Current collector, pole piece, preparation method of pole piece, electrode assembly and secondary battery
Patent Information
- Application Number
- CN202280089525.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-10-28
AI Technical Summary
The bending part of the electrode assembly in the secondary battery is prone to the risk of lithium precipitation, which affects the service life.
Design a current collector. The current collector body has several corner areas spaced apart along the first direction. At least one corner area is provided with perforations along the thickness direction to form perforation features so that lithium ions can flow on both sides of the pole piece and reduce the risk of lithium precipitation.
Through perforation, the lithium ion concentration on both sides of the pole piece is balanced, reducing the risk of lithium precipitation at the bending part and extending the service life of the secondary battery.
Smart Images

Figure CN119096380A_ABST
Abstract
Description
Current collector, pole piece and preparation method thereof, electrode assembly and secondary battery Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a current collector, a pole piece and a preparation method thereof, an electrode assembly and a secondary battery. Background Art
[0002] The electrode assembly is the component in a secondary battery where the electrochemical reaction occurs. It is primarily composed of a positive electrode sheet and a negative electrode sheet wound or stacked, typically with a separator between them. When wound, the electrode assembly can form a straight portion and two curved portions on either side of the straight portion.
[0003] Within the folding zone, the negative and positive electrodes are stacked alternately. However, due to structural design flaws in the electrode assembly, lithium deposition is easily generated between the negative and positive electrodes during cycling, seriously impacting the battery's lifespan.
[0004] Summary of the Invention
[0005] Based on this, it is necessary to provide a current collector, an electrode sheet and a preparation method thereof, an electrode assembly and a secondary battery to reduce the risk of lithium plating and increase the service life of the secondary battery.
[0006] In the first aspect, the present application provides a current collector for winding in a first direction, the current collector comprising: a current collector body having a plurality of corner regions spaced apart along the first direction, the corner regions being used to be opposite to the bending portion of the electrode assembly; wherein, at least one corner region is provided with a perforation extending through the thickness direction of the current collector.
[0007] The above-mentioned current collector has a perforation extending through the current collector body in at least one corner region. Thus, an electrode assembly formed by winding pole pieces with this current collector will have perforations within at least one pole piece layer in the bend. During cyclic charging, lithium ions on the convex and concave sides of the pole piece can communicate through the perforations, ensuring a balanced lithium concentration on both sides of the pole piece. This reduces the risk of lithium plating between the negative and positive pole pieces in the bend, thereby extending the service life of the secondary battery.
[0008] In some embodiments, multiple perforations are provided in the corner region, and all of the perforations are spaced apart within the corner region. Thus, providing multiple perforations in the corner region at intervals can help accelerate the rate of lithium ion concentration transfer between the two sides of the electrode, promoting dynamic equilibrium of lithium ion concentration between the two sides of the electrode.
[0009] In some embodiments, within a corner region having perforations, the perforations are spaced apart in rows along the second direction. The sum of the opening areas of any row of perforations is denoted as S0. The sum of the opening areas of each row, S0, decreases as it approaches either end of the corner region along the second direction, with the first direction being perpendicular to the second direction. This helps reduce the number of openings near one end of the corner region, avoids stress concentration caused by excessive openings, and effectively reduces the risk of electrode fracture during the cold pressing process.
[0010] In some embodiments, within a corner region having perforations, the number of perforations in each row of perforations gradually decreases from the middle of the corner region to either end of the corner region along the second direction. This design reduces the number of perforations closer to the corner region, ensuring structural strength at the edges of the current collector and preventing breakage during the cold pressing process.
[0011] In some embodiments, the current collector body includes a coating region for applying the active material layer. The coating region extends along a first direction and sequentially passes through each corner region. The perforations within the corner regions are all located within the coating region in a second direction, with the first and second directions being perpendicular. This confines the perforations to the coating region, enabling efficient lithium ion flow between the two sides of the electrode sheet while also avoiding the possibility of weakening the electrode's structural strength by placing the perforations in the tabs.
[0012] In some embodiments, at least one stress zone is provided within the coating region, extending along an edge of the coating region in the second direction. The perforations within the corner region are all located in the second direction within the coating region, excluding the stress zone. This ensures mechanical strength on at least one side of the current collector, preventing breakage or tearing during processing and improving production efficiency by leaving the stress zone near one edge of the coating region.
[0013] In some embodiments, the width of each stress zone in the second direction is denoted as D, where D ≥ 3 mm. Thus, a minimum threshold for the width of the stress zone is appropriately limited so that a region at an edge of the coating zone along the second direction is free of openings, thereby ensuring mechanical strength on at least one side of the current collector.
[0014] In some embodiments, two stress zones are spaced apart along the second direction within the coating region, with the two stress zones corresponding to opposite edges of the coating region along the second direction. Thus, stress zones are left near opposite edges of the coating region without perforations, ensuring mechanical strength on both sides of the current collector, preventing breakage or tearing during processing, and improving production efficiency.
[0015] In some embodiments, the current collector body further includes a blank area located on at least one side of the coating area along the second direction. Thus, a blank area is reserved on at least one side of the current collector body to facilitate the fabrication of the tab portion required for the electrode assembly, thereby improving fabrication efficiency.
[0016] In some embodiments, the total area of all perforations within a corner region is denoted as S1, and the area of the corner region on the current collector is denoted as S2, where 0.1% ≤ S1 / S2 ≤ 50%. Thus, properly controlling the S1 / S2 ratio ensures smooth lithium ion flow between the two sides of the electrode while maintaining a certain structural strength of the current collector, thereby avoiding the risk of belt breakage.
[0017] In some embodiments, perforations are provided in the first n corner regions starting from the winding start of the current collector body, where n ≤ 6. By providing perforations in the first n corner regions, lithium deposition is targeted at locations in the electrode assembly where lithium deposition is most likely to occur. This reduces the number of perforations required and improves the mechanical strength of the current collector while minimizing the risk of lithium deposition.
[0018] In a second aspect, the present application provides a pole piece, comprising: a current collector as described in any one of the above items; and an active material layer provided on at least one surface of the current collector body.
[0019] On the third aspect, the present application provides a method for preparing a pole piece, which is used to prepare the above pole piece, including the following steps: providing a current collecting body; drilling holes in the corner area of the current collecting body to form a current collector; coating an active material layer on the surface of the current collector; and rolling the coated current collector.
[0020] In some embodiments, the step of rolling the coated current collector includes: pressing the tension roller surface of the pressure roller and the extension roller surfaces located on both sides of the tension roller surface respectively against the active material layer and the blank areas on both sides of the active material layer on the current collector, and controlling the side of the extension roller surface facing the tension roller surface to leave a gap between the area where the perforations are located. In this way, when cold-pressing the active material, a gap is maintained between the side of the extension roller surface and the area where the perforations are located, avoiding the perforations being too close to the extension roller surface, which would cause stress concentration, thereby preventing the electrode sheet from breaking during rolling.
[0021] In a fourth aspect, the present application provides an electrode assembly constructed as a winding structure, comprising a positive electrode sheet, a negative electrode sheet and a separator arranged between the positive electrode sheet and the negative electrode sheet, and the winding structure includes a bending portion; wherein the positive electrode sheet and / or the negative electrode sheet are the above electrode sheets, and the position of the bending portion is opposite to the corner area after winding.
[0022] In a fifth aspect, the present application provides a secondary battery comprising the above electrode assembly.
[0023] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0025] FIG1 is a schematic diagram of the exploded structure of a secondary battery provided in some embodiments of the present application;
[0026] FIG2 is a schematic diagram of the structure of an electrode assembly provided in some embodiments of the present application;
[0027] FIG3 is a schematic diagram of a current collector structure provided in some embodiments of the present application;
[0028] FIG4 is a schematic diagram of a first flow chart of a method for preparing a pole piece according to some embodiments of the present application;
[0029] FIG5 is a second flow chart of a method for preparing a pole piece according to some embodiments of the present application;
[0030] FIG6 is a schematic diagram of the pressure roller structure provided in some embodiments of the present application.
[0031] 100. Secondary battery; 10. Electrode assembly; 20. End cap; 30. Electrode terminal; 40. Housing; 1. Pole piece; 1a. Current collector; 11. Current collector body; 12. Perforation; 13. Corner area; 14. Coating area; 15. Stress area; 16. Blank area; 17. Opening area; 18. Straight area; 2. Positive electrode piece; 3. Negative electrode piece; 4. Separator; 5. Straight portion; 6. Bend portion; 200. Pressure roller; 210. Extension roller surface; 220. Tension roller surface; X, first direction; Y, second direction. DETAILED DESCRIPTION
[0032] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0034] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0035] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0036] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0037] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0038] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.
[0039] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; internal connections between two components or interactions between two components. Those skilled in the art can understand the specific meanings of the above terms in the embodiments of the present application based on specific circumstances.
[0040] Currently, market developments indicate that power batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As power battery applications continue to expand, market demand is also growing.
[0041] The applicant has noted that when the electrode assembly is constructed into a wound structure, it includes a straight portion and bent portions provided on both sides of the straight portion. In the bent portion, there are alternating layers of positive and negative electrode sheets with different curvature radii, and both the positive and negative electrode sheets will form concave and convex surfaces when bent. Taking one layer of the negative electrode sheet as an example (of course, one layer of the positive electrode sheet can also be used as an example for explanation), its concave side and convex side correspond to the inner and outer layers of the positive electrode sheets, respectively, that is, the concave side of the negative electrode sheet is opposite to the convex side of the inner positive electrode sheet, and its convex side is opposite to the concave side of the outer positive electrode sheet.
[0042] Since the radius of curvature of the concave surface of the negative electrode sheet is greater than the radius of curvature of the convex surface of the inner positive electrode sheet, the active material capacity of the concave surface of the negative electrode sheet will be greater than the active material capacity of the convex surface of the positive electrode sheet, and the corresponding NP value of the two is greater than 1, which can also be simply understood as the lithium insertion vacancy concentration is greater than the lithium insertion ion concentration, and there are surplus lithium insertion vacancies. Conversely, since the radius of curvature of the concave surface of the negative electrode sheet is smaller than the radius of curvature of the convex surface of the outer positive electrode sheet, the active material capacity of the concave surface of the negative electrode sheet will be less than the active material capacity of the convex surface of the positive electrode sheet, and the corresponding NP value of the two is less than 1, which can also be simply understood as the lithium insertion vacancy concentration cannot meet the lithium insertion ion insertion, and the risk of lithium plating is prone to occur during charging.
[0043] Based on this, in order to solve the problem that lithium deposition is easily generated between the positive electrode sheet and the negative electrode sheet at the bending part of the electrode assembly, thereby affecting the service life of the secondary battery, the applicant has conducted in-depth research and designed a current collector with perforations penetrating along the thickness direction of the current collector in at least one corner area so that lithium ions on both sides of the current collector can flow to each other.
[0044] The above-mentioned current collector is provided with a perforation penetrating the current collector body in at least one corner area. In this way, the electrode prepared using the current collector, such as a positive electrode or a negative electrode, will allow lithium ions on both sides of the electrode to pass through the perforation, ensuring that the lithium ion concentration on both sides of the electrode is balanced, for example: the side with a high lithium ion concentration flows through the perforation to the side with a low lithium ion concentration, etc.
[0045] After the electrode sheets prepared using this current collector are wound to form an electrode assembly, the electrode assembly will have perforations inside at least one layer of the electrode sheet in the bend. At this time, during the cyclic charging process, the lithium ions on the convex and concave sides of the electrode sheet will communicate with each other through the perforations, ensuring that the lithium insertion concentration on both sides of the electrode sheet is balanced. For example, the lithium ions on the convex side of the negative electrode sheet will flow through the perforations to the lithium ions on the concave side of the negative electrode sheet, reducing the lithium insertion concentration on the convex side, ensuring that the local NP is greater than or equal to 1, reducing the risk of lithium plating between the negative and positive electrode sheets in the bend, and improving the service life of the secondary battery.
[0046] The secondary battery disclosed in the embodiments of the present application can be used, but is not limited to, in electrical devices such as vehicles, ships, or aircraft. A power supply system comprising the secondary battery disclosed in the present application can be used to form the electrical device.
[0047] In a battery system, there can be multiple secondary batteries, and the multiple secondary batteries can be connected in series, in parallel, or in a mixed connection. Mixed connection means that multiple secondary batteries are connected in series and in parallel. Multiple secondary batteries can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple secondary batteries is accommodated in a box; of course, the battery can also be a battery module formed by first connecting multiple secondary batteries in series, in parallel, or in a mixed connection, and then the multiple battery modules are connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in a box. The battery can also include other structures. For example, the battery can also include a busbar component for realizing electrical connection between multiple secondary batteries. Among them, the secondary battery can be cylindrical, flat, rectangular, or other shapes.
[0048] Please refer to Figure 1, which is a schematic diagram of the exploded structure of a secondary battery 100 provided in some embodiments of the present application. Secondary battery 100 is the smallest unit of a battery. As shown in Figure 1, secondary battery 100 includes an end cap 20, a housing 40, an electrode assembly 10, and other functional components.
[0049] The end cap 20 is a component that covers the opening of the housing 40 to isolate the internal environment of the secondary battery 100 from the external environment. Without limitation, the shape of the end cap 20 can be adapted to the shape of the housing 40 to match the housing 40. Optionally, the end cap 20 can be made of a material with a certain hardness and strength (such as an aluminum alloy). This makes the end cap 20 less likely to deform when subjected to compression or collision, giving the secondary battery 100 greater structural strength and improved safety. Functional components such as electrode terminals 30 can be provided on the end cap 20. The electrode terminals 30 can be used to electrically connect to the electrode assembly 10 for outputting or inputting electrical energy into or out of the secondary battery 100. In some embodiments, the end cap 20 can also be provided with a pressure relief mechanism for relieving internal pressure when the internal pressure or temperature of the secondary battery 100 reaches a threshold. The end cap 20 can also be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application are not particularly limited in this regard. In some embodiments, an insulating member may be provided inside the end cap 20 to isolate the electrical connection components in the housing 40 from the end cap 20 to reduce the risk of short circuit.
[0050] The housing 40 is a component that cooperates with the end cap 20 to form the internal environment of the secondary battery 100, wherein the formed internal environment can be used to accommodate the electrode assembly 10, electrolyte, and other components. The housing 40 and the end cap 20 can be independent components. An opening can be provided in the housing 40, and the internal environment of the secondary battery 100 is formed by closing the end cap 20 at the opening. Without limitation, the end cap 20 and the housing 40 can also be integrated. Specifically, the end cap 20 and the housing 40 can form a common connection surface before other components are inserted into the housing. When the interior of the housing 40 needs to be enclosed, the end cap 20 is closed to the housing 40. The housing 40 can be of various shapes and sizes, such as a rectangular parallelepiped, a cylindrical shape, a hexagonal prism, etc. Specifically, the shape of the housing 40 can be determined according to the specific shape and size of the electrode assembly 10. The housing 40 can be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, plastic, etc., and the embodiments of the present application do not impose any particular limitations on this.
[0051] Please refer to Figure 2. The electrode assembly 10 is a component in the secondary battery 100 where electrochemical reactions occur. One or more electrode assemblies 10 may be contained in the shell 40. The electrode assembly 10 is mainly formed by winding or stacking a positive electrode sheet 2 and a negative electrode sheet 3, and a separator 4 is usually provided between the positive electrode sheet 2 and the negative electrode sheet 3. The parts of the positive electrode sheet 2 and the negative electrode sheet 3 with active materials constitute the main body of the electrode assembly 10, and the parts of the positive electrode sheet 2 and the negative electrode sheet 3 without active materials each constitute a tab. The positive electrode tab and the negative electrode tab may be located together at one end of the main body or respectively at both ends of the main body. During the charge and discharge process of the battery, the positive electrode active material and the negative electrode active material react with the electrolyte, and the tabs are connected to the electrode terminals 30 to form a current loop.
[0052] According to some embodiments of the present application, referring to FIG. 2 and FIG. 3 , a current collector 1a is provided for winding in a first direction X. The current collector 1a includes a current collector body 11. The current collector body 11 has a plurality of corner regions 13 spaced apart along the first direction X. The corner regions 13 are configured to oppose the bend 6 of the electrode assembly 10. A perforation 12 is defined within at least one corner region 13 along the thickness of the current collector 1a.
[0053] The current collector body 11 refers to the core structure of the main components of the current collector 1a. Of course, it can also be understood as the components on the current collector 1a except for features such as the perforation 12. The current collector body 11 can not only carry active substances, but also collect and output the current generated by the electrode active substances. The material of the current collector body 11 can be selected differently according to the polarity of the electrode 1. For example: in the positive electrode 2, the material of the current collector body 11 can be but not limited to metal materials such as aluminum and nickel, and can also be composite materials such as conductive resin, titanium-nickel shape memory alloy, and carbon-coated aluminum foil. In the positive electrode 2, the material of the current collector body 11 can be but not limited to metal materials such as copper, and of course it can also be composite materials such as conductive resin, titanium-nickel shape memory alloy, and so on.
[0054] The corner regions 13 refer to the bends formed in several sections of the current collecting body 11 when the current collecting body 11 is wound along the first direction X during the preparation of the electrode assembly 10. The areas corresponding to these bends in the current collecting body 11 are the corner regions 13. Meanwhile, referring to FIG2 , the wound electrode assembly 10 forms a bent portion 6, which includes the current collecting bodies 11 with multiple stacked corner regions 13. That is, the corner regions 13 are used to correspond to the bent portion 6 of the electrode assembly 10. This can be understood as follows: the wound corner regions 13 are located at the same location as or overlap with the bent portion 6 of the electrode assembly 10.
[0055] Several corner regions 13 are arranged at intervals along the first direction X on the current collecting body 11. A straight region 18 is left between two adjacent corner regions 13, opposite the straight portion 5 of the electrode assembly 10. Furthermore, after winding, the two adjacent corner regions 13 are located on different bends 6 of the electrode assembly 10. For ease of understanding, the two bends 6 of the electrode assembly 10 can be defined as a left bend 6 and a right bend 6, respectively. During winding, the first corner region 13 is wound around the left bend 6, and the second corner region 13 is wound around the right bend 6; then, the third corner region 13 is wound around the left bend 6, and the fourth corner region 13 is wound around the right bend 6, and so on. Following this logic, the remaining corner regions 13 are wound around different bends 6.
[0056] Among all the corner areas 13 on the current collecting body 11 , only some of the corner areas 13 may be provided with the through holes 12 , or all of the corner areas 13 may be provided with the through holes 12 .
[0057] The perforations 12 must be provided in the corner region 13 along the thickness direction of the current collector 1a to ensure that the electrode 1 has a channel for lithium ions to pass through. The number and shape of the perforations 12 can be designed in a variety of ways. For example, the number of perforations 12 in the corner region 13 can be one or more, and the shape of the perforations 12 in the corner region 13 can be regular shapes such as, but not limited to, circular, triangular, square, pentagonal, and elliptical. Of course, irregular shapes are also possible.
[0058] A perforation 12 is provided in at least one corner region 13, extending through the current collector body 11. Thus, the electrode assembly 10 formed by winding the electrode sheet 1 with the current collector 1a will have a perforation 12 feature within at least one electrode sheet 1 layer in the bend 6. During the charging cycle, lithium ions on the convex and concave sides of the electrode sheet 1 can communicate with each other through the perforation 12, ensuring a balanced lithium concentration on both sides of the electrode sheet 1. This reduces the risk of lithium plating between the negative electrode sheet 3 and the positive electrode sheet 2 in the bend 6, thereby improving the service life of the secondary battery 100.
[0059] According to some embodiments of the present application, referring to FIG. 3 , in a corner region 13 having a through-hole 12 , there are multiple through-holes 12 , and all of the through-holes 12 are distributed at intervals within the corner region 13 .
[0060] In the same corner area 13 , the plurality of through-holes 12 are spaced apart and there are various ways to space the through-holes 12 . For example, the plurality of through-holes 12 can be arranged in a matrix, concentric rings, etc. in the corner area 13 ; or they can be arranged in an irregular dense pattern.
[0061] Providing a plurality of through holes 12 at intervals in the corner area 13 is beneficial to accelerating the passing rate of lithium ion concentration on both sides of the electrode piece 1 and promoting the dynamic balance of lithium ion concentration on both sides of the electrode piece 1 .
[0062] According to some embodiments of the present application, referring to FIG. 3 , within a corner region 13 having perforations 12 , the perforations 12 are spaced apart in rows in the second direction Y. The sum of the opening areas of the perforations 12 in any row is denoted as S0. The sum of the opening areas S0 of the rows decreases as it approaches either end of the corner region 13 in the second direction Y. The first direction X is perpendicular to the second direction Y.
[0063] The perforations 12 are arranged in rows and spaced apart in the corner area 13, which should be understood as a plurality of perforations 12 linearly spaced apart in rows along the first direction X, with the rows spaced apart along the second direction Y. In the same row, the opening areas of the perforations 12 may be consistent or inconsistent.
[0064] The sum of the opening areas S0 is related to the number of perforations 12 in each row and the opening area of each perforation 12. The opening area of each perforation 12 can be consistent or inconsistent between rows; the number of perforations 12 can also be consistent or inconsistent between rows, but it should be noted that these two parameters cannot be kept consistent at the same time.
[0065] The closer to either end of the corner region 13 along the second direction Y, the smaller the sum of the opening areas of the through-holes 12 closer to one end of the corner region 13 in the second direction Y. With this design, the through-holes 12 in the corner region 13 are smaller at both ends and larger in the middle. In some embodiments, the sum of the opening areas S0 of each row of through-holes 12 gradually decreases from the middle of the corner region 13 to either end of the corner region 13 along the second direction Y. Furthermore, the first direction X can be the length direction of the current collecting body 11, and the second direction Y can be the width direction of the current collecting body 11.
[0066] Such a design is conducive to reducing the number of openings near one end of the corner area 13, avoiding stress concentration caused by too many openings, and thus effectively avoiding the risk of fracture of the pole piece 1 during the cold pressing process.
[0067] According to some embodiments of the present application, referring to FIG. 3 , in the corner region 13 having the through holes 12 , the number of openings in each row of through holes 12 gradually decreases from the middle of the corner region 13 to either end of the corner region 13 along the second direction Y.
[0068] During the hole-opening process, the number of perforations 12 at one end of the corner area 13 along the second direction Y can be designed to be zero, that is, no holes are opened at one end of the corner area 13. At this time, a non-perforated area 17 is left between the perforation 12 closest to one end of the corner area 13 and one end of the corner area 13.
[0069] The opening areas of the individual through-holes 12 in each row may be consistent or inconsistent. When the opening areas of the individual through-holes 12 in each row are inconsistent, it is necessary to ensure that the sum S0 of the opening areas of each row is designed to be smaller as it approaches the corner area 13.
[0070] The middle of the corner area 13 should be understood as: the corner area 13 is in the middle position in the second direction Y, and can also be understood as the middle position of the current collecting body 11 along its own width direction.
[0071] This design reduces the number of openings at one end closer to the corner area 13 , ensures the structural strength of the edge of the current collecting body 11 , and prevents breakage during the cold pressing process.
[0072] According to some embodiments of the present application, referring to FIG. 3 , the current collector body 11 has a coating region 14 for coating the active material layer. The coating region 14 extends along a first direction X and sequentially passes through each corner region 13. The perforations 12 within the corner region 13 are all located within the coating region 14 along a second direction Y. The first direction X is perpendicular to the second direction Y.
[0073] The coating region 14 refers to the area on the current collector 11 where the active material can be applied. The coating region 14 can overlap with each corner region 13 or directly cover each corner region 13. When the coating region 14 covers each corner region 13, this indicates that the width of the coating region 14 along the second direction Y is consistent with the width of the current collector 11, meaning that the entire surface of the current collector 11 is coated with active material. In this case, the tab portion can be processed by cutting the current collector 1a in an earlier step to obtain a strip tab; alternatively, strip tabs can be welded to the current collector 1a.
[0074] The fact that the through-holes 12 in the corner region 13 are all located within the coating region 14 in the second direction Y should be understood as follows: the through-holes 12 in the corner region 13 will not extend beyond the edge of the coating region 14 in the second direction Y. It should be noted that if the through-holes 12 are opened beyond the coating region 14, it means that the through-holes 12 are also present in the portion not coated with the active material layer. This portion is usually used as the tab portion in the electrode assembly 10. Therefore, opening holes in this portion not only fails to achieve effective lithium ion flow, but also weakens the structural strength of the tab portion.
[0075] The opening position of the through hole 12 is limited to the coating area 14, so that lithium ions can flow effectively on both sides of the electrode 1; at the same time, it is also avoided that the through hole 12 is opened in the electrode ear part, which will cause its structural strength to be weakened.
[0076] According to some embodiments of the present application, please refer to Figure 3, at least one stress zone 15 is provided in the coating area 14, and the stress zone 15 extends along an edge of the coating area 14 in the second direction Y. The through holes 12 in the corner area 13 are all located in the area of the coating area 14 excluding the stress zone 15 in the second direction Y.
[0077] The perforations 12 in the corner region 13 are all located in the area of the coating region 14 excluding the stress region 15, that is, in the second direction Y, there is an unperforated area 17 between the perforations 12 and one edge of the coating region 14. Since stress concentration occurs at the edge of the coating region 14 during the roller cold pressing of the electrode 1, if a hole is opened near one edge of the coating region 14, a weak point will be formed, causing the current collector 1a or the electrode 1 to break, thereby causing the electrode 1 to be scrapped, reducing production efficiency and increasing costs. To this end, the perforated area 17 on the current collector 1a avoids the stress region 15, which can ensure the mechanical strength of at least one side of the current collector 1a, avoid breakage or tearing during processing, and improve production efficiency.
[0078] The open area 17 can be understood as the area enclosed by all the through holes 12 in the corner area 13 .
[0079] A stress zone 15 is left near one edge of the coating zone 14 without the perforation 12, thereby ensuring the mechanical strength of at least one side of the current collector 1a, avoiding breakage or tearing during processing, and improving production efficiency.
[0080] According to some embodiments of the present application, referring to FIG. 3 , the width of each stress region 15 in the second direction Y is denoted as D, where D is ≥ 3 mm.
[0081] The width D of the stress region 15 may be greater than 3 mm. Of course, the specific value of the width D of the stress region 15 may also be determined according to the overall width of the current collector 1 a.
[0082] The minimum threshold of the width of the stress region 15 is reasonably limited so that a region at an edge of the coating region 14 along the second direction Y has no openings, thereby ensuring the mechanical strength of at least one side of the current collector 1 a .
[0083] According to some embodiments of the present application, referring to FIG. 3 , two stress regions 15 are spaced apart in the coating region 14 along the second direction Y. The two stress regions 15 are adjacent to two opposite edges of the coating region 14 along the second direction Y, respectively.
[0084] In the second direction Y, there are two stress areas 15 spaced apart in the coating area 14 . In this case, the through hole 12 in the corner area 13 should be located between the two stress areas 15 .
[0085] Stress areas 15 are left near the two opposite edges of the coating area 14 without perforations 12, thereby ensuring the mechanical strength of both sides of the current collector 1a, avoiding breakage or tearing during processing, and improving production efficiency.
[0086] According to some embodiments of the present application, the current collecting body 11 further has a blank area 16. The blank area 16 is located on at least one side of the coating area 14 along the second direction Y.
[0087] The blank area 16 refers to the area of the current collector 11 other than the coating area 14, that is, the area not coated with the active material layer and not opened. This part can be used as the tab part in the production of the electrode assembly 10, for example: the blank area 16 is wound to form a full tab structure.
[0088] There can be one or two blank areas 16. When there are two blank areas 16, the two blank areas 16 are located on opposite sides of the coating area 14 along the second direction Y. In some embodiments, the position of the perforation 12 in the same corner area 13 constitutes an open area 17, and a stress area 15 is provided between the open area 17 and the blank area 16. To facilitate understanding of the width relationship between the respective areas, the width of the open area 17 along the second direction Y is recorded as C, the width of the coating area 14 is recorded as B, the width of the blank area 16 is recorded as A, and the width of the current collecting body 11 is recorded as L. At this time, the width of the open area 17 satisfies the condition: C≤B=Ln×A, where n can be 0, 1 or 2. It should be noted that the width of the opening area 17 can be reversed in the subsequent right confirmation by the following method, such as: taking the perforations 12 on the outermost sides of the second direction Y in the corner area 13, and making tangents of the two perforations 12 with lines parallel to the first direction X, and obtaining the maximum distance between the two tangents as the width C of the opening area 17.
[0089] A blank area 16 is reserved on at least one side of the current collecting body 11 to facilitate the manufacture of the tab portion required for the electrode assembly 10 , thereby improving manufacturing efficiency.
[0090] According to some embodiments of the present application, in the corner area 13 having the through-holes 12 , the sum of the opening areas of all the through-holes 12 is recorded as S1 , and the area of the corner area 13 on the current collecting body 11 is recorded as S2 , wherein 0.1%≤S1 / S2≤50%.
[0091] The corner region 13 having the through-hole 12 should be understood as one of the corner regions 13 having the through-hole 12 , rather than all the corner regions 13 having the through-hole 12 .
[0092] S1 / S2 can take a value between 0.1% and 50%, for example, S1 / S2 can be, but is not limited to, 0.1% and 50%. It should be noted that the ratio of S1 / S2 should not be too large. If the ratio is greater than 50%, the structural strength of the corner area 13 may be weakened, thereby causing the risk of tape breakage during the cold pressing process.
[0093] Reasonable control of the ratio range of S1 / S2 can not only ensure that lithium ions flow smoothly on both sides of the electrode 1, but also ensure that the current collecting body 11 has a certain structural strength to avoid the risk of belt breakage.
[0094] According to some embodiments of the present application, starting from the starting end of the winding of the current collecting body 11 , the first n corner regions 13 are each provided with a through hole 12 , where n≤6.
[0095] The starting end of the winding of the current collecting body 11 refers to the end where the winding of the current collecting body 11 begins first when the current collecting body 11 is wound along the first direction X.
[0096] The first n corner regions 13 refer to the first to nth corner regions 13 counted from the starting end of the current collecting body 11. Here, n is a positive integer, for example, it can be 1, 2, 3, 4, 5, or 6.
[0097] After in-depth research by the applicant, it was found that the areas most susceptible to lithium deposition during cyclic charge and discharge of the secondary battery 100 are concentrated between the innermost and third circles of the electrode assembly 10, corresponding to the first six corner regions 13 of the current collector body 11. Therefore, the applicant has opened holes in the first n corner regions 13 to effectively address the lithium deposition problem in the electrode assembly 10.
[0098] Drilling holes in the first n corner areas 13 can specifically improve the locations of the electrode assembly 10 where lithium deposition problems are likely to occur. While ensuring that the lithium deposition problem is reduced, the number of drilling operations can be reduced and the mechanical strength of the current collector 1a can be improved.
[0099] According to some embodiments of the present application, a pole piece 1 is provided. The pole piece 1 includes an active material layer and a current collector 1a as described in any of the above solutions. The active material layer is provided on at least one surface of a current collector body 11 .
[0100] The active material layer refers to the active material coated on the current collector 1a. Its material can be selected based on the polarity of the electrode 1. For example, in the positive electrode 2, the active material layer can be made of, but not limited to, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, or a ternary material. In the negative electrode 3, the active material layer can be made of, but not limited to, graphite or silicon oxide. The active material layer can be applied to only one side of the current collector 1a or simultaneously to both opposing sides.
[0101] The above-mentioned electrode 1 adopts the above-mentioned current collector 1a. During the cyclic charging process, the lithium ions on the convex side and the concave side of the electrode 1 will communicate with each other through the perforation 12, ensuring that the lithium insertion concentration on both sides of the electrode 1 is balanced, reducing the risk of lithium plating between the negative electrode 3 and the positive electrode 2 in the bent portion 6, which is beneficial to improving the service life of the secondary battery 100.
[0102] According to some embodiments of the present application, referring to FIG. 3 and FIG. 4 , the present application provides a method for preparing a pole piece 1 , which is used to prepare the pole piece 1 described above, comprising the following steps:
[0103] S100, providing a current collecting body 11;
[0104] S200 , drilling holes 12 in the corner regions 13 of the current collecting body 11 to form the current collector 1 a ;
[0105] S300, coating an active material layer on the surface of the current collector 1a;
[0106] S400 , rolling the coated current collector 1 a .
[0107] The current collector body 11 in step S100 refers to a non-perforated current collector 1a, such as aluminum foil, copper foil, etc.
[0108] In step S200 , there are various ways to drill holes in the corner area 13 , such as laser drilling, mechanical cutting, etc.
[0109] In step S300, coating involves evenly applying a suspension containing positive and negative electrode active materials onto a sheet of aluminum or copper foil using appropriate equipment, followed by drying to form a film. The coating process includes at least shear coating, wetting and leveling, and drying. The detailed operations of these steps are not detailed here; reference is made to existing literature.
[0110] In step S300, roller pressing is usually arranged after the coating and drying process. It is the process of compacting the coated powder electrode material on the positive and negative metal current collectors 1a through a roller press, which is used for the rearrangement and densification of the powder.
[0111] The preparation method of the above-mentioned electrode 1 is to open a perforation 12 on the current collecting body 11, so that the lithium ions on both sides of the electrode 1 can flow to each other through the perforation 12. In this way, during the cyclic charging process, the lithium ions on the convex side and the concave side of the electrode 1 will communicate with each other through the perforation 12, ensuring that the lithium insertion concentration on both sides of the electrode 1 is balanced, reducing the risk of lithium plating between the negative electrode 3 and the positive electrode 2 in the bending portion 6, which is beneficial to improving the service life of the secondary battery 100.
[0112] According to some embodiments of the present application, referring to FIG. 5 and FIG. 6 , S400 , the step of rolling the coated current collector 1 a , includes:
[0113] S410, press the tension roller surface 220 of the pressure roller 200 and the extension roller surface 210 located on both sides of the tension roller surface 220 respectively on the active material layer and the blank area 16 on both sides of the active material layer on the current collector 1a, and control the extension roller surface 210 to leave a gap between the side facing the tension roller surface 220 and the area where the perforation 12 is located.
[0114] Referring to Figure 6 , the pressure roller 200 is the component that presses against the coated current collector 1a to compact the active material. The surface of the pressure roller 200 includes a tension roller surface 220 and extension roller surfaces 210 located on either side of the tension roller surface 220. The extension roller surface 210 presses against the blank area 16 of the current collector 1a, while the tension roller surface 220 presses against the active material layer of the current collector 1a. Both the extension roller surface 210 and the tension roller surface 220 extend circumferentially on the pressure roller 200, with the diameter of the extension roller surface 210 being larger than that of the tension roller surface 220.
[0115] When cold pressing the active material, a gap is left between one side of the stretching roller surface 210 and the area where the perforation 12 is located to avoid the perforation 12 being close to the stretching roller surface 210 and causing stress concentration, thereby preventing the electrode 1 from being easily broken during rolling.
[0116] According to some embodiments of the present application, referring to FIG. 2 , the present application provides an electrode assembly 10 configured as a wound structure. The electrode assembly 10 includes a positive electrode sheet 2, a negative electrode sheet 3, and a separator 4 disposed between the positive electrode sheet 2 and the negative electrode sheet 3, and the wound structure includes a bend 6. The positive electrode sheet 2 and / or the negative electrode sheet 3 are the above-described electrode sheet 1, and the bend 6 is located opposite the corner region 13 after winding.
[0117] According to some embodiments of the present application, please refer to FIG. 1 . The present application provides a secondary battery 100 including the above electrode assembly 10 .
[0118] According to some embodiments of the present application, please refer to Figures 1 to 6. The present application provides a current collector 1a. According to the winding size of the electrode assembly 10, the position of the corner area 13 on the current collector 1a is determined, and then the perforations 12 are punched in the corner area 13. The shape and arrangement of the perforations 12 are not limited. The ratio of the opening area of all perforations 12 to the area of the corner area 13 is 0.1 to 50%. The width of the area where the perforations 12 are located along the second direction Y is limited to the coating area 14, and the sum of the opening areas of each row gradually decreases from the middle to both sides. Outside the edge of the coating area 14 is a blank area 16, and the blank area 16 (the area not coated with active material) is not punched.
[0119] In order to make the purpose, technical solutions and advantages of this application more concise and clear, this application is illustrated with the following specific examples, but this application is by no means limited to these examples. The embodiments described below are only preferred embodiments of this application and can be used to describe this application. They should not be understood as limiting the scope of this application. It should be pointed out that any modifications, equivalent replacements and improvements made within the spirit and principles of this application should be included in the scope of protection of this application.
[0120] In order to better illustrate the present application, the present application is further described below in conjunction with the embodiments. The following are specific embodiments.
[0121] Comparative Example 1
[0122] Positive electrode 2:
[0123] The positive electrode active material ternary material nickel cobalt manganese (NCM811), the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were mixed uniformly in a mass ratio of 97:2:1 and added to the solvent NMP to prepare a positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil, dried at 85°C, cold pressed, and then die-cut and slit to prepare a lithium-ion battery positive electrode sheet 2.
[0124] The coating weight of the active material of the positive electrode sheet 2 is 17.6 mg / cm2. 2 ), the thickness of the current collector 1a of the positive electrode sheet 2 is 13 microns (μm).
[0125] Negative electrode 3:
[0126] Graphite (a negative electrode active material), acetylene black (a conductive agent), sodium carboxymethyl cellulose (CMC) (a thickener), and styrene-butadiene rubber (SBR) (a binder) were added to solvent water at a mass ratio of 96:2:1:1 and mixed evenly to form a negative electrode slurry. The negative electrode slurry was evenly coated on copper foil, dried at 85°C, and then cold pressed to form a negative electrode sheet 3.
[0127] The coating weight of the negative electrode sheet 3 is 10 mg / cm 2 The thickness of the current collector 1a of the negative electrode sheet 3 is 8 μm, the width of the current collector 1a is 170 mm, and the width of the active material coating area 14 of the negative electrode sheet 3 is 100 mm. In addition, the corner area 13 of the current collector 1a of the negative electrode sheet 3 does not have a perforation 12.
[0128] Diaphragm 4:
[0129] A polyethylene microporous film is used as a porous isolation membrane substrate, and inorganic alumina powder, polyvinylpyrrolidone, and acetone solvent are evenly mixed in a weight ratio of 3:1.5:5.5 to form a slurry, which is then coated on one side of the substrate and dried to obtain an isolation membrane.
[0130] Electrolyte:
[0131] Lithium hexafluorophosphate is dissolved in a mixed solvent of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate (the volume ratio of ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate is 1:2:1) to obtain a lithium ion battery electrolyte.
[0132] Preparation of Secondary Battery 100:
[0133] The positive electrode sheet 2, the negative electrode sheet 3 and the separator are wound to obtain a bare cell, which is then packaged, injected, formed, vented and other processes to produce a lithium-ion battery. The battery has a designed charging N / P of 1.03 and a designed cell capacity of 160Ah.
[0134] Comparative Example 2
[0135] It is basically the same as Comparative Example 1, except that holes are opened in the first six corner areas 13 of the current collector 1a of the negative electrode sheet 3, and the ratio of the opening area to the area of the corner area 13 is 10%, and the width of the opening area 17 is 120 mm.
[0136] Example 1
[0137] It is basically the same as Comparative Example 1, except that holes are opened in the first six corner areas 13 of the current collector 1a of the negative electrode sheet 3, and the ratio of the opening area to the area of the corner area 13 is 1%, and the width of the opening area 17 is 100 mm.
[0138] Example 2
[0139] It is basically the same as Comparative Example 1, except that holes are opened in the first six corner areas 13 of the current collector 1a of the negative electrode sheet 3, and the ratio of the opening area to the area of the corner area 13 is 10%, and the width of the opening area 17 is 100 mm.
[0140] Example 3
[0141] It is basically the same as Comparative Example 1, except that holes are opened in the first six corner areas 13 of the current collector 1a of the negative electrode sheet 3, and the ratio of the opening area to the area of the corner area 13 is 10%, and the width of the opening area 17 is 80 mm.
[0142] Example 4
[0143] It is basically the same as Comparative Example 1, except that holes are opened in the first six corner areas 13 of the current collector 1a of the negative electrode sheet 3, and the ratio of the opening area to the area of the corner area 13 is 20%, and the width of the opening area 17 is 60 mm.
[0144] The secondary batteries 100 prepared in the comparative examples and examples above were used to record the frequency of fractures during the cold pressing process. Furthermore, after the secondary batteries 100 were completed, they were charged to 4.25V at a constant current and constant voltage of 0.5C. The cells were then disassembled to observe whether lithium deposition occurred at the bend 6 of the electrode assembly 10. The specific results can be found in Table 1.
[0145] Table 1
[0146]
[0147] As can be seen from Table 1, by comparing Examples 2 to 4 with Comparative Example 1, it can be concluded that drilling the holes 12 in the corner area 13 of the current collector 1 a can effectively reduce the lithium deposition problem at the bend 6 .
[0148] At the same time, when Example 1 and Example 2 are compared with Comparative Example 1, it can be seen that if the width of the opening area 17 is the same as the width of the active material coating area 14, the mechanical strength of the electrode 1 will be weakened, causing the electrode 1 to easily break during the cold pressing process.
[0149] Comparing Example 2, Example 3 and Example 4 with Comparative Example 2, it can be seen that if the width of the opening area 17 is smaller than the width of the active material coating area 14, a stress area 15 without an opening is left between the edge of the opening area 17 and the coating area 14, which can effectively reduce the number of times the electrode 1 breaks.
[0150] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A current collector (1a) for winding in a first direction (X), the current collector (1a) comprising: The current collecting body (11) has a plurality of corner areas (13) spaced apart along the first direction (X), and the corner areas (13) are used to be opposite to the bent portion (6) of the electrode assembly (10); Wherein, a perforation (12) is provided in at least one of the corner regions (13) along the thickness direction of the current collector (1a).
2. The current collector (1a) according to claim 1, wherein In the corner area (13) having the perforations (12), there are a plurality of perforations (12), and all the perforations (12) are distributed at intervals in the corner area (13).
3. The current collector (1a) according to claim 2, wherein In a corner area (13) having the perforations (12), the perforations (12) are spaced apart in rows in a second direction (Y), the sum of the opening areas of the perforations (12) in any row is recorded as S0, and the sum of the opening areas S0 of each row becomes smaller as it approaches any end of the corner area (13) along the second direction (Y), and the first direction (X) is perpendicular to the second direction (Y).
4. The current collector (1a) according to claim 3, wherein In the corner area (13) having the perforations (12), the number of openings of each row of the perforations (12) gradually decreases from the middle of the corner area (13) to either end of the corner area (13) along the second direction (Y).
5. The current collector (1a) according to claim 2, wherein The current collecting body (11) has a coating area (14) for coating an active material layer, the coating area (14) extends along the first direction (X) and passes through each of the corner areas (13) in sequence, the perforations (12) in the corner areas (13) are all located in the coating area (14) in the second direction (Y), and the first direction (X) is perpendicular to the second direction (Y).
6. The current collector (1a) according to claim 5, wherein At least one stress zone (15) is provided in the coating zone (14), and the stress zone (15) extends along an edge of the coating zone (14) in the second direction (Y). The perforations (12) in the corner zone (13) are all located in the area of the coating zone (14) excluding the stress zone (15) in the second direction (Y).
7. The current collector (1a) according to claim 6, wherein The width of each stress zone (15) in the second direction (Y) is recorded as D, wherein D≥3mm.
8. The current collector (1a) according to claim 6, wherein Two stress zones (15) are spaced apart in the coating zone (14) along the second direction (Y), and the two stress zones (15) are respectively adjacent to two opposite edges of the coating zone (14) along the second direction (Y).
9. The current collector (1a) according to any one of claims 5 to 8, wherein: The current collecting body (11) also has a blank area (16), and the blank area (16) is located on at least one side of the coating area (14) along the second direction (Y).
10. The current collector (1a) according to any one of claims 1 to 9, wherein: In the corner area (13) having the perforations (12), the sum of the opening areas of all the perforations (12) is recorded as S1, and the area of the corner area (13) on the current collecting body (11) is recorded as S2, wherein 0.1%≤S1 / S2≤50%.
11. The current collector (1a) according to any one of claims 1 to 10, wherein: Starting from the starting end of the winding of the current collecting body (11), the first n corner areas (13) are all provided with the perforations (12), wherein n≤6.
12. A pole piece (1), comprising: The current collector (1a) according to any one of claims 1 to 11; The active material layer is provided on at least one surface of the current collecting body (11).
13. A method for preparing a pole piece, for preparing the pole piece (1) according to claim 12, comprising the following steps: Providing a current collecting body (11); A perforation (12) is formed in a corner region (13) on the current collecting body (11) to form a current collecting body (1a); coating an active material layer on the surface of the current collector (1a); The coated current collector (1a) is roll-pressed.
14. The method for preparing a pole piece according to claim 13, wherein: The step of rolling the coated current collector (1a) comprises: The tension roller surface (220) of the pressure roller (200) and the extension roller surfaces (210) located on both sides of the tension roller surface (220) are respectively pressed against the active material layer and the blank areas (16) on both sides of the active material layer on the current collector (1a), and a distance is left between the side of the extension roller surface (210) facing the tension roller surface (220) and the area where the perforation (12) is located.
15. An electrode assembly (10) constructed as a wound structure, comprising a positive electrode sheet (2), a negative electrode sheet (3), and a separator (4) disposed between the positive electrode sheet (2) and the negative electrode sheet (3), wherein the wound structure comprises a bent portion (6); in, The positive electrode sheet (2) and / or the negative electrode sheet (3) is the electrode sheet (1) according to claim 12, and the bending portion (6) is located opposite to the corner area (13) after winding.
16. A secondary battery (100) comprising the electrode assembly (10) according to claim 15.
Citation Information
Patent Citations
Secondary battery
CN103022408A
Lithium battery positive plate and preparation method thereof
CN114551787A
Positive plate with through holes and non-deformable secondary battery
CN115207276A
Electrode assembly, battery cell, battery and electric device
CN213692108U
Positive plate with through holes and secondary battery
CN217933852U