The intermediate layer 14 is not limited to the present embodiment, and a layer composed of a medium refractive index material may be stacked appropriately.
[0171] Examples of the low refractive index material include SiO2 (silicon dioxide), Al2O3-added SiO2 (alumina-added silicon dioxide), etc. However, the low refractive index material is not limited to these.
[0172] Examples of high refractive index materials include titanium oxide-lanthanum oxide mixed materials containing aluminum oxide, titanium oxide, other mixed oxides with titanium oxide as the main component, zirconium oxide, mixed materials with zirconium oxide as the main component, niobium oxide, mixed materials with niobium oxide as the main component, tantalum oxide, mixed materials with tantalum oxide as the main component, tungsten oxide, mixed materials with tungsten oxide as the main component, etc. However, the high refractive index material is not limited to this.
[0173] Examples of the medium refractive index material include aluminum oxide, other mixed compounds containing aluminum oxide as a main component, magnesium oxide, other mixed compounds containing magnesium oxide as a main component, yttrium fluoride, cerium fluoride, etc. However, the medium refractive index material is not limited thereto.
[0174] Regarding the intermediate layer 14 and the layers constituting the intermediate layer 14 ( Figure 2 The thickness of the intermediate layer 14 (hereinafter referred to as 14a, 14b, 14c, 14d) is not particularly limited, but for example, the thickness of each layer constituting the intermediate layer 14 is 10nm to 200nm, and the necessary number of layers can be stacked to constitute the intermediate layer 14.
[0175] In addition, although the intermediate layer 14 in the present embodiment has a four-layer structure, the present disclosure is not limited in any way, and the number of layers may be any number.
[0176] In addition, although in the present embodiment, as described above, an intermediate layer 14 is provided as a part of an antireflection film formed by alternately stacking low refractive index layers and high refractive index layers, the present disclosure is not subject to any restriction. For example, at least one layer having functions selected from other filters, mirrors, antistatic, anti-scratch hard coatings, etc. may be formed between the matrix 11 and the intermediate layer 14.
[0177] In addition, the base material, the base layer, and the surface layer in the second embodiment as the surface layer may be the same as those in the first embodiment of the surface layer.
[0178] Optical components
[0179] Figure 3 It is a schematic diagram showing the structure of the optical component in the first embodiment.
[0180] The present embodiment is an optical component that can be used for eyeglass lenses.
[0181] Figure 3 The optical component includes a base material 11 composed of a resin, a hard coating layer 15 for scratch prevention, an intermediate layer 14 having an antireflection function described in the second embodiment of the surface layer, a base layer 12, and a surface layer 13. Figure 3 In the embodiment, as the intermediate layer 14, a double layer structure is adopted in which the intermediate layer 14a stacked at the odd number from the base material 11 side is composed of a low refractive index material, and the intermediate layer 14b stacked at the even number is composed of a high refractive index material, but it is not limited to this, and the number of layers can be any number. In addition, the layer composed of the medium refractive index material can be appropriately stacked.
[0182] Furthermore, as the hard coat layer 15, for example, melamine resin, polyurethane resin, acrylic resin, a mixture of these resins, silane compound, etc. can be used. However, the material used for the hard coat layer is not limited thereto.
[0183] In addition, the optical component represented by the structure in the first embodiment is not limited to eyeglass lenses, and can be used for other well-known uses.
[0184] Figure 4 It is a schematic diagram showing the structure of a second embodiment of an optical component.
[0185] The present embodiment is an optical component that can be used for an optical lens used in a camera or the like.
[0186] Figure 4 The optical component includes a base material 11 composed of glass, an intermediate layer 14 having an antireflection function described in the second embodiment of the surface layer, a base layer 12 and a surface layer 13. Figure 4 In the embodiment, as the intermediate layer 14, a double layer structure is adopted in which the intermediate layer 14a stacked at the odd number from the base material 11 side is composed of a low refractive index material, and the intermediate layer 14b stacked at the even number is composed of a high refractive index material, but it is not limited to this, and the number of layers can be any number. In addition, the layer composed of the medium refractive index material can be appropriately stacked.
[0187] Furthermore, the optical component represented by the structure in the second embodiment is not limited to an optical lens for a camera, and can be used for an optical filter, a touch panel for a display, various films, and the like.
[0188] "Glasses"
[0189] Figure 5 This is a schematic diagram showing the structure of one embodiment of glasses using the optical component of the present disclosure.
[0190] This embodiment is constituted by the above-mentioned eyeglass lens 31 and eyeglass frame 32 of the optical components of the present disclosure.
[0191] The surface layer forming material disclosed in the present invention is a surface layer forming material comprising at least component A and component B, wherein:
[0192] The component A has a siloxane group containing at least a siloxane bond,
[0193] The component B is an alkyl compound having an organic group and having a structure represented by the following general formula (3), wherein the organic group has at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond,
[0194] R3-Y-R4(3)
[0195] The group represented by Y contains one or more selected from [C i H 2i-2 ] j1 , [C i H 2i ] j2 , [C6H4] j3、 [C i+1 H 2i- 1Cl] j4 , [C i H i Cl] j5、 [C5H4O3] j6 、[C3H6N] j7 and [C4H6O2N] j8 A group consisting of at least one bond in the group,
[0196] i, j1, j2, j3, j4, j5, j6, j7 and j8 satisfy 32≤i×(j1+j2+j3+j4+j5+j6+j7+j8)≤750, and j1, j2, j3, j4, j5, j6, j7 and j8 are each independently an integer greater than 0,
[0197] The i in each group is independently an integer greater than 1,
[0198] The R3 and the R4 are independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom,
[0199] The mass ratio of component B to component A in the surface layer forming material is 0.04 to 3.00.
[0200] The surface layer forming material according to the present disclosure will be described.
[0201] Component A and component B constituting the surface layer forming material of the present disclosure are the same as component A and component B constituting the surface layer of the present disclosure.
[0202] The mass ratio of component A to component B in the surface layer forming material disclosed herein is in the range of 0.04 to 3.00 when the mass of component A is 1. That is, the mass ratio of component B to component A in the surface layer forming material is 0.04 to 3.00. The mass ratio is preferably 0.10 to 1.00, and more preferably 0.20 to 0.60.
[0203] Although the surface layer formed by using the surface layer forming material exhibits antifouling properties when the mass ratio of component B relative to component A is less than 0.04, the friction force does not increase when a high load is applied during the processing of a base material or an optical component having the surface layer, and the sliding property is not suppressed, so the processing of the base material or the optical component becomes difficult. In addition, when the mass ratio of component B relative to component A is greater than 3.00, even within the range of the load used by the user in daily life, the friction force is high, and not only the antifouling properties of the surface layer formed by using the surface layer forming material will decrease, but also difficulties will arise in the sense of use such as the cloth being stuck when wiping dirt.
[0204] The mass ratio of component B to component A in the surface layer forming material can be determined using liquid chromatography-mass spectrometry or using the mass of component A and component B measured using a balance when preparing the surface layer forming material.
[0205] The surface layer forming material involved in the present disclosure is not particularly limited as long as the mass ratio of component B in the surface layer forming material to component A is in the range of 0.04 to 3.00, and other materials may also be included. The surface layer forming material may be solid or liquid. For example, component A and component B may be dissolved in an organic solvent such as hexane or toluene to form a solution as a liquid. When the surface forming material is a liquid, the surface layer may be formed by a coating method.
[0206] The surface forming material may contain an organic solvent. The organic solvent is not particularly limited, but for example, at least one selected from the group consisting of ketone solvents such as acetone and methyl ethyl ketone; ether solvents such as dimethyl ether, diethyl ether, tetrahydrofuran, etc.; aromatic hydrocarbon solvents such as benzene, toluene, chlorobenzene, xylene, etc.; and aliphatic hydrocarbon solvents such as isohexane (i.e., 2-methylpentane), 3-methylpentane, 2,2-dimethylbutane and 2,3-dimethylbutane, n-hexane, heptane, and cyclohexane.
[0207] The content of the organic solvent is not particularly limited, but can be, for example, 50 to 150 parts by mass when the total content of component A and component B in the surface layer forming material is 100 parts by mass.
[0208] Example
[0209] The present disclosure will be described in more detail below with reference to the following examples, but the present disclosure is not limited to the following examples.
[0210] [Example 1]
[0211] (Preparation of Surface Layer Forming Material)
[0212] The compound (A-3) described in Table 2-1 is used as component A, and the compound (a-3) described in Table 5 is used as component B. The mixture is mixed in a metal container in such a manner that the mass ratio of component B to component A becomes 0.20 to obtain a surface layer forming material 1.
[0213] (Preparation of base layer)
[0214] On a 3 mm thick borosilicate glass substrate 11, a vacuum deposition apparatus (dome diameter Φ900 mm, deposition distance 890 mm) was used to form a 10 nm thick underlayer 12 composed of SiO2 by a deposition method. The thickness of the underlayer 12 was measured by a spectroscopic ellipsometer (ESM300, manufactured by JA WOOLLAM).
[0215] (Preparation of Surface Layer)
[0216] On the base layer 12, a vacuum evaporation device (dome diameter Φ900mm, evaporation distance 890mm) was used to form the surface layer 13 of the present disclosure composed of the surface layer forming material 1 by evaporation method to prepare the optical component of Example 1. The thickness of the surface layer 13 was measured using a spectroscopic ellipsometer (JA WOOLLAM Co., Ltd. -ESM300), which was 10nm. In addition, the composition ratio of component B in the obtained surface layer relative to component A was measured by a micro Raman spectrometer, which was the same as the mass ratio of component B to component A in the surface layer forming material, which was 0.20.
[0217] The structure of the optical component obtained is similar to that having Figure 1 The structures of the optical components of the surface layers of the present disclosure are shown to be the same.
[0218] (Evaluation of friction force)
[0219] With regard to the surface layer of the prepared optical component, the friction force of the surface layer was measured in the following manner.
[0220] As a friction force measuring device, an automatic friction and wear analysis device Triboster 500 manufactured by Kyowa Interface Science Co., Ltd. was used. As a contact point for measuring friction force, a 2 mm cut 2 A rubber pad (lens stop pad manufactured by 3M) was placed in contact with the surface layer of the optical component to measure the friction force. At this time, the applied load of the device was adjusted so that the load applied to the surface layer became 14kgf and 70kgf, and the test was carried out. The friction speed was implemented under the condition of 2.5mm / sec. The results are shown in Table 7-1.
[0221] (Evaluation of antifouling properties)
[0222] Regarding the surface layer of the produced optical member, the antifouling property of the surface layer was evaluated in the following manner.
[0223] As an index showing the antifouling property, the repellency of the fluorescent pen ink and the ease of wiping off were used as evaluation indexes, and the evaluation was performed based on the following criteria. The results are shown in Table 7-1.
[0224] (Evaluation Criteria)
[0225] A: After the pen tip is attached to the surface layer, the ink will become a ball and bounce off after 1 to 5 seconds, and can be wiped off with cleaning paper.
[0226] B: After the pen tip is attached to the surface layer, the ink will not bounce off even if it exceeds 5 seconds, and can only be wiped off with a piece of wiping paper.
[0227] [Examples 2 to 214]
[0228] The composition ratio of the compounds recorded in Table 2-1 and Table 2-2 used as component A, the compounds recorded in Table 5 and Table 6 used as component B, and the component B after the surface layer is formed relative to component A, is changed to as described in Table 7-1, Table 7-2, Table 8-1 and Table 8-2, respectively. In addition, similarly to Example 1, blending is carried out in a metal container, and after preparing the surface layer forming material, a base layer and a surface layer are formed to prepare an optical component with a surface layer disclosed in the present invention. In addition, the evaluation of friction and the evaluation of antifouling performance are carried out similarly to Example 1. The results are shown in Table 7-1, Table 7-2, Table 8-1 and Table 8-2.
[0229] In Examples 2 to 214, as in Example 1, the composition ratio of component B to component A in the obtained surface layer was consistent with the mass ratio of component B to component A in the surface layer forming material.
[0230] [Table 7-1]
[0231] Table 7-1
[0232]
[0233] [Table 7-2]
[0234] [Table 7-2]Table 7-2
[0235]
[0236] [Table 8-1]
[0237] [Table 8-1]Table 8-1
[0238]
[0239] [Table 8-2]
[0240] [Table 8-2]
[0241] Table 8-2
[0242]
[0243] [Comparative Example 1]
[0244] Only the compound (A-3) described in Table 2-1 was injected into a metal container to prepare a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to prepare an optical component. In addition, the evaluation of frictional force and the evaluation of antifouling performance were carried out in the same manner as in Example 1. The results are shown in Table 9.
[0245] [Comparative Example 2]
[0246] Only the compound (A-8) described in Table 2-1 was injected into a metal container to prepare a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to prepare an optical component. In addition, the evaluation of frictional force and the evaluation of antifouling performance were carried out in the same manner as in Example 1. The results are shown in Table 9.
[0247] [Comparative Example 3]
[0248] Only the compound (B-3) listed in Table 2-2 was injected into a metal container to prepare a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to prepare an optical component.
[0249] [Comparative Example 4]
[0250] Only the compound (C-1) listed in Table 2-2 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0251] [Comparative Example 5]
[0252] Only the compound (D-1) listed in Table 2-2 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0253] [Comparative Example 6]
[0254] Only the compound (a-3) listed in Table 5 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0255] [Comparative Example 7]
[0256] Only the compound (a-4) listed in Table 5 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0257] [Comparative Example 8]
[0258] Only the compound (b-3) listed in Table 5 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0259] [Comparative Example 9]
[0260] Only the compound (b-4) listed in Table 5 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0261] [Comparative Example 10]
[0262] Only the compound (c-1) listed in Table 5 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0263] [Comparative Example 11]
[0264] Only the compound (c-2) listed in Table 5 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0265] [Comparative Example 12]
[0266] Only the compound (d-1) listed in Table 6 was poured into a metal container to obtain a surface layer forming material, and then a base layer and a surface layer were formed in the same manner as in Example 1 to produce an optical component.
[0267] [Comparative Examples 13 and 14]
[0268] Each compound described in Table 2-1 used as component A, each compound described in Table 5 used as component B, and the composition ratio of component A to component B after the surface layer is formed are changed to as described in Table 9, respectively. In addition, the base layer and the surface layer are formed in the same manner as in Example 1 to prepare an optical component. The results are shown in Table 9. In addition, in Comparative Examples 13 and 14, as in Example 1, the composition ratio of component B in the obtained surface layer relative to component A is consistent with the mass ratio of component B in the surface layer forming material relative to component A.
[0269] [Table 9]
[0270] Table 9
[0271]
[0272] OL in Table 9 means that the friction force could not be measured due to overload.
[0273] [Example 215]
[0274] The optical component (glass lens) prepared in the same manner as in Example 5 was processed and assembled on a commercially available frame to prepare spectacles. The friction force and antifouling performance of the optical component of the prepared spectacles were evaluated in the same manner as in Example 1. The results are shown in Table 7-1.
[0275] [Example 216]
[0276] (Preparation of Surface Layer Forming Material)
[0277] The compound (A-3) described in Table 2-1 is used as component A, and the compound (a-3) described in Table 5 is used as component B. After being mixed in a glass container in such a manner that the mass ratio of component B to component A is 0.30, isohexane (trade name: isohexane, manufactured by Tokyo Chemical Industry Co., Ltd.) having the same weight as the total weight of component A and component B is placed in the glass container containing component A and component B, and the mixture in the glass container is stirred until component A and component B can no longer be confirmed by visual observation, thereby obtaining material 2 for surface layer formation.
[0278] (Preparation of Surface Layer)
[0279] By coating the surface layer forming material 2 on a borosilicate glass having a thickness of 3 mm as a base material 11 using a rod coater, and further drying at 25° C. for 24 hours, an optical component having a surface layer of the present disclosure is prepared. In addition, the evaluation of frictional force and the evaluation of antifouling performance are carried out in the same manner as in Example 1. The results are shown in Table 7-1. In addition, in Example 216, as in Example 1, the composition ratio of component B in the obtained surface layer relative to component A is consistent with the mass ratio of component B in the surface layer forming material relative to component A.
[0280] Description of symbols
[0281] 11. Base material
[0282] 12 Basal layer
[0283] 13 Surface layer
[0284] 14 Middle Layer
[0285] 14a, 14c have an intermediate layer of low refractive index material
[0286] 14b, 14d have an intermediate layer of high refractive index material
[0287] 15 Hard coating
[0288] 31 glasses
[0289] 32 Eyeglass frames.
Claims
1. A surface layer comprising at least component A and component B, It is characterized in that The component A has a siloxane group containing a siloxane bond, The component B is an alkyl compound having an organic group and having a structure represented by the following general formula (3), wherein the organic group has at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond, R 3 -Y-R 4 (3) The group represented by Y contains one or more selected from [C i H 2i-2 ] j1 , [C i H 2i ] j2 , [C 6 H 4 ] j3 , [C i+1 H 2i-1 Cl] j4 , [C i H i Cl] j5 , [C 5 H 4 O 3 ] j6 , [C 3 H 6 N] j7 and [C 4 H 6 O 2 N] j8 A group consisting of at least one bond in the group, The i, j 1 、j 2 、j 3 、j 4 、j 5 、j 6 、j 7 and 8 Satisfies 32≤i×(j 1 +j 2 +j 3 +j 4 +j 5 +j 6 +j 7 +j 8 )≤750, The 1 、j 2 、j 3 、j 4 、j 5 、j 6 、j 7 and 8 are each independently an integer greater than 0, The i in each group is independently an integer greater than 1, The R 3 And the R 4 are independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom, The composition ratio of component B to component A in the surface layer is 0.04 to 3.
00.
2. The surface layer according to claim 1, It is characterized in that The siloxane group containing the siloxane bond is at least one group selected from the group consisting of a dimethylsiloxane group, a diphenylsiloxane group, a methylphenylsiloxane group, a methylhydrogensiloxane group, and a phenylhydrogensiloxane group.
3. The surface layer according to claim 1 or 2, It is characterized in that The component A is a compound having a structure represented by the following general formula (2), R 1 -X-R 2 (2) The group represented by X is selected from [SiC 2 H 6 -O] m1 、[SiC 12 H 10 -O] m2 、[SiC 7 H 8 -O] m3 、[SiCH 4 -O] m4 And [SiC 6 H 6 -O] m5 Any combination of at least one group of The m 1 、m 2 、m 3 、m 4 and m 5 Satisfy 2≤m 1 +m 2 +m 3 +m 4 +m 5 ≤150, The m 1 、m 2 、m 3 、m 4 and m 5 are each independently an integer greater than 0, The R 1 And the R 2 Each of them is independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom.
4. The surface layer according to any one of claims 1 to 3, It is characterized in that The group represented by the above Y includes a group containing at least one bond selected from the group consisting of the following formulae (Y-1) to (Y-10), The k 1 , k 2 , k 3 , k 4 , k 5 , k 6 , k 7 , k 8 , k 9 and k 10 Satisfy 8≤k 1 +k 2 +k 3 +k 4 +k 5 +k 6 +k 7 +k 8 +k 9 +k 10 ≤180, The k 1 , k 2 , k 3 , k 4 , k 5 , k 6 , k 7 , k 8 , k 9 and k 10 Each independently represents an integer greater than 0.
5. The surface layer according to any one of claims 1 to 4, It is characterized in that The component B has an organic group, and the organic group has an unsaturated hydrocarbon bond, The unsaturated hydrocarbon bond is derived from at least one compound selected from the group consisting of 1,2-polybutadiene, 1,4-polybutadiene, 1,2-polyisoprene, 1,4-polyisoprene, 1,2-polychloroprene, and 1,4-polychloroprene.
6. The surface layer according to any one of claims 1 to 5, It is characterized in that The component B has a polyolefin having an organic group in a side chain, the organic group having at least one bond selected from the group consisting of an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond.
7. The surface layer according to any one of claims 1 to 6, It is characterized in that The component A has a dimethylsiloxane group, The component B has an organic group, and the organic group has an unsaturated hydrocarbon bond, The unsaturated hydrocarbon bond is derived from at least one compound selected from the group consisting of 1,2-polybutadiene and 1,2-polyisoprene.
8. An optical component, It is characterized in that A surface layer according to any one of claims 1 to 7.
9. A pair of glasses, It is characterized in that An optical component according to claim 8.
10. A surface layer forming material comprising at least component A and component B, It is characterized in that The component A has a siloxane group containing at least a siloxane bond, The component B is an alkyl compound having an organic group and having a structure represented by the following general formula (3), wherein the organic group has at least one bond selected from the group consisting of a saturated hydrocarbon bond, an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond, R 3 -Y-R 4 (3) The group represented by Y contains one or more selected from [C i H 2i-2 ] j1 , [C i H 2i ] j2 , [C 6 H 4 ] j3 , [C i+1 H 2i-1 Cl] j4 , [C i H i Cl] j5 , [C 5 H 4 O 3 ] j6 , [C 3 H 6 N] j7 and [C 4 H 6 O 2 N] j8 A group consisting of at least one bond in the group, The i, j 1 、j 2 、j 3 、j 4 、j 5 、j 6 、j 7 and 8 Satisfies 32≤i×(j 1 +j 2 +j 3 +j 4 +j 5 +j 6 +j 7 +j 8 )≤750, The 1 、j 2 、j 3 、j 4 、j 5 、j 6 、j 7 and 8 are each independently an integer greater than 0, The i in each group is independently an integer greater than 1, The R 3 And the R 4 are independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a silyl group containing a hydrolyzable group, an alkylsilyl group or a hydrogen atom, The mass ratio of component B to component A in the surface layer forming material is 0.04 to 3.
00.
11. The surface layer forming material according to claim 10, It is characterized in that The siloxane group containing the siloxane bond is at least one group selected from the group consisting of a dimethylsiloxane group, a diphenylsiloxane group, a methylphenylsiloxane group, a methylhydrogensiloxane group, and a phenylhydrogensiloxane group.
12. The surface layer forming material according to claim 10 or 11, It is characterized in that The component A is a compound having a structure represented by the following general formula (2), R 1 -X-R 2 (2) The group represented by X is selected from [SiC 2 H 6 -O] m1 、[SiC 12 H 10 -O] m2 、[SiC 7 H 8 -O] m3 、[SiCH 4 -O] m4 And [SiC 6 H 6 -O] m5 Any combination of at least one group of The m 1 、m 2 、m 3 、m 4 and m 5 Satisfy 2≤m 1 +m 2 +m 3 +m 4 +m 5 ≤150, The m 1 、m 2 、m 3、 m 4 and m 5 are each independently an integer greater than 0, The R 1 And the R 2 Each of them is independently a hydrolyzable group, a silanol group, a hydroxyl group, a reactive organic group, an organic group containing a hydrolyzable silyl group, an alkylsilyl group or a hydrogen atom.
13. The surface layer forming material according to any one of claims 10 to 12, It is characterized in that The group represented by the above Y includes a group containing at least one bond selected from the group consisting of the following formulae (Y-1) to (Y-10), The k 1 , k 2 , k 3 , k 4 , k 5 , k 6 , k 7 , k 8 , k 9 and k 10 Satisfy 8≤k 1 +k 2 +k 3 +k 4 +k 5 +k 6 +k 7 +k 8 +k 9 +k 10 ≤180, The k 1 , k 2 , k 3 , k 4 , k 5 , k 6 , k 7 , k 8 , k 9 and k 10 Each independently represents an integer greater than 0.
14. The surface layer forming material according to any one of claims 10 to 13, It is characterized in that The component B has an organic group, and the organic group has an unsaturated hydrocarbon bond, The unsaturated hydrocarbon bond is derived from at least one compound selected from the group consisting of 1,2-polybutadiene, 1,4-polybutadiene, 1,2-polyisoprene, 1,4-polyisoprene, 1,2-polychloroprene, and 1,4-polychloroprene.
15. The surface layer forming material according to any one of claims 10 to 14, It is characterized in that The component B has a polyolefin having an organic group in a side chain, the organic group having at least one bond selected from the group consisting of an unsaturated hydrocarbon bond, a carbon-oxygen double bond, and a carbon-nitrogen double bond.
16. The surface layer forming material according to any one of claims 10 to 15, It is characterized in that The component A has a dimethylsiloxane group, The component B has an organic group, and the organic group has an unsaturated hydrocarbon bond, The unsaturated hydrocarbon bond is derived from at least one compound selected from the group consisting of 1,2-polybutadiene and 1,2-polyisoprene.
17. A surface layer, It is characterized in that The surface layer is formed from the surface layer forming material according to any one of claims 10 to 16.
18. An optical component, It is characterized in that A surface layer according to claim 17.
19. A pair of glasses, It is characterized in that An optical component according to claim 18.