Energy storage device

By using a high aspect ratio carbon element network and water-processable polymer additives in lithium-ion battery electrodes, the problem of toxic solvents and poor contact in traditional electrodes is solved, and the strong electrical performance and machinery of the electrode are achieved Stability improves battery performance and safety.

CN119096319APending Publication Date: 2024-12-06FASTCAP SYSTEMS CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035811.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-01
Filing Date
2023-03-01
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The adhesives used in conventional lithium-ion battery electrodes usually require toxic or environmentally unfriendly solvents, and it is difficult to maintain sufficient contact between the electrode material and the current collector during charging and discharging, affecting the electrochemical characteristics.

Method used

Using a high aspect ratio carbon element network and polymer additives, including multi-walled carbon nanotubes and single-walled carbon nanotubes, provides mechanical support through polymer additives and improves the adhesion of electrode materials to current collectors, ensuring the charging and discharging process Good contact and mechanical stability are maintained in the process, and no environmentally unfriendly solvents are used.

Benefits of technology

The strong electrical performance and mechanical stability of lithium-ion battery electrodes are achieved, while avoiding the use of toxic solvents, which improves the service life and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096319A_ABST
    Figure CN119096319A_ABST
Patent Text Reader

Abstract

Disclosed herein is an energy storage device comprising a positive electrode and a negative electrode wherein at least one of the negative electrode and the positive electrode comprises an active layer comprising: a network of high aspect ratio carbon elements defining void spaces within the network; and a plurality of electrode active material particles disposed in the void spaces within the network; and the network of high aspect ratio carbon elements has a crossover density of at least 0.1 / [mu] m2.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Application No. 63 / 315,170, filed on March 1, 2022, which is incorporated herein by reference in its entirety. Background Art

[0003] Lithium batteries are used in many products, including medical devices, electric vehicles, aircraft, and consumer products such as laptops, cell phones, and cameras. Due to their high energy density, high operating voltage, and low self-discharge, lithium-ion batteries have surpassed the secondary battery market and continue to find new uses in products and developing industries.

[0004] Typically, a lithium-ion battery ("LIB" or "LiB") includes a negative electrode, a positive electrode, and an electrolyte material such as an organic solvent containing a lithium salt. More specifically, the negative electrode and the positive electrode (collectively referred to as "electrodes") are formed by mixing a negative electrode active material or a positive electrode active material with a binder and a solvent to form a paste or slurry, which is then coated on a current collector (such as aluminum or copper) and dried on the current collector to form a thin film on the current collector. The negative electrode and the positive electrode are layered or wound and then loaded into a pressurized casing containing an electrolyte material, which together form a lithium-ion battery.

[0005] In conventional electrodes, the binder used has sufficient adhesion and chemical properties so that the film coated on the current collector will maintain contact with the current collector even when it is manipulated to be installed in a pressurized battery case. Since the film contains the electrode active material, if the film does not maintain adequate contact with the current collector, it may cause significant interference with the electrochemical characteristics of the battery. In addition, it is important to select a binder that is mechanically compatible with the electrode active material so that it can withstand the degree of expansion and contraction of the electrode active material during battery charging and discharging.

[0006] Therefore, binders such as cellulose binders or cross-linked polymer binders have been used to provide good mechanical properties. However, in traditional electrodes, the selected binders usually require the use of environmentally unfriendly or toxic solvents for processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] The following is a brief description of the drawings, wherein like elements have like numerals, and which are presented for the purpose of illustrating exemplary embodiments disclosed herein and not for the purpose of limiting the same.

[0008] Figure 1A is a diagram of electrodes according to various embodiments.

[0009] Figure 1Bis a diagram of electrodes according to various embodiments.

[0010] Figure 1C is a diagram of electrodes according to various embodiments.

[0011] Figure 2 is a diagram of electrodes according to various embodiments.

[0012] Figure 3 is a diagram of electrodes according to various embodiments.

[0013] Figure 4 are examples of electron micrographs of active layers according to various embodiments.

[0014] Figure 5A is a diagram of electrodes according to various embodiments.

[0015] Figure 5B is a diagram of electrodes according to various embodiments.

[0016] Figure 5C is a diagram of electrodes according to various embodiments.

[0017] Figure 6 are examples of electron micrographs of active layers according to various embodiments.

[0018] Figure 7 It is a schematic diagram of the energy storage device.

[0019] Figure 8 is a flow chart of a method for preparing an electrode according to various embodiments.

[0020] Fig. 9 is a cross-sectional view of the energy storage device.

[0021] Fig.10 A schematic diagram of an energy storage device such as a pouch cell is shown.

[0022] Fig.11 are schematic cross-sectional diagrams depicting aspects of an energy storage device (ESD).

[0023] Figures 12 to 21 are graphs depicting various aspects of the electrical performance of energy storage cells assembled according to various embodiments.

[0024] Fig. 22 is a schematic diagram depicting aspects of an energy storage cell assembled according to various embodiments.

[0025] Fig.23 is a schematic diagram depicting aspects of an energy storage cell assembled according to various embodiments.

[0026] Fig.24is a graph depicting the electrical performance of energy storage cells assembled according to various embodiments.

[0027] Figures 25 to 38 are graphs and charts depicting various aspects of the electrical performance of energy storage cells assembled according to various embodiments. DETAILED DESCRIPTION

[0028] A more complete understanding of the components, processes, and devices disclosed herein may be obtained by reference to the accompanying drawings. These figures are merely schematic representations based on convenience and ease of demonstrating the present disclosure, and are therefore not intended to indicate the relative size and dimensions of the device or its components and / or to define or limit the scope of the exemplary embodiments. Although specific terms are used in the following description for clarity, these terms are intended only to refer to the specific structures of the embodiments selected for illustration in the accompanying drawings, and are not intended to define or limit the scope of the present disclosure. In the accompanying drawings and the following description below, it should be understood that the same reference numerals refer to components of the same function.

[0029] Various embodiments provide an electrode and an energy storage device, which exhibits strong electrical properties and strong mechanical stability, and includes polymer additives that promote safe and clean manufacturing processes. Various embodiments provide electrodes that do not include (e.g., do not contain) one or more polymer additives that are insoluble in water or alcohols (such as ethanol). In some embodiments, the electrode is substantially free of one or more polymer additives that are insoluble in water or alcohols (such as ethanol). In some embodiments, the active layer of the electrode does not contain or is substantially free of one or more polymer additives that are insoluble in water or alcohols (such as ethanol). For example, any polymer additive for the electrode according to various embodiments is soluble in one or more of water and alcohols.

[0030] According to various embodiments, the energy storage device includes a positive electrode, a negative electrode and an electrolyte. In an embodiment, the positive electrode includes an active layer, and the active layer includes: (i) a high aspect ratio carbon element network, which defines the void space within the network, (ii) a plurality of electrode active material particles, which are arranged in the void space within the network, and (iii) a polymer additive, the polymer additive being (a) selected from the polyamide family or (b) at least one of a modified polyamide or a polyamide derivative. In some embodiments, the negative electrode includes an active layer, and the active layer includes: (i) a high aspect ratio carbon element network, which defines the void space within the network, (ii) a plurality of electrode active material particles, which are arranged in the void space within the network, wherein the active material particles include silicon, and (iii) a polymer additive. In some embodiments, the silicon included in the active material particles includes one or more of silicon oxide and microsilicon. In some embodiments, the polymer additive is water-processable.

[0031] As used herein, the term "high aspect ratio carbon element" refers to a carbonaceous element having a size in one or more dimensions ("major dimensions") that is significantly larger than the size of the element in lateral dimensions ("minor dimensions").

[0032] According to various embodiments, the energy storage device is included in at least one of a vehicle corresponding to a car, a scooter, a motorcycle, a boat, an airplane, and a sports and leisure vehicle.

[0033] Positive electrode:

[0034] According to various embodiments, the positive electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are arranged in the void space within the network, and (iii) a polymer additive, the polymer additive being (a) selected from the polyamide family or (b) at least one of a modified polyamide or a polyamide derivative. In some embodiments, the high aspect ratio carbon element network that defines the void space within the network includes a first group of carbon nanotubes and a second group of carbon nanotubes. The first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles. The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles. The second group of carbon nanotubes has one or more properties different from the first group of carbon nanotubes. According to various embodiments, the first group of carbon nanotubes includes multi-walled nanotubes, and the second group of carbon nanotubes includes single-walled nanotubes. As an example, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:1. In some embodiments, the multi-walled carbon nanotubes include an average diameter between 6nm and 10nm; an average wall thickness between 6nm and 7nm; an average length between 13 microns and 17 microns. In some embodiments, the average length of the multi-walled carbon nanotubes is about 13 microns. In some embodiments, the average length of the multi-walled carbon nanotubes is about 15 microns. In some embodiments, the average length of the multi-walled carbon nanotubes is about 16 microns. In some embodiments, the single-walled carbon nanotubes include an average diameter between 1nm and 2nm and an average length of about 5 microns. In some embodiments, the single-walled carbon nanotubes include an average diameter between 3nm and 5nm and an average length between 7 microns and 8 microns.

[0035] According to various embodiments, the positive electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that is soluble in at least one of (a) water and (b) alcohols. The high aspect ratio carbon element network that defines the void space within the network may include a group of multi-walled carbon nanotubes. According to various embodiments, the distribution of the length of the group of multi-walled carbon nanotubes is skewed toward the nominal length of the multi-walled carbon nanotubes. For example, the multi-walled carbon nanotubes are processed and / or applied in a manner that reduces or minimizes the fracture or rupture of the multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the high aspect ratio carbon element network is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more severely skewed toward the nominal length. In some embodiments, at least 75% of the multi-walled carbon nanotubes in the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns.

[0036] According to various embodiments, the positive electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that is soluble in water or alcohols, wherein the active layer exhibits an adhesion of at least 90 N / m to the foil of the electrode. In some embodiments, the active layer exhibits an adhesion of at least 100 N / m to the foil of the positive electrode. In some embodiments, the active layer exhibits an adhesion of about 100 N / m to the foil of the positive electrode. The high aspect ratio carbon element network may include multi-walled carbon nanotubes. The adhesion of the active layer to the foil of the positive electrode can be determined according to the peel test described herein.

[0037] According to various embodiments, the positive electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that is soluble in water or alcohols, wherein the active layer does not exhibit cracks when the positive electrode is wound around a mandrel having a diameter of at least 6 mm. The high aspect ratio carbon element network may include multi-walled carbon nanotubes. In some embodiments, the observation that the active layer does not exhibit any cracks in the active layer is determined based on human observation of the active layer (e.g., the surface of the active layer). In some embodiments, human observation of the active layer is performed by analyzing the positive electrode under a microscope. An example of a test for determining whether the active layer exhibits cracks includes winding a sample positive electrode around a set of mandrels (e.g., from the smallest diameter to the largest diameter), opening the sample positive electrode to observe cracks on the front and back sides, and repeating with a thicker mandrel until no cracks are observed.

[0038] According to various embodiments, the positive electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that is soluble in water or alcohols, wherein the active layer exhibits less than 20% expansion when wetted with an electrolyte. In some embodiments, the active layer exhibits less than 10% expansion when wetted with an electrolyte. In some embodiments, the active layer exhibits expansion between 5% and 20% when wetted with an electrolyte. In some embodiments, the active layer exhibits expansion between 5% and 15% when wetted with an electrolyte. In some embodiments, the active layer exhibits expansion between 5% and 10% when wetted with an electrolyte. The high aspect ratio carbon element network may include multi-walled carbon nanotubes.

[0039] As used herein, "peel test" refers to a 90-degree peel test. A sample having a size of 2.54 cm x 10 cm (e.g., an electrode having an active layer adhered to a foil) is used. The test procedure for the peel test includes (i) cutting the double-sided electrode sample into a size of 10 cm*2.54 cm, (ii) applying double-sided tape on one side and sticking it to the metal plate of the tester; fixing one end of the transparent tape with a clamp and the other end flatly attached to the electrode surface at a 90-degree angle, (iii) zeroing the system: setting the moving mode to "cycle mode"; (iv) opening the test file named "sw-1x-v3" and selecting "com 5" from the settings menu; (v) clicking "clear all data" in the left menu list, setting "set sampling rate" to 0.2s, and selecting "continuous sampling" while starting the tester; (vi) selecting "stop sampling" in the left menu list and stopping the tester; and saving the file.

[0040] Figure 1A is a diagram of an electrode according to various embodiments. In the example shown, an electrode 100 (e.g., a positive electrode) is provided. According to various embodiments, the electrode 100 includes a current collector 102 and an active layer 106. The electrode 100 may optionally include an adhesion layer 104. As an example, the adhesion layer 104 includes a material that promotes adhesion between the current collector 102 and the active layer 106.

[0041] In some embodiments, the current collector 102 is an electrical layer. For example, the current collector 102 may be a metal, a metal alloy, etc. As another example, the current collector 102 is a metal foil. In some embodiments, the current collector 102 is an aluminum foil or an aluminum alloy foil. In some embodiments, the current collector 102 is a copper foil or a copper alloy foil. The current collector 102 has a thickness of less than 15 μm. The current collector 102 has a thickness of less than 10 μm. The current collector 102 has a thickness of less than 8 μm. The current collector 102 has a thickness of less than 5 μm. The current collector 102 has a thickness of less than 15 μm. In some preferred embodiments, the current collector 102 has a thickness between about 6 μm and about 8 μm. In some embodiments, the current collector 102 is an aluminum foil or an aluminum alloy foil, and the current collector 102 has a thickness of about 6 μm.

[0042] In some embodiments, the active layer 106 may include a three-dimensional network of high aspect ratio carbon elements 108 that define void spaces within the network. A plurality of active material particles 110 are disposed in the void spaces within the network. Thus, the active material particles 110 are meshed or entangled in the network, thereby increasing the cohesion of the active layer 106. In some embodiments, the three-dimensional network of high aspect ratio carbon elements 108 provides mechanical support for the active material particles 110.

[0043] According to various embodiments, the three-dimensional network of high aspect ratio carbon elements 108 includes one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanostructures, fragments of single-walled carbon nanotubes, fragments of multi-walled carbon nanotubes, fragments of carbon nanostructures, carbon black, etc. Various other high aspect ratio carbon elements may be implemented.

[0044] According to various embodiments, the active layer 106 (eg, three-dimensional network of high aspect ratio carbon elements 108) includes multi-walled carbon nanotubes. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 106 is between 0.25% and 2% by weight of the active layer.

[0045] The active layer 106 has an average thickness between 20 microns and 200 microns. In some embodiments, the active layer 106 has an average thickness of 20 microns to 30 microns. In some embodiments, the active layer 106 has an average thickness of about 100 microns. Typically, the active layer swells when wetted in an electrolyte. An example for measuring the amount of swelling (e.g., expansion at least in the thickness direction) may include obtaining a sample electrode having a diameter of 1 inch, such as by punching out a sample from a large sheet of electrode with a 1 inch diameter round punch, measuring the thickness of the active layer and recording it, placing the sample electrode in a button cell box, injecting the sample electrolyte into the button cell box, allowing the sample (e.g., with the injected electrolyte) to stand for 1 hour, and after 1 hour, measuring the thickness and recording it, then placing the electrode (such as soaked in electrolyte) in a drying chamber, covering it with a metal tray for 48 hours, and after standing for 48 hours, measuring and recording the thickness of the electrode. According to various embodiments, when wetted with electrolyte, the volume active layer 106 expands (e.g., swells) less than 10%. For example, the thickness of the active layer 106 after wetting with the electrolyte is less than 110% of the thickness of the active layer 106 in the absence of the electrolyte.

[0046] According to various embodiments, in the case where the active layer 106 includes multi-walled carbon nanotubes and single-walled carbon nanotubes, when wetted with an electrolyte in an energy storage device including the electrode 100, the multi-walled carbon nanotubes swell more than the single-walled carbon nanotubes. In some embodiments, when wetted with an electrolyte in an energy storage device including the electrode 100, the multi-walled carbon nanotubes swell at least 15% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes expands at least 15% more than the length of the single-walled carbon nanotubes. In some embodiments, when wetted with an electrolyte in an energy storage device including the electrode 100, the multi-walled carbon nanotubes swell at least 25% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes expands at least 25% more than the length of the single-walled carbon nanotubes. In some embodiments, when wetted with an electrolyte in an energy storage device including the electrode 100, the multi-walled carbon nanotubes swell at least 50% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes expands by at least 50% compared to the length of the single-walled carbon nanotubes. In some embodiments, the multi-walled carbon nanotubes swell up to 50% when wetted (e.g., after being wetted with an electrolyte, the length of the multi-walled carbon nanotubes increases by 50%, and / or after being wetted, the diameter of the multi-walled carbon nanotubes increases by 50%, etc.).

[0047] According to various embodiments, the three-dimensional network of high aspect ratio carbon elements 108 includes carbon nanotubes, and the carbon nanotubes are only multi-walled carbon nanotubes and / or fragments of carbon nanotubes. For example, the three-dimensional network of high aspect ratio carbon elements 108 does not include single-walled carbon nanotubes or fragments of single-walled carbon nanotubes. According to various embodiments, the three-dimensional network of high aspect ratio carbon elements 108 includes at least 99% carbon by weight. In some embodiments, the three-dimensional network of high aspect ratio carbon elements 108 includes a network of electrically interconnected carbon elements that exhibits connectivity above a percolation threshold, and wherein the network defines one or more highly conductive pathways having a length greater than 100 μm;

[0048] According to various embodiments, the high aspect ratio carbon element network defines the void space within the network, and the high aspect ratio carbon element network includes a first group of carbon nanotubes and a second group of carbon nanotubes. Preferably, the first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles, and the second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles. The second group of carbon nanotubes has one or more properties different from the first group of carbon nanotubes. For example, the second group of carbon nanotubes has a number of layers (e.g., walls) different from the number of layers (e.g., walls) of the first group of carbon nanotubes. In some embodiments, the first group of carbon nanotubes includes multi-walled carbon nanotubes. In some embodiments, the second group of carbon nanotubes includes single-walled carbon nanotubes. For example, the high aspect ratio carbon element network includes a group of multi-walled carbon nanotubes and a group of single-walled carbon nanotubes. The group of multi-walled carbon nanotubes may have fragments of multi-walled carbon nanotubes, and / or the group of single-walled carbon nanotubes may have fragments of multi-walled carbon nanotubes. According to various embodiments, the active layer includes a larger amount of multi-walled carbon nanotubes than single-walled carbon nanotubes. Preferably, the active layer includes the first group of carbon nanotubes to the second group of carbon nanotubes in a ratio of about 2:1 by weight.

[0049] In the energy storage device of the related art, the network of carbon elements includes fragmented carbon nanotubes, such as fragmented multi-walled carbon nanotubes. The related art process for manufacturing electrodes is. For example, the fragmented multi-walled carbon nanotubes included in the related art electrode generally have an average length significantly less than the nominal length of the multi-walled carbon nanotubes (e.g., the length of the multi-walled carbon nanotubes before being input into the process for manufacturing the electrode (such as creating an active layer or applying the active layer to the current collector)). The fragmented multi-walled carbon nanotubes included in the related art electrode generally have an average length significantly less than half of the nominal length of the multi-walled carbon nanotubes. The fragmented multi-walled carbon nanotubes included in the related art electrode generally have an average length significantly less than one-third of the nominal length of the multi-walled carbon nanotubes. The method for preparing multi-walled carbon nanotubes or for preparing / manufacturing / applying an active layer for a related art electrode does not gently treat the multi-walled carbon nanotubes and causes the multi-walled carbon nanotubes to break or be crushed. Longer multi-walled carbon nanotubes generally provide better mechanical support for the active material particles in the active layer. For example, when the active material particles expand / contract during the charge / discharge cycle, the longer multi-walled carbon nanotubes provide better mechanical support for the active material particles (e.g., the active material particles are better meshed between the relatively longer multi-walled carbon nanotubes). In addition, the longer multi-walled carbon nanotubes can form a longer interconnected network, and the highly conductive paths formed in the network can provide long conductive paths to facilitate the flow of current within and through the active layer (e.g., in the active layer (such as Figure 1A The conductive path is on the order of the thickness of the active layer 106 of the electrode 100).

[0050] According to various embodiments, the electrode includes relatively longer multi-walled carbon nanotubes compared to the multi-walled carbon nanotubes included in the related art electrode. It is found that the use of relatively long multi-walled carbon nanotubes in the electrode has beneficial mechanical and / or electrical properties. For example, multi-walled carbon nanotubes provide relatively good power at low density. As another example, shorter multi-walled carbon nanotubes are generally not swollen (e.g., expanded) like longer multi-walled carbon nanotubes. Therefore, using shorter multi-walled carbon nanotubes will lose (or reduce) some beneficial properties associated with carbon nanotube swelling. As an extreme example, carbon black does not show swelling because carbon black is only carbon particles without entanglements, such as the entanglements shown by a group of multi-walled carbon nanotubes. Observations during the calendering process indicate that a certain amount of multi-walled carbon nanotubes have a length exceeding a threshold length and therefore have sufficient swelling properties-relatively large amounts of pressure or effects associated with applying to the foil to calender the slurry indicate that the collective swelling (e.g., average swelling) of the multi-walled carbon nanotubes in the active layer will meet a specific performance threshold. However, multi-walled carbon nanotubes are generally difficult to process. The processing of multi-walled carbon nanotubes related to the preparation / formation of active layer and / or electrode is gentler than the processing of related art electrodes. Therefore, the method according to various embodiments keeps longer multi-walled carbon nanotubes (e.g., fewer multi-walled carbon nanotubes are crushed, fragmented, broken, etc.). In some embodiments, the active layer of the electrode includes a group of multi-walled carbon nanotubes, and its average length is greater than the average length of the multi-walled carbon nanotubes in the related art electrodes. According to various embodiments, the distribution of the length of this group of multi-walled carbon nanotubes is skewed toward the nominal length of the multi-walled carbon nanotubes. As an example, the nominal length of the multi-walled carbon nanotubes is about 16 microns. For example, multi-walled carbon nanotubes are processed and / or applied in a manner to reduce or minimize the fracture or rupture of multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the high aspect ratio carbon element network is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more seriously skewed toward the nominal length. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 8 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns.In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 50% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 60% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 75% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, the amount of multi-walled carbon nanotubes having a length shorter than half the nominal length of the multi-walled carbon nanotubes is less than 50% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes having a length shorter than half the nominal length of the multi-walled carbon nanotubes is less than 30% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes having a length shorter than half the nominal length of the multi-walled carbon nanotubes is less than 25% by weight of the active layer.

[0051] Compared with the multi-walled carbon nanotubes in the related art electrodes, the multi-walled carbon nanotubes included in the electrode exhibit an average higher aspect ratio, such as having a longer length. A slurry with high viscosity is prepared and subjected to relatively low shear forces during processing. Therefore, the aspect ratio of the multi-walled carbon nanotubes is retained. In some embodiments, at least a subset of the multi-walled carbon nanotubes included in the active layer is a branched carbon nanotube. In some embodiments, at least a subset of the multi-walled carbon nanotubes included in the active layer is branched, interdigitated, entangled and / or shares a common wall. The characteristics of the multi-walled carbon nanotubes can be obtained using a scanning electron microscope (SEM). According to various embodiments, the multi-walled carbon nanotubes include an average length of at least 5 microns. In some embodiments, the multi-walled carbon nanotubes include an average length of at least 10 microns. In some embodiments, the multi-walled carbon nanotubes include an average length between 10 microns and 15 microns. According to various embodiments, the multi-walled carbon nanotubes include an average diameter between 6nm and 15nm. In some embodiments, the multi-walled carbon nanotubes include an average diameter between 6nm and 10nm. According to various embodiments, the multi-walled carbon nanotubes include an average of 3 to 15 layers. In some embodiments, the multi-walled carbon nanotubes include an average of 3 to 15 layers. In some embodiments, the multi-walled carbon nanotubes include an average of 5 to 10 layers. In some embodiments, the multi-walled carbon nanotubes include an average of 6 to 7 layers. In some embodiments, the multi-walled carbon nanotubes include an average of at least 6 layers. In some embodiments, the multi-walled carbon nanotubes include an average aspect ratio of at least 100. In some embodiments, the multi-walled carbon nanotubes include an average aspect ratio between 200 and 1000.

[0052] According to various embodiments, the electrode includes a material selected from the group consisting of LiCoO2, LiNiO2, LiMn2O4, LiCoPO4, LiFePO4, LiNiMhCoO2, and LiNi1-x-y-z Co x M1 y M2 z O z Particles of at least one electrode active material in the group consisting of (wherein M1 and M2 are each independently selected from the group consisting of Al, Ni, Co, Fe, Mn, V, Cr, Ti, W, Ta, Mg and Mo, and x, y and z represent the atomic fractions of the corresponding constituent elements of the oxide, and satisfy the relationship 0≦x<0.5, 0≦y<0.5, 0≦z<0.5).

[0053] According to various embodiments, the plurality of active material particles 110 include a lithium-based material. In some embodiments, the plurality of active material particles 110 include iron phosphate. In some embodiments, the plurality of active material particles 110 include lithium metal oxide. In some embodiments, the plurality of active material particles 110 include one or more of lithium metal oxide, lithium sulfur, and lithium cobalt oxide. In some embodiments, the plurality of active material particles 110 include lithium nickel manganese cobalt oxide. In some embodiments, the plurality of active material particles 110 include lithium nickel cobalt aluminum oxide. In some embodiments, the plurality of active material particles 110 include lithium nickel cobalt manganese aluminum oxide.

[0054] Active layer 106 includes a relatively large amount of active material particles. In some embodiments, active layer 106 includes at least 98.5% active material particles by weight of the active layer. In some embodiments, active layer 106 includes between 96.0% and 98.5% active material particles by weight of the active layer.

[0055] According to various embodiments, the active layer 106 includes a polymer additive. The polymer additive may provide mechanical support for at least a subset of the plurality of active material particles 110 and / or at least a portion of the three-dimensional network of high aspect ratio carbon elements 108. For example, the polymer additive may bond or adhere to the active material particles or carbon elements such as carbon nanotubes (e.g., multi-walled carbon nanotubes and / or single-walled carbon nanotubes). According to various embodiments, electrochemically stable polymers have been found to have beneficial properties as polymer additives for the active layer 106. The polymer additive may be selected to be a polymer that is completely soluble or highly soluble in a solvent used in the process electrode 100. For example, the polymer additive may be soluble or highly soluble in water or alcohols such as ethanol.

[0056] Related Art Electrodes often use polymer binders that are soluble only in toxic or environmentally unfriendly solvents. Polymer binders are used to disperse, adhere, bind particles, and survive in harsh environments. Energy storage device batteries may slowly lose capacity after hundreds or thousands of cycles and charge / discharges. Polymer binders can help maintain the capacity of energy storage devices over their service life.

[0057] According to various embodiments, the electrode 100 and / or the active layer 106 do not include (e.g., are free of) polymer additives that are insoluble in one or more of water or alcohols (such as ethanol). In some embodiments, the electrode 100 is substantially free of polymer additives that are insoluble in one or more of water or alcohols (such as ethanol). In some embodiments, the electrode 100 and / or the active layer 106 of the electrode 100 is free of or substantially free of polymer additives that are insoluble in one or more of water or alcohols (such as ethanol). For example, any polymer additive of the electrode 100 may be soluble in one or more of water and alcohols.

[0058] The polymer additive may be selected based at least in part on its reaction with certain electrolytes used in an energy storage device including the electrode 100. In some embodiments, a polymer additive having a relatively high (e.g., very high) molecular weight is selected because such polymer additives are generally resistant to solvents. For example, polymer additives with high molecular weights do not dissolve in solvents, while polymers with low molecular weights become viscous. In some embodiments, the polymer additive is selected as a polymer that does not become soft (e.g., softer than a softness threshold) when mixed with an electrolyte. In some embodiments, the polymer additive is selected as a polymer that does not substantially swell (e.g., swells or expands beyond a predetermined swelling threshold) when wetted / mixed with an electrolyte used in an energy storage device.

[0059] Active layer 106 may include a polymer additive that is soluble in water and / or alcohols (such as ethanol). In some embodiments, the polymer additive has a relatively high molecular weight. For example, the polymer additive has a molecular weight greater than 200 g / mol. In some embodiments, the polymer additive has a molecular weight greater than 500,000 g / mol. In some embodiments, the polymer additive has a molecular weight greater than 1,000,000 g / mol. In some embodiments, the polymer additive has a molecular weight between 500,000 g / mol and 1,500,000 g / mol.

[0060] The polymer additive may have a 3 With 2.5g / cm 3 In some embodiments, the polymer additive has a specific gravity greater than 1.135 g / cm 3 In some embodiments, the polymer additive has a specific gravity greater than 1.20 g / cm 3 The specific gravity of the polymer additive can be measured according to the ASTM D792 test method.

[0061] The polymer additive may have a specific heat between 1.5 J / g°C at 23°C and 3.5 J / g°C at 23°C. In some embodiments, the polymer additive has a specific heat greater than 2.0 J / g°C at 23°C. In some embodiments, the polymer additive has a specific heat greater than 2.2 J / g°C at 23°C. In some embodiments, the polymer additive has a specific heat of about 2.4 J / g°C at 23°C. The specific heat of the polymer additive may be measured based on a DSC measurement.

[0062] When the polymer additive is dry, the polymer additive may have a tensile strength between 4MPa and 100MPa. As an example, when the polymer additive is dry, the polymer additive has a tensile strength between 4MPa and 70MPa. In some embodiments, the polymer additive has a tensile strength less than 70MPa measured when the polymer additive is dry. In some embodiments, the polymer additive has a tensile strength less than 50MPa measured when the polymer additive is dry. In some embodiments, the polymer additive has a tensile strength less than 25MPa measured when the polymer additive is dry. In some embodiments, the polymer additive has a tensile strength less than 10MPa measured when the polymer additive is dry. In some embodiments, the polymer additive has a tensile strength less than 7.5MPa measured when the polymer additive is dry. In some embodiments, the polymer additive has a tensile strength between 5MPa and 6MPa measured when the polymer additive is dry. The tensile strength of the polymer additive can be measured based on the ASTM D638 test method.

[0063] The polymer additive may have an elongation at yield greater than 4%. As an example, the polymer additive has an elongation at yield greater than 4% and less than 50% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 5% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 10% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 20% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 25% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield between 20% and 30% measured when the polymer additive is dry. The elongation at yield of the polymer additive can be measured based on the ASTM D638 test method.

[0064] According to various embodiments, the active layer 106 includes a polymer additive selected from the polyamide family, or a modified polyamide or a polyamide derivative. The polymer additive is soluble in water or alcohols such as ethanol. In some embodiments, the polymer additive has a relatively high molecular weight. The polymer additive may be at least partially disposed in at least one void space defined by a high aspect ratio carbon element network. In some embodiments, the polymer additive acts as a polymer binder. When the mixture of the polymer additive and ethyl cellosolve is cooled, the polymer additive exhibits gelation. As an example, the polymer additive is completely soluble in each of water, ethylene glycol, benzyl alcohol, acetic acid, and isobutyl alcohol. As an example, the polymer additive is completely soluble in N-methylpyrrolidone. The solubility of the polymer additive can be measured by adding 10g of the polymer additive to 100ml of a specific solvent, stirring the mixture at 80°C for about 3 hours, and after stirring, cooling the mixture to room temperature, and then observing the mixture.

[0065] Because the polymer additive provides mechanical support for the electrode 100 (e.g., provides mechanical support for the active material particles and / or carbon elements), the polymer additive is selected so that the polymer additive has a glass transition temperature that is typically outside the operating temperature of the energy storage device. In some embodiments, the polymer additive has a glass transition temperature of less than 0°C. In some embodiments, the polymer additive has a glass transition temperature of less than -10°C. In some embodiments, the polymer additive has a glass transition temperature of less than -25°C. In some embodiments, the polymer additive has a glass transition temperature of less than -30°C. In some embodiments, the polymer additive has a glass transition temperature of less than -40°C. In some embodiments, the polymer additive has a glass transition temperature of less than -45°C. In some embodiments, the polymer additive has a glass transition temperature between -50°C and -40°C. The glass transition temperature of the polymer additive can be measured based on DSC measurements.

[0066] According to various embodiments, the polymer additive has a 5% weight reduction temperature between 375° C. and 400° C. In some embodiments, the polymer additive has a 5% weight reduction temperature of about 385° C. The polymer additive may be selected such that an aqueous solution of the polymer additive and at least one of water and an alcohol exhibits a viscosity of at least 60 Pa·s at a concentration of about 50% by weight of the polymer additive.

[0067] The active layer 106 may include less than 5% of the polymer additive by weight of the active layer. In some embodiments, the active layer 106 includes approximately 0.5% of the polymer additive by weight of the active layer. In some embodiments, the active layer 106 includes between 0.25% and 1.5% of the polymer additive by weight of the active layer. In some embodiments, the active layer 106 includes less than 1.5% of the polymer additive by weight of the active layer.

[0068] Examples of polymer additives include polyethylene oxide (PEO), polyethers, poly(ethylene glycol) (PEG) derivatives, fluoropolymers (particularly poly(vinylidene fluoride) (PVDF)), polyurethanes (PU), polytetrafluoroethylene (PTFE), alginate (Alg), refolded DNA / Alg, Alg-catechol, PAA-catechol, carboxymethyl chitosan, guar gum, agarose, konjac glucomannan, carboxymethylated gellan gum, PDA-PAA-PEO, pectin / PAA, partially lithiated PAA and Nafion, sequence-defined peptoids, PMDOPA, branched PAA, NaPAA-g-CMC, CS-g-PAANa, PVA-g-PAA, GC-g-LiPAA, PVDF-g-P AA, branched PAA-PEG, CS-g-PANI, hyperbranched β-cyclodextrin, double helical natural xanthan gum, Li-Nafion, PAA / CMC, cross-linked PAA / PVA, glycerol cross-linked PEDOT:PSS, MAH cross-linked corn starch, MAH cross-linked CMC, cross-linked natural GG polymer, cross-linked chitosan, CS-CG+GA, cross-linked dextrin, cross-linked CMC-PEG, cross-linked hyperbranched PEI, cross-linked PAM hydrogel, cross-linked PU elastomer, cross-linked PVA-PEI, TMM functionalized PVA network, polymers including polyamides (e.g., nylon), functionalized polyamides, copolymers of PEO and polyamide, self-healing polymers, PAA-Upy supramolecular, self-healing PAU-g-PEG, Ca 2+ Cross-linked SA hydrogel, (Fe 3+ ) cross-linked (PANa 0.8 Fe y )、Sn 4+ Cross-linked PEDOT:PSS, PAA-PEG-PBI, cross-linked CMC-CPAM, metal polymers, Si@Fe 3+-PDA-PAA, β-CDp / 6AD, slide ring PR-PAA, conductive PFFOMB, PEG-grafted PFP, PF-COONa, PFPQ-COONa, pyrene (PPyE), pyrene (PPyMAA), pyrene (PPyMADMA), PANI, FA-doped PEDOT:PSS, stretchable conductive glue, poly (phenanthrenequinone), cyclized PAN, PAA-P (HEA-co-DMA), PEDOT:PSS / PEO / PEI, PAA / PVA+elastic gel polymer electrolyte, PAA+BFPU, mixture of PU and poly (acrylic acid) (PAA), copolymers of any subset of the foregoing, etc. Zhao, YM. et al. 2021, "Various other polymers may be implemented as the polymeric additive", InfoMat, Vol. 3, No. 5, pp. 460-501 (hereinafter referred to as "Zhao") provides a description of various polymers that can be implemented as polymer additives. Zhao is incorporated herein in its entirety for all purposes.

[0069] In some embodiments, the surface treatment 202 (not shown, see Figure 2 ) is applied on the surface of the high aspect ratio carbon element 108 of the network. The surface treatment promotes adhesion between the high aspect ratio carbon element and the active material particles 110. The surface treatment may also promote adhesion between the high aspect ratio carbon element and the current collector 102 (also referred to herein as a "conductive layer"), the optional adhesion layer 104 and / or at least a subset of the active material particles 110. The surface treatment may include a surfactant layer bonded to the high aspect ratio carbon element 108 and including a plurality of surfactant elements, each surfactant element having a hydrophobic end and a hydrophilic end, wherein the hydrophobic end is disposed proximal to one of the surfaces in the high aspect ratio carbon element 108 and the hydrophilic end is disposed distal to one of the surfaces in the high aspect ratio carbon element 108. In some embodiments, the surface treatment 202 includes at least a portion of a polymer additive. In some embodiments, the surface treatment includes a material soluble in a solvent having a boiling point below 202°C. In some embodiments, the surface treatment includes a material soluble in a solvent having a boiling point below 185°C.

[0070] According to various embodiments, the active layer 106 includes a dispersant. The dispersant can be selected based on compatibility with water and / or alcohols (such as ethanol). In some embodiments, the dispersant is a water-soluble polymer. In some embodiments, the dispersant corresponds to or includes polyvinyl pyrrolidone (PVP). The PVP used for the dispersant can be a PVP with a relatively high molecular weight.

[0071] According to various embodiments, the active layer 106 includes about 25% of the dispersant by weight of the active layer 106. In some embodiments, the amount of dispersant included in the active layer 106 is between 10% and 50% by weight of the active layer 106. In some embodiments, the amount of dispersant included in the active layer 106 is between 15% and 40% by weight of the active layer 106. In some embodiments, the amount of dispersant included in the active layer 106 is between 20% and 30% by weight of the active layer 106.

[0072] According to various embodiments, the electrode 100 (e.g., the active layer 106) includes active material particles 110 including lithium iron phosphate (LFP). LFP is generally cheaper than nickel or cobalt, such as in the case of an electrode including nickel cobalt aluminum oxide. In addition, electrodes including LFP generally have relatively low toxicity. However, the energy density of LFP is lower than that of lithium cobalt oxide. In the case where the electrode 100 and / or the active layer 106 include LFP, the active layer 106 includes a polymer additive in an amount between 0.5% and 5% by weight of the active layer 106. For example, even if the absolute amount of the polymer additive is equal between an electrode including LFP and an electrode including cobalt or nickel, because LFP is lighter than cobalt or nickel, the relative weight percentage of LFP is higher. In some embodiments, the LFP included in the active layer 106 is in the form of nanoparticles. Therefore, a larger absolute amount of polymer additive may be required compared to an electrode including nickel or cobalt. According to various embodiments, an electrode including LFP includes carbon between 0.5% and 5% by weight in the active layer 106. In some embodiments, the electrode including LFP includes multi-walled carbon nanotubes in an amount between 0.5% and 5% by weight in the active layer 106. The polymer additive used in conjunction with the positive electrode including LFP can be water-soluble. For example, the processing of LFP is typically a water-based process. In the case where the positive electrode includes LFP, the active layer 106 includes a dispersant in an amount between 0.1% and 2% by weight of the active layer 106. In some embodiments, the active layer 106 includes a dispersant in an amount between 0.5% and 1.5% by weight of the active layer 106.

[0073] Figure 1B is a diagram of an electrode according to various embodiments. In the example shown, an electrode 125 (e.g., a positive electrode) is provided. According to various embodiments, the electrode 125 includes a current collector 128 and an active layer 132. The electrode 125 may optionally include an adhesion layer 130. As an example, the adhesion layer 130 includes a material that promotes adhesion between the current collector 128 and the active layer 132. In some embodiments, the current collector 128 corresponds to (or is similar to) Figure 1A The current collector 102 is provided.

[0074] In some embodiments, the active layer 132 corresponds to (or is similar to) Figure 1A The current active layer 106 of the electrode. According to various embodiments, the active layer of the electrode includes a group of multi-walled carbon nanotubes (e.g., represented by 134 and shown in solid lines) and a group of single-walled carbon nanotubes (e.g., represented by 136 and shown in dashed lines). In some embodiments, the average aspect ratio of the group of multi-walled carbon nanotubes is greater than the average aspect ratio of the group of single-walled carbon nanotubes.

[0075] According to various embodiments, the active layer 132 includes multi-walled carbon nanotubes and single-walled carbon nanotubes. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 132 is between 0.25% and 2% by weight of the active layer. In some embodiments, the amount of single-walled carbon nanotubes included in the active layer 136 is between 0.01% and 0.25% by weight of the active layer. According to various embodiments, the ratio of multi-walled carbon nanotubes in the active layer 132 to single-walled carbon nanotubes in the active layer 136 by weight of the active layer is about 2:1.

[0076] In some embodiments, the amount of multi-walled carbon nanotubes included in active layer 132 is between 0.25% and 2% by weight of the active layer. In some embodiments, the amount of single-walled carbon nanotubes included in active layer 132 is between 0.01% and 0.25% by weight of the active layer.

[0077] The single-walled carbon nanotubes included in the electrode show a longer length than the single-walled carbon nanotubes in the related art electrode on average. Prepare a slurry with high viscosity and withstand relatively low shear force during processing. The characteristics of multi-walled carbon nanotubes can be obtained using a scanning electron microscope (SEM). According to various embodiments, the single-walled carbon nanotube includes a length range between 1nm and 34nm. The average length of the single-walled carbon nanotube can be between 7 microns and 8 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 1nm and 2nm and an average length of about 5 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 3nm and 5nm and an average length of at least 200 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 3nm and 5nm and an average length between 7 microns and 8 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 5nm and 6nm and an average length between 7 microns and 8 microns. In some embodiments, the single-walled carbon nanotube includes an average of 1 or 2 layers of wall.

[0078] Figure 1C 1 is a diagram of an electrode according to various embodiments. In the example shown, the active layer of the electrode 150 includes a functionalized carbon element. As an example, the functionalized carbon element can be based at least in part on Figure 1AThe high aspect ratio carbon elements 108 (eg, a group of multi-walled carbon nanotubes and / or a group of single-walled carbon nanotubes, etc.) of the active layer 106 of the electrode 100 shown in FIG. 1 are obtained by surface treatment.

[0079] In some embodiments, the functionalized carbon element is formed from a dried (eg, freeze-dried) aqueous dispersion comprising nanoform carbon and a functionalizing material (such as a surfactant). In some such embodiments, the aqueous dispersion is substantially free of materials that would damage the carbon element, such as an acid.

[0080] In some embodiments, the surface treatment of the high aspect ratio carbon element comprises a thin polymer layer disposed on the carbon element that promotes adhesion of the active material to the network. In some such embodiments, the thin polymer layer comprises a self-assembling and / or self-limiting polymer layer. In some embodiments, the thin polymer layer is bonded to the active material, for example via hydrogen bonding.

[0081] In some embodiments, the thickness of the thin polymer layer in a direction perpendicular to the outer surface of the carbon element may be less than 3, 2, 1, 0.5, 0.1 (or less) times the minor dimension of the element.

[0082] In some embodiments, the thin polymer layer includes functional groups (e.g., pendant functional groups) bonded to the active material, e.g., via non-covalent bonds (such as π-π bonds). In some such embodiments, the thin polymer layer can form a stable covering layer on at least a portion of the carbon element.

[0083] In some embodiments, the thin polymer layer on some elements may be bonded to a current collector or an adhesion layer disposed thereon and located below an active layer comprising an energy storage (i.e., active) material. For example, in some embodiments, the thin polymer layer includes side functional groups bonded to the surface of the current collector or the adhesive layer, for example, via non-covalent bonds (such as π-π bonds). In some such embodiments, the thin polymer layer may form a stable covering layer on at least a portion of the element. In some embodiments, this arrangement provides excellent mechanical stability of the electrode.

[0084] In some embodiments, the polymeric material is miscible in a solvent of the type described in the above examples. For example, in some embodiments, the polymeric material is miscible in a solvent comprising alcohols such as methanol, ethanol or 2-propanol (isopropanol, sometimes referred to as IPA) or a combination thereof. In some embodiments, the solvent may include one or more additives for further improving the properties of the solvent, such as low boiling point additives, such as acetonitrile (ACN), deionized water and tetrahydrofuran. In this example, the mixture is formed in a solvent without NMP.

[0085] In yet further exemplary embodiments, the surface treatment may be formed of a carbonaceous material layer produced by pyrolysis of a polymeric material disposed on a high aspect ratio carbon element. The carbonaceous material layer (e.g., graphite or amorphous carbon) may be attached (e.g., via covalent bonds) to or otherwise promote adhesion to the active material particles. Examples of suitable pyrolysis techniques are described in U.S. Patent Application Serial No. 63 / 028,982 filed on May 22, 2020, which is incorporated herein in its entirety for all purposes. One polymeric material suitable for use in this technology is polyacrylonitrile (PAN)

[0086] According to various embodiments, the active layer 106 includes a dispersant. The dispersant can be selected based on compatibility with water and / or alcohols (such as ethanol). In some embodiments, the dispersant is a water-soluble polymer. In some embodiments, the dispersant corresponds to or includes polyvinyl pyrrolidone (PVP). The PVP used for the dispersant can be a PVP with a relatively high molecular weight.

[0087] Figure 2 2 is a diagram of an electrode according to various embodiments. In the example shown, a detailed view of a high aspect ratio carbon element 201 of a network 200 is provided (eg, Figure 1A and 1B ), which is located near a number of active material particles 300. In the illustrated embodiment, the surface treatment 202 on the element 201 is an outer layer of a surfactant layer bonded to the surface of the element 201. As shown, the surfactant layer includes a plurality of surfactant elements 210, each having a hydrophobic end 211 and a hydrophilic end 212, wherein the hydrophobic end is disposed proximal to the surface of the carbon element 201 and the hydrophilic end 212 is disposed distal to the surface.

[0088] In some embodiments where the carbon element 201 is hydrophobic (typically the case for nanoform carbon elements such as carbon nanotubes, carbon nanotube bundles, and graphene flakes), the hydrophobic end 211 of the surfactant element 210 will be attracted to the carbon element 201. Thus, in some embodiments, the surface treatment 202 can be a self-assembled layer. For example, as described in detail below, in some embodiments, when the carbon element 201 is mixed with the surfactant element 210 in a solvent to form a slurry, the surface treatment 202 layer self-assembles on the surface due to electrostatic interactions between the element 201 and the surfactant element 210 within the slurry.

[0089] In some embodiments, the surface treatment 202 is applied to a three-dimensional network of high aspect ratio carbon elements (e.g., Figure 1A The surface treatment promotes the bonding of the high aspect ratio carbon element with the active material particles 300 (e.g., Figure 1AThe surface treatment may also promote adhesion between the high aspect ratio carbon element and the current collector (also referred to herein as the "conductive layer"), such as Figure 1A The current collector 102 of the electrode 100 and / or the optional adhesion layer (e.g., Figure 1A Adhesion layer 104 of electrode 100).

[0090] In some embodiments, the surface treatment 202 can be a self-limiting layer. For example, as described in detail below, in some embodiments, when the element 201 is mixed with the surfactant element 210 in a solvent to form a slurry, due to the electrostatic interaction between the element 201 and the surfactant element 210 in the slurry, the surface treatment 202 layer is self-assembled on the surface. In some such embodiments, once the area on the surface of the element 201 is covered by the surfactant element 210, additional surfactant elements 210 will not be attracted to the area. In some embodiments, once the surface of the element 201 is covered by the surfactant element 202, further elements are repelled from the layer, thereby causing a self-limiting process. For example, in some embodiments, the surface treatment 202 can be formed in a self-limiting process, thereby ensuring that the layer is very thin, such as a single molecule or a few molecules thick.

[0091] In some embodiments, the hydrophilic ends 212 of at least a portion of the surfactant elements form bonds with the active material particles 300. Thus, the surface treatment 202 can provide good adhesion between the elements 201 of the network 200 and the active material particles. In some embodiments, the bonds can be covalent bonds, or non-covalent bonds, such as π-π bonds, hydrogen bonds, electrostatic bonds, or combinations thereof.

[0092] For example, in some embodiments, the hydrophilic end 212 of the surfactant element 210 has a polar charge of a first polarity; while the surface of the active material particles 300 carries a polar charge of a second polarity opposite to the first polarity, and thus attract each other.

[0093] For example, in some embodiments, during the formation of layer 100, active material particles 300 are combined in a solvent with carbon elements 201 bearing surface treatment 202 (as described in more detail below), and the outer surface particles 300 of the active material can be characterized by having a zeta potential (as known in the art) of opposite sign to the zeta potential of the outer surface of surface treatment 202. Thus, in some such embodiments, the attraction between carbon elements 201 bearing surface treatment 202 and active material product 300 promotes self-assembly of a structure in which active material particles 300 are meshed with carbon elements 201 of network 200.

[0094] In some embodiments, the hydrophilic end 212 of at least a portion of the surfactant element forms a bond with a current collector layer or an adhesion layer located below the active material layer 100. Thus, the surface treatment 202 can provide good adhesion between the element 201 of the network 200 and such an underlying layer. In some embodiments, the bond can be a covalent bond, or a non-covalent bond, such as a π-π bond, a hydrogen bond, an electrostatic bond, or a combination thereof. In some embodiments, this arrangement provides excellent mechanical stability of the electrode 10, as discussed in more detail below.

[0095] In various embodiments, the surfactant used to form the surface treatment 202 as described above may include any suitable material. For example, in some embodiments, the surfactant may include one or more of the following: hexadecyltrimethylammonium hexafluorophosphate (CTAP), hexadecyltrimethylammonium tetrafluoroborate (CTAB), hexadecyltrimethylammonium acetate, hexadecyltrimethylammonium nitrate, high amidopropyl betaine, N-(cocoalkyl)-N,N,N-methyltrimethylammonium sulfate, and cocamidopropyl betaine. Additional suitable materials are described below.

[0096] In some embodiments, the surfactant layer 202 can be formed by dissolving a compound in a solvent such that the surfactant layer is formed from ions from the compound (e.g., in a self-limiting process as described above). In some such embodiments, the active layer 100 will include residual counter ions 214 of the surfactant ions that form the surface treatment 202.

[0097] In some embodiments, these surfactant counterions 214 are selected to be compatible with use in an electrochemical cell. For example, in some embodiments, the counterions are selected to be non-reactive or mildly reactive with materials used in the cell (e.g., electrolyte, separator, housing, etc.). For example, if an aluminum housing is used, the counterions may be selected to be non-reactive or mildly reactive with the aluminum housing.

[0098] For example, in some embodiments, the residual counter ions contain no or substantially no halide groups. For example, in some embodiments, the residual counter ions contain no or substantially no bromine.

[0099] In some embodiments, the residual counterions may be selected to be compatible with the electrolyte used in the energy storage cell comprising the active layer 200. For example, in some embodiments, the residual counterions may be the same ion species used in the electrolyte itself. For example, if the electrolyte includes a dissolved Li PF6 salt, the electrolyte anion is PF6. In such cases, the surfactant may be selected, for example, CTA PF6, such that the surface treatment 202 is formed as an anionic layer from CTA PF6, while the residual surfactant counterions are PF6 anions from CTA PF6 (thereby matching the anions of the electrolyte).

[0100] In some embodiments, the surfactant material used is soluble in a solvent that exhibits favorable properties. For example, in some embodiments, the solvent may include water or alcohols, such as methanol, ethanol or 2-propanol (isopropanol, sometimes referred to as IPA) or a combination thereof. In some embodiments, the solvent may include one or more additives for further improving the properties of the solvent, such as low boiling point additives, such as acetonitrile (ACN), deionized water and tetrahydrofuran.

[0101] For example, if a low boiling point solvent is used in the formation of the surface treatment 202, a thermal drying process (e.g., of the type described in more detail below) performed at a relatively low temperature can be used to quickly remove the solvent. As will be appreciated by those skilled in the art, this can increase the speed and / or cost of manufacturing the active layer 202.

[0102] For example, in some embodiments, the surface treatment 202 is formed of a material that is soluble in a solvent having a boiling point less than 250°C, 225°C, 202°C, 200°C, 185°C, 180°C, 175°C, 150°C, 125°C, or lower, such as less than or equal to 100°C.

[0103] In some embodiments, the solvent may exhibit other advantageous properties. In some embodiments, the solvent may have a low viscosity, such as a viscosity at 20° C. less than or equal to 3.0 centipoise, 2.5 centipoise, 2.0 centipoise, 1.5 centipoise, or less. In some embodiments, the solvent may have a low surface tension, such as a surface tension at 20° C. less than or equal to 40 mN / m, 35 mN / m, 30 mN / m, 25 mN / m, or less. In some embodiments, the solvent may have a low toxicity, such as a toxicity comparable to that of alcohols such as isopropanol.

[0104] It is noteworthy that this is in contrast to the process for forming a conventional electrode active layer, which is characterized by a bulk binder material (such as polyvinylidene fluoride or polyvinylidene fluoride (PVDF)). Such bulk binders require an aggressive solvent characterized by a high boiling point. One such example is n-methyl-2-pyrrolidone (NMP). Using NMP (or other pyrrolidone-based solvents) as a solvent requires the use of a high temperature drying process to remove the solvent. In addition, NMP is expensive, requires a complex solvent recovery system, and is highly toxic, with significant safety issues. On the contrary, as described in further detail below, in various embodiments, active layer 200 can be formed without using NMP or similar compounds (such as pyrrolidone compounds).

[0105] Although one class of exemplary surface treatments 202 is described above, it should be understood that other treatments may be used. For example, in various embodiments, the surface treatment 202 may be formed by functionalizing the high aspect ratio carbon element 201 using any suitable technique as described herein or known in the art. The functional groups applied to the element 201 may be selected to promote adhesion between the active material particles 300 and the network 200. For example, in various embodiments, the functional groups may include carboxyl groups, hydroxyl groups, amine groups, silane groups, or combinations thereof.

[0106] As will be described in more detail below, in some embodiments, the functionalized carbon element 201 is formed from a dried (e.g., freeze-dried) aqueous dispersion comprising nanoform carbon and a functionalizing material (such as a surfactant). In some such embodiments, the aqueous dispersion is substantially free of materials that can damage the carbon element 201, such as an acid.

[0107] Figure 3 is a diagram of electrodes according to various embodiments.

[0108] refer to Figure 3 In some embodiments, the surface treatment 202 on the high aspect ratio carbon element 201 includes polymer particles disposed on the carbon element that promote adhesion of the active material to the network. In some such embodiments, the polymer particles include a self-assembling and / or self-limiting polymer layer. In some embodiments, the polymer particles bond to the active material, for example via hydrogen bonding.

[0109] In some embodiments, the polymer particles include functional groups (eg, pendant functional groups) bonded to the active material, eg, via non-covalent bonds (such as π-π bonds). In some such embodiments, the polymer particles may form a stable covering layer on at least a portion of element 201 .

[0110] In some embodiments, the polymer particles on some of the elements 201 may be bonded to the current collector 101 or the adhesion layer 102 located below the active layer 200. For example, in some embodiments, the polymer particles include side functional groups that are bonded to the surface of the current collector 101 or the adhesion layer 102, for example, via non-covalent bonds (such as π-π bonds). In some such embodiments, the polymer particles may form a stable covering layer on at least a portion of the element 201. In some embodiments, this arrangement provides excellent mechanical stability of the electrode 10, as discussed in more detail below.

[0111] In some embodiments, the polymeric material is miscible in solvents of the types described in the examples above. For example, in some embodiments, the polymeric material is miscible in solvents including alcohols such as methanol, ethanol, or 2-propanol (isopropanol, sometimes referred to as IPA), or combinations thereof. In some embodiments, the solvent may include one or more additives to further improve the properties of the solvent, such as low boiling point additives such as acetonitrile (ACN), deionized water, and tetrahydrofuran.

[0112] Suitable examples of materials that can be used for the polymeric particles include water-soluble polymers, such as polyvinylpyrrolidone.Additional exemplary materials are provided below.

[0113] Figure 4 are examples of electron micrographs of active layers according to various embodiments.

[0114] refer to Figure 4 , shows an electron micrograph of an exemplary active material layer of the type described herein. Tendril-like high aspect ratio carbon elements 201 (formed from CNT bundles) are clearly shown intermeshing active material particles 300. In some embodiments, the active layer lacks any bulk polymer material occupying space within the layer.

[0115] Negative electrode:

[0116] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, wherein the active material particles include silicon, and (iii) a polymer additive. In some embodiments, the silicon included in the active material particles includes one or more of silicon oxide and microsilicon. In some embodiments, the polymer additive is water-processable.

[0117] In some embodiments, the polymer additive includes one or more of a polyolefin, a poly(acrylic acid), and a styrene-butadiene rubber (SBR). In some embodiments, the amount of the polymer material included in the active layer is about 8% by weight of the active layer. In some embodiments, the amount of the polymer material included in the active layer is equal to or less than 8% by weight of the active layer. In some embodiments, the amount of the polymer material included in the active layer is about 10% by weight of the active layer. In some embodiments, the amount of the polymer material included in the active layer is equal to or less than 10% by weight of the active layer. In some embodiments, the amount of the polymer material included in the active layer is less than 12% by weight of the active layer. In some embodiments, the amount of the polymer material included in the active layer is less than 15% by weight of the active layer.

[0118] According to various embodiments, the active layer includes a polymer additive, which includes a polyolefin. In some embodiments, the average particle size of the polyolefin is 1 μm or less. In some embodiments, the polyolefin includes an unsaturated hydrocarbon with 3 to 6 carbon atoms, and is at least one of a propylene component and a 1-butene component. In some embodiments, the polymer additive including the polyolefin is manufactured using a polyolefin resin including 50% to 98% by mass of unsaturated hydrocarbons with 3 to 6 carbon atoms and 0.5% to 20% by mass of unsaturated carboxylic acid units. In some embodiments, the polyolefin includes an ethylene component. In some embodiments, the polyolefin includes (i) an unsaturated hydrocarbon with 3 to 6 carbon atoms, and is at least one of a propylene component and a 1-butene component, and (ii) an ethylene component. In some embodiments, the polyolefin includes a crosslinking agent and / or a tackifier. In some embodiments, the polyolefin includes at least one selected from the group consisting of maleic anhydride, acrylic acid and methacrylic acid.

[0119] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive. In some embodiments, the polymer additive includes one or more of polyolefins, poly(acrylic acid) and styrene-butadiene rubber (SBR). In some embodiments, the silicon included in the active material particles includes one or more of silicon oxide and microsilicon. In some embodiments, the active layer includes silicon-based particles between 20% and 95% by weight relative to the weight of the active layer. In some embodiments, the active layer includes silicon-based particles between 50% and 95% by weight relative to the weight of the active layer. In some embodiments, the active layer includes silicon-based particles greater than 75% by weight relative to the weight of the active layer. In some embodiments, the active layer includes silicon-based particles greater than 80% by weight relative to the weight of the active layer. In some embodiments, the active layer includes silicon-based particles between 20% and 75% by weight relative to the weight of the active layer. In some embodiments, the active layer comprises greater than 20% silicon particles (e.g., micro-silicon) by weight relative to the weight of the active layer. In some embodiments, the active layer comprises between 20% and 40% silicon particles (e.g., micro-silicon) by weight relative to the weight of the active layer. In some embodiments, the active layer comprises between 30% and 40% silicon particles (e.g., micro-silicon) by weight relative to the weight of the active layer. In some embodiments, the active layer comprises greater than 50% silicon oxide particles by weight relative to the weight of the active layer. In some embodiments, the active layer comprises between 60% and 70% silicon oxide particles by weight relative to the weight of the active layer.

[0120] According to various embodiments, the active layer includes silicon-based particles. In some embodiments, the active layer includes both microsilicon particles and silicon oxide particles. In some embodiments, the active layer includes microsilicon particles and is substantially free of silicon oxide particles (e.g., the active layer does not include any silicon oxide particles). The silicon oxide particles do not appear to expand to the same extent as microsilicon (e.g., pure silicon). For example, the oxide layer around silicon is large enough so that the expansion of silicon in silicon oxide does not generally cause the silicon oxide to expand too significantly. In contrast, microsilicon expands and contracts to a greater extent than silicon oxide, thereby creating more challenges to maintaining the electrical and / or mechanical properties of an electrode (e.g., a negative electrode). For example, the expansion of microsilicon can destroy electrical connections within an electrode (e.g., in an active layer), or the mechanical stability of an electrode. Various embodiments provide a network of high aspect ratio carbon elements that maintain electrical connections and mechanical support during charge / discharge cycles.

[0121] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network, which defines the void space within the network, (ii) a plurality of electrode active material particles, which are arranged in the void space within the network, and the plurality of electrode active material particles include a plurality of silicon-based particles (e.g., micro-silicon, silicon oxide, etc.), and (iii) a polymer additive. The polymer additive has a relatively high molecular weight. In some embodiments, the polymer additive has a molecular weight of at least 400,000 g / mol. In some embodiments, the polymer additive has a molecular weight of at least 1,000,000 g / mol. In some embodiments, the polymer additive has a molecular weight of at least 1,500,000 g / mol. In some embodiments, the polymer additive has a molecular weight between 700,000 g / mol and 1,500,000 g / mol. In some embodiments, the polymer additive has a molecular weight between 500,000 g / mol and 1,000,000 g / mol.

[0122] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, the plurality of electrode active material particles including a plurality of silicon-based particles (e.g., micro-silicon, silicon oxide, etc.), and (iii) a polymer additive. The polymer additive has a relatively high tensile strength. For example, the polymer additive includes a polymer that is difficult to stretch. In some embodiments, the polymer additive has a relatively high tensile strength and can be processed in water or alcohols. In some embodiments, the polymer additive has a relatively high tensile strength and can be processed in water (e.g., it is relatively easy to process using water). In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 20MPa at a strain of about 10%. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 30MPa at a strain of about 10%. In some embodiments, the polymer additive includes a polymer that exhibits a stress between 30MPa and 35MPa at a strain of about 10%. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 10MPa at a strain of about 20%. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 20MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 25MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress between 25MPa and 30MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 15MPa at 5% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 18MPa at 5% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 20MPa at 5% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress between 15MPa and 25MPa at 5% strain. In some embodiments, the polymer additive includes a polymer with a maximum strength greater than 20MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength greater than 25MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength greater than 30MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength between 30MPa and 35MPa. In some embodiments, the polymer additive comprises a polymer having a maximum strength of about 33 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus greater than 5.5 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus greater than 7 MPa.In some embodiments, the polymer additive comprises a polymer having a Young's modulus greater than 7.5 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus of about 8 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 5.5 MPa and 10 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 7 MPa and 10 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 7 MPa and 8.5 MPa.

[0123] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive. In some embodiments, the silicon included in the active material particles includes one or more of silicon oxide and microsilicon. In some embodiments, the polymer additive includes one or more of polyolefins, poly (acrylic acid) and styrene-butadiene rubber (SBR). In some embodiments, the high aspect ratio carbon element network that defines the void space within the network includes a first group of carbon nanotubes and a second group of carbon nanotubes. In some embodiments, the high aspect ratio carbon element network further includes a third group of carbon elements. The third group of carbon elements may include graphite. The first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles. The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles. The second group of carbon nanotubes has one or more properties different from the first group of carbon nanotubes. According to various embodiments, the first group of carbon nanotubes includes multi-walled nanotubes, and the second group of carbon nanotubes includes single-walled nanotubes. As an example, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:1. In some embodiments, the multi-walled carbon nanotubes include an average diameter between 6nm and 10nm; an average wall thickness between 6nm and 7nm; an average length between 13 microns and 17 microns. In some embodiments, the average length of the multi-walled carbon nanotubes is about 13 microns. In some embodiments, the average length of the multi-walled carbon nanotubes is about 15 microns. In some embodiments, the average length of the multi-walled carbon nanotubes is about 16 microns. In some embodiments, the single-walled carbon nanotubes include an average diameter between 1nm and 2nm and an average length of about 5 microns. In some embodiments, the single-walled carbon nanotubes include an average diameter between 3nm and 5nm and an average length between 7 microns and 8 microns.

[0124] According to various embodiments, the network of high aspect ratio carbon elements included in the active layer of the electrode includes a first group of carbon nanotubes and a second group of carbon nanotubes. The first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles. The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles. The second group of carbon nanotubes has one or more properties different from the first group of carbon nanotubes. In some embodiments, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:1. In some embodiments, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 9:1. In some embodiments, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is at least 5:1. In some embodiments, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is at least 7:1.

[0125] In some embodiments, the network of high aspect ratio carbon elements further includes a third group of carbon elements. The third group of carbon elements may include graphite. Graphite can be used to increase Coulomb effectiveness. Graphite is conductive and can eliminate swelling shapes. In some embodiments, the active layer of the electrode includes at least 5% graphite by weight of the active layer. In some embodiments, the active layer of the electrode includes about 5% graphite by weight of the active layer. In some embodiments, the active layer of the electrode includes at least 10% graphite by weight of the active layer. In some embodiments, the active layer of the electrode includes at least 15% graphite by weight of the active layer. In some embodiments, the active layer of the electrode includes at least 20% graphite by weight of the active layer.

[0126] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that is soluble in at least one of (a) water and (b) alcohols. The high aspect ratio carbon element network that defines the void space within the network may include a group of multi-walled carbon nanotubes. According to various embodiments, the distribution of the length of the group of multi-walled carbon nanotubes is skewed toward the nominal length of the multi-walled carbon nanotubes. For example, the multi-walled carbon nanotubes are processed and / or applied in a manner that reduces or minimizes the fracture or rupture of the multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the high aspect ratio carbon element network is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more severely skewed toward the nominal length. In some embodiments, at least 75% of the multi-walled carbon nanotubes in the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns.

[0127] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network, which defines a void space within the network, (ii) a plurality of electrode active material particles, which are arranged in the void space within the network, and (iii) a polymer additive, which is soluble in water or alcohols, wherein the active layer exhibits at least 75N / m of adhesion to the foil of the electrode. In some embodiments, the active layer exhibits at least 90N / m of adhesion to the foil of the electrode. In some embodiments, the active layer exhibits at least 100N / m of adhesion to the foil of the electrode. In some embodiments, the active layer exhibits about 100N / m of adhesion to the foil of the electrode. In some embodiments, the active layer exhibits at least 125N / m of adhesion to the foil of the electrode. In some embodiments, the active layer exhibits at least 150N / m of adhesion to the foil of the electrode. The high aspect ratio carbon element network may include multi-walled carbon nanotubes. The adhesion of the active layer to the foil of the electrode can be determined according to the peel test described herein. In some embodiments, the foil includes copper and / or a copper alloy. According to various embodiments, the foil is coated on both sides (e.g., opposite sides). Coating on both sides of the foil can prevent the foil from folding during the drying process of drying the active layer (e.g., after the active layer is applied to the foil). For example, the drying of the active layer can cause the active layer to shrink, which can apply force to the foil and cause the foil to fold / shrink accordingly. In order to help avoid foil shrinkage, a thicker foil can be selected or the foil can be coated on opposite sides of the foil. In some embodiments, the foil (e.g., the thickness of the foil) is at least partially determined based on a tensile strength sufficient to withstand the force applied to the foil by the shrinkage of the active layer during the drying process and / or the force caused during the charge / discharge cycle (e.g., the force caused by the expansion / shrinkage of silicon during charge / discharge). In an embodiment, the foil has a thickness of less than 10 microns. In an embodiment, the foil has a thickness of less than 8 microns. In an embodiment, the foil has a thickness of less than 7 microns. In an embodiment, the foil has a thickness of less than 6 microns. In an embodiment, the foil has a thickness of less than 5 microns. In an embodiment, the foil has a thickness of about 6 microns.

[0128] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that is soluble in water or alcohols, wherein the active layer does not exhibit cracks when the electrode is wrapped around a mandrel having a diameter of at least 6 mm. The high aspect ratio carbon element network may include multi-walled carbon nanotubes. In some embodiments, the observation that the active layer does not exhibit any cracks in the active layer is determined based on human observation of the active layer (e.g., the surface of the active layer). In some embodiments, human observation of the active layer is performed using an electrode analyzed under a microscope. An example of a test for determining whether the active layer exhibits cracks includes wrapping a sample electrode around a set of mandrels (e.g., from the smallest diameter to the largest diameter), opening the sample electrode to observe cracks on the front and back sides, and repeating with a thicker mandrel until no cracks are observed.

[0129] According to various embodiments, the negative electrode includes an active layer. In some embodiments, the active layer includes: (i) a high aspect ratio carbon element network that defines a void space within the network, (ii) a plurality of electrode active material particles that are disposed in the void space within the network, and (iii) a polymer additive that can be processed in water or alcohols, wherein the active layer exhibits less than 50% expansion when wetted with an electrolyte. The polymer additive is soluble in water or alcohols. In some embodiments, the active layer exhibits less than 40% expansion when wetted with an electrolyte. In some embodiments, the active layer exhibits less than 30% expansion when wetted with an electrolyte. In some embodiments, the active layer exhibits less than 10% expansion when wetted with an electrolyte. In some embodiments, the active layer exhibits less than 10% expansion when wetted with an electrolyte. In some embodiments, the active layer exhibits expansion between 5% and 20% when wetted with an electrolyte. In some embodiments, the active layer exhibits expansion between 5% and 15% when wetted with an electrolyte. In some embodiments, the active layer exhibits expansion between 5% and 10% when wetted with an electrolyte. The network of high aspect ratio carbon elements may include multi-walled carbon nanotubes.

[0130] Figure 5A is a diagram of an electrode according to various embodiments. According to various embodiments, electrode 500 includes current collector 502 and active layer 506. Electrode 500 may optionally include adhesion layer 504. As an example, adhesion layer 504 includes a material that promotes adhesion between current collector 502 and active layer 506.

[0131] In some embodiments, the current collector 502 is an electrical layer. For example, the current collector 502 may be a metal, a metal alloy, etc. As another example, the current collector 502 is a metal foil. In some embodiments, the current collector 502 is an aluminum foil or an aluminum alloy foil. In some embodiments, the current collector 502 is a copper foil or a copper alloy foil. The current collector 502 has a thickness of less than 15 μm. The current collector 502 has a thickness of less than 10 μm. The current collector 502 has a thickness of less than 8 μm. The current collector 502 has a thickness of less than 5 μm. The current collector 502 has a thickness of less than 15 μm. In some preferred embodiments, the current collector 502 has a thickness between about 6 μm and about 8 μm. In some preferred embodiments, the current collector 502 has a thickness between about 5 μm and about 8 μm. In some embodiments, the current collector 502 is an aluminum foil or an aluminum alloy foil, and the current collector 502 has a thickness of about 6 μm. In some embodiments, the electrode includes a foil, and an active layer is provided on the opposite side of the foil.

[0132] In some embodiments, the active layer 506 may include a three-dimensional network of high aspect ratio carbon elements 508 that define void spaces within the network. A plurality of active material particles 510 are disposed in the void spaces within the network. Thus, the active material particles 510 are meshed or entangled in the network, thereby increasing the cohesion of the active layer 506. In some embodiments, the three-dimensional network of high aspect ratio carbon elements 508 provides mechanical support for the active material particles 510.

[0133] According to various embodiments, the three-dimensional network of high aspect ratio carbon elements 508 includes one or more of single-walled carbon nanotubes, multi-walled carbon nanotubes, a group of carbon nanotubes with a small number of walls (e.g., less than 6 walls), a group of carbon nanotubes with a large number of walls (e.g., greater than 6 walls), carbon nanostructures, fragments of single-walled carbon nanotubes, fragments of multi-walled carbon nanotubes, fragments of carbon nanostructures, carbon black, etc. Various other high aspect ratio carbon elements may be implemented. The three-dimensional network of high aspect ratio carbon elements 508 maintains electrical connection between high aspect ratio carbon elements (e.g., carbon nanotubes) during the charge / discharge cycle of the electrode. For example, when silicon particles included in the active layer expand and / or shrink during the charge / discharge cycle, the three-dimensional network of high aspect ratio carbon elements 508 maintains electrical connection between high aspect ratio carbon elements (e.g., carbon nanotubes). When silicon expands (e.g., silicon particles can expand by about 300%), multi-walled carbon nanotubes (or carbon nanotubes with a large number of walls) provide good bonding or coverage for silicon particles (such as silicon oxide). When silicon expands during charge / discharge cycles, single-walled carbon nanotubes (or carbon nanotubes with a small number of walls) can expand along with the silicon, and thus such carbon nanotubes generally do not reduce energy transfer.

[0134] According to various embodiments, the active layer 506 (e.g., the three-dimensional network of high aspect ratio carbon elements 508) includes multi-walled carbon nanotubes or a group of carbon nanotubes having a large number of walls (e.g., greater than 5 walls, or having 5 walls, etc.). In some embodiments, the amount of multi-walled carbon nanotubes (or a group of carbon nanotubes having a large number of walls) included in the active layer 506 is between 2% and 5% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes (or a group of carbon nanotubes having a large number of walls) included in the active layer 506 is between 3% and 5% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes (or a group of carbon nanotubes having a large number of walls) included in the active layer 506 is between 3.75% and 5% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes (or a group of carbon nanotubes having a large number of walls) included in the active layer 106 is about 4% by weight of the active layer.

[0135] The active layer 506 has an average thickness between 10 microns and 200 microns. In some embodiments, the active layer 506 has an average thickness of 15 microns to 50 microns. In some embodiments, the active layer 506 has an average thickness of 10 microns to 25 microns. In some embodiments, the active layer 506 has an average thickness of about 100 microns. In some embodiments, the active layer 506 has an average thickness of about 50 microns. In some embodiments, the active layer 506 has an average thickness between 25 microns and 50 microns. Typically, the active layer swells when wetted in an electrolyte. Examples for measuring the amount of swelling (e.g., expansion in at least the thickness direction) may include obtaining a sample electrode having a 1 inch diameter, such as by punching out a sample from a large sheet of electrode with a 1 inch diameter round punch, measuring the thickness of the active layer and recording it, placing the sample electrode in a button cell box, injecting the sample electrolyte into the button cell box, allowing the sample (e.g., with the injected electrolyte) to stand for 1 hour, and after 1 hour, measuring the thickness and recording it, then placing the electrode (as soaked with the electrolyte) in a drying chamber, covering it with a metal tray for 48 hours, and after standing for 48 hours, measuring and recording the thickness of the electrode. According to various embodiments, the volume expansion (e.g., swelling) of the active layer 506 when wetted with the electrolyte is less than 10%. For example, the thickness of the active layer 506 after being wetted with the electrolyte is less than 110% of the thickness of the active layer 106 in the absence of the electrolyte. According to various embodiments, the volume expansion (e.g., swelling) of the active layer 106 when wetted with the electrolyte is less than 20%. For example, the thickness of the active layer 506 after wetting with the electrolyte is less than 120% of the thickness of the active layer 506 in the absence of the electrolyte.

[0136] According to various embodiments, in the case where the active layer 506 includes multi-walled carbon nanotubes and single-walled carbon nanotubes, when wetted with an electrolyte in an energy storage device including the electrode 500, the multi-walled carbon nanotubes swell more than the single-walled carbon nanotubes. In some embodiments, when wetted with an electrolyte in an energy storage device including the electrode 500, the multi-walled carbon nanotubes swell at least 15% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes expands at least 15% more than the length of the single-walled carbon nanotubes. In some embodiments, when wetted with an electrolyte in an energy storage device including the electrode 500, the multi-walled carbon nanotubes swell at least 25% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes expands at least 25% more than the length of the single-walled carbon nanotubes. In some embodiments, when wetted with an electrolyte in an energy storage device including the electrode 100, the multi-walled carbon nanotubes swell at least 50% more than the single-walled carbon nanotubes. For example, when wetted with an electrolyte, the length of the multi-walled carbon nanotubes expands by at least 50% compared to the length of the single-walled carbon nanotubes. In some embodiments, the multi-walled carbon nanotubes swell up to 50% when wetted (e.g., after being wetted with an electrolyte, the length of the multi-walled carbon nanotubes increases by 50%, and / or after being wetted, the diameter of the multi-walled carbon nanotubes increases by 50%, etc.).

[0137] According to various embodiments, the three-dimensional network of high aspect ratio carbon elements 508 includes carbon nanotubes, and the carbon nanotubes are only multi-walled carbon nanotubes and / or fragments of carbon nanotubes. For example, the three-dimensional network of high aspect ratio carbon elements 508 does not include single-walled carbon nanotubes or fragments of single-walled carbon nanotubes. According to various embodiments, the three-dimensional network of high aspect ratio carbon elements 508 includes at least 99% carbon by weight. In some embodiments, the three-dimensional network of high aspect ratio carbon elements 508 includes a network of electrically interconnected carbon elements that exhibit connectivity above the percolation threshold, and wherein the network defines one or more highly conductive paths having a length greater than 500 μm. In some embodiments, when the silicon particles included in the active layer expand or contract during the charge / discharge cycle of the electrode 500, the three-dimensional network of high aspect ratio carbon elements 508 remains electrically connected.

[0138] According to various embodiments, the high aspect ratio carbon element network defines the void space within the network, and the high aspect ratio carbon element network includes a first group of carbon nanotubes and a second group of carbon nanotubes. Preferably, the first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles, and the second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles. The second group of carbon nanotubes has one or more properties different from the first group of carbon nanotubes. For example, the second group of carbon nanotubes has a number of layers (e.g., walls) different from the number of layers (e.g., walls) of the first group of carbon nanotubes. In some embodiments, the first group of carbon nanotubes includes multi-walled carbon nanotubes. In some embodiments, the second group of carbon nanotubes includes single-walled carbon nanotubes. For example, the high aspect ratio carbon element network includes a group of multi-walled carbon nanotubes and a group of single-walled carbon nanotubes. The group of multi-walled carbon nanotubes may have fragments of multi-walled carbon nanotubes, and / or the group of single-walled carbon nanotubes may have fragments of multi-walled carbon nanotubes. According to various embodiments, the active layer includes a larger amount of multi-walled carbon nanotubes than single-walled carbon nanotubes. Preferably, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes included in the active layer is about 1.5:1. Preferably, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes included in the active layer is at least 1.5:1. Preferably, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes included in the active layer is about 2:1. Preferably, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes included in the active layer is at least 5:1. Preferably, the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes included in the active layer is about 9:1.

[0139] In the energy storage device of the related art, the network of carbon elements includes fragmented carbon nanotubes, such as fragmented multi-walled carbon nanotubes. The related art process for manufacturing electrodes is. For example, the fragmented multi-walled carbon nanotubes included in the related art electrode generally have an average length significantly less than the nominal length of the multi-walled carbon nanotubes (e.g., the length of the multi-walled carbon nanotubes before being input into the process for manufacturing the electrode (such as creating an active layer or applying the active layer to the current collector)). The fragmented multi-walled carbon nanotubes included in the related art electrode generally have an average length significantly less than half of the nominal length of the multi-walled carbon nanotubes. The fragmented multi-walled carbon nanotubes included in the related art electrode generally have an average length significantly less than one-third of the nominal length of the multi-walled carbon nanotubes. The method for preparing multi-walled carbon nanotubes or for preparing / manufacturing / applying an active layer for a related art electrode does not gently treat the multi-walled carbon nanotubes and causes the multi-walled carbon nanotubes to break or be crushed. Longer multi-walled carbon nanotubes generally provide better mechanical support for the active material particles in the active layer. For example, when the active material particles expand / contract during the charge / discharge cycle, the longer multi-walled carbon nanotubes provide better mechanical support for the active material particles (e.g., the active material particles are better meshed between the relatively longer multi-walled carbon nanotubes). In addition, the longer multi-walled carbon nanotubes can form a longer interconnected network, and the highly conductive paths formed in the network can provide long conductive paths to facilitate the flow of current within and through the active layer (e.g., in the active layer (such as Figure 5A The conductive path is on the order of the thickness of the active layer 506 of the electrode 500).

[0140] According to various embodiments, the electrode includes relatively longer multi-walled carbon nanotubes compared to the multi-walled carbon nanotubes included in the related art electrode. It is found that the use of relatively long multi-walled carbon nanotubes in the electrode has beneficial mechanical and / or electrical properties. For example, multi-walled carbon nanotubes provide relatively good power at low density. As another example, shorter multi-walled carbon nanotubes are generally not swollen (e.g., expanded) like longer multi-walled carbon nanotubes. Therefore, using shorter multi-walled carbon nanotubes will lose (or reduce) some beneficial properties associated with carbon nanotube swelling. As an extreme example, carbon black does not show swelling because carbon black is only carbon particles without entanglements, such as the entanglements shown by a group of multi-walled carbon nanotubes. Observations during the calendering process indicate that a certain amount of multi-walled carbon nanotubes have a length exceeding a threshold length and therefore have sufficient swelling properties-relatively large amounts of pressure or effects associated with applying to the foil to calender the slurry indicate that the collective swelling (e.g., average swelling) of the multi-walled carbon nanotubes in the active layer will meet a specific performance threshold. However, multi-walled carbon nanotubes are generally difficult to process. The processing of multi-walled carbon nanotubes related to the preparation / formation of active layer and / or electrode is gentler than the processing of related art electrodes. Therefore, the method according to various embodiments keeps longer multi-walled carbon nanotubes (e.g., fewer multi-walled carbon nanotubes are crushed, fragmented, broken, etc.). In some embodiments, the active layer of the electrode includes a group of multi-walled carbon nanotubes, and its average length is greater than the average length of the multi-walled carbon nanotubes in the related art electrodes. According to various embodiments, the distribution of the length of this group of multi-walled carbon nanotubes is skewed toward the nominal length of the multi-walled carbon nanotubes. As an example, the nominal length of the multi-walled carbon nanotubes is about 16 microns. For example, multi-walled carbon nanotubes are processed and / or applied in a manner to reduce or minimize the fracture or rupture of multi-walled carbon nanotubes. The length of the multi-walled carbon nanotubes in the high aspect ratio carbon element network is generally the nominal length of the multi-walled carbon nanotubes, or the length of such multi-walled carbon nanotubes tends to be more seriously skewed toward the nominal length. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 75% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 10% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 12 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 8 microns. In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network have a length of at least 13 microns.In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 50% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 60% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, at least 50% of the multi-walled carbon nanotubes within the high aspect ratio carbon element network are within 75% of the nominal length (e.g., between 13.4 microns and about 15 microns). In some embodiments, the amount of multi-walled carbon nanotubes having a length shorter than half the nominal length of the multi-walled carbon nanotubes is less than 50% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes having a length shorter than half the nominal length of the multi-walled carbon nanotubes is less than 30% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes having a length shorter than half the nominal length of the multi-walled carbon nanotubes is less than 25% by weight of the active layer.

[0141] Compared with the multi-walled carbon nanotubes in the related art electrodes, the multi-walled carbon nanotubes included in the electrode exhibit an average higher aspect ratio, such as having a longer length. A slurry with high viscosity is prepared and subjected to relatively low shear forces during processing. Therefore, the aspect ratio of the multi-walled carbon nanotubes is retained. In some embodiments, at least a subset of the multi-walled carbon nanotubes included in the active layer is a branched carbon nanotube. In some embodiments, at least a subset of the multi-walled carbon nanotubes included in the active layer is branched, interdigitated, entangled and / or shares a common wall. The characteristics of the multi-walled carbon nanotubes can be obtained using a scanning electron microscope (SEM). According to various embodiments, the multi-walled carbon nanotubes include an average length of at least 5 microns. In some embodiments, the multi-walled carbon nanotubes include an average length of at least 10 microns. In some embodiments, the multi-walled carbon nanotubes include an average length between 10 microns and 15 microns. According to various embodiments, the multi-walled carbon nanotubes include an average diameter between 6nm and 15nm. In some embodiments, the multi-walled carbon nanotubes include an average diameter between 6nm and 10nm. According to various embodiments, the multi-walled carbon nanotubes include an average of 3 to 15 layers. In some embodiments, multi-walled carbon nanotubes include an average of 3 to 15 layers. In some embodiments, multi-walled carbon nanotubes include an average of 5 to 10 layers. In some embodiments, multi-walled carbon nanotubes include an average of 6 to 7 layers. In some embodiments, multi-walled carbon nanotubes include at least 6 layers on average. In some embodiments, multi-walled carbon nanotubes (e.g., a group of carbon nanotubes with a large number of walls) include an average aspect ratio of at least 100. In some embodiments, multi-walled carbon nanotubes include an average aspect ratio between 200 and 1000. In some embodiments, high aspect ratio carbon elements may include sheet-like or plate-like elements having two major dimensions and one minor dimension. For example, in some such embodiments, the length ratio of each of the major dimensions may be at least 5 times, 10 times, 100 times, 500 times, 1,000 times, 5,000 times, 10,000 times or more of the length ratio of the minor dimension.

[0142] According to various embodiments, the electrode includes particles of silicon-based active material. In some embodiments, the electrode includes at least one electrode active material selected from the group consisting of silicon (e.g., microsilicon), silicon oxide (e.g., SiOx), SiOx powder (Shin-Etsu 7131). Various other silicon-based particles may be implemented. In some embodiments, the active material includes one or more of graphite, hard carbon, activated carbon, nanocarbon, silicon, silicon oxide, and carbon-encapsulated silicon nanoparticles.

[0143] According to various embodiments, the plurality of active material particles 510 include microsilicon.

[0144] Active layer 506 includes a relatively large amount of active material particles. In some embodiments, active layer 506 includes at least 50.0% active material particles by weight of the active layer. In some embodiments, active layer 106 includes between 70.0% and 90.0% active material particles by weight of the active layer. In some embodiments, active layer 106 includes greater than 80% active material particles by weight of the active layer.

[0145] According to various embodiments, the active layer 506 includes a polymer additive. The polymer additive may provide mechanical support for at least a subset of the plurality of active material particles 510 and / or at least a portion of the three-dimensional network of high aspect ratio carbon elements 508. For example, the polymer additive may bond or adhere to the active material particles or carbon elements such as carbon nanotubes (e.g., multi-walled carbon nanotubes and / or single-walled carbon nanotubes). According to various embodiments, electrochemically stable polymers have been found to have beneficial properties as polymer additives for the active layer 506. The polymer additive may be selected to be a polymer that is completely soluble or highly soluble in the solvent used in the treatment electrode 500. For example, the polymer additive may be soluble or highly soluble in water or alcohols such as ethanol. In some embodiments, the polymer additive may be processed in water.

[0146] According to various embodiments, the polymer additive has a relatively high tensile strength. For example, the polymer additive includes a polymer that is difficult to stretch. In some embodiments, the polymer additive has a relatively high tensile strength and can be processed in water or alcohols. In some embodiments, the polymer additive has a relatively high tensile strength and can be processed in water (for example, it is relatively easy to process using water). In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 20MPa at about 10% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 30MPa at about 10% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress between 30MPa and 35MPa at about 10% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 10MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 20MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 25MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress between 25MPa and 30MPa at about 20% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 15MPa at 5% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 18MPa at 5% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress greater than 20MPa at 5% strain. In some embodiments, the polymer additive includes a polymer that exhibits a stress between 15MPa and 25MPa at 5% strain. In some embodiments, the polymer additive includes a polymer with a maximum strength greater than 20MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength greater than 25MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength greater than 30MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength between 30MPa and 35MPa. In some embodiments, the polymer additive includes a polymer with a maximum strength of about 33MPa. In some embodiments, the polymer additive includes a polymer with a Young's modulus greater than 5.5MPa. In some embodiments, the polymer additive includes a polymer with a Young's modulus greater than 7MPa. In some embodiments, the polymer additive includes a polymer with a Young's modulus greater than 7.5MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus of about 8 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 5.5 MPa and 10 MPa.In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 7 MPa and 10 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 7 MPa and 8.5 MPa.

[0147] In some embodiments, the polymer additive comprises one or more of a polyolefin, a poly(acrylic acid), and a styrene-butadiene rubber (SBR). In some embodiments, the polymer additive comprises an AquaCharge adhesive.

[0148] According to various embodiments, the electrode includes 89wt.% Wacker microsilica powder + 1wt.% pre-dispersed single-walled carbon nanotube Neocarbonix ethanol-based suspension + 10wt.% AquaCharge binder (10wt.% water-based solution). AQUACHARGE is a trade name for an aqueous binder for electrodes, which is developed by applying water-soluble resin technology. AQUACHARGE is produced by Sumitomo Seika Chemicals Co., Ltd. of Hyogo Prefecture, Japan. A similar example is provided in U.S. Patent No. 8,124,277, entitled "Binder for electrode formation, slurry for electrode formation using the binder, electrode using the slurry, rechargeable battery using the electrode, and capacitor using the electrode", and is incorporated herein by reference in its entirety. Further examples include polyacrylic acid (PAA), which is a synthetic high molecular weight polymer of acrylic acid; and sodium polyacrylate, which is the sodium salt of polyacrylic acid.

[0149] Related Art Electrodes often use polymer binders that are soluble only in toxic or environmentally unfriendly solvents. Polymer binders are used to disperse, adhere, bind particles, and survive in harsh environments. Energy storage device batteries may slowly lose capacity after hundreds or thousands of cycles and charge / discharges. Polymer binders can help maintain the capacity of energy storage devices over their service life.

[0150] According to various embodiments, the electrode 500 and / or the active layer 506 do not include (e.g., are free of) polymer additives that are not processable or insoluble in water or one or more of alcohols (such as ethanol). In some embodiments, the electrode is substantially free of polymer additives that are not processable or insoluble in water or one or more of alcohols (such as ethanol). In some embodiments, the electrode 500 and / or the active layer 506 of the electrode 500 does not include or is substantially free of polymer additives that are insoluble in water or one or more of alcohols (such as ethanol). For example, any polymer additive of the electrode 500 according to various embodiments may be soluble in one or more of water and alcohols (e.g., methanol, ethanol, etc.).

[0151] The polymer additive may be selected based at least in part on its reaction with certain electrolytes used in an energy storage device including the electrode 500. In some embodiments, a polymer additive having a relatively high (e.g., very high) molecular weight is selected, such as because such polymer additives are generally resistant to solvents. For example, polymer additives with high molecular weights do not dissolve in solvents, while polymers with low molecular weights become viscous. In some embodiments, the polymer additive is selected as a polymer that does not become soft (e.g., softer than a softness threshold) when mixed with an electrolyte. In some embodiments, the polymer additive is selected as a polymer that does not substantially swell (e.g., swells or expands beyond a predetermined swelling threshold) when wetted / mixed with an electrolyte used in an energy storage device.

[0152] Active layer 506 may include a polymer additive that is processable or soluble in water and / or alcohols (such as ethanol). In some embodiments, the polymer additive has a relatively high molecular weight. For example, the polymer additive has a molecular weight greater than 200 g / mol. In some embodiments, the polymer additive has a molecular weight greater than 400,000 g / mol. In some embodiments, the polymer additive has a molecular weight greater than 500,000 g / mol. In some embodiments, the polymer additive has a molecular weight greater than 1,000,000 g / mol. In some embodiments, the polymer additive has a molecular weight between 500,000 g / mol and 1,500,000 g / mol.

[0153] The polymer additive may have a specific gravity between 1.0 g / cm3 and 2.5 g / cm3. In some embodiments, the polymer additive has a specific gravity greater than 1.135 g / cm3. In some embodiments, the polymer additive has a specific gravity greater than 1.20 g / cm3. The specific gravity of the polymer additive may be measured according to the ASTM D792 test method.

[0154] The polymer additive may have a specific heat between 1.5 J / g°C at 23°C and 3.5 J / g°C at 23°C. In some embodiments, the polymer additive has a specific heat greater than 2.0 J / g°C at 23°C. In some embodiments, the polymer additive has a specific heat greater than 2.2 J / g°C at 23°C. In some embodiments, the polymer additive has a specific heat of about 2.4 J / g°C at 23°C. The specific heat of the polymer additive may be measured based on a DSC measurement.

[0155] When the polymer additive is dried, the polymer additive may have a tensile strength between 4MPa and 100MPA. As an example, when the polymer additive is dried, the polymer additive has a tensile strength between 4MPa and 70MPA. In some embodiments, the polymer additive has a tensile strength of less than 70MPa measured when the polymer additive is dried. In some embodiments, the polymer additive has a tensile strength of less than 50MPa measured when the polymer additive is dried. In some embodiments, the polymer additive includes a polymer exhibiting a stress between 15MPa and 25MPa at 5% strain. In some embodiments, the polymer additive includes a polymer having a maximum strength greater than 20MPa. In some embodiments, the polymer additive includes a polymer having a maximum strength greater than 25MPa. In some embodiments, the polymer additive includes a polymer having a maximum strength greater than 30MPa. In some embodiments, the polymer additive includes a polymer having a maximum strength between 30MPa and 35MPa. In some embodiments, the polymer additive includes a polymer having a maximum strength of about 33MPa. In some embodiments, the polymer additive includes a polymer having a Young's modulus greater than 5.5MPa. In some embodiments, the polymer additive includes a polymer having a Young's modulus greater than 7MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus greater than 7.5 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus of about 8 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 5.5 MPa and 10 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 7 MPa and 10 MPa. In some embodiments, the polymer additive comprises a polymer having a Young's modulus between 7 MPa and 8.5 MPa. The tensile strength of the polymer additive can be measured based on the ASTM D638 test method.

[0156] The polymer additive may have an elongation at yield greater than 4%. As an example, the polymer additive has an elongation at yield greater than 4% and less than 50% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 5% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 10% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 20% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield greater than 25% measured when the polymer additive is dry. In some embodiments, the polymer additive has an elongation at yield between 20% and 30% measured when the polymer additive is dry. The elongation at yield of the polymer additive can be measured based on the ASTM D638 test method.

[0157] According to various embodiments, the active layer 506 includes a polymer additive selected from the polyamide family, or a modified polyamide or a polyamide derivative. The polymer additive is soluble in water or alcohols such as ethanol. In some embodiments, the polymer additive has a relatively high molecular weight. The polymer additive may be at least partially disposed in at least one void space defined by a high aspect ratio carbon element network. In some embodiments, the polymer additive acts as a polymer binder. When the mixture of the polymer additive and ethyl cellosolve is cooled, the polymer additive may exhibit gelation. As an example, the polymer additive may be completely soluble in each of water, ethylene glycol, benzyl alcohol, acetic acid, and isobutyl alcohol. As an example, the polymer additive may be completely soluble in N-methylpyrrolidone. The solubility of the polymer additive can be measured by adding 10g of the polymer additive to 100ml of a specific solvent, stirring the mixture at 80°C for about 3 hours, and after stirring, cooling the mixture to room temperature, and then observing the mixture.

[0158] Because the polymer additive provides mechanical support for the electrode 100 (e.g., provides mechanical support for the active material particles and / or carbon elements), the polymer additive is selected so that the polymer additive has a glass transition temperature that is typically outside the operating temperature of the energy storage device. In some embodiments, the polymer additive has a glass transition temperature of less than 0°C. In some embodiments, the polymer additive has a glass transition temperature of less than -10°C. In some embodiments, the polymer additive has a glass transition temperature of less than -25°C. In some embodiments, the polymer additive has a glass transition temperature of less than -30°C. In some embodiments, the polymer additive has a glass transition temperature of less than -40°C. In some embodiments, the polymer additive has a glass transition temperature of less than -45°C. In some embodiments, the polymer additive has a glass transition temperature between -50°C and -40°C. The glass transition temperature of the polymer additive can be measured based on DSC measurements.

[0159] According to various embodiments, the polymer additive has a 5% weight reduction temperature between 375° C. and 400° C. In some embodiments, the polymer additive has a 5% weight reduction temperature of about 385° C. The polymer additive may be selected such that an aqueous solution of the polymer additive and at least one of water and an alcohol exhibits a viscosity of at least 60 Pa·s at a concentration of about 50% by weight of the polymer additive.

[0160] The active layer 506 may include less than 5% of the polymer additive by weight of the active layer. In some embodiments, the amount of polymer material included in the active layer 506 is about 8% by weight of the active layer. In some embodiments, the amount of polymer material included in the active layer 506 is equal to or less than 8% by weight of the active layer. In some embodiments, the amount of polymer material included in the active layer 506 is about 10% by weight of the active layer. In some embodiments, the amount of polymer material included in the active layer 506 is equal to or less than 10% by weight of the active layer. In some embodiments, the amount of polymer material included in the active layer 506 is less than 12% by weight of the active layer. In some embodiments, the amount of polymer material included in the active layer 506 is less than 15% by weight of the active layer.

[0161] Examples of polymer additives include polyolefins, poly(acrylic acid), styrene-butadiene rubber (SBR), polyethylene oxide (PEO), polyethers, poly(ethylene glycol) (PEG) derivatives, fluoropolymers (particularly poly(vinylidene fluoride) (PVDF)), polyurethanes (PU), polytetrafluoroethylene (PTFE), alginate (Alg), refolded DNA / Alg, Alg-catechol, PAA-catechol, carboxymethyl chitosan, guar gum, agarose, konjac glucomannan, carboxymethylated gellan gum, PDA-PAA-PEO, pectin / PAA, partially lithiated PAA and Nafion, sequence-defined peptoids, PMDOPA, branched PAA, NaPAA-g-CMC, CS-g-PAANa, PVA-g-PAA, GC-g-LiPAA, PVDF-g-PAA, branched PAA-PEG, CS-g-PANI, hyperbranched β-cyclodextrin, double-helical natural xanthan gum, Li-Nafion, PAA / CMC, cross-linked PAA / PVA, glycerol-cross-linked PEDOT:PSS, MAH-cross-linked corn starch, MAH-cross-linked CMC, cross-linked natural GG polymer, cross-linked chitosan, CS-CG + GA, cross-linked dextrin, cross-linked CMC-PEG, cross-linked hyperbranched PEI, cross-linked PAM hydrogel, cross-linked PU elastomer, cross-linked PVA-PEI, TMM functionalized PVA network, polymers including polyamides (e.g., nylon), functionalized polyamides, copolymers of PEO and polyamide, self-healing polymers, PAA-Upy supramolecules, self-healing PAU-g-PEG, Ca2+ cross-linked SA hydrogel, (Fe3+) cross-linked (PANa0.8Fey), Sn4+ cross-linked PEDOT:PSS, PAA-PEG-PBI, cross-linked CMC- CPAM, metal polymer, Si@Fe3+-PDA-PAA, β-CDp / 6AD, slide-ring PR-PAA, conductive PFFOMB, PEG-grafted PFP, PF-COONa, PFPQ-COONa, pyrene (PPyE), pyrene (PPyMAA), pyrene (PPyMADMA), PANI, FA-doped PEDOT:PSS, stretchable conductive adhesive, poly(phenanthrenequinone), cyclized PAN, PAA-P(HEA-co-DMA), PEDOT:PSS / PEO / PEI, PAA / PVA + elastic gel polymer electrolyte, PAA+BFPU, mixture of PU and poly(acrylic acid) (PAA), copolymers of any subset of the foregoing, etc.Zhao, YM. et al. 2021, "Various other polymers may be implemented as the polymeric additive", InfoMat, Vol. 3, No. 5, pp. 460-501 (hereinafter referred to as "Zhao") provides a description of various polymers that can be implemented as polymeric additives. Zhao is incorporated herein in its entirety for all purposes.

[0162] In some embodiments, the surface treatment 202 (not shown, see Figure 2 ) is applied on the surface of the high aspect ratio carbon element 108 of the network. The surface treatment promotes adhesion between the high aspect ratio carbon element and the active material particles 510. The surface treatment may also promote adhesion between the high aspect ratio carbon element and the current collector 502 (also referred to herein as a "conductive layer"), the optional adhesion layer 504 and / or at least a subset of the active material particles 510. The surface treatment may include a surfactant layer bonded to the high aspect ratio carbon element 508 and including a plurality of surfactant elements, each surfactant element having a hydrophobic end and a hydrophilic end, wherein the hydrophobic end is disposed proximal to one of the surfaces in the high aspect ratio carbon element 508 and the hydrophilic end is disposed distal to one of the surfaces in the high aspect ratio carbon element 508. In some embodiments, the surface treatment 202 includes at least a portion of a polymer additive. In some embodiments, the surface treatment includes a material soluble in a solvent having a boiling point below 202°C. In some embodiments, the surface treatment includes a material soluble in a solvent having a boiling point below 185°C.

[0163] In some embodiments, the surface treatment 202 may be formed by a carbonaceous material layer, which is produced by the pyrolysis of a polymeric material disposed on a high aspect ratio carbon element. The carbonaceous material layer (e.g., graphite or amorphous carbon) may be attached (e.g., via a covalent bond) to active material particles or otherwise promote adhesion to active material particles. Examples of suitable pyrolysis techniques are described in U.S. Patent Application Serial No. 63 / 028,982 filed May 22, 2020. A suitable polymeric material for this technology is polyacrylonitrile (PAN).

[0164] According to various embodiments, the active layer 106 includes a dispersant. The dispersant can be selected based on compatibility with water and / or alcohols (such as ethanol). In some embodiments, the dispersant is a water-soluble polymer. In some embodiments, the dispersant is an alcohol-soluble polymer. In some embodiments, the dispersant is a polymer that can be processed in water or alcohols. In some embodiments, the dispersant corresponds to or includes polyvinyl pyrrolidone (PVP). The PVP used for the dispersant can be a PVP with a relatively high molecular weight.

[0165] According to various embodiments, the active layer 506 includes about 25% dispersant by weight of the active layer 506. In some embodiments, the amount of dispersant included in the active layer 506 is between 10% and 50% by weight of the active layer 106. In some embodiments, the amount of dispersant included in the active layer 106 is between 15% and 40% by weight of the active layer 506. In some embodiments, the amount of dispersant included in the active layer 506 is between 20% and 30% by weight of the active layer 506.

[0166] Figure 5B is a diagram of an electrode according to various embodiments. According to various embodiments, electrode 525 includes current collector 528 and active layer 532. Electrode 525 may optionally include adhesion layer 530. As an example, adhesion layer 530 includes a material that promotes adhesion between current collector 528 and active layer 532. In some embodiments, current collector 528 corresponds to (or is similar to) Figure 5A The current collector 502 is provided.

[0167] In some embodiments, the active layer 532 corresponds to (or is similar to) Figure 5A The current active layer 506 of the electrode. According to various embodiments, the active layer of the electrode includes a group of multi-walled carbon nanotubes (e.g., represented by 543 and shown in solid lines) and a group of single-walled carbon nanotubes (e.g., represented by 536 and shown in dashed lines). In some embodiments, the average aspect ratio of the group of multi-walled carbon nanotubes is greater than the average aspect ratio of the group of single-walled carbon nanotubes.

[0168] According to various embodiments, the active layer 532 includes multi-walled carbon nanotubes and single-walled carbon nanotubes. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 532 is between 0.25% and 4% by weight of the active layer. In some embodiments, the amount of single-walled carbon nanotubes included in the active layer 536 is between 0.01% and 2% by weight of the active layer. In some embodiments, the amount of single-walled carbon nanotubes included in the active layer 536 is between 0.5% and 1.5% by weight of the active layer. According to various embodiments, the multi-walled carbon nanotubes in the active layer 532 and the active layer 536 are The ratio of single-walled carbon nanotubes in layer 532 by weight of the active layer is about 2: 1. In some embodiments, the ratio of multi-walled carbon nanotubes in active layer 532 to single-walled carbon nanotubes in active layer 532 by weight of the active layer is about 5: 1. In some embodiments, the ratio of multi-walled carbon nanotubes in active layer 532 to single-walled carbon nanotubes in active layer 532 by weight of the active layer is about 9: 1. In some embodiments, the ratio of multi-walled carbon nanotubes in active layer 532 to single-walled carbon nanotubes in active layer 532 by weight of the active layer is at least 7: 1.

[0169] In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 132 is between 0.25% and 5% by weight of the active layer. In some embodiments, the amount of single-walled carbon nanotubes included in the active layer 532 is between 0.01% and 2% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 532 is between 3% and 6% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 532 is between 3% and 5% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 532 is between 4% and 5% by weight of the active layer. In some embodiments, the amount of multi-walled carbon nanotubes included in the active layer 532 is about 4% by weight of the active layer.

[0170] In some embodiments, the active layer 532 further comprises graphite. Graphite can be used to increase the Coulomb effectiveness. Graphite is conductive and can eliminate swelling shapes. In some embodiments, the active layer 532 of the electrode comprises at least 5% graphite by weight of the active layer 532. In some embodiments, the active layer 532 of the electrode comprises between 4% and 7% graphite by weight of the active layer 532. In some embodiments, the active layer 132 of the electrode comprises about 5% graphite by weight of the active layer 132. In some embodiments, the active layer 132 of the electrode comprises at least 10% graphite by weight of the active layer 532. In some embodiments, the active layer 532 comprises at least 15% graphite by weight of the active layer 532. In some embodiments, the active layer 532 comprises at least 20% graphite by weight of the active layer 532.

[0171] The single-walled carbon nanotubes included in the electrode show a longer length than the single-walled carbon nanotubes in the related art electrode on average. Prepare a slurry with high viscosity and withstand relatively low shear force during processing. The characteristics of multi-walled carbon nanotubes can be obtained using a scanning electron microscope (SEM). According to various embodiments, the single-walled carbon nanotube includes a length range between 1nm and 34nm. The average length of the single-walled carbon nanotube can be between 7 microns and 8 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 1nm and 2nm and an average length of about 5 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 3nm and 5nm and an average length of at least 200 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 3nm and 5nm and an average length between 7 microns and 8 microns. In some embodiments, the single-walled carbon nanotube includes an average diameter between 5nm and 6nm and an average length between 7 microns and 8 microns. In some embodiments, the single-walled carbon nanotube includes an average of 1 or 2 layers of wall.

[0172] Figure 5C5 is a diagram of an electrode according to various embodiments. In the example shown, the active layer of the electrode 550 includes a functionalized carbon element. As an example, the functionalized carbon element can be based at least in part on Figure 5A The high aspect ratio carbon elements 508 (eg, a group of multi-walled carbon nanotubes and / or a group of single-walled carbon nanotubes, etc.) of the active layer 506 of the electrode 500 shown in FIG. 5 are obtained by surface treatment.

[0173] In some embodiments, the functionalized carbon element is formed from a dried (eg, freeze-dried) aqueous dispersion comprising nanoform carbon and a functionalizing material (such as a surfactant). In some such embodiments, the aqueous dispersion is substantially free of materials that would damage the carbon element, such as an acid.

[0174] In some embodiments, the surface treatment of the high aspect ratio carbon element comprises a thin polymer layer disposed on the carbon element that promotes adhesion of the active material to the network. In some such embodiments, the thin polymer layer comprises a self-assembling and / or self-limiting polymer layer. In some embodiments, the thin polymer layer is bonded to the active material, for example via hydrogen bonding.

[0175] In some embodiments, the thickness of the thin polymer layer in a direction perpendicular to the outer surface of the carbon element may be less than 3, 2, 1, 0.5, 0.1 (or less) times the minor dimension of the element.

[0176] In some embodiments, the thin polymer layer includes functional groups (e.g., pendant functional groups) bonded to the active material, e.g., via non-covalent bonds (such as π-π bonds). In some such embodiments, the thin polymer layer can form a stable covering layer on at least a portion of the carbon element.

[0177] In some embodiments, the thin polymer layer on some elements may be bonded to a current collector or an adhesion layer disposed thereon and located below an active layer comprising an energy storage (i.e., active) material. For example, in some embodiments, the thin polymer layer includes side functional groups bonded to the surface of the current collector or the adhesive layer, for example, via non-covalent bonds (such as π-π bonds). In some such embodiments, the thin polymer layer may form a stable covering layer on at least a portion of the element. In some embodiments, this arrangement provides excellent mechanical stability of the electrode.

[0178] In some embodiments, the polymeric material is miscible in a solvent of the type described in the above examples. For example, in some embodiments, the polymeric material is miscible in a solvent comprising alcohols such as methanol, ethanol or 2-propanol (isopropanol, sometimes referred to as IPA) or a combination thereof. In some embodiments, the solvent may include one or more additives for further improving the properties of the solvent, such as low boiling point additives, such as acetonitrile (ACN), deionized water and tetrahydrofuran. In this example, the mixture is formed in a solvent without NMP.

[0179] In yet further exemplary embodiments, the surface treatment may be formed by a layer of carbonaceous material produced by pyrolysis of a polymeric material disposed on a high aspect ratio carbon element. The carbonaceous material layer (e.g., graphite or amorphous carbon) may be attached (e.g., via covalent bonds) to or otherwise promote adhesion to the active material particles. Examples of suitable pyrolysis techniques are described in U.S. Patent Application Serial No. 63 / 028,982 filed on May 22, 2020, which is incorporated herein in its entirety for all purposes. One polymeric material suitable for use in this technology is polyacrylonitrile (PAN)

[0180] According to various embodiments, the active layer 506 includes a dispersant. The dispersant can be selected based on compatibility with water and / or alcohols (such as ethanol). In some embodiments, the dispersant is a water-soluble polymer. In some embodiments, the dispersant corresponds to or includes polyvinyl pyrrolidone (PVP). The PVP used for the dispersant can be a PVP with a relatively high molecular weight.

[0181] Dispersants and additives can be added to the mixture. An example of a dispersant is PVP. Polyvinylpyrrolidone (PVP), also commonly referred to as "polyvidone" or "povidone", is a water-soluble polymer made from the monomer N-vinylpyrrolidone. Typically, dispersants act as emulsifiers and disintegrants in solution polymerization, and act as surfactants, reducing agents, shape controllers, and dispersants in nanoparticle synthesis and self-assembly thereof. Another example of a dispersant includes AQUACHARGE, a trade name for an aqueous binder for electrodes, developed by applying water-soluble resin technology. AQUACHARGE is produced by Sumitomo Seika Chemicals Co., Ltd. of Hyogo Prefecture, Japan. A similar example is provided in U.S. Patent No. 8,124,277, entitled "Binder for electrode formation, slurry forelectrode formation using the binder, electrode using the slurry, rechargeable battery using the electrode, and capacitor using the electrode", and is incorporated herein by reference in its entirety. Further examples include polyacrylic acid (PAA), which is a synthetic high molecular weight polymer of acrylic acid; and sodium polyacrylate, which is the sodium salt of polyacrylic acid.

[0182] Table III

[0183] Dispersant addition and mixing

[0184]

[0185] Target viscosity range of slurry

[0186] Shear rate (rpm) Viscosity (mPa s) 6 20000-10000 12 6000-3000 30 3000-1500 60 1200-800

[0187] Figure 6 is an example of an electron micrograph of an active layer according to various embodiments. Figure 6 , shows an electron micrograph of an exemplary active material layer of the type described herein. Tendril-like high aspect ratio carbon elements (formed from CNT bundles) are clearly shown as intermeshing active material particles. In some embodiments, the active layer lacks any bulk polymer material that occupies space within the layer.

[0188] Energy Storage Batteries

[0189] According to various embodiments, the energy storage battery includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode may correspond to (or be similar to) Figure 1A Electrode 100 or Figure 1B The negative electrode may correspond to (or be similar to) Figure 5A Electrode 500 or Figure 5B Electrode 525. The electrolyte may be selected based at least in part on the positive electrode and / or the negative electrode. For example, the electrolyte is selected to facilitate charge transfer between the positive electrode and the negative electrode. The selection of the electrolyte may be based on one or more characteristics of the positive electrode, one or more characteristics of the negative electrode, or both.

[0190] In various embodiments, one or both of the positive electrode and the negative electrode include a network of high aspect ratio carbon elements defining void spaces within the network.

[0191] Figure 7 It is a schematic diagram of the energy storage device.

[0192] refer to Figure 7 , shows an energy storage cell 700, which includes a first electrode 701, a second electrode 702, a permeable separator 703 disposed between the first electrode 701 and the second electrode 702, and an electrolyte 704 that wets the first and second electrodes. One or both of the electrodes 701, 702 may be of the type described herein. In some embodiments, the first electrode 701 is a Figure 1A Electrode 100 or Figure 1B In some embodiments, the second electrode 702 is a positive electrode corresponding to or similar to Figure 5A Electrode 500 or Figure 5B The electrode 525 is the negative electrode.

[0193] In some embodiments, the energy storage cell 700 may be a battery, such as a lithium-ion battery. In some such embodiments, the electrolyte may be a lithium salt dissolved in a solvent, for example, the type described in Qi Li, June Chen, Lei Fan, Xueqian Kong, Yingying Lu, Progress in electrolytes for rechargeable Li-based batteries and beyond, Green Energy & Environment, Vol. 1, No. 1, pp. 18-42, the entire contents of which are incorporated herein by reference.

[0194] In some such embodiments, the energy storage cell 700 has an operating voltage within the range of 1.0 V to 5.0 V or any sub-range thereof, such as 2.3 V - 4.3 V.

[0195] In some such embodiments, energy storage cell 700 has an operating temperature range that includes -40°C to 100°C or any sub-range thereof, such as -10°C to 60°C.

[0196] In some such embodiments, the energy storage cell 700 has a gravimetric energy density of at least 100 Wh / kg, 200 Wh / kg, 300 Wh / kg, 400 Wh / kg, 500 Wh / kg, 1000 Wh / kg, or more.

[0197] In some such embodiments, the energy storage cell 700 has a volumetric energy density of at least 200Wh / L, 400Wh / L, 600Wh / L, 800Wh / L, 1,000Wh / L, 1,500Wh / L, 2,000Wh / L, or more.

[0198] In some such embodiments, energy storage cell 700 has a C-rate in the range of 0.1 to 50.

[0199] In some such embodiments, the energy storage cell 700 has a cycle life of at least 1,000, 1500, 2,000, 2,500, 3,000, 3,500, 4,000, or more charge and discharge cycles.

[0200] In some embodiments, the energy storage battery 700 may be a lithium ion capacitor of the type described in U.S. Patent Application Serial No. 63 / 021,492, filed on May 8, 2020, the entire contents of which are incorporated herein by reference.

[0201] In some such embodiments, energy storage cell 700 has an operating temperature range that includes -60°C to 100°C or any sub-range thereof, such as -40°C to 85°C.

[0202] In some such embodiments, the energy storage cell 700 has a gravimetric energy density of at least 10Wh / kg, 15Wh / kg, 20Wh / kg, 30Wh / kg, 40Wh / kg, 50Wh / kg, or more.

[0203] In some such embodiments, the energy storage cell 700 has a volumetric energy density of at least 20Wh / L, 30Wh / L, 40Wh / L, 50Wh / L, 60Wh / L, 70Wh / L, 80Wh / L, or more.

[0204] In some such embodiments, the energy storage cell 700 has a gravimetric energy density of at least 5 kW / kg, 7.5 kW / kg, 10 kW / kg, 12.5 kW / kg, 14 kW / kg, 15 kW / kg, or more.

[0205] In some such embodiments, the energy storage cell 700 has a volumetric energy density of at least 10 kW / L, 15 kW / L, 20 kW / L, 22.5 kW / L, 25 kW / L, 28 kW / L, 30 kW / L, or more.

[0206] In some such embodiments, energy storage cell 700 has a C-rate in the range of 1.0 to 100.

[0207] In some such embodiments, energy storage cell 700 has a cycle life of at least 100,000, 500,000, 1,000,000, or more charge and discharge cycles.

[0208] Manufacturing method

[0209] As described herein include Figure 1A The electrode 100 includes an active layer 106, Figure 1B The electrode 125 of the active layer 132 includes Figure 5A The electrode 500 includes an active layer 506 and includes Figure 5B The electrode 532 of the active layer can be manufactured using any suitable manufacturing process. As will be appreciated by those skilled in the art, in some embodiments, electrodes 100, 125, 500, and 525 can be manufactured using a wet coating technique of the type described in International Patent Publication No. WO / 2018 / 102652 published on June 7, 2018, further considering the teachings described herein.

[0210] Figure 8 is a flow chart of a method for preparing an electrode according to various embodiments. Figure 1A The process 600 can be similarly implemented in conjunction with manufacturing electrodes according to various embodiments disclosed herein, including Figure 1B Electrode 125, Figure 5A The electrodes 500 and Figure 5B Electrode 525.

[0211] refer to Figure 8 In some embodiments, the active layer 106 of the electrode 100 can be formed using process 800. At 810, the high aspect ratio carbon element 201 and a surface treatment material (eg, a surfactant or polymer material as described herein) are combined with a solvent (of the type described herein) to form an initial slurry.

[0212] At 820, the initial slurry is treated to ensure good dispersion of the solid material in the slurry. In some embodiments, the treatment includes introducing mechanical energy into the mixture of the solvent and the solid material (e.g., using a sonicator, which may also sometimes be referred to as a "sonicator") or other suitable mixing device (e.g., a high shear mixer). In some embodiments, the mechanical energy introduced into the mixture is at least 0.4 kilowatt-hours / kilogram (kWh / kg), 0.5 kWh / kg, 0.6 kWh / kg, 0.7 kWh / kg, 0.8 kWh / kg, 0.9 kWh / kg, 1.0 kWh / kg or greater. For example, the mechanical energy introduced into the mixture per kilogram of the mixture may be in the range of 0.4 kWh / kg to 1.0 kWh / kg or any sub-range thereof, such as 0.4 kWh / kg to 0.6 kWh / kg.

[0213] In some embodiments, an ultrasonic bath mixer can be used. In other embodiments, a probe sonicator can be used. When compared with an ultrasonic bath for nanoparticle applications, probe sonication may be significantly more powerful and effective. The high shear forces generated by ultrasonic cavitation can break up particle agglomerates and produce smaller and more consistent particle sizes. Among them, sonication can cause solids to form a stable and uniform suspension in the slurry. Typically, this will result in dispersion and deagglomeration of solids and other decompositions. Examples of probe sonication devices include the Q series probe sonicators available from QSonica LLC in Newtown, Connecticut. Another example includes the BransonDigital SFX-450 sonicator available from Thomas Scientific in Swedesboro, New Jersey.

[0214] However, in some embodiments, the local nature of each probe within the probe assembly may result in uneven mixing and suspension. For example, this may be the case for large samples. This can be addressed by using a device with a continuous flow cell and appropriate mixing. For example, with such a setup, mixing of the slurry will achieve a fairly consistent dispersion.

[0215] In some embodiments, the initial slurry, once processed, will have a viscosity in the range of 5,000 cps to 25,000 cps, or any sub-range thereof, such as 6,000 cps to 19,000 cps.

[0216] At 830, the surface treatment 202 may be formed completely or partially on the high aspect ratio carbon element 201 in the initial slurry. In some embodiments, at this stage, the surface treatment 202 may be formed as described above with reference to Figure 2 and Figure 3 The resulting surface treatment 201 may include functional groups or other features that may promote adhesion between the high aspect ratio carbon element 201 and the active material particles 300 as described in further steps below.

[0217] At 840 , the active material particles 300 may be combined with the initial slurry to form a final slurry that includes the active material particles 300 and the high aspect ratio carbon elements 201 having the surface treatment 202 formed thereon.

[0218] In some embodiments, active material 300 may be added directly to the initial slurry. In other embodiments, active material 300 may first be dispersed in a solvent (e.g., using the techniques described above with respect to the initial solvent) to form an active material slurry. This active material slurry may then be combined with the initial slurry to form a final slurry.

[0219] At 850, the final slurry is processed to ensure good dispersion of the solid materials in the final slurry. In various embodiments, any suitable mixing method known in the art can be used. In some embodiments, the processing can use the techniques described above with reference to 820. In some embodiments, a planetary mixer can be used, such as a multi-axis (e.g., three-axis or more) planetary mixer. In some such embodiments, the planetary mixer can have multiple blades, such as two or more mixing blades and one or more (e.g., two, three or more) dispersion blades, such as disc dispersion blades.

[0220] In some embodiments, during 850, the matrix 200 engaging the active material 300 may be fully or partially self-assembled, as described above with reference to Figure 2 and Figure 3 In some embodiments, the interaction between the surface treatment 202 and the active material 300 promotes the self-assembly process.

[0221] In some embodiments, the final slurry, once processed, will have a viscosity in the range of 1,000 cps to 10,000 cps or any sub-range thereof, for example, 2,500 cps to 6000 cps.

[0222] At 860, active layer 106 is formed from the final slurry. In some embodiments, the final slurry may be wet cast directly onto current collector conductive layer 102 (or optional adhesion layer 104) and dried. As an example, casting may be performed by applying at least one of heat and vacuum until substantially all solvent and any other liquid has been removed, thereby forming active layer 106. In some such embodiments, it may be desirable to protect portions of the underlying layer. For example, where electrode 100 is intended for two-sided operation, it may be desirable to protect the underside of conductive layer 102. Protection may include preventing solvents, such as by masking certain areas or providing drains to divert solvents away.

[0223] In other embodiments, the final slurry may be at least partially dried elsewhere and then transferred to the adhesive layer 104 or the conductive layer 102 using any suitable technique (e.g., roll-to-roll application) to form the active layer 106. In some embodiments, the wet combined slurry may be placed on an intermediate material having an appropriate surface and dried to form a layer (e.g., active layer 106). Although any material having an appropriate surface may be used as an intermediate material, an exemplary intermediate material includes PTFE because its properties facilitate subsequent removal from the surface. In some embodiments, the specified layer is formed in a press to provide a layer exhibiting a desired thickness, area, and density.

[0224] In some embodiments, the final slurry may be formed into a sheet and applied to the adhesion layer 104 or the conductive layer 102 as appropriate. For example, in some embodiments, the final slurry may be applied by a slot die to control the thickness of the applied layer. In other embodiments, the slurry may be applied and then leveled to the desired thickness, for example, using a scraper. A variety of other techniques may be used to apply the slurry. For example, the coating technique may include, but is not limited to: comma coating; comma reverse coating; blade coating; slot die extrusion coating; direct gravure coating; air knife coating (air knife); chamber blade coating; offset gravure coating; one roll kiss coating; reverse kiss coating using a small diameter gravure roller; rod coating; three reverse roll coating (top feed); three reverse roll coating (fountain die); reverse roll coating, etc.

[0225] The viscosity of the final slurry may vary depending on the application technique. For example, for comma coating, the viscosity may range from about 1,000 cps to about 200,000 cps. Lip die coating provides for coating with a slurry exhibiting a viscosity between about 500 cps and about 300,000 cps. Reverse kiss coating provides for coating with a slurry exhibiting a viscosity between about 5 cps and 1,000 cps. In some applications, the respective layers may be formed by a plurality of passages.

[0226] In some embodiments, the active layer 106 formed from the final slurry may be compressed (e.g., using a calendaring device) before or after being applied to the electrode 100. In some embodiments, the slurry may be partially or completely dried (e.g., by applying heat, vacuum, or a combination thereof) before or during the compression process. For example, in some embodiments, the active layer may be compressed to a final thickness (e.g., in a direction perpendicular to the current collector layer 102) that is less than 90%, 80%, 70%, 50%, 40%, 30%, 20%, 10% or less of its pre-compression thickness.

[0227] In various embodiments, when a partially dried layer is formed during the coating or compression process, the layer may subsequently be fully dried (eg, by applying heat, vacuum, or a combination thereof). In some embodiments, substantially all of the solvent is removed from the active layer 106 .

[0228] In some embodiments, the solvent used to form the slurry is recovered and recycled into the slurry manufacturing process.

[0229] In some embodiments, the active layer 106 may be compressed, for example to break some of the constituent high aspect ratio carbon elements or other carbonaceous materials, to increase the surface area of ​​the corresponding layer. In some embodiments, the compression process may increase one or more of the adhesion between layers, the ion transport rate within the layer, and the surface area of ​​the layer. In various embodiments, the compression may be applied before or after the corresponding layer is applied to or formed on the electrode 100.

[0230] In some embodiments where calendaring is used to compress the active layer 106, the calendaring equipment may be set to have a gap spacing equal to less than 90%, 80%, 70%, 50%, 40%, 30%, 20%, 10% or less of the pre-compression thickness of the layer (e.g., set to about 33% of the pre-compression thickness of the layer). The calendaring rollers may be configured to provide a suitable pressure, for example, greater than 1 ton per cm of roller length, greater than 1.5 tons per cm of roller length, greater than 2.0 tons per cm of roller length, greater than 2.5 tons per cm of roller length, or greater. In some embodiments, the active layer after compression will have a density in the range of 1 g / cc to 10 g / cc, or any sub-range thereof, such as 2.5 g / cc to 4.0 g / cc. In some embodiments, the calendaring process may be performed at a temperature in the range of 20°C to 140°C or any sub-range thereof. In some embodiments, the active layer 106 may be preheated prior to calendaring, for example, at a temperature in the range of 20°C to 100°C or any sub-range thereof.

[0231] Once the electrode 100 has been assembled, the electrode 100 can be used to assemble an energy storage device. The assembly of the energy storage device can follow conventional steps for assembling the electrode with the separator and placing it in a housing (such as a can or bag), and can further include additional steps for electrolyte addition and sealing the housing.

[0232] In various embodiments, process 800 may include any of the following features (alone or in any suitable combination):

[0233] In some embodiments, the initial slurry has a solids content in the range of 0.1%-20.0% by weight (or any subrange thereof). In some embodiments, the final slurry has a solids content in the range of 10.0%-80% by weight (or any subrange thereof).

[0234] In various embodiments, the solvent used can be any solvent described herein with respect to the formation of surface treatment 202. In some embodiments, the surfactant material used to form surface treatment 202 is soluble in a solvent that exhibits favorable properties. For example, in some embodiments, the solvent can include water or an alcohol such as methanol, ethanol, or 2-propanol (isopropanol, sometimes referred to as IPA) or a combination thereof. In some embodiments, the solvent can include one or more additives for further improving the properties of the solvent, such as low boiling point additives such as acetonitrile (ACN), deionized water, and tetrahydrofuran.

[0235] In some embodiments, if a low boiling point solvent is used, a thermal drying process performed at a relatively low temperature can be used to quickly remove the solvent. As will be appreciated by those skilled in the art, this can increase the manufacturing speed and / or cost of the electrode 100. For example, in some embodiments, the solvent can have a boiling point of less than 250°C, 225°C, 202°C, 200°C, 185°C, 180°C, 175°C, 150°C, 125°C or less, for example, less than or equal to 100°C.

[0236] In some embodiments, the solvent may exhibit other advantageous properties. In some embodiments, the solvent may have a low viscosity, such as a viscosity at 20° C. less than or equal to 3.0 centipoise, 2.5 centipoise, 2.0 centipoise, 1.5 centipoise, or less. In some embodiments, the solvent may have a low surface tension, such as a surface tension at 20° C. less than or equal to 40 mN / m, 35 mN / m, 30 mN / m, 25 mN / m, or less. In some embodiments, the solvent may have a low toxicity, such as a toxicity comparable to that of alcohols such as isopropanol.

[0237] In some embodiments, during the formation of the active layer, the material forming the surface treatment may be dissolved in a solvent that is substantially free of pyrrolidone compounds. In some embodiments, the solvent is substantially free of n-methyl-2-pyrrolidone.

[0238] In some embodiments, surface treatment 201 is formed from a material that includes a surfactant of the type described herein.

[0239] In some embodiments, dispersing the high aspect ratio carbon elements and the surface treatment material in a solvent to form an initial slurry includes applying a force to the agglomerated carbon elements to cause the elements to slide apart from each other in a direction transverse to the short axis of the elements. In some embodiments, the techniques for forming such dispersions may be adapted from those disclosed in International Patent Publication No. WO / 2018 / 102652, published on June 7, 2018, which is hereby incorporated herein in its entirety for all purposes with further consideration of the teachings described herein.

[0240] In some embodiments, the high aspect ratio carbon element 201 can be functionalized prior to forming a slurry for forming the electrode 100. For example, in one aspect, a method is disclosed that includes dispersing the high aspect ratio carbon element 201 and a surface treatment material in an aqueous solvent to form an initial slurry, wherein the dispersing step results in the formation of a surface treatment on the high aspect ratio carbon element; drying the initial slurry to remove substantially all of the water, thereby obtaining a dry powder of high aspect ratio carbon having the surface treatment thereon. In some embodiments, the dry powder can be combined, for example, with a slurry of a solvent and an active material to form a final solution of the type described above with reference to method 800.

[0241] In some embodiments, drying the initial slurry comprises freeze-drying (freeze-drying) the initial slurry. In some embodiments, the aqueous solvent and the initial slurry are substantially free of substances that damage the high aspect ratio carbon elements. In some embodiments, the aqueous solvent and the initial slurry are substantially free of acid. In some embodiments, the initial slurry is substantially composed of high aspect ratio carbon elements, surface treatment materials and water.

[0242] Some embodiments further include dispersing a dry powder of high aspect ratio carbon with a surface treatment in a solvent and adding an active material to form a secondary slurry; coating the secondary slurry on a substrate; and drying the secondary slurry to form an electrode active layer. In some embodiments, further considering the teachings described herein, the aforementioned steps can be performed using techniques adapted from those disclosed in International Patent Publication No. WO / 2018 / 102652 published on June 7, 2018.

[0243] In some embodiments, the final slurry may include a polymer additive such as polyacrylic acid (PAA), poly(vinyl alcohol) (PVA), poly(vinyl acetate) (PVAc), polyacrylonitrile (PAN), polyisoprene (PIpr), polyaniline (PANi), polyethylene (PE), polyimide (PI), polystyrene (PS), polyurethane (PU), polyvinyl butyral (PVB), polyvinyl pyrrolidone (PVP). In some embodiments, the active layer may be treated by applying heat to pyrolyze the additive so that the surface treatment 202 may form a carbonaceous material layer produced by pyrolysis of the polymer additive. The carbonaceous material layer (e.g., graphite or amorphous carbon) may be attached (e.g., via covalent bonds) to the active material particles or otherwise promote adhesion to the active material particles 300. The heat treatment may be performed in any suitable manner, such as by applying a laser beam. Examples of suitable pyrolysis techniques are described in U.S. Patent Application Serial No. 63 / 028982, filed May 22, 2020, which is incorporated herein in its entirety for all purposes.

[0244] Surfactants

[0245] The above technique includes surface treating 202 the high aspect ratio carbon nanotubes 201 with a surfactant to promote adhesion with active material particles 300. While several advantageously suitable surfactants have been described, it should be understood that other surfactant materials may be used, including the following.

[0246] Surfactants are molecules or groups of molecules with surface activity, including wetting agents, dispersants, emulsifiers, detergents and foaming agents. Various surfactants can be used to prepare surface treatments as described herein. Typically, the surfactant used comprises a lipophilic non-polar hydrocarbon group and a polar functional hydrophilic group. The polar functional group can be a carboxylate, ester, amine, amide, imide, hydroxyl, ether, nitrile, phosphate, sulfate or sulfonate. Surfactants can be used alone or in combination. Therefore, the combination of surfactants can include anionic, cationic, nonionic, zwitterionic, amphiphilic and amphoteric surfactants, as long as there is a net positive charge or a net negative charge in the head region of the surfactant molecule population. In some cases, a single negatively charged or positively charged surfactant is used in the preparation of the electrode composition of the present invention.

[0247] The surfactant used in the preparation of the electrode composition of the present invention may be an anion, including but not limited to sulfonates such as alkyl sulfonates, alkylbenzene sulfonates, alpha olefin sulfonates, paraffin sulfonates and alkyl ester sulfonates; sulfates such as alkyl sulfates, alkyl alkoxy sulfates and alkyl alkoxylated sulfates; phosphates such as monoalkyl phosphates and dialkyl phosphates; phosphate esters; carboxylates such as fatty acids, alkyl alkoxy carboxylates, sarcosinates, isethionates and taurates. Specific examples of carboxylates are sodium oleate, sodium cocoyl isethionate, sodium methyl oleyl taurate, sodium laureth carboxylate, sodium trideceth carboxylate, sodium lauryl sarcosinate, lauroyl sarcosine and cocoyl sarcosinate. Specific examples of sulfates include sodium dodecyl sulfate (SDS), sodium lauryl sulfate, sodium laureth sulfate, sodium trideceth sulfate, sodium tridecyl sulfate, sodium coconut sulfate and sodium lauric acid monoglyceride sulfate.

[0248] Suitable sulfonate surfactants include, but are not limited to, alkyl sulfonates, aryl sulfonates, mono- and di-alkyl sulfosuccinates, and mono- and di-alkyl sulfosuccinamates. Each alkyl group independently contains from about 2 to 20 carbons, and each alkyl group may also be ethoxylated with up to about 8 units, preferably up to about 6 units (e.g., an average of 2, 3, or 4 units) of ethylene oxide. Illustrative examples of alkyl and aryl sulfonates are sodium tridecylbenzene sulfonate (STBS) and sodium dodecylbenzene sulfonate (SDBS).

[0249] Illustrative examples of sulfosuccinates include, but are not limited to, dimethicone copolyol sulfosuccinate, diamyl sulfosuccinate, dioctyl sulfosuccinate, dicyclohexyl sulfosuccinate, diheptyl sulfosuccinate, dihexyl sulfosuccinate, diisobutyl sulfosuccinate, dioctyl sulfosuccinate, C12-15 pareth sulfosuccinate, cetearyl sulfosuccinate, cocoyl polyglucose sulfosuccinate, cocoyl butylglucose polyether-10 sulfosuccinate, decetheth-5 sulfosuccinate, decetheth-6 sulfosuccinate, dihydroxyethyl sulfosuccinyl undecylenate, hydrogenated cottonseed glycerides sulfosuccinate, isodecyl sulfosuccinate, isostearyl sulfosuccinate, Adipose sulfosuccinate, laureth-5 sulfosuccinate, lauryl ether sulfosuccinate, laureth-12 sulfosuccinate, laureth-6 sulfosuccinate, laureth-9 sulfosuccinate, dodecyl sulfosuccinate, nonoxynol-10 sulfosuccinate, oleth-3 sulfosuccinate, oleyl sulfosuccinate, PEG-10 lauryl citrate sulfosuccinate, silicone alcohol polyether-14 sulfosuccinate, stearyl sulfosuccinate, tallow, tridecyl sulfosuccinate, ditridecyl sulfosuccinate, diethylene glycol castor oil sulfosuccinate, di(1,3-dimethylbutyl) sulfosuccinate and silicone copolyol sulfosuccinate.

[0250] Illustrative examples of sulfosuccinates include, but are not limited to, lauroamido-MEA sulfosuccinate, oleamido PEG-2 sulfosuccinate, cocamido MIPA-sulfosuccinate, cocamido PEG-3 sulfosuccinate, isostearamido MEA-sulfosuccinate, isostearamido MIPA-sulfosuccinate, lauroamido MEA-sulfosuccinate, lauroamido PEG-2 sulfosuccinate, lauroamido PEG-5 sulfosuccinate, myristamido MEA-sulfosuccinate, oleamido MEA-sulfosuccinate, oleamido PIPA-sulfosuccinate, oleamido PIPA-sulfosuccinate, and oleamido PIPA-sulfosuccinate. EG-2 sulfosuccinate, palmitamido PEG-2 sulfosuccinate, palmitoleamido PEG-2 sulfosuccinate, PEG-4 cocamide MIPA-sulfosuccinate, ricinoleamido MEA-sulfosuccinate, stearamido MEA-sulfosuccinate, stearoyl sulfosuccinate, talamido MEA-sulfosuccinate, tallow sulfosuccinate, tallowamido MEA-sulfosuccinate, undecylenamido MEA-sulfosuccinate, undecylenamido PEG-2 sulfosuccinate, wheat germamido MEA-sulfosuccinate and wheat germamido PEG-2 sulfosuccinate.

[0251] Some examples of commercial sulfonates are OT-S, OT-MSO, TR70% (Cytec Inc., West Paterson, NJ), NaSul CA-HT3 (King Industries, Norwalk, Conn.) and C500 (Crompton Co., West Hill, Ontario, Canada). OT-S is dioctyl sodium sulfosuccinate from petroleum distillates. OT-MSO also contains dioctyl sodium sulfosuccinate. TR70% is sodium ditridecyl sulfosuccinate in a mixture of ethanol and water. NaSul CA-HT3 is a calcium dinonylnaphthalene sulfonate / calcium carboxylate complex. C500 is an oil-soluble calcium sulfonate.

[0252] Alkyl or alkyl group refers to a saturated hydrocarbon having one or more carbon atoms, including straight-chain alkyl groups (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc.), cycloalkyl groups (or cycloalkyl or alicyclic or carbocyclic rings) (e.g., cyclopropyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, etc.), branched alkyl groups (e.g., isopropyl, tert-butyl, sec-butyl, isobutyl, etc.), and alkyl-substituted alkyl groups (e.g., alkyl-substituted cycloalkyl groups and cycloalkyl-substituted alkyl groups).

[0253] Alkyl groups may include both unsubstituted alkyl groups and substituted alkyl groups.Substituted alkyl groups refer to alkyl groups having substituents replacing one or more hydrogens on one or more carbons of the hydrocarbon backbone. Such substituents may include alkenyl, alkynyl, halogen, hydroxy, alkylcarbonyloxy, arylcarbonyloxy, alkoxycarbonyloxy, aryloxy, aryloxycarbonyloxy, carboxyl, alkylcarbonyl, arylcarbonyl, alkoxycarbonyl, aminocarbonyl, alkylaminocarbonyl, dialkylaminocarbonyl, alkylthiocarbonyl, alkoxy, phosphate, phosphonate, phosphino, cyano, amino (including alkylamino, dialkylamino, arylamino, diarylamino and alkylarylamino), acylamino (including alkylcarbonylamino, arylcarbonylamino, carbamoyl and ureido), imino, sulfo, alkylthio, arylthio, thiocarboxyl, sulfate, alkylsulfinyl, sulfonate, sulfamoyl, sulfonamido, nitro, trifluoromethyl, cyano, azido, heterocyclyl, alkylaryl or aromatic (including heteroaromatic) groups.

[0254] In some embodiments, the substituted alkyl group may include a heterocyclic group. The heterocyclic group includes a closed ring structure similar to a carbocyclic group, wherein one or more carbon atoms in the ring are elements other than carbon, such as nitrogen, sulfur or oxygen. The heterocyclic group may be saturated or unsaturated. Exemplary heterocyclic groups include aziridine, oxirane (epoxide, oxirane), thiirane (episulfide), dioxirane, azetidine, oxetane, thiamine, dioxetane, dithiamine, dithiamine, oxazolidine, pyrrolidine, pyrroline, tetrahydrofuran, dihydrofuran and furan.

[0255] For anionic surfactants, the counterion is typically sodium, but may alternatively be potassium, lithium, calcium, magnesium, ammonium, an amine (primary, secondary, tertiary or tetramine) or other organic base. Exemplary amines include isopropylamine, ethanolamine, diethanolamine and triethanolamine. Mixtures of the above cations may also be used.

[0256] The surfactant used to prepare the material of the present invention may be cationic. Such cationic surfactants include, but are not limited to, pyridinium-containing compounds and primary, secondary, tertiary or quaternary organic amines. For cationic surfactants, the counterion may be, for example, chlorine, bromine, methosulfate, ethosulfate, lactate, saccharinate, acetate and phosphate. Examples of cationic amines include polyethoxylated oleylamine / stearylamine, ethoxylated tallowamine, coconut alkylamine, oleylamine and tallow alkylamine, and mixtures thereof.

[0257] Examples of quaternary amines having a single long alkyl group are cetyltrimethylammonium bromide (CTAB), benzyldodecyldimethylammonium bromide (BddaBr), benzyldimethylhexadecylammonium chloride (BdhaCl), dodecyltrimethylammonium bromide, myristyltrimethylammonium bromide, octadecyldimethylbenzylammonium chloride, oleyldimethylbenzylammonium chloride, lauryltrimethylammonium sulfate (also known as cocotrimonium sulfate), cetyldimethylhydroxyethylammonium dihydrogen phosphate, basutamidopropyldimethylammonium chloride, cocotrimonium chloride, dioctadecyldimonium chloride, maltamidopropyldimethylammonium chloride, stearyloctyldimethylammonium chloride, isostearylamidopropyldimethylammonium chloride, dihydroxypropyl PEG-5 linoleate ammonium chloride, PEG-2 stearammonium chloride, behentrimonium chloride, dicetyldimonium chloride, tallowtrimonium chloride, and behenamidopropylethyldimethylammonium sulfate.

[0258] Examples of quaternary amines having two long alkyl groups are didodecyldimethylammonium bromide (DDAB), distearyldimethylammonium chloride, dicetyldimethylammonium chloride, stearoctyldimethylammonium sulfate, dihydrogenated palmitoylethyl hydroxyethylammonium methylsulfate, dipalmitoylethyl hydroxyethylammonium methylsulfate, dioleoylethyl hydroxyethylammonium methylsulfate and hydroxypropyl distearyldimethylammonium chloride.

[0259] Quaternary ammonium compounds of imidazoline derivatives include, for example, isostearyl benzyl imidazoline ammonium chloride, cocoyl benzyl hydroxyethyl imidazoline ammonium chloride, cocoyl hydroxyethyl imidazoline PG-chloride phosphate and stearyl hydroxyethyl imidazoline ammonium chloride. Other heterocyclic quaternary ammonium compounds such as dodecylpyridinium chloride, amprolium hydrochloride (AH) and benzethonium hydrochloride (BH) can also be used.

[0260] The surfactant used to prepare the material of the present invention can be nonionic, including but not limited to polyoxyalkylene carboxylates, fatty acid esters, fatty alcohols, ethoxylated fatty alcohols, poloxamers, alkanolamides, alkoxylated alkanolamides, polyethylene glycol monoalkyl ethers and alkyl polysaccharides. Polyoxyalkylene carboxylates have one or two carboxylate moieties each having about 8 to 20 carbons and a polyoxyalkylene moiety comprising about 5 to 200 alkylene oxide units. Ethoxylated fatty alcohols include an ethylene oxide moiety containing about 5 to 150 ethylene oxide units and a fatty alcohol moiety having about 6 to about 30 carbons. The fatty alcohol moiety can be cyclic, linear or branched, and saturated or unsaturated. Some examples of ethoxylated fatty alcohols include glycol ethers of oleyl alcohol, stearyl alcohol, lauryl alcohol and isohexadecanol. Poloxamers are block copolymers of ethylene oxide and propylene oxide, with about 15 to about 100 moles of ethylene oxide. Alkyl polysaccharide ("APS") surfactants (e.g., alkyl polyglycosides) contain a hydrophobic group having from about 6 to about 30 carbons and a polysaccharide (e.g., polyglycoside) as a hydrophilic group. An example of a commercial nonionic surfactant is FOA-5 (Octel Starreon LLC., Littleton, Colo.).

[0261] Specific examples of suitable nonionic surfactants include alkanolamides such as cocamide diethanolamide ("DEA"), cocamide monoethanolamide ("MEA"), cocamide monoisopropanolamide ("MIPA"), PEG-5 cocamide MEA, lauramide DEA, and lauramide MEA; alkylamine oxides such as lauramine oxide, cocamine oxide, cocamidopropylamine oxide, and lauroamidopropylamine oxide; sorbitan laurate, sorbitan distearate, fatty acids or fatty acid esters such as lauric acid, isostearic acid, and PEG-150 distearate; fatty alcohols or ethoxylated fatty alcohols such as lauryl alcohol, alkyl polyglycosides such as decyl glucoside, lauryl glucoside, and coco glucoside.

[0262] The surfactants used to prepare the materials of the present invention may be zwitterionic, having both formal positive and negative charges on the same molecule. The positively charged groups may be quaternary ammonium, phosphonium or sulfonium, while the negatively charged groups may be carboxyl, sulfonate, sulfate, phosphate or phosphate ester. Similar to other classes of surfactants, the hydrophobic portion may contain one or more long, straight, cyclic or branched aliphatic chains of about 8 to 18 carbon atoms. Specific examples of zwitterionic surfactants include alkyl betaines such as cocodimethyl carboxymethyl betaine, lauryl dimethyl carboxymethyl betaine, lauryl dimethyl α-carboxyethyl betaine, hexadecyl dimethyl carboxymethyl betaine, lauryl bis-(2-hydroxyethyl) carboxymethyl betaine, stearyl bis-(2-hydroxypropyl) carboxymethyl betaine, oleyl dimethyl γ-carboxypropyl betaine and lauryl bis-(2-hydroxypropyl) α-carboxyethyl betaine, amidopropyl betaine; and alkyl sulfobetaines such as cocodimethyl sulfopropyl betaine, stearyl dimethyl sulfopropyl betaine, lauryl dimethyl sulfoethyl betaine, lauryl bis-(2-hydroxyethyl) sulfopropyl betaine and alkylamidopropyl hydroxysulfobetaine.

[0263] The surfactant used to prepare the material of the present invention may be amphoteric. Examples of suitable amphoteric surfactants include alkyl amphocarboxy glycinates and alkyl amphocarboxy propionates, alkyl amphodipropionates, alkyl amphodiacetates, alkyl amphoglycinates and alkyl amphopropionates, and ammonium or substituted ammonium salts of alkyl iminopropionates, alkyl iminodipropionates and alkyl amphopropyl sulfonates. Specific examples are cocoamphoacetate, cocoamphopropionate, cocoamphodiacetate, lauroamphoacetate, lauroamphodiacetate, lauroamphodipropionate, lauroamphodiacetate, cocoamphopropyl sulfonate, hexamethylenediacetate, hexamethyleneacetate, hexamethylenedipropionate and stearamphoacetate.

[0264] Surfactants used to prepare the materials of the present invention may also be polymers such as N-substituted polyisobutenyl succinimides and succinates, alkyl methacrylate vinyl pyrrolidone copolymers, alkyl methacrylate-dialkylaminoethyl methacrylate copolymers, alkyl methacrylate polyethylene glycol methacrylate copolymers, polystearamide and polyethylene imine.

[0265] The surfactant used to prepare the material of the present invention can also be a polysorbate type nonionic surfactant, such as polyoxyethylene (20) sorbitan monolaurate (polysorbate 20), polyoxyethylene (20) sorbitan monopalmitate (polysorbate 40), polyoxyethylene (20) sorbitan monostearate (polysorbate 60) or polyoxyethylene (20) sorbitan monooleate (polysorbate 80).

[0266] The surfactant used to prepare the material of the present invention can be an oil-based dispersant, which includes alkyl succinimides, succinates, high molecular weight amines, and Mannich bases and phosphoric acid derivatives. Some specific examples are polyisobutenyl succinimide-polyethylene polyamine, polyisobutenyl succinate, polyisobutenyl hydroxybenzyl-polyethylene polyamine and dihydroxypropyl phosphate.

[0267] The surfactant used to prepare the material of the present invention can be a combination of two or more surfactants of the same or different types selected from the group consisting of anionic, cationic, nonionic, zwitterionic, amphoteric and amphoteric surfactants. Suitable examples of combinations of two or more surfactants of the same type include, but are not limited to, a mixture of two anionic surfactants, a mixture of three anionic surfactants, a mixture of four anionic surfactants, a mixture of two cationic surfactants, a mixture of three cationic surfactants, a mixture of four cationic surfactants, a mixture of two nonionic surfactants, a mixture of three nonionic surfactants, a mixture of four nonionic surfactants, a mixture of two zwitterionic surfactants, a mixture of three zwitterionic surfactants, a mixture of four zwitterionic surfactants, a mixture of two amphoteric surfactants, a mixture of three amphoteric surfactants, a mixture of four amphoteric surfactants, a mixture of two amphoteric surfactants, a mixture of three amphoteric surfactants and a mixture of four amphoteric surfactants.

[0268] Polymer particles

[0269] The above techniques include using a polymer to form a surface treatment 201 on the high aspect ratio carbon nanotubes to promote adhesion with the active material particles 300. While several advantageously suitable polymers have been described, it should be understood that other polymer materials may be used, including the following.

[0270] The polymer used to prepare the material of the present invention can be a polymer material, such as a water-processable polymer material and / or an alcohol-processable polymer material. In various embodiments, any of the following polymers (and combinations thereof) can be used: polyacrylic acid (PAA), poly(vinyl alcohol) (PVA), poly(vinyl acetate) (PVAc), polyacrylonitrile (PAN), polyisoprene (PIpr), polyaniline (PANi), polyethylene (PE), polyimide (PI), polystyrene (PS), polyurethane (PU), polyvinyl butyral (PVB), polyvinyl pyrrolidone (PVP). In some embodiments, another exemplary polymer material is fluoroacrylic mixed latex (TRD202A), and is provided by JSR Corporation.

[0271] Fig. 9 is a cross-sectional view of the energy storage device.

[0272] Fig.10 A schematic diagram of an energy storage device such as a pouch cell is shown.

[0273] Fig.11 are schematic cross-sectional diagrams depicting aspects of an energy storage device (ESD).

[0274] Fig.10 and Fig.11 A schematic diagram of a pouch cell is shown. Fig.10 As shown, the energy storage battery 1000 includes a positive electrode 1010 and a negative electrode 1320, the positive electrode including an active layer 1060, and the negative electrode including an active layer 1340. In some embodiments, the energy storage battery 1300 further includes a negative electrode 1330, the negative electrode including an active layer 1350. According to various embodiments, the positive electrode 1310 may be a double-sided positive electrode, which includes an active layer 1360 on both sides. Each side of the positive electrode 1360 may have an applicable portion of the active layer 1360 applied using the techniques described herein. The positive electrode 1310 may correspond to or may be similar to Figure 1A Electrode 100 or Figure 1B According to various embodiments, the negative electrode 13320 and / or the negative electrode 1330 may correspond to or may be similar to Figure 5A Electrode 500 or Figure 5B Electrode 525.

[0275] According to various embodiments, the teachings herein provide electrodes without PVDF binders in the positive electrode or other conventional binders in the negative electrode. Instead, as described above, the 3D carbon scaffold or matrix holds the active material particles together to form a viscous layer that is also firmly attached to the metal current collector. Such active material structures are formed during slurry preparation and subsequently in roll-to-roll ("R2R") coating and drying processes. One of the main advantages of this technology is its scalability and "insertion" nature, as various embodiments are compatible with conventional electrode manufacturing processes.

[0276] Formation of 3D carbon matrix during slurry preparation using the techniques described herein: Using, for example, a 2-step slurry preparation method (such as described above in reference Figure 8The high aspect ratio carbon material is appropriately dispersed and chemically functionalized (of the type described in process 800). The chemical functionalization is designed to form an organized self-assembled structure with the surface of the active material particles (e.g., NMC particles for the positive electrode or silicon particles ("Si") or silicon oxide ("SiOx") particles in the case of the negative electrode). The slurry so formed can be based on water and / or alcohol solvents for the positive electrode and water for the negative electrode, and such solvents are very easy to evaporate and handle during the manufacturing process. Electrostatic interactions promote self-organized structures in the slurry, and after the drying process, the bonding between the carbon matrix with active material particles so formed and the current collector surface is promoted by surface treatments (e.g., functional groups on the matrix) and strong entanglement of the active material in the carbon matrix.

[0277] As will be appreciated by those skilled in the art, the mechanical properties of the electrode can be readily modified by adjusting the surface functionalization and entanglement effects, depending on the application and mass loading requirements.

[0278] After coating and drying, the electrode undergoes a calendaring step to control the density and porosity of the active material. In NMC positive electrodes, densities of 3.5 g / cc or higher and porosities of 20% porosity or higher can be achieved. Porosity can be optimized depending on mass loading and LIB cell requirements. For SiOx / Si negative electrodes, porosity is specifically controlled to accommodate active material expansion during the lithiation process.

[0279] In some typical applications, the teachings herein can provide up to 20% or more reduction in $ / kWh. By using friendly solvents that evaporate easily, electrode yields are higher, and more importantly, energy consumption in long dryers is significantly reduced. Conventional NMP recovery systems are also greatly simplified when using alcohols or other solvent mixtures.

[0280] The teachings herein provide a 3D matrix that significantly increases the electrode conductivity by 10 to 100 times compared to electrodes using conventional binders (such as PVDF), which enables fast charging at the battery level. Using this technology, thick electrode coatings in the positive electrode with a thickness of up to 150um (or more) on each side of the current collector are possible. The combination of the solvent used in the slurry and the firm 3D carbon matrix is ​​designed to obtain a thick wet coating without cracking during the drying step. Thick positive electrodes with high-capacity negative electrodes can significantly increase energy density to 400Wh / kg or more.

[0281] Fast charging is achieved by combining a high capacity negative electrode lithiated by an alloying process (Si / SiOx) and by reducing the overall impedance of the battery when the negative electrode and positive electrode are combined as described herein. The teachings herein provide fast charging by having high conductivity electrodes, and particularly high conductivity positive electrodes.

[0282] One exemplary embodiment includes a Li-ion battery energy storage device in the form of a pouch cell that combines a Ni-rich NMC active material in the positive electrode and a SiOx and graphite blend active material in the negative electrode, wherein both the negative electrode and the positive electrode are made using a 3D carbon matrix process as described herein.

[0283] Schematic diagram of the electrode arrangement soft pack battery device is shown in Fig. 9 As shown. As shown, a double-sided positive electrode using a positive electrode layer 960 (e.g., an active layer according to various embodiments disclosed herein) on opposite sides of an aluminum foil current collector 910 is disposed between two single-sided negative electrodes 920 and 930, each of which has negative electrode layers 940 and 950 (e.g., an active layer including a network of carbon elements as disclosed herein) disposed on a copper foil current collector. The electrodes are separated by a permeable separator material (not shown) wetted with an electrolyte (not shown). This arrangement can be accommodated in a soft pack battery of a type known in the art.

[0284] These devices can be characterized by high mass loading of Ni-rich NMC cathode electrodes and methods for their manufacture: mass loading = 20-30 mg / cm2, specific capacity > 210 mAh / g. SiOx / graphite anode (SiOx content = ~20 wt.%) based electrodes and material synthesis and manufacturing methods: mass loading 8-14 mg / cm2, reversible specific capacity ≥ 550 mAh / g. Long life performance of Li-ion electrolytes based on SiOx / graphite anodes for batteries: -30 to 60°C. High energy, high power density and long cycle life Ni-rich NMC cathode / SiOx+graphite / carbon+ based Li-ion soft pack batteries: capacity ≥ 5Ah, specific energy ≥ 300Wh / kg, energy density ≥ 800Wh / L, with a cycle life of more than 500 cycles at 1C rate charge and discharge, and ultra-high power fast charge and discharge C rate (up to 5C rate) capability.

[0285] Fig.10 are schematic cross-sectional diagrams depicting aspects of an energy storage device (ESD).

[0286] In general, the examples of energy storage devices (ESD) disclosed herein are illustrative. That is, the energy storage device (ESD) is not limited to the embodiments disclosed herein.

[0287] More specific examples of energy storage devices (ESDs) include supercapacitors, such as double layer capacitors (devices that store charge electrostatically), pseudocapacitors (which store charge electrochemically), and hybrid capacitors (which store charge both electrostatically and electrochemically). Typically, electrostatic double layer capacitors (EDLCs) use carbon electrodes or derivatives that have an electrostatic double layer capacitance much higher than the electrochemical pseudocapacitance, achieving charge separation in the Helmholtz double layer at the interface between the conductive electrode surface and the electrolyte. Typically, electrochemical pseudocapacitors use metal oxide or conductive polymer electrodes that have a large amount of electrochemical pseudocapacitance in addition to the double layer capacitance. Pseudocapacitance is achieved by faradaic electron charge transfer with redox reactions, intercalation, or electrosorption. Hybrid capacitors (such as lithium ion capacitors) use electrodes with different properties: one that exhibits primarily electrostatic capacitance, while the other exhibits primarily electrochemical capacitance.

[0288] Other examples of energy storage devices (ESD) include rechargeable batteries, accumulators, or secondary batteries, which are types of batteries that can be charged, discharged into a load, and recharged multiple times. During charging, the positive active material is oxidized, producing electrons, while the negative active material is reduced, consuming electrons. These electrons constitute the current from the external circuit. Typically, the electrolyte acts as a buffer for the internal ion flow between the electrodes (such as the negative and positive electrodes). Battery charge and discharge rates are often discussed by reference to the "C" rate of the current. The C rate is the rate at which the battery can theoretically be fully charged or discharged in one hour. The "depth of discharge" (DOD) is usually expressed as a percentage of the nominal ampere-hour capacity. For example, zero percent (0%) DOD means no discharge.

[0289] exist Fig.10 , a cross section of an energy storage device (ESD) 1400 is shown. The energy storage device (ESD) 1400 includes a housing 1411. The housing 1411 has two terminals 1410 disposed on the exterior thereof. The terminals 1410 provide internal electrical connections to a battery 1412 housed within the housing 1411 and external electrical connections to an external device, such as a load or a charging device (not shown).

[0290] Fig.11 It is a depiction Fig.10 Schematic cross-sectional view of various aspects of a prior art battery for an energy storage device (ESD).

[0291] Fig. 9A cross-sectional portion of battery 1400 is depicted in FIG. As shown in the figure, battery 1512 includes a multilayer energy storage material roll. That is, sheets or strips of energy storage material are rolled together to form a roll. The energy storage material roll includes opposing electrodes referred to as "negative electrode 1530" and "positive electrode 1540." Negative electrode 1530 and positive electrode 1540 are separated by separator 1550. Not shown in the figure but included as part of battery 1512 is an electrolyte. In general, the electrolyte permeates or wets positive electrode 1540 and negative electrode 1530 and promotes the migration of ions within battery 1512. According to various embodiments, positive electrode 1540 corresponds to or is similar to Figure 1A Electrode 100 or Figure 1B In some embodiments, the positive electrode 1540 corresponds to an electrode including a high aspect ratio carbon element network disclosed herein and / or a polymer additive disclosed herein. According to various embodiments, the negative electrode 1530 corresponds to or is similar to Figure 5A Electrode 500 or Figure 5B The negative electrode 1530 corresponds to an electrode comprising a network of high aspect ratio carbon elements disclosed herein and / or a polymer additive disclosed herein in some embodiments.

[0292] Figures 12 to 21 are graphs depicting various aspects of the electrical performance of energy storage cells assembled according to various embodiments.

[0293] Fig.12 is a graph depicting the C-rate of a half-cell constructed according to the teachings herein. The half-cell includes 22.5 mg / cm 2 The "best process" curve represents the binder-free electrode made according to the teachings of this article. The "old process" curve represents the binder-free electrode made without these surfactants and dispersants disclosed in this article. The "PVDF" curve represents the performance of the battery using electrodes made with the prior art. In this example, the half-cell has a pouch cell structure. The following table provides the initial specificity and C-rate test results. The working electrode size is 45x45mm, and the Li counter electrode is 46x46 mm. The electrolyte is 1M LiPF6 in EC / DMC (1 / 1 by volume) + 1% VC.

[0294] Fig.12 Data

[0295]

[0296] exist Fig.13In the figure, the test results of a complete soft pack battery are shown. In this example, the positive electrode is a 45X45 mm Ni-rich NMC, and the negative electrode is a 46x46 mm graphite electrode. The electrolyte is 1MLiPF6 in EC / DMC (1 / 1 by volume) + 1% VC. N / P ratio = ~1.1. It can be seen that the resistance of HPPC is much lower than that of the traditional PVDF process. Fig.17 As shown, lower charge resistance in the positive electrode results in improved performance at a ten percent state of charge in accordance with the teachings herein. Fig.19 It is shown that the positive electrodes made according to the teachings herein have improved cycling stability.

[0297] Another soft pack battery is constructed for testing. In this embodiment, the positive electrode is a Ni-rich NMC with a mass loading of 45X45 mm and 28-30 mg / cm2, and the negative electrode is a combination of graphite / SiOx (45% SiOx) electrodes with a mass loading of 46x46 mm and 8-9 mg / cm2. The electrolyte is 1.1MLiPF6 in PC:FEC:EMC:DEC=20:10:50:20. N / P ratio =~1.04 to 1.10. Both the NMC positive electrode and the 45% SiOx negative electrode manufacturing processes are used with the processes described herein, and a mixed surfactant and dispersant combined with a 3D nanocarbon matrix (e.g., NX electrode) is used. When the soft pack battery packaging efficiency is 90%, the Li-ion battery full battery specific energy is about 332Wh / kg, and if the packaging efficiency is increased to 95%, it is 351Wh / kg. When the soft-pack battery packaging efficiency is 90% and the soft-pack battery volume expansion is 10%, the energy density is about 808Wh / L; and when the soft-pack battery packaging efficiency is 95% and the soft-pack battery volume expansion is 10%, the energy density is about 853Wh / L. Based on the claimed electrode manufacturing process, the initial first cycle charge specific capacity of the positive and negative electrodes is about 228mAh / g and 852mAh / g; based on the claimed electrode manufacturing process, the initial first cycle discharge specific capacity of the positive and negative electrodes is about 210mAh / g and 750mAh / g. The LiB full battery capacity in this example is 240mAh for the first charge capacity and 216mAh for the first discharge capacity from 4.2V to 2.5V under 0.1C rate constant current charge and discharge. The initial coulomb efficiency is about ~90%. This data and various aspects of the electrical performance of the battery are Figures 14 to 21 Explained in.

[0298] Example properties of a battery using the resulting electrode are listed in the table below. In addition, the example battery exhibited no cracks or stresses that would normally appear in some physical tests.

[0299]

[0300]

[0301] Fig. 22 An example battery cell using an example of an electrode disclosed herein (eg, NX electrode) is shown. Battery cell 2600 has dimensions of approximately 46.5 mm x 48.5 mm x 7.14 mm. Fig. 22 The cells shown correspond to 1.5Ah to 3.5Ah cells. The cells shown (eg, with NX NMC811 electrodes) exhibit a first cycle charge specific capacity greater than or equal to 210 mAh / g, and an area capacity of substantially 5.6 mAh / cm2.

[0302] Fig.23 An example battery cell using an example of an electrode disclosed herein (eg, a NX electrode, such as an electrode including a 3D nanocarbon matrix) is shown. The battery cell 2700 has dimensions of approximately 62 mm x 107 mm x 5.4 mm. Fig.23 The illustrated battery cell 2700 corresponds to a 9.0Ah to 12.0Ah battery cell. The illustrated battery cell 2700 (eg, with NX NMC811 electrodes) exhibits a first cycle charge specific capacity greater than or equal to 1116 mAh / g, and an area capacity of substantially 6.5 mAh / cm2.

[0303] Fig.24 A graph 2800 showing characteristics of various examples of battery cells (e.g., pouch cells). The battery cells have dimensions of approximately 46mm x 46mm x 3mm. For a 9-layer NMC811 cathode and a 10-layer Si anode (e.g., a 1.5Ah cell), the battery cell packing efficiency is about ~86%; however, in large format pouch cells >5Ah with more stacked layers, the battery packing efficiency can be increased to 95% efficiency. The results show that Si anodes (5.5mg / cm2 to 5.0mg / cm2) can increase specific energy and energy density by at least 30% compared to graphite anode electrodes (16mg / cm2 to match 24mg / cm2 NX NMC811 cathodes) with the same small pouch cell format and number of layers.

[0304] Fig.25 Graph 2900 is shown comparing the performance of battery cells including positive electrodes according to various embodiments with control battery cells having conventional PVDF positive electrodes. Fig.19 As shown, using a positive electrode with a 3D nanocarbon matrix (e.g., NXNMC811) reduces the resistance by at least 20%.

[0305] Fig.26Graph 3000 is shown comparing the performance of a battery cell including a positive electrode according to various embodiments with a control battery cell having a conventional PVDF positive electrode. Fig.19 As shown, using a positive electrode with a 3D nanocarbon matrix (e.g., NXNMC811) reduces the resistance by at least 20%.

[0306] Fig. 27 Graph 3100 comparing the performance of battery cells including positive electrodes according to various embodiments with a control battery cell having a conventional PVDF positive electrode is shown. Fig. 20 The battery cells compared in the examples include NX Si-C negative electrodes (e.g., electrodes with a 3D nanocarbon matrix), are 1.5Ah cells, and are measured based on 1C1C cycling from 4.2V to 2.8V. Fig. 27 As shown, the positive electrode using a 3D nanocarbon matrix (e.g., NX NMC811) has a larger discharge density, and the difference in discharge density increases with the number of cycles. After 250 cycles, the battery cell according to various embodiments (e.g., a battery cell having a positive electrode including a 3D nanocarbon matrix) has a discharge capacity of at least 1275mAh, and preferably at least 1375mAh. After 250 cycles, the battery cell according to various embodiments (e.g., a battery cell having a positive electrode including a 3D nanocarbon matrix) has a discharge capacity of approximately 10% greater than that of the control battery cell (e.g., a battery cell having a positive electrode including PVDF).

[0307] Fig.28 A graph 3200 is shown illustrating the performance of a battery cell including electrodes according to various embodiments. Fig.28 The battery cell measured in the experiment includes a NX Si-C negative electrode (e.g., an electrode with a 3D nanocarbon matrix), a positive electrode according to various embodiments (e.g., a positive electrode with a 3D nanocarbon matrix), a 1.5Ah battery, and is measured according to 1C1C cycles from 4.2V to 2.8V. Fig.28 As shown, the battery including the positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity retention rate of about 82.7% after 500 cycles. The battery cell including the positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity drop of less than 300 mAh after 500 cycles.

[0308] Fig.29 Graph 3300 is shown illustrating the performance of a battery cell including electrodes according to various embodiments. Fig.29 A graph of fast charge cycle performance is provided. Fig.29The battery cell measured in the experiment includes a NX Si-C negative electrode (e.g., an electrode with a 3D nanocarbon matrix), a positive electrode according to various embodiments (e.g., a positive electrode with a 3D nanocarbon matrix), a 1.5Ah battery (e.g., a soft pack battery), and is measured at 1C / 1C (3 cycles) + 3.5C (CCCV 15min) / 1C (1 cycle) every 4 cycles in the voltage range of 4.2V to 2.8V. Fig.29 As shown, a battery including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity retention rate of at least 87% after 500 cycles. In some embodiments, a battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity retention rate of 87% to 88% after 500 cycles. A battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity retention rate of less than 300 mAh after 270 cycles.

[0309] Fig.30 A graph 3400 is shown illustrating the performance of a battery cell including electrodes according to various embodiments. Fig.30 A graph of discharge energy versus cycles is provided. Fig.30 The battery cells measured in the experiment include a NX Si-C negative electrode (e.g., an electrode with a 3D nanocarbon matrix), a positive electrode according to various embodiments (e.g., a positive electrode with a 3D nanocarbon matrix), a positive electrode with a load of 5.6 mAh / cm2 and an electrode density of 3.5 g / cc, and are measured in a voltage range of 4.2 V to 3.0 V according to 1C / 1C cycles. Fig.30 As shown, a battery including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity retention rate of at least 70% after 600 cycles, and preferably has a discharge capacity retention rate of at least 80% after 600 cycles. In some embodiments, a battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NXNMC811) has a discharge capacity retention rate of approximately 70% after 1000 cycles. In some embodiments, a battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a discharge capacity retention rate between 80% and 90% after 600 cycles.

[0310] Fig.31 A graph 3100 is shown illustrating the performance of a battery cell including electrodes according to various embodiments. Fig.31 A graph of storage time versus capacity is provided. For example, the battery cells are measured according to the SOC100 calendar life test at 50 degrees Celsius. Fig.31The battery cell measured in is a 1.5Ah soft pack battery cell, which includes a NX Si-C negative electrode (e.g., an electrode with a 3D nanocarbon matrix), a positive electrode according to various embodiments (e.g., a positive electrode with a 3D nanocarbon matrix). Fig.31 As shown, a battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a capacity retention rate of at least 95% after 21 days. In some embodiments, a battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a capacity retention rate of about at least 95% after 28 days. In some embodiments, a battery cell including a positive electrode comprising a 3D nanocarbon matrix (e.g., NX NMC811) has a capacity retention rate of about at least 96% after 28 days. In some embodiments, a battery cell including a positive electrode having a 3D nanocarbon matrix (e.g., NX NMC811) has a capacity retention rate of at least 1% better than a control 1.5Ah soft pack battery cell having a PVDF positive electrode after 28 days.

[0311] Fig.32 and Fig.33 The performance of a battery cell including electrodes according to various embodiments of the present application is shown. Fig.32 and 33 The battery cell that provides the performance is a soft-pack battery with dimensions of 46.5mm x 46.5mm x 7.14mm, and a positive electrode including a 3D nanocarbon matrix (e.g., NX NMC811). Fig.32 A graph 3200 is provided indicating battery capacity design, specific energy, and energy density. Fig.33 A graph 3300 of battery voltage versus capacity is provided.

[0312] Fig.34 Graph 3400 shows weight distribution of battery cells according to various embodiments. Fig.34 The battery cell in which the weight distribution was measured was a 3.4Ah soft pack battery, which included a positive electrode comprising a 3D nanocarbon matrix (e.g., NX NMC811).

[0313] Fig.35 and Fig.36 The performance of a battery cell including electrodes according to various embodiments of the present application is shown. The battery cell providing the performance is a pouch cell including dimensions of 62 mm x 107 mm and 5.4 mm, and a positive electrode including a 3D nanocarbon matrix (eg, NX NMC811). Fig.35 A graph 3500 is provided indicating battery capacity design, specific energy, and energy density. Fig.36A graph 3600 of capacity versus number of DST cycles is provided. According to various embodiments, the battery cell includes a specific energy greater than or equal to 315Wh / kg, an energy density greater than or equal to 820Wh / L, and a battery capacity of 9Ah. The battery cell according to various embodiments exhibits a DST cycle stability of at least about 70% at 1000 cycles, at least 92.5% at 225 cycles, and / or greater than 90 percent at 300 cycles.

[0314] Fig.37 and Fig.38 Graphs 3700 and 3800 show the performance of a battery cell including electrodes according to various embodiments of the present application. Fig.38 As shown, battery cells according to various embodiments (e.g., 9Ah soft pack batteries including a positive electrode including a 3D nanocarbon matrix) exhibit a volume expansion of less than 10% from 0% charge to 100% charge. In some embodiments, such battery cells exhibit a volume expansion of less than 9% from 0% charge to 100%. In some embodiments, such battery cells exhibit a volume expansion of about 8.8% from 0% charge to 100%.

[0315] In summary, an energy storage device includes a positive electrode and a negative electrode, wherein:

[0316] At least one of the negative electrode and the positive electrode includes an active layer, the active layer including a network of high aspect ratio carbon elements defining void spaces within the network; and a plurality of electrode active material particles disposed in the void spaces within the network; and the network of high aspect ratio carbon elements has a particle size of at least 0.1 / μm 2 , preferably at least 0.15 / μm 2 In an embodiment, the cross-density of the high aspect ratio carbon element network is less than 0.5 / μm 2 .

[0317] The network of high aspect ratio carbon elements includes a population of carbon nanotubes that form a percolating electrical pathway through the active layer.

[0318] At least a subset of the plurality of carbon nanotubes maintain electrical connectivity during charge and discharge cycles of the energy storage device. The high aspect ratio carbon element network includes a plurality of carbon nanotubes, and the plurality of carbon nanotubes has an average ratio of a length of a major dimension of the carbon nanotubes to a length of a minor dimension of the corresponding carbon nanotubes of at least 1,000.

[0319] The network of high aspect ratio carbon elements includes a population of carbon nanotubes, and the population of carbon nanotubes has an average ratio of the length of a major dimension of the carbon nanotubes to the length of a corresponding minor dimension of the carbon nanotubes of at least 1,500.

[0320] The network of high aspect ratio carbon elements includes a population of carbon nanotubes; and the population of carbon nanotubes has an average ratio of a length of a major dimension of the carbon nanotubes to a length of a minor dimension of the corresponding carbon nanotubes of at least 2,000.

[0321] The network of high aspect ratio carbon elements includes a population of carbon nanotubes; and the population of carbon nanotubes has an average ratio of the length of a major dimension of the carbon nanotubes to the length of a minor dimension of the corresponding carbon nanotubes of at least 10,000.

[0322] The network of high aspect ratio carbon elements includes a population of multi-walled carbon nanotubes. The population of multi-walled carbon nanotubes includes an average diameter between 6 nm and 10 nm; an average wall thickness between 6 nm and 7 nm; and an average length of about 16 microns.

[0323] In an embodiment, at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 8 microns, and at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 12 microns. In an embodiment, the multi-walled carbon nanotubes have a nominal length of at least 15 microns.

[0324] In an embodiment, the network of high aspect ratio carbon elements includes a plurality of multi-walled carbon nanotubes; and a distribution of lengths of the plurality of multi-walled carbon nanotubes is skewed toward a nominal length of the multi-walled carbon nanotubes.

[0325] In an embodiment, the storage device further comprises an electrolyte, wherein after wetting with the electrolyte, an average thickness of the positive electrode or the negative electrode increases by less than 10%.

[0326] In another embodiment, the network of high aspect ratio carbon elements includes a first group of carbon nanotubes and a second group of carbon nanotubes; and the second group of carbon nanotubes has one or more properties that are different from the first group of carbon nanotubes.

[0327] In one embodiment, the first plurality of carbon nanotubes includes multi-walled carbon nanotubes.

[0328] In another embodiment, the second plurality of carbon nanotubes includes single-walled carbon nanotubes.

[0329] In another embodiment, the first group of carbon nanotubes includes multi-walled carbon nanotubes; the second group of carbon nanotubes includes single-walled carbon nanotubes; and the ratio of the amount by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:1.

[0330] In an embodiment, the positive electrode includes an active layer, and the network of high aspect ratio carbon elements includes a group of multi-walled carbon nanotubes. In an embodiment, the active layer includes between 0.25% and 1.5% multi-walled carbon nanotubes by weight of the active layer. In an embodiment, the active layer includes between 0.2% and 2% multi-walled carbon nanotubes by weight of the active layer. In an embodiment, the first average aspect ratio of the first group of carbon nanotubes is greater than the second average aspect ratio of the second group of carbon nanotubes.

[0331] In an embodiment, the device comprises a positive electrode, wherein the positive electrode comprises an active layer, and the active layer further comprises a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative.

[0332] In an embodiment, the polymer additive is nylon. In an embodiment, the polymer additive is water soluble. In an embodiment, the polymer additive has a molecular weight greater than 1,000,000 g / mol. In an embodiment, the polymer additive has a molecular weight between 500,000 g / mol and 2,000,000 g / mol.

[0333] In an embodiment, the positive electrode comprises an active layer, and the active layer has an average thickness of 20 micrometers to 30 micrometers. In an embodiment, the positive electrode comprises an active layer, and the active layer has an average thickness of between 20 micrometers and 200 micrometers.

[0334] In an embodiment, the positive electrode includes an active layer, and the active material particles include lithium iron phosphate. In an embodiment, the positive electrode includes an active layer, and the active material particles include lithium metal oxide. In an embodiment, the positive electrode includes an active layer, and the active material particles include one or more of lithium metal oxide, lithium sulfur, and lithium cobalt oxide. In an embodiment, the positive electrode includes an active layer, and the active material particles include lithium nickel manganese cobalt oxide. In an embodiment, the positive electrode includes an active layer, and the active material particles include lithium nickel cobalt aluminum oxide. In an embodiment, the positive electrode includes an active layer, and the active material particles include lithium nickel cobalt manganese aluminum oxide.

[0335] In an embodiment, the positive electrode comprises an active layer, and wherein the active layer comprises at least 98.5% active material particles by weight of the active layer. In an embodiment, the positive electrode comprises an active layer, and the active layer comprises between 96.0% and 98.5% active material particles by weight of the active layer. In an embodiment, the storage device comprises a positive electrode, wherein the positive electrode comprises an active layer; wherein the active layer comprises a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative; and the active layer comprises approximately 0.5% of the polymer additive by weight of the active layer.

[0336] In an embodiment, a storage device includes a positive electrode, wherein the positive electrode includes an active layer; the active layer includes a polymer additive, which is (i) selected from the polyamide family or (ii) at least one of a modified polyamide or a polyamide derivative; and the active layer includes between 0.25% and 1.5% of the polymer additive by weight of the active layer.

[0337] In an embodiment, the positive electrode comprises an active layer and the network is at least 99% carbon by weight and comprises a network of electrically interconnected carbon elements exhibiting connectivity above a percolation threshold and wherein the network defines one or more highly conductive pathways having a length greater than 100 μm.

[0338] In yet another embodiment, the positive electrode comprises an active layer; the active layer comprises a polymer additive, the polymer additive being at least one of (i) selected from the polyamide family or (ii) modified polyamide or polyamide derivatives; and the polymer additive is a polymer binder.

[0339] In another embodiment, the positive electrode includes an active layer; the active layer includes a polymer additive, which is (i) selected from the polyamide family or (ii) at least one of a modified polyamide or a polyamide derivative; and the polymer additive is at least partially disposed in at least one void space defined by the high aspect ratio carbon element network.

[0340] In an embodiment, the positive electrode includes an active layer; and the active layer includes a polymer additive, the polymer additive being at least one of (i) selected from a polyamide family or (ii) a modified polyamide or a polyamide derivative.

[0341] In an embodiment, the polymeric additive has a tensile strength of less than 70 MPa measured when the polymeric additive is dry. In an embodiment, the polymeric additive has a tensile strength of less than 50 MPa measured when the polymeric additive is dry. In an embodiment, the polymeric additive has a tensile strength of less than 25 MPa measured when the polymeric additive is dry. In an embodiment, the polymeric additive has a tensile strength of less than 10 MPa measured when the polymeric additive is dry. In an embodiment, the polymeric additive has an elongation at yield of greater than 10% measured when the polymeric additive is dry. In an embodiment, the polymeric additive has an elongation at yield of greater than 20% measured when the polymeric additive is dry.

[0342] In an embodiment, the polymer additive is water soluble. In an embodiment, the polymer additive is soluble in alcohol. In an embodiment, the polymer additive is soluble in each of water and alcohol.

[0343] In an embodiment, an energy storage device includes a negative electrode, wherein the negative electrode includes an active layer; the active material particles include silicon; and the active layer includes a polymer additive, the polymer additive being at least one of a polyolefin, a poly(acrylic acid), and a styrene-butadiene rubber (SBR).

[0344] In an embodiment, the silicon contained in the electrode active material particles is in the form of SiO. In an embodiment, the silicon contained in the electrode active material is micro silicon.

[0345] In an embodiment, the silicon contained in the electrode active material is greater than fifty percent by weight of the active layer. In an embodiment, the silicon contained in the electrode active material is at least eighty percent by weight of the active layer.

[0346] In an embodiment, an energy storage device includes a network of high aspect ratio carbon elements including a carbon nanotube mesh; and the carbon nanotube mesh maintains electrical connections between at least a subset of carbon nanotubes included in the mesh during expansion of silicon.

[0347] In an embodiment, the energy storage device includes a network of high aspect ratio carbon elements. The high aspect ratio carbon elements include a carbon nanotube mesh; and the carbon nanotube mesh maintains electrical connections between at least a subset of the carbon nanotubes included in the mesh during charging and discharging of a battery including the electrode.

[0348] In an embodiment, an energy storage device includes a high aspect ratio carbon element network, which includes a first group of carbon nanotubes, wherein the first group of carbon nanotubes includes: a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; and a second group of carbon nanotubes, wherein the second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and the second group of carbon nanotubes has one or more properties different from those of the first group of carbon nanotubes.

[0349] In an embodiment, the first group of carbon nanotubes includes multi-walled nanotubes, the second group of carbon nanotubes includes single-walled nanotubes, and the ratio by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:1.

[0350] In an embodiment, the first group of carbon nanotubes and the second group of carbon nanotubes form a mesh that maintains electrical connections between the carbon nanotubes contained in the mesh during charging and discharging of a battery in which the electrodes are present.

[0351] In an embodiment, after wetting with the electrolyte, the average thickness of the multi-walled carbon nanotubes increases by less than 10%.In an embodiment, a first average aspect ratio of the first group of carbon nanotubes is greater than a second average aspect ratio of the second group of carbon nanotubes.

[0352] In an embodiment, the first plurality of carbon nanotubes has an average aspect ratio of at least 100 microns.

[0353] In an embodiment, a high aspect ratio carbon element network includes: a first group of carbon nanotubes, wherein the first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; a second group of carbon nanotubes, wherein the second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and the second group of carbon nanotubes has one or more properties different from those of the first group of carbon nanotubes; and graphite particles.

[0354] In an embodiment, the network of high aspect ratio carbon elements comprises about 5% graphite by weight of the active layer.

[0355] In an embodiment, an energy storage device includes a first group of carbon nanotubes including multi-walled carbon nanotubes; a second group of carbon nanotubes including single-walled carbon nanotubes; and a network of high aspect ratio carbon elements that is approximately 2% single-walled carbon nanotubes by weight.

[0356] In an embodiment, an energy storage device comprises: a first group of carbon nanotubes, the first group of carbon nanotubes comprising multi-walled carbon nanotubes; a second group of carbon nanotubes, the second group of carbon nanotubes comprising single-walled carbon nanotubes; wherein the high aspect ratio carbon element network is approximately 0.5% single-walled carbon nanotubes by weight of the active layer.

[0357] In an embodiment, the energy storage device includes a first group of carbon nanotubes, the first group of carbon nanotubes including multi-walled carbon nanotubes; the second group of carbon nanotubes including single-walled carbon nanotubes; the high aspect ratio carbon element network is less than or approximately equal to 2wt% of the single-walled carbon nanotubes by weight of the active layer, preferably less than or approximately equal to 3wt% of the single-walled carbon nanotubes by weight of the active layer, and more preferably less than or approximately equal to 4.5wt% of the single-walled carbon nanotubes by weight of the active layer.

[0358] In an embodiment, the network of high aspect ratio carbon elements is greater than about 3% and less than about 5% multi-walled carbon nanotubes by weight of the active layer.

[0359] In an embodiment, the energy storage device includes an active layer, which includes a first group of carbon nanotubes, the first group of carbon nanotubes includes multi-walled carbon nanotubes; the second group of carbon nanotubes includes single-walled carbon nanotubes; and the ratio of the amount by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is at least 9:1, preferably at least 5:1.

[0360] Various other components may be included and invoked to provide aspects of the teachings herein. For example, additional materials, combinations of materials, and / or omissions of materials may be used to provide additional embodiments within the scope of the teachings herein. A variety of modifications of the teachings herein may be implemented. In general, modifications may be designed based on the needs of a user, designer, manufacturer, or other similar interested party. Modifications may be intended to meet specific performance criteria that the aforementioned parties deem important.

[0361] Unless the phrase "means for" or "step for" is explicitly used in a particular claim, no appended claim or claim element should be construed as invoking 35 USC §112(f).

[0362] When introducing elements of the present invention or embodiments thereof, the articles "a," "an," and "the" are intended to indicate that there are one or more of the elements described. Similarly, the adjective "another" is intended to mean one or more elements when used to introduce an element. The terms "comprising" and "having" are intended to be inclusive so that there may be additional elements in addition to the listed elements. As used herein, the term "exemplary" is not intended to imply the best example. Rather, "exemplary" refers to an example of an embodiment of one embodiment among many possible embodiments.

[0363] The following examples are merely illustrative of various contents disclosed herein and are not intended to limit the scope thereof. Unless otherwise stated, all examples are based on simulations.

[0364] In general, the present invention may alternatively comprise, consist of, or consist essentially of any suitable components disclosed herein.

Claims

1. An energy storage device, comprising: positive electrode; as well as negative electrode, in: At least one of the negative electrode and the positive electrode includes an active layer, and the active layer includes: a network of high aspect ratio carbon elements defining void spaces within the network; and a plurality of electrode active material particles disposed in the void spaces within the network; and and The high aspect ratio carbon element network has a thickness of at least 0.1 / μm 2 The crossover density.

2. The electrode of claim 1, wherein the crossover density of the high aspect ratio carbon element network is at least 0.15 / μm 2 .

3. The electrode of claim 1, wherein the crossover density of the high aspect ratio carbon element network is at least 0.15 / μm 2 .

4. The electrode according to claim 1, wherein the cross-density of the high aspect ratio carbon element network is less than 0.5 / μm 2 . 5 . The energy storage device of claim 1 , wherein the network of high aspect ratio carbon elements comprises a group of carbon nanotubes, and the carbon nanotubes included in the group of carbon nanotubes correspond to electrical pathways.

6. The energy storage device of claim 5, wherein at least a subset of the plurality of carbon nanotubes maintain electrical connectivity during charge and discharge cycles of the energy storage device.

7. The energy storage device according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a group of carbon nanotubes; and The population of carbon nanotubes has an average ratio of the length of a major dimension of the carbon nanotubes to the length of a minor dimension of the corresponding carbon nanotubes of at least 1,000.

8. The energy storage device according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a group of carbon nanotubes; and The population of carbon nanotubes has an average ratio of the length of a major dimension of the carbon nanotubes to the length of a corresponding minor dimension of the carbon nanotubes of at least 1,500.

9. The energy storage device according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a group of carbon nanotubes; and The population of carbon nanotubes has an average ratio of the length of a major dimension of the carbon nanotubes to the length of a corresponding minor dimension of the carbon nanotubes of at least 2,000.

10. The energy storage device according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a group of carbon nanotubes; and The population of carbon nanotubes has an average ratio of the length of a major dimension of the carbon nanotubes to the length of a corresponding minor dimension of the carbon nanotubes of at least 10,000.

11. The energy storage device of claim 1, wherein the network of high aspect ratio carbon elements comprises a population of multi-walled carbon nanotubes.

12. The energy storage device of claim 11, wherein the plurality of multi-walled carbon nanotubes comprises: An average diameter between 6 nm and 10 nm; Average wall thickness between 6 nm and 7 nm; as well as Average length of about 16 microns.

13. The energy storage device of claim 11, wherein at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 8 microns.

14. The energy storage device of claim 11, wherein at least 50% of the plurality of multi-walled carbon nanotubes have a length greater than 12 microns.

15. The energy storage device of claim 11, wherein the multi-walled carbon nanotubes have a nominal length of at least 15 microns.

16. The energy storage device according to claim 1, wherein: The network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes; and The distribution of the lengths of the plurality of multi-walled carbon nanotubes is skewed toward the nominal length of the multi-walled carbon nanotubes.

17. The energy storage device of claim 1, further comprising an electrolyte, wherein after wetting with the electrolyte, the average thickness of the positive electrode or the negative electrode increases by less than 10%.

18. The energy storage device according to claim 1, wherein: The network of high aspect ratio carbon elements includes a first group of carbon nanotubes and a second group of carbon nanotubes; and The second group of carbon nanotubes has one or more properties that are different from those of the first group of carbon nanotubes.

19. The energy storage device of claim 18, wherein the first group of carbon nanotubes comprises multi-walled carbon nanotubes.

20. The energy storage device of claim 18, wherein the second group of carbon nanotubes comprises single-walled carbon nanotubes.

21. The energy storage device according to claim 18, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; and The ratio of the amount by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:

1.

22. The energy storage device of claim 18, wherein the positive electrode comprises the active layer and the network of high aspect ratio carbon elements comprises a population of multi-walled carbon nanotubes.

23. The energy storage device of claim 22, wherein the active layer comprises between 0.25% and 1.5% multi-walled carbon nanotubes by weight of the active layer.

24. The energy storage device of claim 22, wherein the active layer comprises between 0.2% and 2% multi-walled carbon nanotubes by weight of the active layer.

25. The energy storage device of claim 18, wherein a first average aspect ratio of the first group of carbon nanotubes is greater than a second average aspect ratio of the second group of carbon nanotubes.

26. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active layer further comprises: The polymer additive is (i) at least one selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative.

27. The energy storage device according to claim 26, wherein the polymer additive is: nylon.

28. The energy storage device of claim 26, wherein the polymer additive is water-soluble.

29. The energy storage device of claim 26, wherein the polymer additive has a molecular weight greater than 1,000,000 g / mol.

30. The energy storage device of claim 26, wherein the polymer additive has a molecular weight between 500,000 g / mol and 2,000,000 g / mol. 31 . The energy storage device of claim 1 , wherein the positive electrode comprises the active layer, and the active layer has an average thickness of 20 μm to 30 μm.

32. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active layer has an average thickness between 20 microns and 200 microns.

33. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active material particles comprise lithium iron phosphate.

34. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active material particles comprise lithium metal oxide.

35. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active material particles comprise one or more of lithium metal oxide, lithium sulfur, and lithium cobalt oxide.

36. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active material particles comprise lithium nickel manganese cobalt oxide.

37. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active material particles comprise lithium nickel cobalt aluminum oxide.

38. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active material particles comprise lithium nickel cobalt manganese aluminum oxide.

39. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and wherein the active layer comprises at least 98.5% of the active material particles by weight of the active layer.

40. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the active layer comprises between 96.0% and 98.5% of the active material particles by weight of the active layer.

41. The energy storage device of claim 1, wherein: The positive electrode includes the active layer; The active layer includes a polymer additive, wherein the polymer additive is at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative; and The active layer includes about 0.5% of the polymer additive, based on the weight of the active layer.

42. The energy storage device of claim 1, wherein: The positive electrode includes the active layer; The active layer includes a polymer additive, wherein the polymer additive is at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative; and The active layer includes between 0.25% and 1.5% of the polymer additive by weight of the active layer.

43. The energy storage device of claim 1, wherein the positive electrode comprises the active layer, and the network is at least 99% carbon by weight and comprises a network of electrically interconnected carbon elements that exhibits connectivity above a percolation threshold, and wherein the network defines one or more highly conductive pathways having a length greater than 100 μm; 44. The energy storage device of claim 1, wherein: The positive electrode includes the active layer; The active layer includes a polymer additive, wherein the polymer additive is at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative; and The polymer additive is a polymer binder.

45. The energy storage device of claim 1, wherein: The positive electrode includes the active layer; The active layer includes a polymer additive, wherein the polymer additive is at least one of (i) selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative; and The polymer additive is at least partially disposed in at least one void space defined by the network of high aspect ratio carbon elements.

46. ​​The energy storage device of claim 1, wherein: The positive electrode includes the active layer; and The active layer includes a polymer additive, wherein the polymer additive is at least one of (i) selected from the polyamide family or (ii) modified polyamide or polyamide derivatives.

47. The energy storage device of claim 46, wherein: The polymer additive has a tensile strength of less than 70 MPa measured when the polymer additive is dry.

48. The energy storage device of claim 46, wherein the polymer additive has a tensile strength of less than 50 MPa measured when the polymer additive is dry.

49. The energy storage device of claim 46, wherein the polymer additive has a tensile strength of less than 25 MPa measured when the polymer additive is dry.

50. The energy storage device of claim 46, wherein the polymer additive has a tensile strength of less than 10 MPa measured when the polymer additive is dry.

51. The energy storage device of claim 46, wherein the polymer additive has an elongation at yield greater than 10% measured when the polymer additive is dry.

52. The energy storage device of claim 46, wherein the polymer additive has an elongation at yield greater than 20% measured when the polymer additive is dry.

53. The energy storage device of claim 46, wherein the polymer additive is water soluble.

54. The energy storage device of claim 46, wherein the polymer additive is soluble in alcohol.

55. The energy storage device of claim 46, wherein the polymer additive is soluble in each of water and alcohols.

56. The energy storage device of claim 1, wherein: The negative electrode includes the active layer; The active material particles include silicon; and The active layer includes a polymer additive, wherein the polymer additive is at least one of polyolefin, poly(acrylic acid), and styrene-butadiene rubber (SBR).

57. The energy storage device of claim 56, wherein the silicon included in the electrode active material particles is in the form of SiO.

58. The energy storage device according to claim 56, wherein the silicon included in the electrode active material is micro silicon.

59. The energy storage device of claim 56, wherein the silicon included in the electrode active material is greater than fifty percent by weight of the active layer.

60. The energy storage device of claim 56, wherein the silicon included in the electrode active material is at least eighty percent by weight of the active layer.

61. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements comprises a carbon nanotube mesh; and The carbon nanotube mesh maintains electrical connections between at least a subset of the carbon nanotubes included in the mesh during expansion of the silicon.

62. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements comprises a carbon nanotube mesh; and The carbon nanotube grid maintains electrical connections between at least a subset of the carbon nanotubes included in the grid during charging and discharging of a battery including the electrode.

63. The energy storage device of claim 56, wherein the network of high aspect ratio carbon elements comprises: a first group of carbon nanotubes, wherein the first group of carbon nanotubes comprises a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; as well as A second group of carbon nanotubes, wherein: The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and The second group of carbon nanotubes has one or more properties that are different from those of the first group of carbon nanotubes.

64. The energy storage device of claim 63, wherein the first group of carbon nanotubes comprises multi-walled nanotubes.

65. The energy storage device of claim 63, wherein the second plurality of carbon nanotubes comprises single-walled nanotubes.

66. The energy storage device of claim 63, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; and The ratio of the amount by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is about 2:

1.

67. The energy storage device of claim 63, wherein the first group of carbon nanotubes and the second group of carbon nanotubes form a grid that maintains electrical connections between carbon nanotubes included in the grid during charging and discharging of a battery including the electrode.

68. The energy storage device of claim 63, wherein the average thickness of the multi-walled carbon nanotubes increases by less than 10% after wetting with electrolyte.

69. The energy storage device of claim 63, wherein a first average aspect ratio of the first group of carbon nanotubes is greater than a second average aspect ratio of the second group of carbon nanotubes.

70. The energy storage device of claim 63, wherein the first plurality of carbon nanotubes have an average aspect ratio of at least 100 microns.

71. The energy storage device of claim 56, wherein the network of high aspect ratio carbon elements comprises: a first group of carbon nanotubes, wherein the first group of carbon nanotubes comprises a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; A second group of carbon nanotubes, wherein: The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and The second group of carbon nanotubes has one or more properties that are different from the first group of carbon nanotubes; and Graphite particles.

72. The energy storage device of claim 71, wherein the network of high aspect ratio carbon elements comprises approximately 5% graphite by weight of the active layer.

73. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The network of high aspect ratio carbon elements is approximately 2% by weight single wall carbon nanotubes.

74. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The network of high aspect ratio carbon elements is about 0.5% single wall carbon nanotubes by weight of the active layer.

75. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The network of high aspect ratio carbon elements is less than or about equal to 2% single wall carbon nanotubes by weight of the active layer.

76. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The network of high aspect ratio carbon elements is approximately 3% multi-walled carbon nanotubes by weight of the active layer.

77. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The network of high aspect ratio carbon elements is approximately 4.5% multi-walled carbon nanotubes by weight of the active layer.

78. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The network of high aspect ratio carbon elements is greater than about 3% and less than about 5% multi-walled carbon nanotubes by weight of the active layer.

79. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The ratio of the amount by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is at least 9:

1.

80. The energy storage device of claim 71, wherein: The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; The ratio of the amount by weight of the first group of carbon nanotubes to the second group of carbon nanotubes is at least 5:

1.

81. The energy storage device of claim 71, wherein the multi-walled carbon nanotubes comprise: An average diameter between 6 nm and 10 nm; Average wall thickness between 6 nm and 7 nm; as well as Average length of about 16 microns.

82. The energy storage device of claim 71, wherein the single-walled carbon nanotubes comprise: An average diameter between 1 nm and 2 nm; Average length of about 5 microns.

83. The energy storage device of claim 71, wherein the single-walled carbon nanotubes comprise: An average diameter between 3 nm and 5 nm; as well as An average length of at least 200 microns.

84. The energy storage device of claim 71, wherein the single-walled carbon nanotubes comprise: An average diameter between 3 nm and 5 nm; as well as Average length between 7 and 8 microns.

85. The energy storage device of claim 71, wherein the single-walled carbon nanotubes comprise 1 or 2 walls on average.

86. The energy storage device of claim 71, wherein the single-walled carbon nanotubes comprise: An average diameter between 5 nm and 6 nm; Average length between 7 and 8 microns.

87. The energy storage device of claim 71, wherein the single-walled carbon nanotubes comprise: Length range between 1 nm and 34 nm; Average length between 7 and 8 microns.

88. The energy storage device of claim 71, wherein the average thickness of the active layer increases by less than 10% after wetting with electrolyte.

89. The energy storage device of claim 88, wherein upon wetting with electrolyte, one or more portions of the active layer swell to cause the thickness of the active layer to increase.

90. The energy storage device of claim 71, wherein the average thickness of the active layer increases by less than 15% after wetting with electrolyte.

91. The energy storage device of claim 71, wherein the average thickness of the active layer increases by less than 5% after wetting with electrolyte.

92. The energy storage device of claim 71, wherein a first average aspect ratio of the first group of carbon nanotubes is greater than a second average aspect ratio of the second group of carbon nanotubes.

93. The energy storage device of claim 71, wherein the first plurality of carbon nanotubes have an average aspect ratio of at least 100.

94. The energy storage device of claim 71, wherein the first group of carbon nanotubes has an average aspect ratio between 200 and 1000.

95. The electrode of claim 1, wherein: The network of high aspect ratio carbon elements includes a set of multi-walled carbon nanotubes, the set of multi-walled carbon nanotubes including a plurality of multi-walled carbon nanotubes; The plurality of multi-walled carbon nanotubes have an average length greater than 5 microns.

96. The electrode of claim 1, wherein: The network of high aspect ratio carbon elements includes a set of multi-walled carbon nanotubes, the set of multi-walled carbon nanotubes including a plurality of multi-walled carbon nanotubes; The plurality of multi-walled carbon nanotubes have an average length greater than 10 microns.

97. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements includes a set of carbon nanostructures.

98. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes, the set of multi-walled carbon nanotubes comprising a plurality of multi-walled carbon nanotubes; and The plurality of multi-walled carbon nanotubes have at least 6 walls.

99. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes, the set of multi-walled carbon nanotubes comprising a plurality of multi-walled carbon nanotubes; and The plurality of multi-walled carbon nanotubes have at least 7 walls.

100. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements comprises a set of multi-walled carbon nanotubes, the set of multi-walled carbon nanotubes comprising a plurality of multi-walled carbon nanotubes; and The plurality of multi-walled carbon nanotubes have 6 or 7 walls.

101. The energy storage device of claim 56, wherein the network of high aspect ratio carbon elements comprises at least one material selected from the group consisting of: carbon nanostructures, fragments of carbon nanostructures, and broken multi-walled carbon nanotubes.

102. The energy storage device of claim 56, wherein: The high aspect ratio carbon element network includes a plurality of carbon nanotubes; and The distribution of the lengths of the plurality of carbon nanotubes is skewed toward the nominal length of the carbon nanotubes.

103. The energy storage device of claim 102, wherein the nominal length of the carbon nanotubes is at least 15 microns.

104. The energy storage device of claim 56, wherein: The network of high aspect ratio carbon elements comprises a plurality of multi-walled carbon nanotubes; and The distribution of the lengths of the plurality of multi-walled carbon nanotubes is skewed toward the nominal length of the multi-walled carbon nanotubes.

105. The energy storage device of claim 104, wherein the nominal length of the multi-walled carbon nanotubes is at least 15 microns.

106. The energy storage device of claim 56, further comprising: Electrolytes; in: The network of high aspect ratio carbon elements further comprises: graphite; The first group of carbon nanotubes includes multi-walled carbon nanotubes; The second group of carbon nanotubes includes single-walled carbon nanotubes; and When wetted with the electrolyte, the multi-walled nanotubes included in the first group of carbon nanotubes swell less than the single-walled carbon nanotubes included in the second group of carbon nanotubes.

107. The energy storage device of claim 56, wherein: The high aspect ratio carbon element network comprises: A first group of carbon nanotubes, wherein: The first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; The multi-walled carbon nanotubes include: An average diameter between 6 nm and 10 nm; An average wall thickness between 6 nm and 7 nm; and An average length of approximately 16 microns; and A second group of carbon nanotubes, wherein: The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and The second group of carbon nanotubes has one or more properties that are different from those of the first group of carbon nanotubes.

108. The energy storage device of claim 56, wherein: The high aspect ratio carbon element network comprises: A first group of carbon nanotubes, wherein: The first group of carbon nanotubes includes a plurality of first carbon nanotubes or a plurality of first carbon nanotube bundles; and A second group of carbon nanotubes, wherein: The second group of carbon nanotubes includes a plurality of second carbon nanotubes or a plurality of second carbon nanotube bundles; and The second group of carbon nanotubes has one or more properties that are different from the first group of carbon nanotubes; and The single-walled carbon nanotubes include: Average diameters of 1 nm and 6 nm; Average length of about 5 microns.

109. The energy storage device of claim 56, wherein the active layer comprises at least 98.5% by weight of the active material particles.

110. The energy storage device of claim 56, wherein the active layer comprises between 96.0% and 98.5% by weight of the active material particles.

111. The energy storage device of claim 56, wherein the network is at least 99% carbon by weight and comprises a network of electrically interconnected carbon elements that exhibits connectivity above a percolation threshold, and wherein the network defines one or more highly conductive pathways having a length greater than 100 μm; 112. The energy storage device of claim 56, further comprising: foil; in: The active layer is disposed on the foil; and The thickness of the foil is equal to or less than 8 micrometers.

113. The energy storage device of claim 112, wherein the foil is copper.

114. The energy storage device of claim 112, wherein the thickness of the foil is equal to or less than 6 microns.

115. The energy storage device of claim 56, wherein the active layer comprises at least 50% by weight of the active material particles.

116. The energy storage device of claim 56, wherein the active layer comprises between 50% and 98.5% by weight of the active material particles.

117. The energy storage device of claim 56, wherein the active layer comprises at least 5% by weight of the polymer additive.

118. The energy storage device of claim 56, wherein the active layer comprises between 8% by weight of the polymer additive.

119. The energy storage device of claim 56, wherein the active layer comprises less than 12% by weight of the polymer additive.

120. The energy storage device of claim 56, wherein the network is at least 99% carbon by weight and comprises a network of electrically interconnected carbon elements exhibiting connectivity above a percolation threshold, and wherein the network defines one or more highly conductive pathways having a length greater than 100 μm.

121. The electrode of claim 1, wherein the polymer additive is from the family of at least one of polyolefins, poly(acrylic acid), and SBR.

122. An energy storage device, comprising: A positive electrode comprising: An active layer comprising: a network of high aspect ratio carbon elements defining void spaces within said network; a plurality of electrode active material particles disposed in the void spaces within the network; and A polymer additive, wherein the polymer additive is (i) at least one selected from the polyamide family or (ii) a modified polyamide or a polyamide derivative; and A negative electrode comprising: An active layer comprising: a network of high aspect ratio carbon elements defining void spaces within said network; a plurality of electrode active material particles disposed in the void spaces within the network, wherein the active material particles include silicon; and The polymer additive is at least one of polyolefin, poly(acrylic acid) and styrene-butadiene rubber (SBR).

123. An electric vehicle comprising an energy storage device, wherein the energy storage device comprises: Negative and positive electrodes, where: At least one of the negative electrode and the positive electrode includes an active layer, and the active layer includes: a network of high aspect ratio carbon elements defining void spaces within the network; and a plurality of electrode active material particles disposed in the void spaces within the network; and The high aspect ratio carbon element network has a thickness of at least 0.1 / μm 2 The crossover density.

124. An electric vehicle according to claim 123, wherein the electric vehicle corresponds to at least one of a car, a scooter, a motorcycle, a boat, an airplane, and a sports and leisure vehicle.