Method for manufacturing electrode

The clamp matches the thermal expansion amount of the sealing member with the current collector in electrode manufacturing, reduces the difference in shrinkage amount after cooling, solves the problem of current collector folds in electrode manufacturing, and improves the electrode quality.

CN119096385APending Publication Date: 2024-12-06TOYOTA INDUSTRIES CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380035087.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-22
Filing Date
2023-04-13
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the electrode manufacturing process, heating expansion and cooling of the sealing member lead to a difference in the shrinkage amount from the current collector, which may cause wrinkles of the current collector.

Method used

When pressurized heating is performed by using a clamp, the thermal expansion amount of the sealing member and the current collector is closer by deformation of the heater part and the pressing part, reducing the difference in shrinkage after cooling, and using a pair of clamps to uncoated the current collector. The part and the sealing member are heated and welded.

Benefits of technology

The current collector wrinkles caused by the difference in shrinkage amount between the sealing member and the current collector are effectively suppressed, and the production quality of the electrode is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096385A_ABST
    Figure CN119096385A_ABST
Patent Text Reader

Abstract

A method for manufacturing an electrode (11), the method including: an arrangement step in which a sealing member (140) is arranged in an uncoated portion of a collector (12); and a welding step in which the sealing member is welded to the current collector by performing pressure heating using a jig (60) in which the sealing member is heated in a state in which the sealing member is pressed against the uncoated portion. The jig is provided with: a heater unit (61) which is deformable and is configured so as to heat the sealing member; and a pressing part (64) configured to press the heater part against the sealing member. The disposing step includes disposing the sealing member in the uncoated portion such that an exposed portion where the sealing member is not disposed is formed in the uncoated portion. The welding step includes heating the sealing member and the exposed portion in a state in which the heater portion is pressed against the sealing member and the exposed portion while deforming the heater portion so as to follow compressive deformation of the pressing portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing an electrode. Background Art

[0002] In order to insulate collectors from each other in a power storage device formed by stacking a plurality of electrodes, a sealing member is sometimes welded to a collector when manufacturing an electrode. For example, in a method for manufacturing an electrode described in Patent Document 1, a sealing member is welded to a collector by performing pressurized heating in which a heater is pressed against the sealing member disposed on the collector.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-106963 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] When the sealing member is welded to the current collector by pressurizing and heating the sealing member, the sealing member expands as it is heated. When the heating of the heater stops during the welding of the sealing member to the current collector, the expanded sealing member is cooled, and the sealing member shrinks as it cools. When the difference in shrinkage between the sealing member and the current collector is large, the current collector is compressed as the sealing member shrinks, so that wrinkles may be generated on the current collector.

[0008] Solutions for solving problems

[0009] According to one embodiment of the present disclosure, a method for manufacturing an electrode is provided. The electrode comprises: a current collector having a first surface and a second surface on the opposite side of the first surface; an active material layer provided on the first surface and the second surface; and a sealing member fused to the current collector. The first surface and the second surface each have a portion where the active material layer is provided and an uncoated portion where the active material layer is not provided. The manufacturing method comprises: a configuration step of configuring the sealing member on the uncoated portion of at least one of the first surface and the second surface; and a welding step of welding the sealing member to the current collector by heating the sealing member under pressure against the uncoated portion using a jig. The jig comprises: a heater portion that is deformable and configured to heat the sealing member; and a pressing portion that is configured to press the heater portion against the sealing member. The direction in which the pressing portion presses the sealing member is a pressing direction. The pressing portion is located in parallel with the heater portion and the sealing member in the pressing direction, and is configured to be compressed and deformed in the pressing direction as the heater portion is pressed. The arranging step includes arranging the sealing member in the uncoated portion in such a manner that an exposed portion is formed in the uncoated portion as a portion where the sealing member is not arranged and is located between the active material layer and the sealing member. The welding step includes deforming the heater portion in a manner that follows the compression deformation of the pressing portion, while heating the sealing member arranged in the uncoated portion and the exposed portion while pressing the heater portion against the two.

[0010] According to the above method, the sealing member is fused to the collector by deforming the heater portion in a manner that follows the compression deformation of the pressing portion, and heating the sealing member and the exposed portion while pressing the heater portion against the two. Compared with the case where the exposed portion is not pressurized and heated but only the sealing member is pressurized and heated, in the above method, the thermal expansion of the collector caused by the heat transfer from the heater portion becomes larger. Therefore, the difference in thermal expansion between the sealing member and the collector becomes smaller, thereby reducing the difference in shrinkage between the sealing member and the collector caused by the cooling of the collector and the sealing member. Therefore, when the sealing member is fused to the collector, the generation of wrinkles in the collector caused by the difference in shrinkage between the sealing member and the collector can be suppressed.

[0011] In the method for manufacturing an electrode, the clamp may be a pair of clamps located on both sides of the current collector in the pressing direction, and each of the pair of clamps includes the heater portion and the pressing portion. The configuration step may include configuring the sealing member on the uncoated portion of the first surface and the second surface. The welding step may include using the pair of clamps to pressurize and heat the sealing member configured on the uncoated portion of the first surface and the second surface, and the exposed portion of the first surface and the second surface.

[0012] According to the above method, the heater portion can be deformed in a manner following the compression deformation of the pressing portion, while the sealing member and the exposed portion are heated while the heater portion is pressed against the first and second surfaces of the current collector. As a result, the sealing member can be welded to the uncoated portions on both surfaces of the current collector through the heater portion and the pressing portion.

[0013] In the method for manufacturing an electrode, the sealing member may include: a main body portion disposed on the uncoated portion; and a protrusion portion extending from the main body portion and protruding from an outer edge of the current collector. The welding step may include heating the sealing member while the heater portion is pressed against at least a portion of the protrusion portion.

[0014] According to the above method, heating is performed while the heater portion is pressed against the sealing member excluding at least a portion of the protrusion. Therefore, by heating while the heater portion is pressed against the main body, the sealing member can be fused to the collector. Even if the entire protrusion is not pressurized and heated by the heater portion, the sealing member can be fused to the collector. Therefore, compared with the case where the entire sealing member is pressurized and heated by the heater portion, the thermal expansion of the sealing member can be reduced. As a result, the shrinkage of the sealing member caused by the cooling of the sealing member can be reduced. Therefore, the difference between the shrinkage of the sealing member and the collector can be further reduced, thereby suppressing the generation of wrinkles in the collector.

[0015] Effects of the Invention

[0016] According to the present invention, it is possible to suppress the generation of wrinkles in the current collector which would otherwise occur due to the difference in shrinkage between the sealing member and the current collector when the sealing member is welded to the current collector. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a cross-sectional view of a power storage device according to one embodiment.

[0018] Figure 2 Yes Figure 1A cross-sectional view showing an enlarged portion of a power storage device.

[0019] Figure 3 is a diagram for explaining a method for manufacturing an electrode according to an embodiment, and shows a method for arranging a sealing member in a structure Figure 1 A plan view showing the state of the current collector of the electrode of the power storage device.

[0020] Figure 4 is a diagram for explaining a method for manufacturing an electrode according to an embodiment, and is a diagram showing a configuration having Figure 3 A cross-sectional view of a sealing member in a state before the current collector is subjected to pressurized heating.

[0021] Figure 5 is a diagram for explaining a method for manufacturing an electrode according to an embodiment, and is a diagram showing a configuration having Figure 3 A cross-sectional view of a sealing member in a state where a current collector is pressurized and heated.

[0022] Figure 6 is a diagram for explaining a method for manufacturing an electrode according to an embodiment, and shows a method for manufacturing an electrode by applying pressure and heating. Figure 3 A cross-sectional view of an electrode in a state where a sealing member is integrated.

[0023] Figure 7 is a diagram for explaining a method for manufacturing a power storage device according to an embodiment, and shows Figure 6 A cross-sectional view of a stacked body showing a stacked state of electrodes, separators and spacers.

[0024] Figure 8 is a diagram for explaining a method for manufacturing an electrode according to a modified example, and is a diagram showing a configuration having Figure 3 A cross-sectional view of a sealing member in a state before the current collector is subjected to pressurized heating. DETAILED DESCRIPTION

[0025] Below, use Figure 1 to Figure 7 Hereinafter, for the sake of convenience, the power storage device and the electrode will be described before the method for manufacturing the electrode.

[0026] <Electricity storage device>

[0027] like Figure 1 As shown, the power storage device 10 includes a stacked body 10a and a sealing body 15. The stacked body 10a is formed by stacking a plurality of electrodes 11 between a positive terminal electrode 36 and a negative terminal electrode 37. The power storage device 10 of this embodiment is a lithium ion secondary battery. Hereinafter, the direction in which the plurality of electrodes 11 are stacked is referred to as a stacking direction X.

[0028] <Electrode>

[0029] like Figure 1 and Figure 2 As shown, each of the plurality of electrodes 11 includes a current collector 12, a positive electrode active material layer 23 as an active material layer, and a negative electrode active material layer 33 as an active material layer. The current collector 12 is in sheet form. Active material layers are provided on both sides of the current collector 12. The current collector 12 has a first face 12a and a second face 12b which are opposite to each other in the stacking direction X. The positive electrode active material layer 23 is provided on the first face 12a of the current collector 12, and the negative electrode active material layer 33 is provided on the second face 12b. Each of the plurality of electrodes 11 is a bipolar electrode composed of such a current collector 12. In the stack 10a, the plurality of electrodes 11 are stacked in such a manner that the first face 12a of the current collector 12 of one of the two electrodes 11 adjacent to each other in the stacking direction X is opposite to the second face 12b of the current collector 12 of the other electrode 11.

[0030] In a top view viewed from the stacking direction X (hereinafter referred to as a top view), the positive electrode active material layer 23 is formed in the central portion of the first surface 12a of the current collector 12. The peripheral portion of the first surface 12a of the current collector 12 in a top view becomes a positive electrode uncoated portion 12c as an uncoated portion where the positive electrode active material layer 23 is not provided. The positive electrode uncoated portion 12c is configured to surround the positive electrode active material layer 23 in a top view. In a top view, the negative electrode active material layer 33 is formed in the central portion of the second surface 12b of the current collector 12. The peripheral portion of the second surface 12b of the current collector 12 in a top view becomes a negative electrode uncoated portion 12d as an uncoated portion where the negative electrode active material layer 33 is not provided. The negative electrode uncoated portion 12d is configured to surround the negative electrode active material layer 33 in a top view.

[0031] The positive electrode active material layer 23 and the negative electrode active material layer 33 are arranged to face each other in the stacking direction X. The negative electrode active material layer 33 is formed, for example, slightly larger than the positive electrode active material layer 23. In a plan view, the entire region where the positive electrode active material layer 23 is formed is located within the region where the negative electrode active material layer 33 is formed.

[0032] <Details of current collector>

[0033] In the present embodiment, the current collector 12 is formed by integrating a sheet-shaped positive electrode current collector 22 and a sheet-shaped negative electrode current collector 32. The first surface 12a of the current collector 12 is formed by one surface of the positive electrode current collector 22, and the second surface 12b is formed by one surface of the negative electrode current collector 32. The integration of the positive electrode current collector 22 and the negative electrode current collector 32 can also be performed by bonding the surface of the positive electrode current collector 22 on the side opposite to the first surface 12a to the surface of the negative electrode current collector 32 on the side opposite to the second surface 12b. The shapes of the positive electrode current collector 22 and the negative electrode current collector 32 when viewed from above are the same shape.

[0034] like Figure 3 As shown, the current collector 12 has four sides 12f in a plan view and is rectangular. The outer edge 12e of the current collector 12 is composed of the four sides 12f. Two sides 12f are also referred to as short sides 12g, and two sides 12f longer than the short sides 12g are also referred to as long sides 12h.

[0035] like Figure 1 As shown, the positive electrode collector 22 and the negative electrode collector 32 are chemically inert electrical conductors for allowing current to continue to flow through the positive electrode active material layer 23 and the negative electrode active material layer 33 during discharge or charge of the lithium ion secondary battery. The material constituting the positive electrode collector 22 and the negative electrode collector 32 can be, for example, a metal material, a conductive resin material, a conductive inorganic material, etc.

[0036] The conductive resin material may be, for example, a conductive polymer material or a resin obtained by adding a conductive filler to a non-conductive polymer material as required. The positive electrode collector 22 and the negative electrode collector 32 may also include a plurality of layers including one or more layers containing a metal material or a conductive resin material. The surfaces of the positive electrode collector 22 and the negative electrode collector 32 may also be coated with a known protective layer. The surfaces of the positive electrode collector 22 and the negative electrode collector 32 may also be plated with metal by a known method such as plating treatment.

[0037] The positive electrode collector 22 and the negative electrode collector 32 may have, for example, a form of foil, sheet, film, wire, rod, mesh or clad material. When the positive electrode collector 22 and the negative electrode collector 32 are metal foils, the positive electrode collector 22 and the negative electrode collector 32 may be, for example, aluminum foil, copper foil, nickel foil, titanium foil or stainless steel foil. The positive electrode collector 22 and the negative electrode collector 32 may also be alloy foils of the above metals. When the positive electrode collector 22 and the negative electrode collector 32 are metal foils, the thickness of the positive electrode collector 22 and the negative electrode collector 32 is, for example, 1 to 100 μm. The positive electrode collector 22 of the present embodiment is aluminum foil. The negative electrode collector 32 of the present embodiment is copper foil. Furthermore, in order to improve the structural stability of the stack 10a, for example, the thickness of the current collectors 12 of the positive terminal electrode 36 and the negative terminal electrode 37 and the current collectors 12 of some of the plurality of electrodes 11 constituting the bipolar electrode may be set to be 100 μm or more.

[0038] In addition, the current collector 12 is not limited to the form of integrating the positive electrode current collector 22 and the negative electrode current collector 32, and may be a sheet-shaped current collector made of a metal material, a conductive resin material, a conductive inorganic material, etc. In addition, the current collector 12 may be an object in which a coating layer is formed on one surface of the sheet-shaped current collector by plating treatment, etc. In these cases, the single current collector 12 functions as the positive electrode current collector 22 and the negative electrode current collector 32.

[0039] <Details of positive electrode active material layer and negative electrode active material layer>

[0040] The positive electrode active material layer 23 contains a positive electrode active material that can absorb and release lithium ions as charge carriers. The positive electrode active material can be, for example, olivine-type lithium iron phosphate (LiFePO 4 ) and other polyanion compounds, lithium composite metal oxides having a layered rock salt structure, and metal oxides having a spinel structure. The positive electrode active material is a substance that can be used as a positive electrode active material for a power storage device 10 such as a lithium ion secondary battery.

[0041] The negative electrode active material layer 33 contains a negative electrode active material that can absorb and release charge carriers such as lithium ions. The negative electrode active material can be used without particular limitation as long as it is a single substance, alloy or compound that can absorb and release charge carriers such as lithium ions. For example, the negative electrode active material can be Li or carbon, a metal compound, an element that can be alloyed with lithium or a compound thereof. Carbon can be, for example, natural graphite, artificial graphite, hard carbon (difficult to graphitize carbon) or soft carbon (easy to graphitize carbon). Artificial graphite can be, for example, highly oriented graphite or mesophase carbon microbeads. Elements that can be alloyed with lithium can be, for example, silicon or tin.

[0042] The positive electrode active material layer 23 and the negative electrode active material layer 33 may contain other components such as a conductive additive, a binder, an electrolyte (polymer matrix, an ion conductive polymer, a liquid electrolyte, etc.) for improving electrical conductivity, and an electrolyte supporting salt (lithium salt) for improving ion conductivity as required. The types of other components contained in the positive electrode active material layer 23 and the negative electrode active material layer 33 and their blending ratios are not particularly limited.

[0043] Conductive aids may be, for example, acetylene black, carbon black or graphite. Binders may be, for example, fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene, fluorine rubber, thermoplastic resins such as polypropylene and polyethylene, imide resins such as polyimide and polyamide-imide, alkoxysilyl-containing resins, acrylic resins such as poly(methyl)acrylic acid, styrene-butadiene rubber, carboxymethyl cellulose, sodium alginate, alginate such as ammonium alginate, water-soluble cellulose ester crosslinks or starch-acrylic acid graft polymers. These binders may be used alone or in multiples. Solvents or dispersion media may be, for example, water, N-methyl-2-pyrrolidone, etc.

[0044] <Isolation>

[0045] The power storage device 10 includes a separator 35. The separator 35 is disposed between the positive electrode active material layer 23 and the negative electrode active material layer 33. The separator 35 is a member that prevents short circuits caused by contact between the two electrodes by isolating the positive electrode active material layer 23 and the negative electrode active material layer 33 and allows charge carriers such as lithium ions to pass through.

[0046] The separator 35 may be, for example, a porous sheet or nonwoven fabric containing a polymer that absorbs and retains an electrolyte. The electrolyte impregnated into the separator 35 may be, for example, a liquid electrolyte containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent, or a polymer gel electrolyte containing an electrolyte retained in a polymer matrix. In this embodiment, a liquid electrolyte is used as the electrolyte. The electrolyte salt of the liquid electrolyte may be LiClO 4 、LiAsF 6 、LiPF 6 , LiBF 4 、LiCF 3 SO 3 、LiN(FSO 2 ) 2 、LiN(CF 3 SO 2 ) 2 The non-aqueous solvent may be a known lithium salt such as cyclic carbonates, cyclic esters, chain carbonates, chain esters or ethers. In addition, two or more of these known solvent materials may be used in combination. The material constituting the separator 35 may be, for example, polypropylene, polyethylene, polyolefin or polyester. The separator 35 may have a single-layer structure or a multi-layer structure. The multi-layer structure may have, for example, an adhesive layer and a ceramic layer as a heat-resistant layer.

[0047] <Positive terminal electrode and negative terminal electrode>

[0048] In the stacking direction X, the plurality of electrodes 11 are located between the positive terminal electrode 36 and the negative terminal electrode 37. The positive terminal electrode 36 includes a current collector 12 and a positive electrode active material layer 23 provided on the first surface 12a of the current collector 12, and is configured in the same manner as the electrode 11 except that the negative electrode active material layer 33 is not provided. The negative terminal electrode 37 includes a current collector 12 and a negative electrode active material layer 33 provided on the second surface 12b of the current collector 12, and is configured in the same manner as the electrode 11 except that the positive electrode active material layer 23 is not provided. The current collector 12 of the positive terminal electrode 36 is located at one end of the stack 10a in the stacking direction X. The current collector 12 of the negative terminal electrode 37 is located at the other end of the stack 10a in the stacking direction X.

[0049] The second surface 12b of the current collector 12 of the positive terminal electrode 36 constitutes a first outer surface 32a which is an outer surface at one end of the stacking direction X of the stack 10a. The first surface 12a of the current collector 12 of the negative terminal electrode 37 constitutes a second outer surface 22a which is an outer surface at the other end of the stack 10a in the stacking direction X. The first outer surface 32a and the second outer surface 22a are planes extending in a manner perpendicular to the stacking direction X.

[0050] <Interior Space>

[0051] The internal space S is located between two current collectors 12 adjacent to each other in the stacking direction X. The internal space S is divided by the positive current collector 22 and the negative current collector 32 adjacent to each other in the stacking direction X, and the sealing body 15. One internal space S is divided for each group of positive current collectors 22 and negative current collectors 32 adjacent to each other in the stacking direction X. The positive electrode active material layer 23, the negative electrode active material layer 33, the separator 35, and the liquid electrolyte (not shown) are arranged in the internal space S. The liquid electrolyte is, for example, a so-called electrolyte solution containing a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent.

[0052] <Positive and negative current conducting plates>

[0053] The power storage device 10 includes a positive electrode current plate 38 and a negative electrode current plate 39. The positive electrode current plate 38 and the negative electrode current plate 39 are made of a material with excellent conductivity. The material constituting the positive electrode current plate 38 and the negative electrode current plate 39 may be a metal material such as aluminum, copper or stainless steel. The stack 10a is arranged between the positive electrode current plate 38 and the negative electrode current plate 39 in the stacking direction X.

[0054] The positive electrode current-carrying plate 38 is electrically connected to the first outer surface 32a of the stack 10a. The negative electrode current-carrying plate 39 is electrically connected to the second outer surface 22a of the stack 10a. The positive electrode current-carrying plate 38 and the negative electrode current-carrying plate 39 are each provided with a terminal (not shown). The power storage device 10 is charged and discharged through the terminals provided on the positive electrode current-carrying plate 38 and the negative electrode current-carrying plate 39.

[0055] <Closed body>

[0056] The sealing body 15 is arranged to surround the positive electrode active material layer 23 and the negative electrode active material layer 33 of the plurality of electrodes 11, the positive electrode terminal electrode 36, and the negative electrode terminal electrode 37 as viewed from the stacking direction X. Hereinafter, the electrode 11, the positive electrode terminal electrode 36, and the negative electrode terminal electrode 37 may be simply referred to as the electrode 11a. The sealing body 15 seals between the current collectors 12 adjacent to each other in the stacking direction X.

[0057] like Figure 2 As shown, the sealing body 15 has a plurality of sealing portions 40 fused to each of the collectors 12 of the plurality of electrodes 11a. That is, each of the plurality of electrodes 11a has a sealing portion 40. The plurality of sealing portions 40 are made of resin. Each of the sealing portions 40 has: two first sealing portions 41; and a second sealing portion 42. The first sealing portion 41 is a portion disposed between the first surface 12a of the collector 12 of one electrode 11a of the electrodes 11a adjacent to each other in the stacking direction X and the second surface 12b of the collector 12 of the other electrode 11a. That is, the first sealing portion 41 is disposed on the inner side than the outer edge 12e of the collector 12 as viewed in the stacking direction X. The two first sealing portions 41 are disposed on both sides of each collector 12 in the stacking direction X. The two first sealing portions 41 are fused to the first surface 12a and the second surface 12b of the collector 12. The two first sealing portions 41 are welded to the first surface 12a and the second surface 12b via the welding portion 41a. The two first sealing portions 41 are welded to the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d. In other words, the sealing portion 40 is welded to the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d as uncoated portions.

[0058] The first sealing portion 41 located on the positive electrode uncoated portion 12c is arranged to surround the positive electrode active material layer 23. The first sealing portion 41 located on the negative electrode uncoated portion 12d is arranged to surround the negative electrode active material layer 33. The first sealing portion 41 has a rectangular frame shape.

[0059] The first sealing portion 41 located on the positive electrode uncoated portion 12c is separated from the positive electrode active material layer 23. As a result, a portion of the positive electrode uncoated portion 12c becomes a positive electrode exposed portion 17 where the positive electrode active material layer 23 and the first sealing portion 41 are not configured. The positive electrode exposed portion 17 as an exposed portion is a portion of the positive electrode uncoated portion 12c as an uncoated portion where the positive electrode active material layer 23 as an active material layer and the sealing portion 40 are not configured. The positive electrode exposed portion 17 is located between the positive electrode active material layer 23 and the sealing portion 40. The positive electrode exposed portion 17 is in a rectangular frame shape when viewed from above. The positive electrode exposed portion 17 is located at a position surrounding the positive electrode active material layer 23 from the outside and is located at a position closer to the inside than the first sealing portion 41 located on the positive electrode uncoated portion 12c.

[0060] The first sealing portion 41 located on the negative electrode uncoated portion 12d is separated from the negative electrode active material layer 33. As a result, a portion of the negative electrode uncoated portion 12d becomes a negative electrode exposed portion 18 where the negative electrode active material layer 33 and the first sealing portion 41 are not configured. The negative electrode exposed portion 18 as an exposed portion is a portion of the negative electrode uncoated portion 12d as an uncoated portion where the negative electrode active material layer 33 as an active material layer and the sealing portion 40 are not configured. The negative electrode exposed portion 18 is located between the negative electrode active material layer 33 and the sealing portion 40. The negative electrode exposed portion 18 is in a rectangular frame shape when viewed from above. The negative electrode exposed portion 18 is located at a position surrounding the negative electrode active material layer 33 from the outside and is located at a position closer to the inside than the first sealing portion 41 located on the negative electrode uncoated portion 12d.

[0061] The second sealing portion 42 is a portion extending from the first sealing portion 41 to the outside of the outer edge 12e of the collector 12. More specifically, the second sealing portion 42 is a portion located at a position outside the outer edge 12e of the collector 12 when viewed from the stacking direction X. The second sealing portion 42 is configured to surround the collector 12 as viewed from the stacking direction X. The second sealing portion 42 is in the shape of a rectangular frame. The second sealing portion 42 covers the end face of the collector 12 that connects the first face 12a and the second face 12b. The second sealing portion 42 connects the outer periphery of the first sealing portion 41 located on the positive electrode uncoated portion 12c with the outer periphery of the first sealing portion 41 located on the negative electrode uncoated portion 12d.

[0062] The sealing body 15 has a plurality of spacer portions 50. The plurality of spacer portions 50 are made of resin. The spacer portions 50 are each sandwiched between the collectors 12 adjacent in the stacking direction X by the first sealing portion 41 located on the positive electrode uncoated portion 12c and the first sealing portion 41 located on the negative electrode uncoated portion 12d. Thus, the spacer portion 50 is sandwiched between the collectors 12 adjacent in the stacking direction X by the first sealing portion 41. The spacer portion 50 is configured to surround the positive electrode active material layer 23 and the negative electrode active material layer 33 as viewed from the stacking direction X. The spacer portion 50 is in the shape of a rectangular frame.

[0063] In the embodiment, both surfaces of the spacer 50 in the stacking direction X are not fused to the first sealing portion 41. Both surfaces of the spacer 50 in the stacking direction X may be in contact with the first sealing portion 41 or may be separated from the first sealing portion 41.

[0064] The first sealing portion 41 and the separator portion 50 are located between the current collectors 12 adjacent to each other in the stacking direction X. Thus, the first sealing portion 41 and the separator portion 50 maintain a gap between the positive electrode current collector 22 of one current collector 12 and the negative electrode current collector 32 of the other current collector 12 of two current collectors 12 adjacent to each other in the stacking direction X and insulate them. In this way, the sealing portion 40 and the separator portion 50 suppress short circuits between the positive electrode current collector 22 and the negative electrode current collector 32.

[0065] The sealing body 15 has a sealing portion 16. The sealing portion 16 is made of resin. The sealing portion 16 is in a cylindrical shape extending in the stacking direction X. The sealing portion 16 is located at a position surrounding the sealing portion 40, the separator portion 50, and the plurality of current collectors 12 from the outside of the stacked body 10a.

[0066] The sealing portion 16 seals the internal space S between the current collectors 12 adjacent to each other in the stacking direction X. The sealing portion 16 can suppress the intrusion of moisture from the outside of the power storage device 10 into the internal space S. The sealing portion 16 can suppress the leakage of the liquid electrolyte contained in the internal space S to the outside of the power storage device 10.

[0067] <Method for manufacturing electrode and power storage device>

[0068] Next, a method for manufacturing the electrode 11 and the power storage device 10 will be described. In the following, the electrode 11 will be described, but the positive terminal electrode 36 and the negative terminal electrode 37 are also manufactured in the same manner.

[0069] like Figure 4 As shown, when manufacturing the electrode 11, a sealing member 140 is arranged on the current collector 12 having the positive electrode active material layer 23 and the negative electrode active material layer 33. Next, in the manufacturing method of the electrode 11, the sealing member 140 is welded using a pair of clamps 60 to the current collector 12 having the positive electrode active material layer 23 and the negative electrode active material layer 33 as active material layers on both sides. The sealing member 140 is welded to the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d as uncoated portions using the clamps 60. The manufactured electrode 11 has: the current collector 12 having active material layers on both sides; and the sealing member 140, which is welded to the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d as uncoated portions of the current collector 12.

[0070] The sealing member 140 is a precursor of the sealing portion 40 and the sealing portion 16. The sealing member 140 is arranged on each of the uncoated portions of the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d of the collector 12. The collector 12 is sandwiched by two sealing members 140 from both sides of the thickness direction of the collector 12. The sealing member 140 protrudes from the collector 12 to the outside of the outer edge 12e of the collector 12. That is, from the direction in which the collector 12 and the sealing member 140 are stacked, each sealing member 140 is arranged on the collector 12 in a manner having both a portion overlapping with the collector 12 and a portion not overlapping with the collector 12.

[0071] The sealing member 140 disposed on the positive electrode uncoated portion 12c is also referred to as a first sealing member 141. The first sealing member 141 is located at a position surrounding the positive electrode active material layer 23. The sealing member 140 disposed on the negative electrode uncoated portion 12d is also referred to as a second sealing member 142. The second sealing member 142 is located at a position surrounding the negative electrode active material layer 33. That is, the sealing member 140 is disposed on both surfaces of the current collector 12 in a manner surrounding the positive electrode active material layer 23 and the negative electrode active material layer 33.

[0072] The sealing member 140 includes a protrusion 140b protruding from the outer edge 12e of the current collector 12. The protrusion 140b of the first sealing member 141 and the protrusion 140b of the second sealing member 142 are separated from each other. The portion of the sealing member 140 that is arranged on the uncoated portion of the current collector 12 is called the main body 140a. The first sealing member 141 and the second sealing member 142 each include a main body 140a and a protrusion 140b. The main body 140a of the first sealing member 141 is a portion of the first sealing member 141 located on the positive electrode uncoated portion 12c. The main body 140a of the second sealing member 142 is a portion of the second sealing member 142 located on the negative electrode uncoated portion 12d. In the first sealing member 141 and the second sealing member 142, the protrusion 140b extends from the main body 140a. The protrusion 140b of the first sealing member 141 is a portion of the first sealing member 141 that is not located on the positive electrode uncoated portion 12c. The protrusion 140b of the second sealing member 142 is a portion of the second sealing member 142 that is not located on the negative electrode uncoated portion 12d.

[0073] The main body 140a of the first sealing member 141 is separated from the positive electrode active material layer 23. As a result, a part of the positive electrode uncoated portion 12c becomes a positive electrode exposed portion 17 where the positive electrode active material layer 23 and the first sealing member 141 are not arranged. The positive electrode exposed portion 17 is frame-shaped when viewed from above. When viewed from above, the positive electrode exposed portion 17 is located outside the positive electrode active material layer 23 and inside the first sealing member 141.

[0074] The main body 140a of the second sealing member 142 is separated from the negative electrode active material layer 33. As a result, a part of the negative electrode uncoated portion 12d becomes a negative electrode exposed portion 18 where the negative electrode active material layer 33 and the second sealing member 142 are not configured. The negative electrode exposed portion 18 is frame-shaped when viewed from above. When viewed from above, the negative electrode exposed portion 18 is located outside the negative electrode active material layer 33 and inside the second sealing member 142.

[0075] In the present embodiment, the positive electrode exposed portion 17 and the negative electrode exposed portion 18 are portions of the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d as uncoated portions where the active material layer and the sealing member 140 are not arranged, and are portions located between the active material layer and the sealing member 140. The positive electrode exposed portion 17 and the negative electrode exposed portion 18 of the present embodiment correspond to the exposed portions.

[0076] The portion of the positive electrode uncoated portion 12c where the sealing member 140 is arranged is referred to as a positive electrode covering portion 19. In a plan view, the positive electrode covering portion 19 is frame-shaped and is located outside the positive electrode exposed portion 17. The positive electrode uncoated portion 12c is composed of the positive electrode exposed portion 17 and the positive electrode covering portion 19. The positive electrode exposed portion 17 and the positive electrode covering portion 19 are adjacent to each other.

[0077] The portion of the negative electrode uncoated portion 12d where the sealing member 140 is arranged is referred to as a negative electrode covering portion 20. In a plan view, the negative electrode covering portion 20 is frame-shaped and is located outside the negative electrode exposed portion 18. The negative electrode uncoated portion 12d is composed of the negative electrode exposed portion 18 and the negative electrode covering portion 20. The negative electrode exposed portion 18 and the negative electrode covering portion 20 are adjacent to each other.

[0078] like Figure 3 As shown, the sealing member 140 is configured to extend along the edge 12f of the collector 12. In more detail, the sealing member 140 is configured to extend along each of the two long sides 12h and the two short sides 12g of the collector 12. The sealing member 140 includes four sealing member pieces that are respectively arranged along the four sides 12f and are separated from each other. Each sealing member piece is in the shape of a strip having a long side direction along the corresponding side 12f and a short side direction in a direction intersecting the corresponding side 12f. One sealing member piece in the first sealing member 141 and one sealing member piece in the second sealing member 142 are arranged along one side 12f.

[0079] The sealing member sheets can be configured so that the ends of the sealing member sheets in the long side direction overlap each other, or can be configured so that the ends of the sealing member sheets in the long side direction do not overlap each other. In the present embodiment, the ends of the sealing member sheets in the long side direction arranged along the long side 12h overlap each other with the ends of the sealing member sheets in the long side direction arranged along the short side 12g. In the sealing member 140 arranged on each of the first surface 12a and the second surface 12b, the sealing member sheets arranged along the long side 12h and the sealing member sheets arranged along the short side 12g are arranged in a frame shape. The negative electrode active material layer 33 is surrounded by the second sealing member 142 including the sealing member sheets arranged along the long side 12h and the sealing member sheets arranged along the short side 12g. Although in Figure 3 Although not shown in the figure, the positive electrode active material layer 23 is surrounded by a first sealing member 141 including a sealing member piece arranged along the long side 12 h and a sealing member piece arranged along the short side 12 g .

[0080] In the present embodiment, a pair of clamps 60 are used to weld the sealing member sheets arranged along the two long sides 12h of the collector 12 to both sides of the collector 12. Then, a pair of clamps 60 are used to weld the sealing member sheets arranged along the two short sides 12g of the collector 12 to both sides of the collector 12. In addition, the long side welding process of welding the sealing member sheets arranged along the two long sides 12h of the collector 12 to both sides of the collector 12 can be implemented on both sides at the same time, or one side at a time. In addition, the short side welding process of welding the sealing member sheets arranged along the two short sides 12g of the collector 12 to both sides of the collector 12 can be implemented on both sides at the same time, or one side at a time. In addition, the long side welding process and the short side welding process can be implemented first.

[0081] like Figure 4As shown, a pair of clamps 60 each include a heater portion 61 and a pressing portion 64. The heater portion 61 is, for example, a metal plate with an electric heating wire (not shown) built in. By adjusting the amount of current flowing through the electric heating wire, the heating and heating stop of the heater portion 61 can be switched. The heater portion 61 is used to heat the sealing member 140 and is deformable. The pressing portion 64 is used to press the heater portion 61 to the sealing member 140 so that the sealing member 140 is pressed to the collector 12. Hereinafter, the direction in which the pressing portion 64 presses the sealing member 140 is referred to as the pressing direction D. That is, the pressing direction D refers to a direction orthogonal to the first surface 12a and the second surface 12b, and is a direction from the clamp 60 to the sealing member 140. The pressing portion 64 includes a rubber portion 62 and a base portion 63. The rubber portion 62 is, for example, made of silicone rubber. The rubber portion 62 is located at a position overlapping with the heater portion 61 in the pressing direction D. That is, the pressing portion 64 is located at a position overlapping the heater portion 61 in the pressing direction D. Thus, the pressing portion 64 is located in parallel with the heater portion 61 and the sealing member 140 in the pressing direction D. The heater portion 61 is fixed to the rubber portion 62. The rubber portion 62 is compressibly deformable.

[0082] The base portion 63 is made of metal, for example. The rubber portion 62 is located between the base portion 63 and the heater portion 61. Thus, the rubber portion 62 insulates the base portion 63 from the heater portion 61. The rubber portion 62 suppresses heat transfer from the heater portion 61 to the base portion 63. The rubber portion 62 is fixed to the base portion 63. Thus, the heater portion 61 and the pressing portion 64 are integrated. By operating an operating device not shown in the figure, the position of the base portion 63 relative to the sealing member and the collector foil as the welding object is changed by the operator. That is, the base portion 63 is configured to be displaceable relative to the welding object. When the position of the base portion 63 relative to the welding object is changed, the heater portion 61 and the rubber portion 62 integrated with the base portion 63 will be displaced as a whole with the base portion 63.

[0083] When the sealing member 140 is welded to the collector 12, a pair of clamps 60 are respectively arranged at positions opposite to the sealing member 140 on both sides of the thickness direction of the collector 12. The thickness direction of the collector 12 coincides with the pressing direction D. Hereinafter, the heater portion 61 arranged on the side facing the first surface 12a relative to the collector 12 is also referred to as the first heater portion 61a, and the heater portion 61 arranged on the side facing the second surface 12b relative to the collector 12 is also referred to as the second heater portion 61b. The heater portion 61 is arranged at a position separated from the positive electrode active material layer 23 and the negative electrode active material layer 33 in a direction orthogonal to the pressing direction D. The first heater portion 61a is opposite to the positive electrode exposed portion 17 and the first sealing member 141, and the second heater portion 61b is opposite to the negative electrode exposed portion 18 and the second sealing member 142. The pair of jigs 60 are displaced so that their respective base portions 63 approach the facing sealing member 140 , and are displaced so as to approach each other with the sealing member 140 and the current collector 12 interposed therebetween.

[0084] like Figure 5 As shown, when the heater portion 61 moves to a predetermined position, the displacement of the base portion 63 stops, thereby stopping the displacement of the pair of clamps 60. At this time, the first heater portion 61a contacts the positive electrode exposed portion 17 and the first sealing member 141. The second heater portion 61b contacts the negative electrode exposed portion 18 and the second sealing member 142.

[0085] The first heater portion 61a is pressed against the main body 140a and the positive electrode exposed portion 17 of the first sealing member 141. In addition, the second heater portion 61b is pressed against the main body 140a and the negative electrode exposed portion 18 of the second sealing member 142. Moreover, the first heater portion 61a is pressed against a portion that is a part of the protrusion 140b of the first sealing member 141 and connected to the main body 140a. The second heater portion 61b is pressed against a portion that is a part of the protrusion 140b of the second sealing member 142 and connected to the main body 140a. The portion of the protrusion 140b of the first sealing member 141 and the second sealing member 142 that is separated from the main body 140a is not pressed by the heater portion 61. That is, in the present embodiment, the heater portion 61 is pressed against the sealing member 140 except for a part of the protrusion 140b. In addition, in the present embodiment, the pair of clamps 60 are displaced so as to approach each other, and the sealing member 140 and the current collector 12 are clamped by the pair of clamps 60, and in this state, the heater portion of each clamp is pressed against the sealing member 140 and the exposed portion. Therefore, one of the pair of clamps 60 also functions as a supporting member that receives the pressing force of the other clamp.

[0086] The first heater portion 61a abuts against the first sealing member 141 while deforming along the positive electrode exposed portion 17. The second heater portion 61b abuts against the second sealing member 142 while deforming along the negative electrode exposed portion 18. The pressing portion 64 presses the heater portion 61 against the sealing member 140. As the heater portion 61 presses the sealing member 140, the rubber portion 62 is compressed and deformed in the pressing direction D. In detail, the portion of the rubber portion 62 that overlaps with the portion of the heater portion 61 abutting against the sealing member 140 is compressed and deformed to a greater extent than the portion that overlaps with the portion of the heater portion 61 abutting against the positive electrode exposed portion 17 and the negative electrode exposed portion 18. The rubber portion 62 is compressed and deformed while the displacement of the position of the rubber portion 62 is suppressed by the base portion 63. In this way, as the heater portion 61 presses the sealing member 140, the pressing portion 64 is compressed and deformed in the pressing direction D. The pressing portion 64 pressing the first heater portion 61 a can apply uniform surface pressure to the first sealing member 141 and the positive electrode exposure portion 17 , and the pressing portion 64 pressing the second heater portion 61 b ​​can apply uniform surface pressure to the second sealing member 142 and the negative electrode exposure portion 18 .

[0087] like Figure 5 and Figure 6 As shown, the heater portion 61 is heated in a state where the heater portion 61 is in contact with the sealing member 140, the positive electrode exposed portion 17, and the negative electrode exposed portion 18. In addition, the heating of the heater portion 61 may be started before the heater portion 61 is in contact with the sealing member 140, the positive electrode exposed portion 17, and the negative electrode exposed portion 18, or after the heater portion 61 is in contact with the sealing member 140, the positive electrode exposed portion 17, and the negative electrode exposed portion 18. The first sealing member 141 and the second sealing member 142, which are the sealing member 140 disposed in the uncoated portion, and the positive electrode exposed portion 17 and the negative electrode exposed portion 18, which are the exposed portions, are pressurized and heated while the heater portion 61 is deformed in a manner following the compression deformation of the pressing portion 64 and the heater portion 61 is pressed against them. The sealing member 140 is welded to the two surfaces of the collector 12 by applying the above-mentioned pressure and heating to the uncoated portions of the sealing member 140 disposed on both sides of the collector 12 and the positive electrode exposed portion 17 and the negative electrode exposed portion 18 as the exposed portions on both sides of the collector 12 using a pair of clamps 60. The pressure and heating of the positive electrode exposed portion 17 and the negative electrode exposed portion 18 by the heater unit 61 and the pressure and heating of the sealing member 140 by the heater unit 61 are started at the same timing. Thus, the sealing member 140 is welded to the collector 12. As a result, the first sealing portion 41 welded to the collector 12 is formed.

[0088] The pair of jigs 60 heats the body 140a of each of the first sealing member 141 and the second sealing member 142 while pressing the heater portion 61 against them. Thus, the body 140a of the first sealing member 141 is welded to the positive electrode coating 19. In addition, the body 140a of the second sealing member 142 is welded to the negative electrode coating 20. The welded portion 41a is formed at the boundary between the body 140a of the first sealing member 141 and the positive electrode coating 19, and at the boundary between the body 140a of the second sealing member 142 and the negative electrode coating 20. By welding the sealing member 140 to the collector 12, the electrode 11 in which the collector 12 and the sealing member 140 are integrated is formed.

[0089] Furthermore, the fixture 60 heats the first sealing member 141 and the second sealing member 142 while pressing the heater portion 61 against the portion connected to the main body portion 140a in the protruding portion 140b. Thus, in the first sealing member 141 and the second sealing member 142, the portions of the protruding portion 140b that are pressurized and heated by the heater portion 61 are melted and connected to each other, thereby forming the second sealing portion 42. After the second sealing portion 42 is formed, the first sealing member 141 and the second sealing member 142 are integrated into one sealing member 140.

[0090] The portion of the protrusion 140b separated from the main body 140a does not melt because it is not pressed and heated by the heater 61. That is, in this embodiment, heating is performed while the heater 61 is pressed against the sealing member 140 except for a portion of the protrusion 140b.

[0091] After the welded portion 41a is formed, the welding process of the sealing member 140 to the collector 12 by the pair of clamps 60 is terminated. The welding process of the sealing member 140 to the collector 12 by the pair of clamps 60 is terminated by stopping the heating of the heater unit 61. The pressurization and heating of the positive electrode exposed portion 17 and the negative electrode exposed portion 18 by the heater unit 61 and the pressurization and heating of the sealing member 140 by the heater unit 61 are terminated at the same timing. In addition, before the welded portion 41a is completely cooled, it is preferred to maintain the sealing member 140 and the collector 12 clamped by the pair of clamps 60, and the pair of clamps 60 can also be displaced together with the heating stop of the heater unit 61 so that the heater unit 61 is separated from the sealing member 140.

[0092] As the welding process of the sealing member 140 to the current collector 12 by the pair of clamps 60 is completed, the welded portion 41a is cooled, thereby completing the welding of the sealing member 140 to the current collector 12. Such welding of the sealing member 140 to the current collector 12 is performed on the sealing member 140 arranged on all sides 12f of the current collector 12. By repeatedly welding the sealing member 140 to the current collector 12 by the pair of clamps 60, the electrode 11 in which the current collector 12 and the sealing member 140 are integrated is sequentially formed.

[0093] like Figure 7 As shown in FIG. 1 , the electrode 11a integrated with the sealing member 140, the separator 35, and the spacer unit 50 are sequentially stacked in the stacking direction X. The separator 35 is interposed between the positive electrode active material layer 23 of one electrode 11a of the two electrodes 11a adjacent to each other in the stacking direction X and the negative electrode active material layer 33 of the other electrode 11a. Thus, the stacked body 10a is formed. The spacer unit 50 is interposed between the sealing member 140 integrated with one electrode 11a of the two electrodes 11a adjacent to each other in the stacking direction X and the sealing member 140 integrated with the other electrode 11a of the two electrodes 11a.

[0094] Next, the sealing member 140 and the spacer portion 50 are welded. The sealing member 140 and the spacer portion 50 can be welded in a non-contact manner using, for example, a welding jig 70. The welding jig 70 is, for example, an infrared heater. In this case, the welding jig 70 is opposed to the sealing member 140 and the spacer portion 50 from the outside of the laminate 10a in a state separated in a direction intersecting the lamination direction X. The protruding portion 140b of the sealing member 140 and a portion of the spacer portion 50 are melted by the heat generated by the infrared rays irradiated from the welding jig 70.

[0095] like Figure 2 and Figure 7 As shown, when the spacer portion 50 and the protrusion 140b are melted by the welding jig 70, the portion of the spacer portion 50 overlapping with the protrusion 140b in the stacking direction X is welded to the protrusion 140b, thereby forming the sealing portion 16. The portion of the sealing member 140 where the sealing portion 16 is not formed corresponds to the sealing portion 40 of the power storage device 10.

[0096] [Function and Effect]

[0097] According to the above-described embodiment, the following operations and effects can be obtained.

[0098] (1) In the manufacturing method of the electrode 11 of the present embodiment, the sealing member 140 disposed in the positive electrode uncoated portion 12c of the current collector 12 and the positive electrode exposed portion 17 of the positive electrode uncoated portion 12c of the current collector 12, which is a portion where the positive electrode active material layer 23 and the sealing member 140 are not disposed, are pressurized and heated. In addition, the sealing member 140 disposed in the negative electrode uncoated portion 12d of the current collector 12 and the negative electrode exposed portion 18 of the negative electrode uncoated portion 12d of the current collector 12, which is a portion where the negative electrode active material layer 33 and the sealing member 140 are not disposed, are pressurized and heated. Specifically, while the heater portion 61 is deformed in a manner following the compression deformation of the pressing portion 64, the sealing member 140, the positive electrode uncoated portion 12c, and the negative electrode uncoated portion 12d are heated while the heater portion 61 is pressed against them. Thus, the sealing member 140 is fused to the current collector 12. Compared with the case where only the sealing member 140 is pressurized and heated without pressurizing and heating the positive electrode exposed portion 17 and the negative electrode exposed portion 18, the thermal expansion amount of the current collector 12 caused by the heat transfer from the heater portion 61 becomes larger. Therefore, the difference in the thermal expansion amount between the sealing member 140 and the current collector 12 becomes smaller, so that the difference in the shrinkage amount of the sealing member 140 and the current collector 12 caused by the cooling of the current collector 12 and the sealing member 140 can be reduced. Therefore, when the sealing member 140 is welded to the current collector 12, the generation of wrinkles in the current collector 12 caused by the difference in the shrinkage amount of the sealing member 140 and the current collector 12 can be suppressed.

[0099] (2) A pair of clamps 60 each includes a heater 61 and a pressing portion 64. A pair of clamps 60 are used to pressurize and heat the sealing member 140 of the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d, which are uncoated portions arranged on both sides of the collector 12, and the positive electrode exposed portion 17 and the negative electrode exposed portion 18, which are exposed portions on both sides of the collector 12. As a result, the sealing member 140 is fused to both sides of the collector 12. Therefore, on both sides of the first side 12a and the second side 12b of the collector 12, the heater portion 61 can be deformed in a manner that follows the compression deformation of the pressing portion 64, while the sealing member 140 and the exposed portion are heated while the heater portion 61 is pressed against the two sides. As a result, the sealing member 140 can be fused to the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d, which are uncoated portions on both sides of the collector 12, through the heater portion 61 and the pressing portion 64.

[0100] (3) The sealing member 140 includes: a main body 140a disposed on the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d of the current collector 12; and a protrusion 140b extending from the main body 140a and protruding from the outer edge 12e of the current collector 12. The heating is performed in a state where the heater unit 61 is pressed against the sealing member 140 except for a part of the protrusion 140b. Therefore, by heating in a state where the heater unit 61 is pressed against the main body 140a, the sealing member 140 can be welded to the current collector 12. Even if the entire protrusion 140b is not pressurized and heated by the heater unit 61, the sealing member 140 can be welded to the current collector 12. Therefore, compared with the case where the entire sealing member 140 is pressurized and heated by the heater unit 61, the thermal expansion amount of the sealing member 140 can be reduced. As a result, the shrinkage amount of the sealing member 140 caused by the cooling of the sealing member 140 can be reduced. Therefore, the difference in the amount of shrinkage between the sealing member 140 and the current collector 12 can be further reduced, and thus the generation of wrinkles in the current collector 12 can be further suppressed.

[0101] [Example of Change]

[0102] In addition, the above-mentioned embodiment can be implemented by the following modifications. The above-mentioned embodiment and the following modifications can be implemented in combination with each other within the range that there is no technical contradiction.

[0103] ○ If Figure 8 As shown, it is also possible to configure a sheet 65 between the heater portion 61 and the collector 12 and the sealing member 140. It is also possible that the sheet 65 is configured to be spaced apart from the heater portion 61 and spaced apart from the collector 12 and the sealing member 140 before a pair of clamps 60 clamp the sealing member 140 and the collector 12. The sheet 65 is, for example, a strip-shaped member extending in the long side direction of the sealing member sheet. It is also possible that the sheet 65 is maintained in a state where a predetermined tension is applied in the long side direction by a holding mechanism not shown. Furthermore, it is also possible that when the sealing member 140 is welded to the collector 12, the sealing member 140 is heated while the heater portion 61 is pressed against the collector 12 and the sealing member 140 through the sheet 65. Thus, it is possible to suppress the molten sealing member 140 from adhering to the heating surface of the heater portion 61. In addition, by displacing the pair of clamps 60 so that the heater portion 61 is separated from the sealing member 140 , the sheet 65 is separated from the sealing member 140 by the applied tension.

[0104] The sheet material 65 can be, for example, a material obtained by applying a fluorine resin coating having heat resistance, poor adhesion and sliding properties on the surface of a substrate sheet. In addition, the sheet material 65 can also be a material obtained by impregnating a fluorine compound such as polytetrafluoroethylene into a substrate sheet having heat resistance. The illustrated sheet material 65 is, for example, a glass cloth impregnated with a fluorine compound. The glass cloth is composed of a glass cloth having a higher thermal conductivity than the fluorine compound. Therefore, by using a sheet material 65 in which a substrate sheet is composed of glass cloth, heat transfer from the heater portion 61 to the sealing member 140 can be appropriately performed. In addition, the sheet material 65 can also be, for example, a resin sheet obtained by forming the resin containing the above-mentioned fluorine compound itself into a sheet shape.

[0105] When the sealing member 140 is arranged to extend along the side 12f of the current collector 12, the sealing member 140 may be temporarily fixed (temporarily welded) to the current collector 12 by spot welding (spot welding) using ultrasound, heat, etc. Thus, the sealing member 140 can be prevented from shifting from a predetermined position until welding using the heater portion 61 is performed.

[0106] ○ It is also possible that the sealing member 140 uses a sealing material cut from a long strip-shaped sealing substrate. In such a long strip-shaped sealing substrate, the linear expansion coefficient of the sealing substrate in the TD direction, which is the short side direction of the sealing substrate, is smaller than the linear expansion coefficient of the sealing substrate in the MD direction, which is the long side direction of the sealing substrate. Based on this, the sealing member sheet in the sealing member 140 is cut out from the sealing substrate in such a manner that the TD direction of the sealing substrate is consistent with the long side direction of the sealing member sheet. In addition, the sealing member sheet may be arranged on the collector 12 in such a manner that the long side direction of the sealing member sheet is along the edge 12f of the collector 12. In this case, compared with, for example, the case where the sealing member sheet is cut out from the sealing substrate in such a manner that the MD direction of the sealing substrate is consistent with the long side direction of the sealing member sheet, the amount of heat shrinkage of the sealing member 140 during welding to the collector 12 can be reduced.

[0107] ○ Alternatively, after the sealing member pieces arranged along the two short sides 12g are welded to the current collector 12, the sealing member pieces arranged along the two long sides 12h are welded to the current collector 12. The sealing member pieces arranged along the four sides 12f of the current collector 12 may be welded to the current collector 12 in sequence, or they may be welded to the current collector 12 at the same time.

[0108] The sealing member pieces arranged along the four sides 12f of the current collector 12 may be integrated with each other. In this case, the sealing member 140 is a frame-shaped body composed of four integrated sealing member pieces.

[0109] ○ The pressing portion 64 may also have a resin portion instead of the rubber portion 62. The resin portion in this case is formed of, for example, a fluororesin such as polytetrafluoroethylene. The resin portion may also be located between the heater portion 61 and the sealing member 140 in the pressing direction D. The resin portion as the pressing portion 64 is located in parallel with the heater portion 61 and the sealing member 140 in the pressing direction D. In this case, the sealing member 140 arranged in the positive electrode uncoated portion 12c and the negative electrode uncoated portion 12d, and the positive electrode exposed portion 17 and the negative electrode exposed portion 18 can also be heated by pressing the heater portion 61 against them while deforming the heater portion 61 in a manner that follows the compression deformation of the resin portion.

[0110] ○ The sealing portion 40 may also be provided only on any one of the first surface 12a and the second surface 12b of the current collector 12. In addition, the sealing member 140 may also be welded in a state where it is provided only on any one of the first surface 12a and the second surface 12b of the current collector 12. In this case, the pair of clamps 60 may be replaced by a first clamp having a heater portion 61 and a second clamp having a pressing portion 64 to form a clamp. For example, when the sealing portion 40 is provided on the first surface 12a, the first clamp is configured to be opposite to the sealing member 140 configured to the positive electrode uncoated portion 12c and the positive electrode exposed portion 17. The second clamp is configured so that it is opposite to the portion of the negative electrode uncoated portion 12d that overlaps with the sealing member 140 and the positive electrode exposed portion 17 configured to the positive electrode uncoated portion 12c in the pressing direction D. The pressing portion 64 in this case is located in parallel with the heater portion 61 and the sealing member 140 in the pressing direction D. In this case, the sealing member 140 disposed on the positive electrode uncoated portion 12 c and the positive electrode exposed portion 17 can also be heated while the heater portion 61 is deformed in a manner following the compression deformation of the pressing portion 64 and the heater portion 61 is pressed against the two.

[0111] ○ The sealing member 140 disposed on the positive electrode uncoated portion 12c of the current collector 12 and the sealing member 140 disposed on the negative electrode uncoated portion 12d may also be integrated with each other. The sealing member 140 in this case has, for example, a portion located along the outer edge 12e of the current collector 12. The sealing member 140 is integrated by connecting the portion of the sealing member 140 located on the positive electrode uncoated portion 12c and the portion of the sealing member 140 located on the negative electrode uncoated portion 12d by the portion located along the outer edge 12e.

[0112] ○ The start timing of the pressurization and heating of the positive electrode exposed portion 17 and the negative electrode exposed portion 18 by the heater unit 61 may be staggered from the start timing of the pressurization and heating of the sealing member 140 by the heater unit 61. In this case, the same effect as the above-mentioned embodiment can be obtained by performing the pressurization and heating of the positive electrode exposed portion 17 and the negative electrode exposed portion 18 by the heater unit 61 and the pressurization and heating of the sealing member 140 by the heater unit 61 in parallel. In addition, it is preferred that the pressurization and heating of the positive electrode exposed portion 17 and the negative electrode exposed portion 18 by the heater unit 61 and the pressurization and heating of the sealing member 140 by the heater unit 61 end at the same timing.

[0113] ○ The portion of the sealing member 140 that is heated when pressed against the heater portion 61 is at least a portion of the sealing member 140, and the range can be appropriately changed. For example, when the sealing member 140 is welded to the collector 12, the heater portion 61 may be pressed against the sealing member 140 except for the entire protrusion 140b and heated. In this case, after the sealing member 140 is welded to the collector 12, the second sealing portion 42 may not be formed.

[0114] The protruding portion 140b may be omitted from the sealing member 140. In this case, the sealing member 140 is composed of the main body portion 140a. The sealing portion 16 may be formed using a resin material different from that of the sealing member 140.

[0115] Next, technical ideas that can be grasped from the above-mentioned embodiment and modified examples are described below.

[0116] (Supplementary Note 1) The current collector is composed of a positive electrode current collector and a negative electrode current collector integrated together.

[0117] Description of Reference Numerals

[0118] D…pressing direction; 11, 11a…electrodes; 12…collector; 12a…first surface; 12b…second surface; 12e…outer edge; 23…positive electrode active material layer; 33…negative electrode active material layer; 60…clamp; 61…heater portion; 64…pressing portion; 140…sealing member; 140a…main body portion; 140b…protrusion.

Claims

1. A method for manufacturing an electrode, It is characterized in that The electrode comprises: a current collector having a first surface and a second surface opposite to the first surface; an active material layer provided on the first surface and the second surface; and a sealing member welded to the current collector. The first surface and the second surface each have a portion where the active material layer is provided and an uncoated portion where the active material layer is not provided. The manufacturing method comprises: a step of disposing the sealing member on the uncoated portion of at least one of the first surface and the second surface; as well as a welding step of welding the sealing member to the collector by heating the sealing member under pressure against the uncoated portion using a jig, The fixture has: a heater portion that is deformable and configured to heat the sealing member; and a pressing portion configured to press the heater portion against the sealing member, wherein a direction in which the pressing portion presses the sealing member is a pressing direction, The pressing portion is located in parallel with the heater portion and the sealing member in the pressing direction, and is configured to be compressed and deformed in the pressing direction as the heater portion is pressed. The step of arranging includes arranging the sealing member in the uncoated portion so that an exposed portion is formed in the uncoated portion as a portion where the sealing member is not arranged and located between the active material layer and the sealing member, The welding step includes heating the sealing member disposed in the uncoated portion and the exposed portion while the heater portion is pressed against the sealing member and the exposed portion, while deforming the heater portion so as to follow the compressive deformation of the pressing portion.

2. The method for producing an electrode according to claim 1, in, The clamps are a pair of clamps located on both sides of the current collector in the pressing direction, Each of the pair of clamps includes the heater portion and the pressing portion, The arranging step includes arranging the sealing member on the uncoated portions of the first surface and the second surface, The welding step includes applying pressure and heating the sealing member disposed at the uncoated portions of the first surface and the second surface and the exposed portions of the first surface and the second surface using the pair of jigs.

3. The method for manufacturing an electrode according to claim 1 or claim 2, in, The sealing member includes: a main body portion disposed on the uncoated portion; and a protrusion portion extending from the main body portion and protruding from an outer edge of the current collector. The welding step includes heating in a state where the heater portion is pressed against the sealing member excluding at least a portion of the protruding portion.

4. The method for manufacturing an electrode according to claim 1 or claim 2, in, The welding step includes starting pressurizing and heating the exposed portion and the sealing member by the heater portion at the same timing, and ending pressurizing and heating the exposed portion and the sealing member by the heater portion at the same timing.

Citation Information

Patent Citations

  • Power storage module and manufacturing method thereof

    JP2018106963A