AI Technical Summary
The thermal safety performance of secondary batteries decreases when the temperature rises, resulting in poor cycle performance and inability to meet high performance requirements.
An isolation film composed of organic particles and inorganic particles with a specific particle size ratio is used to form a coating on the substrate, and the overlap and extrusion between particles are used to reduce the shrinkage of the substrate, improve the electrolyte infiltration effect, and enhance thermal insulation. Safety and cycle performance.
It significantly improves the thermal safety performance and cycle performance of the secondary battery, reduces the probability of short circuit between the positive and negative electrode pieces, and improves the energy density and ion transmission characteristics.
Smart Images

Figure CN119096406A_ABST
Abstract
Description
Separator and preparation method thereof, secondary battery and electric device Technical Field
[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to an isolation membrane and a preparation method thereof, a secondary battery, and an electrical device. Background Art
[0002] In recent years, secondary batteries have been widely used in electrical devices such as power tools, electric vehicles, energy storage devices, etc. due to their good electrochemical properties and safety performance.
[0003] With the promotion and application of secondary batteries, performance requirements are becoming increasingly stringent. However, in related technologies, as the temperature of secondary batteries rises, their thermal safety performance deteriorates, and may even cause safety issues. Furthermore, the increase in temperature of secondary batteries may also reduce their cycling performance, resulting in secondary batteries failing to meet current requirements.
[0004] Summary of the Invention
[0005] The purpose of this application is to provide an isolation membrane and its preparation method, a secondary battery and an electrical device, wherein the isolation membrane has good heat resistance and good infiltration and liquid retention effects on the electrolyte, so that the secondary battery has better thermal safety and cycle performance.
[0006] In a first aspect, the present application provides an isolation film, comprising a substrate and a coating, wherein the coating is disposed on at least one side of the substrate, wherein the coating comprises first particles and second particles, wherein the first particles are organic particles, the average particle size of the first particles is denoted as D1, and the average particle size D2 of the second particles is denoted as D2, and the coating satisfies: 1 <D1 / D2≤10。
[0007] In the separator provided herein, the first particles are organic particles, and the coating satisfies the aforementioned relationship, enabling the first and second particles to alternately overlap within the coating. When the substrate contracts due to heat, the organic particles exhibit excellent heat resistance, and the organic particles, the second particles, and / or the second particles can rapidly squeeze each other, exerting a force on the substrate opposite to the direction of contraction, thereby improving the thermal safety of the secondary battery. Furthermore, the second particles filling the gaps between the first particles creates more voids in the coating, thereby enhancing the electrolyte's wetting effect on the separator, facilitating ion transport within the separator and thus improving the cycling performance of the secondary battery.
[0008] In any embodiment of the present application, the coating satisfies: 2≤D1 / D2≤8; optionally, 3≤D1 / D2≤7. Satisfying the above relationship can help the particles better overlap each other. When the substrate shrinks due to heat, the rapid contact and compression between the particles can provide a force opposite to the direction of substrate contraction, further reducing the degree of substrate contraction and enhancing the substrate's deformation resistance. This reduces the probability of short circuits between the positive and negative electrode sheets in the secondary battery, further improving its thermal safety performance.
[0009] In any embodiment of the present application, 0.02 μm ≤ D1 ≤ 3 μm, and optionally, 0.5 μm ≤ D1 ≤ 2 μm. The average particle size D1 of the first particles within the above-mentioned suitable range not only facilitates electrolyte wetting of the separator to improve the cycle performance of the secondary battery, but also facilitates the overlap between the particles. Furthermore, when the separator is heated, a force acting in the opposite direction of the heat of the separator is quickly provided, thereby reducing the degree of shrinkage of the separator when heated and improving the thermal safety performance of the secondary battery.
[0010] In any embodiment of the present application, 0.01 μm ≤ D2 ≤ 2 μm; alternatively, 0.1 μm ≤ D2 ≤ 1 μm. The average particle size D2 of the second particles within the above-mentioned suitable range not only facilitates electrolyte wetting of the separator to improve the cycle performance of the secondary battery, but also facilitates the overlapping of the particles. Furthermore, when the separator is heated, it quickly provides a force in the opposite direction of the heat of the separator, thereby reducing the degree of shrinkage of the separator when heated and improving the thermal safety performance of the secondary battery.
[0011] In any embodiment of the present application, the volume distribution particle size D of the first particles is 1 v90≤3.0μm, optional 0.1μm≤D 1 v90≤2.0μm. Volume distribution particle size D of the first particle 1 When v90 is within the above range, the stacking density can be increased while the coating layer can have a suitable thickness to improve the energy density of the secondary battery.
[0012] In any embodiment of the present application, the volume distribution particle size D of the first particles is 1 v50≤2μm, optional 0.01μm≤D 1 v50≤1.5μm. Volume distribution particle size D of the first particle 1When v50 is within the above range, it can help to enhance the close contact between the first particles and enable adjacent particles to overlap together. When the substrate shrinks due to heat, the rapid contact and extrusion between the particles can provide a force opposite to the shrinkage direction of the substrate, thereby further reducing the shrinkage degree of the substrate and enhancing the deformation resistance of the substrate, thereby reducing the probability of short circuit between the positive and negative pole pieces in the secondary battery, and further improving its thermal safety performance.
[0013] In any embodiment of the present application, the specific surface area of the first particles is greater than or equal to 3m 2 / g, optionally, 10m 2 / g-100m 2 The specific surface area of the first particles is set within the above-mentioned suitable range, which can increase the contact area between the first particles and the electrolyte, thereby helping to improve the electrolyte's wetting effect on the separator and the electrolyte retention effect.
[0014] In any embodiment of the present application, the particle size distribution (D 1 v90-D 1 v10) / D 1 v50≤1.5, optional 0.5≤(D 1 v90-D 1 v10) / D 1 v50≤1.0.
[0015] In any embodiment of the present application, the volume distribution particle size D of the second particles is 2 v90≤2μm; optional 0.3μm≤D 2 v90≤1.5μm.
[0016] In any embodiment of the present application, the volume distribution particle size D of the second particles is 2 v50≤1.5μm; optional 0.2μm≤D 2 v50≤1μm.
[0017] In any embodiment of the present application, the specific surface area of the second particles is greater than or equal to 10 m 2 The specific surface area of the second particles is set within the above-mentioned suitable range, which can increase the contact area between the second particles and the electrolyte, thereby helping to improve the electrolyte's wetting effect on the separator and the electrolyte retention effect.
[0018] In any embodiment of the present application, the particle size distribution (D 2 v90-D 2 v10) / D 2 v50≤1.0, optional 0.2≤(D 2 v90-D 2v10) / D 2 v50≤0.8.
[0019] In any embodiment of the present application, the weight proportion of the first particles in the coating is recorded as A, and the weight proportion of the second particles in the coating is recorded as B, then the coating satisfies: 1
[0020] In any embodiment of the present application, the weight proportion of the first particles in the coating is recorded as A, and the weight proportion of the second particles in the coating is recorded as B, then the coating satisfies: A ≥ 50%, optionally 70% ≤ A ≤ 90%; and / or, the coating satisfies: B ≤ 35%, optionally 5% ≤ B ≤ 25%.
[0021] In any embodiment of the present application, the first particles include one or more of silicone particles, melamine formaldehyde resin particles, phenolic resin particles, polyester particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, and polyaryletherketone particles. Optionally, the first particles include silicone particles.
[0022] In any embodiment of the present application, the first particles include organosilicon particles, the organosilicon particles include a first polymer, and the first polymer includes a first structural unit, a second structural unit, and a third structural unit;
[0023] The first structural unit has a structure as shown in formula (I):
[0024]
[0025] In formula (I), R1 includes a hydrogen atom, or one or more substituted or unsubstituted C1-C5 alkyl groups; alternatively, R1 includes a hydrogen atom, or one or more substituted or unsubstituted C1-C3 alkyl groups;
[0026] R2 includes one or more of a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C3-C20 cycloalkyl group, or a substituted or unsubstituted C1-C20 hydroxyalkyl group; alternatively, R2 includes one or more of a C1-C12 alkyl group, a C3-C12 cycloalkyl group, or a C1-C12 hydroxyalkyl group;
[0027] The second structural unit is shown in formula (II):
[0028]
[0029] In formula (II), R3 includes one or more of a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; optionally, R3 includes one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group;
[0030] The third structural unit is as shown in formula (III):
[0031]
[0032] In formula (III), R4 to R 11 each independently includes one or more of a substituted or unsubstituted C1-C10 alkyl group, or a structural unit as shown in formula (III-1), wherein at least one of R4 to R 11 is a structural unit as shown in formula (III-1),
[0033]
[0034] In formula (III-1), R 12 includes a hydrogen atom, or one or more of a substituted or unsubstituted C1-C5 alkyl group; optionally, R 12 includes a hydrogen atom, or one or more of a substituted or unsubstituted C1-C3 alkyl group;
[0035] R 13 is selected from a substituted or unsubstituted C1-C10 alkyl group; optionally, R 13 is selected from a substituted or unsubstituted C3-C10 alkyl group.
[0036] In any embodiment of the present application, based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the first structural unit is denoted as a%, 65 ≤ a ≤ 95; optionally, 70 ≤ a ≤ 85; and / or, based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the second structural unit is denoted as b%, 0 < b ≤ 15; optionally, 5 ≤ b ≤ 10; and / or, based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the third structural unit is denoted as c%, 0 < c ≤ 10; optionally, 5 ≤ c ≤ 9.
[0037] In any embodiment of the present application, based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the first structural unit is denoted as a%, the molar content of the second structural unit is denoted as b%, and the molar content of the third structural unit is denoted as c%; the organosilicon particles satisfy one or more of the conditions (1) to (3):
[0038] (1) 7 ≤ a / b ≤ 14;
[0039] (2)8≤a / c≤16;
[0040] (3)a:b:c is (13-15):(2-4):(2-4).
[0041] In any embodiment of the present application, the organosilicon particles further include a second polymer, and the second polymer includes a structural unit represented by formula (a):
[0042]
[0043] In formula (a), R 14 and R 15 Each independently comprises one or more of substituted or unsubstituted C1-C10 alkyl, hydroxyl or amino; optionally, R 14 and R 15 Each independently includes one or more of a substituted or unsubstituted C1-C6 alkyl group, a hydroxyl group or an amino group.
[0044] Optionally, the second polymer includes one or more of polymethylsiloxane, polydimethylsiloxane, polydiethylsiloxane, polymethylhydroxysiloxane, and polymethylaminosiloxane.
[0045] In any embodiment of the present application, the number average molecular weight of the organosilicon particles is 30,000-70,000, and can optionally be 40,000-50,000. When the number average molecular weight of the organosilicon particles is within this range, it is advantageous to form organosilicon particles with a smaller particle size. When applied to a separator, this allows for a thinner coating of the separator, reducing the overall thickness of the separator, thereby facilitating an increase in the energy density of the secondary battery. Furthermore, the risk of organosilicon particles clogging the separator substrate can be reduced, thereby improving the overall air permeability and other properties of the separator.
[0046] In any embodiment of the present application, based on the mass of the organosilicon particles, the moisture content of the organosilicon particles is less than or equal to 3000 μg / g; optionally, it can be 600 μg / g-2800 μg / g.
[0047] In any embodiment of the present application, the second particles include one or more of inorganic particles and polymer particles; alternatively, the second particles include inorganic particles.
[0048] In any embodiment of the present application, the inorganic particles include one or more selected from inorganic particles having a dielectric constant of 5 or higher, inorganic particles capable of transporting active ions, and inorganic particles capable of electrochemical oxidation and reduction.
[0049] In any embodiment of the present application, the polymer particles include one or more of silicone particles, melamine formaldehyde resin particles, phenolic resin particles, polyester particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles and polyaryletherketone particles.
[0050] In any embodiment of the present application, the thickness of the substrate is less than or equal to 16 μm, and can be optionally 3 μm-9 μm.
[0051] In any embodiment of the present application, the porosity of the substrate is greater than or equal to 20%, and can be optionally 25%-45%.
[0052] In any embodiment of the present application, the coating has a thickness of 0.1 μm-5 μm, optionally 0.5 μm-3 μm. The coating thickness H within the above range can help improve the close packing between particles in the coating, thereby further improving the thermal safety performance of the secondary battery.
[0053] In any embodiment of the present application, the porosity of the coating is greater than or equal to 20%, and can optionally be between 25% and 50%. When the coating contains organosilicon particles, a porosity within the above range can further enhance the electrolyte's wetting and retention of the separator, thereby facilitating ion transport within the separator and improving the cycling performance of the secondary battery.
[0054] In any embodiment of the present application, the longitudinal thermal shrinkage of the separator at 150° C. for 1 hour is less than or equal to 3%.
[0055] In any embodiment of the present application, the transverse thermal shrinkage of the separator at 150° C. for 1 hour is less than or equal to 2%.
[0056] In any embodiment of the present application, the air permeability of the isolation membrane is less than or equal to 200s / 100mL, and can be optionally 150s / 100mL-200s / 100mL.
[0057] In any embodiment of the present application, the longitudinal tensile strength of the separator is greater than or equal to 2700 kg / cm 2 .
[0058] In any embodiment of the present application, the transverse tensile strength of the separator is greater than or equal to 2500 kg / cm 2 .
[0059] In any embodiment of the present application, the wetted length of the isolation membrane is 20 mm to 100 mm, and optionally 40 mm to 70 mm.
[0060] A second aspect of the present application provides a method for preparing the isolation film of the first aspect of the present application, comprising the following steps:
[0061] providing a substrate;
[0062] mixing the first particles and the second particles in a solvent to prepare a coating slurry;
[0063] Applying the coating slurry on at least one side of the substrate to form a slurry coating layer, and drying the slurry coating layer to form a coating layer to obtain a release film;
[0064] The first particles are organic particles, the average particle size of the first particles is recorded as D1, the average particle size of the second particles is recorded as D2, and the average particle size of the first particles is recorded as D1. <D1 / D2≤10。
[0065] A third aspect of the present application provides a secondary battery, comprising the isolation membrane of the first aspect of the present application or the isolation membrane obtained by the preparation method of the second aspect of the present application.
[0066] A fourth aspect of the present application provides an electrical device comprising the secondary battery of the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0067] In order to more clearly illustrate the technical solutions of the embodiments of this application, the following briefly introduces the drawings required for use in the embodiments of this application. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0068] FIG1 is a schematic diagram of an embodiment of a secondary battery of the present application.
[0069] FIG. 2 is an exploded schematic diagram of an embodiment of the secondary battery of FIG. 1 .
[0070] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.
[0071] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.
[0072] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .
[0073] FIG6 is a schematic diagram of an embodiment of an electric device including the secondary battery of the present application as a power source.
[0074] In the accompanying drawings, the drawings are not necessarily drawn to scale.
[0075] The following are the descriptions of the reference numerals:
[0076] 1-battery pack, 2-upper box, 3-lower box, 4-battery module, 5-secondary battery, 51-housing, 52-electrode assembly, 53-cover. DETAILED DESCRIPTION
[0077] Below, the embodiments of the separator and its preparation method, secondary battery, and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided to enable those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0078] " scope " disclosed in the application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and selected lower limit and upper limit define the boundary of special scope.The scope that this mode limits can be to include end value or not include end value, and can be combined arbitrarily, and promptly any lower limit can form a scope with any upper limit combination.For example, if the scope of 60-120 and 80-110 is listed for specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected.In addition, if the minimum range value 1 and 2 listed, and if the maximum range value 3,4 and 5 listed, then the following scope can all be expected: 1-3,1-4,1-5,2-3,2-4 and 2-5.In the application, unless otherwise specified, numerical range " ab " represents the abbreviation of any real number combination between a and b, and wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0079] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0080] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0081] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0082] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0083] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0084] In this application, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance.
[0085] In this application, the terms "plurality" and "multiple" refer to two or more.
[0086] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.
[0087] Unless otherwise stated, the numerical values of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in the embodiments of this application.
[0088] Secondary batteries are widely used in electrical devices such as power tools, electric vehicles, energy storage devices, etc. due to their good electrochemical properties and safety performance.
[0089] With the promotion and application of secondary batteries, the performance requirements for them are becoming increasingly higher. Among them, the thermal safety performance and cycle performance of secondary batteries have become two focuses of attention. Generally speaking, a secondary battery includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is placed between the positive and negative electrode sheets, mainly preventing short circuits between the positive and negative electrodes, while allowing active ions to pass freely to form a circuit. Therefore, it can be seen that the separator is a key component to improve its thermal safety performance and cycle performance.
[0090] Currently, separators are typically made of polyolefin films, which experience significant thermal shrinkage when heated. This can cause short circuits between the positive and negative electrodes in secondary batteries, impacting the thermal safety and cycling performance of the secondary battery. Therefore, there is an urgent need to improve the thermal safety and cycling performance of secondary batteries.
[0091] In view of this, the present application provides an isolation membrane and its preparation method, a secondary battery and an electrical device. The isolation membrane has good heat resistance and good infiltration and liquid retention effects on the electrolyte, so that the secondary battery has good thermal safety performance and cycle performance.
[0092] Isolation film
[0093] In a first aspect, an embodiment of the present application provides an isolation film, comprising a substrate and a coating, wherein the coating is disposed on at least one side of the substrate, wherein the coating comprises first particles and second particles, the first particles being organic particles, the average particle size of the first particles being denoted as D1, and the average particle size D2 of the second particles being denoted as D2, and the coating satisfies: 1 <D1 / D2≤10。
[0094] In the separator provided herein, the first particles are organic particles, and the coating satisfies the aforementioned relationship, enabling the first and second particles to alternately overlap within the coating. When the substrate contracts due to heat, the organic particles exhibit excellent heat resistance, and the organic particles, the second particles, and / or the second particles can rapidly squeeze each other, exerting a force on the substrate opposite to the direction of contraction, thereby improving the thermal safety of the secondary battery. Furthermore, the second particles filling the gaps between the first particles creates more voids in the coating, thereby enhancing the electrolyte's wetting effect on the separator, facilitating ion transport within the separator and thus improving the cycling performance of the secondary battery.
[0095] In this application, the average particle size of a material has a well-known meaning in the art and can be measured using instruments and methods known in the art. For example, an image of the material or separator can be obtained by measuring the image using a scanning electron microscope, a transmission electron microscope, or a particle size distribution instrument. Multiple (e.g., 100 or more) test particles (e.g., the first particles and the second particles of this application) can be randomly selected from the image, and the average value of the shortest diagonal length of the particles can be calculated as the average particle size.
[0096] In some embodiments of the present application, the coating satisfies the relationship: 2≤D1 / D2≤8, optionally, 3≤D1 / D2≤7. The average particle size D1 of the first particles and the average particle size of the second particles satisfying the aforementioned relationship can facilitate better overlap between the particles. Consequently, when the substrate shrinks due to heat, the rapid contact and compression between the particles can provide a force opposite to the direction of substrate shrinkage, further reducing the degree of substrate shrinkage and enhancing the substrate's resistance to deformation, thereby reducing the probability of short circuits between the positive and negative electrode sheets in the secondary battery and further improving its thermal safety performance.
[0097] In some embodiments of the present application, the average particle size D1 of the first particles is 0.02μm-3.0μm, optionally 0.5μm-2μm. The average particle size D1 of the first particles is within the above-mentioned suitable range. While helping the electrolyte to infiltrate the isolation membrane to improve the cycle performance of the secondary battery, it can also help the overlap between the particles, and then when the isolation membrane is heated, it quickly provides a force in the opposite direction of the heating of the isolation membrane, thereby reducing the degree of shrinkage of the isolation membrane when heated to improve the thermal safety performance of the secondary battery. Exemplarily, the average particle size D1 of the first particles can also be, but is not limited to, 0.04μm-2.5μm, 0.1μm-2.3μm, 0.5μm-2μm, 0.8μm-1.8μm, 1.0μm-1.5μm, 1.2μm-1.4μm.
[0098] In some specific examples, the average particle size D1 of the first particles may be, but is not limited to, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.80 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1.0 μm, 1.05 μm, 1.1 μm, 1.15 μm, 1.2 μm, 1 .25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm, 1.55μm, 1.60μm, 1.65μm , 1.7μm, 1.75μm, 1.8μm, 1.85μm, 1.9μm, 1.95μm, 2.0μm, 2.05μm, 2.1μm, 2.15μm, 2.2μm, 2.25μm, 2.3μm, 2.35μm, 2.4μm, 2.45μm, 2.5μm, 2.55μm , 2.6μm, 2.65μm, 2.7μm, 2.75μm, 2.8μm, 2.85μm, 2.9μm, 2.95μm, 3.0μm.
[0099] In some embodiments of the present application, the volume distribution particle size D of the first particles is 1 v90≤3.0μm, optional 0.1μm≤D 1 v90≤2.0μm. Volume distribution particle size D of the first particle 1 When v90 is within the above range, the stacking density can be increased while the coating layer can have a suitable thickness to improve the energy density of the secondary battery.
[0100] In some specific examples, the volume distribution particle size D1v90 of the first particles can be, but is not limited to, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.80 μm, 0.85 μm, 0.9 μm, 0.95 μm, 1.0 μm, 1.05 μm, 1.1 μm, 1.15 μm, 1 .2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm, 1.55μm, 1.60μm, 1. 65μm, 1.7μm, 1.75μm, 1.8μm, 1.85μm, 1.9μm, 1.95μm, 2.0μm, 2.05μm, 2.1 μm, 2.15μm, 2.2μm, 2.25μm, 2.3μm, 2.35μm, 2.4μm, 2.45μm, 2.5μm, 2.55μm m, 2.6μm, 2.65μm, 2.7μm, 2.75μm, 2.8μm, 2.85μm, 2.9μm, 2.95μm, 3.0μm.
[0101] In any embodiment of the present application, the volume distribution particle size D of the first particles is 1 v50≤2μm, optional 0.01μm≤D 1 v50≤1.5μm. Volume distribution particle size D of the first particle 1 When v50 is within the above range, it can help to enhance the close contact between the first particles and enable adjacent particles to overlap together. When the substrate shrinks due to heat, the rapid contact and extrusion between the particles can provide a force opposite to the shrinkage direction of the substrate, thereby further reducing the shrinkage degree of the substrate and enhancing the deformation resistance of the substrate, thereby reducing the probability of short circuit between the positive and negative pole pieces in the secondary battery, and further improving its thermal safety performance.
[0102] In some examples, the volume distribution particle size D of the first particles is 1v50 can be, but is not limited to, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55μm, 0.6μm, 0.65μm, 0.7μm, 0.75μm, 0.80μm, 0.85μm, 0.9μm, 0.95μm, 1.0μm , 1.05μm, 1.1μm, 1.15μm, 1.2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm.
[0103] In some embodiments of the present application, the particle size distribution (D 1 v90-D 1 v10) / D 1 v50≤1.5, optional 0.5≤D 1 v90-D 1 v10) / D 1 v50≤1.0. When the particle size distribution of the first particles falls within the above range, the first particles have a relatively uniform particle size distribution, which facilitates uniform dispersion of the first particles in the coating, forming a coating with relatively uniform thickness. Furthermore, when the coating slurry is applied to the surface of the substrate, the risk of the first particles falling into the gaps in the substrate is reduced, thereby ensuring the air permeability of the substrate. Because the first particles are primarily distributed in the coating, the overall heat resistance of the coating is maintained.
[0104] For example, (D 1 v90-D 1 v10) / D 1 v50 can be 0.05, 0.1, 0.15, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a range consisting of any two of the above values.
[0105] In this application, the volume distribution particle size Dv90 of a material is generally known in the art and represents the particle size corresponding to 90% of the cumulative volume distribution percentage of the material. This can be measured using instruments and methods known in the art. For example, the particle size distribution can be measured using a laser particle size analyzer (e.g., Master Size 3000) in accordance with GB / T 19077-2016, Laser Diffraction Method.
[0106] In this application, the volume distribution particle size Dv50 of a material is generally known in the art and represents the particle size corresponding to 50% of the cumulative volume distribution percentage of the material. This can be measured using instruments and methods known in the art. For example, the particle size distribution can be measured using a laser particle size analyzer (e.g., Master Size 3000) in accordance with GB / T 19077-2016, Laser Diffraction Method.
[0107] In this application, the volume distribution particle size Dv10 of a material has a well-known meaning in the art, representing the particle size corresponding to 10% of the cumulative volume distribution percentage of the material. It can be measured using instruments and methods known in the art. For example, it can be measured using a laser particle size analyzer (e.g., Master Size 3000) in accordance with GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method.
[0108] In some embodiments of the present application, the specific surface area of the first particles is greater than or equal to 3 m 2 / g, optionally, 10m 2 / g-100m 2 Setting the surface area of the first particles within the above-mentioned suitable range can increase the contact area between the first particles and the electrolyte, thereby helping to improve the electrolyte's wetting effect on the separator and the electrolyte retention effect.
[0109] In some examples, the specific surface area of the first particles may be, but is not limited to, 3 m 2 / g, 3.5m 2 / g、4m 2 / g, 4.5m 2 / g、5m 2 / g, 5.5m 2 / g、6m 2 / g, 6.5m 2 / g、7m 2 / g, 7.5m 2 / g、8m 2 / g、8.5m 2 / g、9m 2 / g, 9.5m 2 / g、10m 2 / g, 10.5m 2 / g、11m 2 / g, 11.5m 2 / g、12m 2 / g, 12.5m 2 / g、13m 2 / g, 13.5m 2 / g、14m 2 / g, 14.5m 2 / g、15m2 / g、15.5m 2 / g、16m 2 / g、16.5m 2 / g、17m 2 / g、17.5m 2 / g、18m 2 / g、19m 2 / g、20m 2 / g、21m 2 / g、22m 2 / g、23m 2 / g、24m 2 / g、25m 2 / g、26m 2 / g、27m 2 / g、28m 2 / g、29m 2 / g、30m 2 / g、31m 2 / g、32m 2 / g、33m 2 / g、34m 2 / g、35m 2 / g、36m 2 / g、37m 2 / g、38m 2 / g、39m 2 / g、40m 2 / g、41m 2 / g、42m 2 / g、43m 2 / g、44m 2 / g、45m 2 / g、46m 2 / g、47m 2 / g、48m 2 / g、49m 2 / g、50m 2 / g、55m 2 / g、60m 2 / g、65m 2 / g、70m 2 / g、75m 2 / g、80m 2 / g、85m 2 / g、90m 2 / g、95m 2 / g、100m 2 / g。
[0110] In an embodiment of the present application, the weight of the first particles and the weight of the second particles in the coating satisfy a suitable ratio relationship, which not only helps to reduce the shrinkage of the isolation membrane to improve the thermal safety performance of the secondary battery, but also enables the first particles to be better overlapped to form more pores, further improving the wetting effect of the electrolyte to improve the cycle performance of the secondary battery.
[0111] In some embodiments of the present application, the weight proportion of the first particles in the coating is recorded as A, and the weight proportion of the second particles in the coating is recorded as B, then the coating satisfies: 1
[0112] In some embodiments of the present application, the weight proportion of the first particles in the coating is recorded as A, and the weight proportion of the second particles in the coating is recorded as B, then the coating satisfies: 50% ≤ A, optionally 70% ≤ A ≤ 90%; and / or, the coating satisfies: B ≤ 35%, optionally 15% ≤ B ≤ 25%.
[0113] In some embodiments of the present application, the first particles include at least one of one or more of silicone particles, melamine formaldehyde resin particles, phenolic resin particles, polyester particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles and polyaryletherketone particles.
[0114] In some embodiments of the present application, the first particles include organosilicon particles. The organosilicon particles refer to organosilicon particles whose main chain is a silicon-oxygen-silicon bond (-Si-O-Si-). Since the silicon-oxygen-silicon bond is an inorganic bond, the bond energy is large, which can give the organosilicon very high heat resistance and chemical stability. For example, the organosilicon can be used for a long time below 200°C. The side chain of the organosilicon may not be grafted with other groups, or it may be grafted with organic groups. When the organic groups are grafted, the organosilicon can be given good dispersibility, etc., which can improve the coating performance of the organosilicon coating and the affinity with the substrate. The organosilicon particles are dispersed in the coating so that the isolation membrane has good heat resistance, thereby improving the thermal safety performance of the secondary battery. In addition, a structure with gaps can be formed between the organosilicon particles, which can enhance the wetting and retention properties of the isolation membrane for the electrolyte, thereby promoting the transmission of active ions in the isolation membrane, so that the isolation membrane can improve the cycle performance of the secondary battery when applied to the secondary battery.
[0115] In some embodiments of the present application, the first particles include organosilicon particles, the organosilicon particles include a first polymer, and the first polymer includes a first structural unit, a second structural unit, and a third structural unit.
[0116] The first structural unit has a structure as shown in formula (I):
[0117]
[0118] In formula (I), R1 includes a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; alternatively, R1 is selected from one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group;
[0119] R2 includes substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 hydroxyalkyl; alternatively, R2 is selected from one or more of C1-C12 alkyl, C3-C12 cycloalkyl, and C1-C12 hydroxyalkyl;
[0120] The second structural unit is shown in formula (II):
[0121]
[0122] In formula (II), R3 includes a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; alternatively, R3 is selected from one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group;
[0123] The third structural unit is shown in formula (III):
[0124]
[0125] In formula (III), R4 to R 11 It includes one or more independently selected from substituted or unsubstituted C1-C10 alkyl groups, or structural units as shown in formula (III-1), wherein R4 to R 11 At least one of them is a structural unit represented by formula (III-1),
[0126]
[0127] In formula (III-1), R 12 Including hydrogen atoms, or substituted or unsubstituted C1-C5 alkyl; Optionally, R 12 is selected from one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group; R 13 is selected from substituted or unsubstituted C1-C10 alkyl; optionally, R 13 is selected from substituted or unsubstituted C3-C10 alkyl groups.
[0128] In the above embodiments, the flexible monomer segment in the molecular segment of the first structural unit can adjust the glass transition temperature of the first polymer and improve the toughness and peel strength of the first polymer, thereby contributing to good bonding performance. The second structural unit can produce excellent anti-swelling and high bonding properties, and also help to improve the ion conductivity of the secondary battery. The polysilsesquioxane in the third structural unit can improve the heat resistance of the first polymer. In addition, the first structural unit and the third structural unit can work together to play a synergistic role in improving the bonding and heat resistance of the first polymer; the first structural unit and the second structural unit can work together to play a synergistic role in improving the thermal stability and anti-swelling properties of the first polymer. Therefore, the first polymer can further enhance the heat resistance of the isolation membrane, thereby further improving the thermal safety performance of the secondary battery.
[0129] In some embodiments of the present application, based on the total molar amount of the first structural unit, the second structural unit and the third structural unit, the molar content of the first structural unit is recorded as a%, 65≤a≤95. When the molar content of the first structural unit is within the above range, the adhesion of the first polymer can be improved. When the first polymer is applied to the isolation membrane, the bonding force between the first polymer and the substrate of the isolation membrane can be significantly improved. Optionally, 70≤a≤90. For example, the molar content of the first structural unit can be 65%, 70%, 75%, 80%, 85%, 90% or a range consisting of any two of the above values.
[0130] In some embodiments of the present application, based on the total molar amount of the first structural unit, the second structural unit and the third structural unit, the molar content of the second structural unit is recorded as b%, 0<b≤15. When the molar content of the second structural unit is within the above range, the thermal stability of the first polymer can be significantly improved. Optionally, 5≤b≤10. Exemplarily, the molar content of the second structural unit can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or a range consisting of any two of the above values.
[0131] In some embodiments of the present application, the molar content of the third structural unit is expressed as c%, based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, where 0 < c ≤ 10. When the molar content of the third structural unit is within the above range, the heat resistance of the first polymer can be further improved. Alternatively, 5 ≤ c ≤ 9. For example, the molar content of the third structural unit can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or a range consisting of any two of the above values.
[0132] The cyano groups in the first and second structural units can synergistically improve the first polymer's anti-swelling and adhesion properties, thereby enhancing the coating's adhesion to the substrate and its deformation resistance, thereby improving the thermal stability of the separator. Therefore, when the molar content a of the first structural unit and the molar content b of the second structural unit further satisfy 7 ≤ a / b ≤ 14, the first structural unit and the second structural unit can further fully exert their synergistic effect, improving the adhesion, stability, and anti-swelling properties of the first polymer. For example, a / b can be 7, 8, 9, 10, 11, 12, 13, 14, or a range consisting of any two of these values.
[0133] The polysilsesquioxane in the third structural unit of the secondary battery can synergize with the first structural unit to improve the heat resistance and bonding properties of the first polymer as a whole, thereby enhancing the heat resistance of the separator and thus improving the thermal safety of the secondary battery. Therefore, when the molar content a of the first structural unit and the molar content b of the second structural unit further satisfy 8≤a / c≤16, the first structural unit can further fully exert the synergistic effect with the third structural unit, improving the bonding and heat resistance of the first polymer. For example, a / c can be 8, 9, 10, 11, 12, 13, 14, 15, 16, or a range consisting of any two of the above values.
[0134] In some embodiments of the present application, the degree of polymerization a of the first structural unit, the degree of polymerization b of the second structural unit, and the degree of polymerization c of the third structural unit satisfy the following ratio: a:b:c = (13-15): (2-4): (2-4). When the degrees of polymerization of the first structural unit, the second structural unit, and the third structural unit satisfy the above ratio, the three structural units can synergize with each other to jointly improve the adhesion, anti-swelling, and heat resistance of the polymer.
[0135] The first structural unit includes a variety of chemical structures, and the specific chemical structure of the first structural unit is described below.
[0136] In some embodiments of the present application, R1 is selected from a hydrogen atom and / or a methyl group.
[0137] In some embodiments of the present application, R2 includes one or more of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-octyl, isooctyl, 2-ethylhexyl, dodecyl or isobornyl.
[0138] Illustratively, the first structural unit includes one or more of the structures represented by formula (I-1) to formula (I-8):
[0139]
[0140]
[0141] The second structural unit includes a variety of chemical structures, and the specific chemical structure of the second structural unit is described below.
[0142] In some embodiments of the present application, R3 includes one or more of a hydrogen atom or a methyl group.
[0143] Illustratively, the second structural unit includes one or more of the structures represented by formula (II-1) to the structures represented by formula (II-4):
[0144]
[0145] The third structural unit includes a variety of chemical structures, and the specific chemical structure of the third structural unit is described below.
[0146] In some embodiments of the present application, R4 to R 11 Each independently selected from the structural unit shown in formula (III-1); optionally, R 12 including one or more of a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group or an n-pentyl group; and / or, R 13 The alkyl radicals include one or more of n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-octyl, isooctyl and 2-ethylhexyl.
[0147] In some embodiments, R4 to R 11 One of them is selected from the structural unit shown in formula (III-1); optionally, R 12 including hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl or n-pentyl; and / or R 13 One or more selected from n-propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, n-pentyl, n-octyl, isooctyl or 2-ethylhexyl.
[0148] In the present application, the group types in the first polymer can be measured using infrared spectroscopy. For example, the infrared spectrum of the material can be tested to determine the characteristic peaks contained therein, thereby determining the type of the modified group. Specifically, the material can be subjected to infrared spectroscopy analysis using instruments and methods well known in the art, for example, using an infrared spectrometer (such as the IS10 Fourier transform infrared spectrometer of Nicolet, USA), and tested according to GB / T 6040-2019 General Rules for Infrared Spectroscopy Analysis Methods.
[0149] In some embodiments of the present application, the first polymer has an infrared spectrum at 1750 cm -1 to 1735cm -1, which indicates the presence of ester groups.
[0150] In some embodiments of the present application, the first polymer has a wavelength of 2260 cm in the infrared spectrum. -1 to 2220cm -1 , which indicates the presence of a cyano group.
[0151] In some embodiments of the present application, the first polymer has an infrared spectrum of 1100 nm. -1 to 1120cm -1 The characteristic peaks of silsesquioxane are shown in FIG1 , which indicates the presence of the Si-O-Si skeleton of silsesquioxane.
[0152] In some embodiments of the present application, the first polymer can be prepared by the following method, which includes:
[0153] Step S100, providing a first monomer, a second monomer and a third monomer;
[0154] In step S200 , a first monomer, a second monomer, and a third monomer are mixed and polymerized under the action of an initiator to generate a first polymer.
[0155] In the present application, the first monomer, the second monomer and the third monomer are mixed and copolymerized, and the formed first polymer is a copolymer of the three monomers.
[0156] The first monomer has a structure represented by formula (IV),
[0157]
[0158] In formula (IV), R1 includes a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; alternatively, R1 is selected from one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group;
[0159] R2 includes substituted or unsubstituted C1-C20 alkyl, substituted or unsubstituted C3-C20 cycloalkyl, substituted or unsubstituted C1-C20 hydroxyalkyl; alternatively, R2 is selected from one or more of C1-C12 alkyl, C3-C12 cycloalkyl, and C1-C12 hydroxyalkyl.
[0160] The first monomer is an acrylic acid ester compound, and when it is polymerized, the carbon-carbon double bond opens to form a first structural unit.
[0161] Illustratively, the first monomer includes one or more of methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, n-pentyl acrylate, n-octyl acrylate, isooctyl acrylate, 2-ethylhexyl acrylate, cyclohexyl acrylate, lauryl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, isobornyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, and 2-hydroxypropyl methacrylate.
[0162] The second monomer has a structure represented by formula (V),
[0163]
[0164] In formula (V), R3 includes a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; alternatively, R3 is selected from one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group.
[0165] The second monomer is an acrylonitrile compound, and when it is polymerized, the carbon-carbon double bond opens to form a second structural unit.
[0166] Illustratively, the second monomer includes acrylonitrile and / or methacrylonitrile.
[0167] The third monomer has a structure shown in formula (VI),
[0168]
[0169] In formula (VI), R 30 to R 37 It includes one or more independently selected from substituted or unsubstituted C1-C10 alkyl groups, or structural units as shown in formula (VI-1), wherein R 30 to R 37 At least one of them is a structural unit represented by formula (VI-1),
[0170]
[0171] In formula (VI-1), R 12 Including hydrogen atoms, or substituted or unsubstituted C1-C5 alkyl; Optionally, R 12 One or more selected from a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group;
[0172] R 13 is selected from substituted or unsubstituted C1-C10 alkyl; optionally, R13is selected from substituted or unsubstituted C3-C10 alkyl groups.
[0173] Illustratively, the third monomer includes one or more of methacryloxypropyl cage polysilsesquioxane, methacryloxypropyl heptaisobutyl polysilsesquioxane, methacryloxypropyl heptaoctyl polysilsesquioxane, acryloxypropyl cage polysilsesquioxane, acryloxypropyl heptaisobutyl polysilsesquioxane, and methacryloxypropyl heptaoctyl polysilsesquioxane.
[0174] In some embodiments of the present application, step S200 specifically includes:
[0175] Step S210, adding a first monomer, a second monomer, and a third monomer into a solvent and an emulsifier and mixing them to form a mixed system;
[0176] In step S220 , an initiator is added to the mixed system, and a polymerization reaction occurs under the action of the initiator to generate a first polymer.
[0177] The present application can copolymerize multiple monomers by emulsion polymerization, which is a simpler polymerization method. Of course, the present application can also adopt other polymerization methods, such as solution polymerization, suspension polymerization, etc. The process parameters used in the polymerization process can be selected from commonly used parameters in the field and will not be repeated here.
[0178] In some embodiments of the present application, the emulsifier includes one or more of sodium lauryl sulfate, sodium dodecylbenzene sulfonate, alkyl diphenyl oxide disulfonate, and ethoxylated alkylphenol ammonium sulfate.
[0179] In some embodiments of the present application, the ratio of the mass percentage of the emulsifier to the mass percentage of the first monomer, the second monomer, and the third monomer, based on the total mass of the mixed system, is 0.1% to 5%, i.e., the amount of the emulsifier used is 0.1% to 5% of the mass of the three monomers. When the mass percentage of the emulsifier is within the above range, the first monomer, the second monomer, and the third monomer can be emulsified and dispersed in the solvent to form a relatively uniform system.
[0180] In some embodiments of the present application, the initiator includes potassium persulfate and / or ammonium persulfate.
[0181] In some embodiments of the present application, the ratio of the mass percentage of the initiator to the mass percentage of the second monomer, the third monomer, and the third monomer, based on the total mass of the mixed system, is 0.15% to 1%. That is, the amount of the initiator used is 0.1% to 5% of the mass of the three monomers. When the mass percentage of the initiator is within this range, sufficient polymerization can be ensured.
[0182] In some embodiments of the present application, the solvent may include water such as deionized water.
[0183] As a specific embodiment, the method includes:
[0184] Preparation of prepolymer: deionized water, emulsifier, first polymerizable monomer, second polymerizable monomer and third polymerizable monomer are mixed and stirred uniformly to obtain a prepolymer;
[0185] Preparation of the first polymer: Add an emulsifier and deionized water to a container, stir and emulsify for 30 to 60 minutes to obtain a uniform and stable emulsion; then slowly dropwise add the prepolymer prepared in the previous step and the initiator solution (the initiator potassium persulfate and / or ammonium persulfate is dissolved in deionized water to form a solution), after the dropwise addition is completed, heat to 90° C. to 110° C. and keep warm for 0.5 hours, cool to 40° C., adjust the pH to 7 to 8 with ammonia water, filter, discharge, and dry to obtain a polymer.
[0186] In some embodiments of the present application, the second particles include organosilicon particles, which further include a second polymer, and the second polymer includes a structural unit represented by formula (a):
[0187]
[0188] In formula (a), R 14 and R 15 Each independently comprises one or more of a substituted or unsubstituted C1-C10 alkyl group, a hydroxyl group or an amino group. 14 and R 15 Each independently includes one or more of a substituted or unsubstituted C1-C6 alkyl group, a hydroxyl group or an amino group.
[0189] In some embodiments of the present application, the second polymer includes one or more of polymethylsiloxane, polydimethylsiloxane, polydiethylsiloxane, polymethylhydroxysiloxane, and polymethylaminosiloxane.
[0190] Illustratively, the organosilicon particles include at least one of the structures represented by formula (a-1) to the structures represented by formula (a-5):
[0191]
[0192]
[0193] The first polymer and the second polymer in this application are only used to distinguish the types of materials and have no limiting effect on the order and quantity.
[0194] In some embodiments of the present application, the number average molecular weight of the organosilicon particles is 30,000-70,000, optionally 40,000-50,000. For example, the number average molecular weight of the organosilicon particles can be 30,000, 35,000, 40,000, 45,000, 50,000, 55,000, 60,000, 65,000, 70,000, or a range consisting of any two of the above values. When the number average molecular weight of the organosilicon particles is within the above range, on the one hand, it can have a relatively high viscosity, which is beneficial for improving the adhesion between the separator and the positive and negative electrode sheets when the organosilicon particles are applied to the separator. On the other hand, it is beneficial to form organosilicon particles with a smaller particle size. When applied to the separator, it can achieve a thin coating of the coating in the separator, reduce the overall thickness of the separator, and thus facilitate the improvement of the energy density of the secondary battery; and the particle size of the organosilicon particles formed by the organosilicon particles will not be too small, which can reduce the risk of the organosilicon particles clogging the substrate in the separator and improve the overall air permeability and other properties of the separator.
[0195] In the present application, the number average molecular weight of the first polymer can be measured by gel permeation chromatography (GPC). Specifically, the measurement is performed using a GPC1515 instrument from Waters, USA. The sample is dissolved in tetrahydrofuran for more than 12 hours at a concentration of 4 mg / mL. The sample is filtered and prepared. The test temperature is 25°C and the test flow rate is 1 ml / min.
[0196] The inventors further discovered that during the long-term charge and discharge process of the secondary battery, the moisture in the isolation membrane will gradually be released and enter the electrolyte, and the electrolyte is highly sensitive to moisture and easily produces hydrofluoric acid HF when it comes into contact with water, thereby increasing the acidity of the electrolyte, causing corrosion of active materials and current collectors, etc., and may cause the dissolution of transition metal ions in the active materials, thereby affecting the electrochemical performance of the secondary battery. Therefore, the present application regulates the moisture content of the organosilicon particles to be less than or equal to 3000μg / g, and can be optionally 600μg / g-2800μg / g, based on the mass of the organosilicon particles. When the moisture content of the organosilicon particles is within the above range, the moisture content contained therein is relatively small, which can reduce the risk of side reactions in the electrolyte during the long-term charge and discharge cycle of the secondary battery, thereby improving the electrochemical performance of the secondary battery. Illustratively, the moisture content of the organosilicon particles may be 600 μg / g, 800 μg / g, 1000 μg / g, 1200 μg / g, 1500 μg / g, 1800 μg / g, 2000 μg / g, 2500 μg / g, 2800 μg / g, or a range consisting of any two of the foregoing values.
[0197] In the present application, the moisture content of the organosilicon particles can be measured by a moisture meter, the testing method can adopt the Karl Fischer moisture determination method, and the testing instrument can adopt the Swiss Metrohm 831 Karl Fischer moisture meter.
[0198] In some embodiments of the present application, the average particle size D2 of the second particles is 0.01 μm-2 μm, and can be 0.1 μm ≤ D2 ≤ 1 μm. The average particle size D2 of the second particles within the above-mentioned suitable range not only helps the electrolyte to infiltrate the separator to improve the cycle performance of the secondary battery, but also facilitates the overlap between the particles. When the separator is heated, it quickly provides a force in the opposite direction of the heat of the separator, thereby reducing the degree of shrinkage of the separator when heated, thereby improving the thermal safety performance of the secondary battery.
[0199] In some examples, the average particle size D2 of the second particles may be, but is not limited to, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.80μm, 0.85μm, 0.9μm, 0.95μm, 1.0μm, 1.05μm, 1.1μm, 1.15μm, 1.2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm, 1.55μm, 1.60μm, 1.65μm, 1.7μm, 1.75μm, 1.8μm, 1.85μm, 1.9μm, 1.95μm, 2.0μm or a range consisting of any two of the above values.
[0200] In some embodiments of the present application, the volume distribution particle size D of the second particles is 2 v90≤2μm; optional 0.3μm≤D 2 v90≤1.5μm. Volume distribution particle size D of the second particle 2 When v90 is within the above range, it can be filled between the organic silicone particles to enhance the contact between the particles.
[0201] In some examples, the volume distribution particle size D of the second particles is 2v90 can be, but is not limited to, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.15 μm, 0.2 μm, 0.25 μm, 0.3 μm, 0.35 μm, 0.4 μm, 0.45 μm, 0.5 μm, 0.55 μm, 0.6 μm, 0.65 μm, 0.7 μm, 0.75 μm, 0.80 μm, 0.85μm, 0.9μm, 0.95μm, 1.0μm, 1.05μm, 1.1μm, 1.15μm, 1.2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm, 1.55μm, 1.60μm, 1.65μm, 1.7μm, 1.75μm, 1.8μm, 1.85μm, 1.9μm, 1.95μm, 2.0μm or a range consisting of any two of the above values.
[0202] In some embodiments of the present application, the volume distribution particle size D of the second particles is 2 v50≤1.5μm; optional 0.2μm≤D 2 v50≤1μm. Volume distribution particle size D of the second particle 2 When v50 is within the above range, it can help to enhance the close contact between the silicone particles and enable adjacent particles to overlap together. When the substrate shrinks due to heat, the rapid contact and extrusion between the particles can provide a force opposite to the shrinkage direction of the substrate, thereby further reducing the degree of shrinkage of the substrate and enhancing the deformation resistance of the substrate, thereby reducing the probability of short circuit between the positive and negative electrodes in the secondary battery and further improving its thermal safety performance.
[0203] In some examples, the volume distribution particle size D of the second particles is 2 v50 can be, but is not limited to, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.15 μm, 0.2μm, 0.25μm, 0.3μm, 0.35μm, 0.4μm, 0.45μm, 0.5μm, 0.55μm, 0.6μm, 0.65μm, 0.7μm, 0.75μm, 0.80μm, 0.85μm, 0.9μm, 0.95μm, 1.0μm, 1.05μm, 1.1μm, 1.15μm, 1.2μm, 1.25μm, 1.3μm, 1.35μm, 1.4μm, 1.45μm, 1.5μm or a range consisting of any two of the above values.
[0204] In some embodiments of the present application, the specific surface area of the second particles is greater than or equal to 10 m 2 The specific surface area of the second particles is set within the above-mentioned suitable range, which can increase the contact area between the second particles and the electrolyte, thereby helping to improve the electrolyte's wetting effect on the separator and the electrolyte retention effect.
[0205] In some embodiments of the present application, the particle size distribution (D 2 v90-D 2 v10) / D 2 v50≤1.0, optional 0.2≤(D 2 v90-D 2 v10) / D 2 v50≤0.8. The particle size distribution of the second particles within the above range can further facilitate the overlap between the particles in the coating, allowing the particles to quickly contact and squeeze each other when the substrate shrinks due to heat, generating a force opposite to the direction of substrate shrinkage, thereby reducing the degree of substrate shrinkage and improving the heat resistance of the separator.
[0206] In some examples, the specific surface area of the second particles may be, but is not limited to, 10 m 2 / g, 10.5m 2 / g、11m 2 / g, 11.5m 2 / g、12m 2 / g, 12.5m 2 / g、13m 2 / g, 13.5m 2 / g、14m 2 / g, 14.5m 2 / g、15m 2 / g, 15.5m 2 / g、16m 2 / g, 16.5m 2 / g、17m 2 / g, 17.5m 2 / g、18m 2 / g、19m 2 / g, 20m 2 / g, 21m 2 / g、22m 2 / g, 23m 2 / g、24m 2 / g, 25m 2 / g、26m 2 / g、27m 2 / g、28m 2 / g、29m 2 / g、30m 2 / g、31m2 / g、32m 2 / g、33m 2 / g、34m 2 / g、35m 2 / g、36m 2 / g、37m 2 / g、38m 2 / g、39m 2 / g, 40m 2 / g、41m 2 / g、42m 2 / g、43m 2 / g、44m 2 / g、45m 2 / g、46m 2 / g、47m 2 / g、48m 2 / g、49m 2 / g, 50m 2 / g、55m 2 / g, 60m 2 / g、65m 2 / g、70m 2 / g、75m 2 / g、80m 2 / g、85m 2 / g、90m 2 / g、95m 2 / g、100m 2 / g or a range consisting of any two of the above values.
[0207] In some embodiments of the present application, the second particles include one or more of inorganic particles and polymer particles.
[0208] Exemplarily, the inorganic particles include one or more selected from inorganic particles having a dielectric constant of 5 or higher, inorganic particles capable of transporting active ions, and inorganic particles capable of electrochemical oxidation and reduction.
[0209] Alternatively, the inorganic particles having a dielectric constant of 5 or more include boehmite, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, zirconium oxide, barium oxide, calcium oxide, magnesium oxide, nickel oxide, tin oxide, cerium oxide, yttrium oxide, hafnium oxide, aluminum hydroxide, magnesium hydroxide, silicon carbide, boron carbide, aluminum nitride, silicon nitride, boron nitride, magnesium fluoride, calcium fluoride, barium fluoride, barium sulfate, magnesium aluminum silicate, lithium magnesium silicate, sodium magnesium silicate, bentonite, hectorite, zirconium titanate, barium titanate, Pb(Zr,Ti)O3 (abbreviated as PZT), Pb 1-m La m Zr 1-n Ti nO3 (abbreviated as PLZT, 0<m<1, 0<n<1), Pb(Mg3Nb 2 / 3 )O3-PbTiO3 (abbreviated as PMN-PT), and one or more of their respective modified inorganic particles. Optionally, the modification method of each inorganic particle may be chemical modification and / or physical modification. Chemical modification methods include coupling agent modification (for example, using silane coupling agents, titanate coupling agents, etc.), surfactant modification, polymer grafting modification, etc. The physical modification method may be mechanical force dispersion, ultrasonic dispersion, high energy treatment, etc. The modification treatment can reduce the agglomeration of inorganic particles; in addition, by selecting coupling agents with specific functional groups and surfactants to modify inorganic particles, it is also helpful to improve the coating's wetting properties for the electrolyte and improve the coating's adhesion.
[0210] Alternatively, inorganic particles having ion conductivity but not storing ions include Li3PO4, lithium titanium phosphate Li x1 Ti y1 (PO4)3, lithium aluminum titanium phosphate Li x2 Al y2 Ti z1 (PO4)3, (LiAlTiP) x3 O y3 Type glass, lanthanum lithium titanate Li x4 La y4 TiO3, lithium germanium thiophosphate Li x5 Ge y5 P z2 S w , lithium nitride Li x6 N y6 、SiS2 type glass Li x7 Si y7 S z3 and P2S5 glass Li x8 P y8 S z4 One or more of the following: 0<x1<2, 0<y1<3, 0<x2<2, 0<y2<1, 0<z1<3, 0<x3<4, 0<y3<13, 0<x4<2, 0<y4<3, 0<x5<4, 0<y5<1, 0<z2<1, 0<w<5, 0<x6<4, 0<y6<2, 0<x7<3, 0<y7<2, 0<z3<4, 0<x8<3, 0<y8<3, 0<z4<7. This can further improve the ion transport properties of the isolation membrane.
[0211] Optionally, the inorganic particles capable of undergoing electrochemical reaction include at least one of lithium-containing transition metal oxides, lithium-containing phosphates, carbon-based materials, silicon-based materials, tin-based materials, and lithium-titanium compounds.
[0212] Optionally, the polymer particles include one or more of organosilicon particles, melamine formaldehyde resin particles, phenolic resin particles, polyester particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles, and polyaryletherketone particles. The organosilicon particles included in the polymer particles are the same as the organosilicon particles included in the first particles.
[0213] In some embodiments of the present application, the coating has a thickness of 0.1 μm-5 μm, optionally 0.5 μm-3 μm. A coating thickness within the above range can help improve the close packing between particles in the coating, thereby further improving the thermal safety performance of the secondary battery.
[0214] In some embodiments of the present application, the coating has a porosity greater than or equal to 20%, and can optionally be between 25% and 50%. When the coating contains organosilicon particles, a porosity within the above range can further enhance the electrolyte's wetting and retention of the separator, thereby facilitating ion transport within the separator and improving the cycling performance of the secondary battery.
[0215] In some embodiments of the present application, the substrate has a thickness of less than or equal to 16 μm. Optionally, the substrate has a thickness of 3 μm to 9 μm. The coating of the present application can improve the thermal safety and cycling performance of the separator, thereby enabling the use of a thinner substrate, thereby further increasing the energy density of the secondary battery.
[0216] In some embodiments of the present application, the substrate has a porous structure, and the porosity of the substrate is greater than or equal to 20%. Optionally, the porosity of the substrate is 25%-50%. When the porosity of the porous substrate is within the above-mentioned suitable range, it is beneficial to further improve the ion transport characteristics of the separator and thus improve the cycle performance of the secondary battery.
[0217] The present application does not particularly limit the material of the substrate. Any known substrate with good chemical and mechanical stability can be selected. For example, the substrate can include at least one of a porous polyolefin-based resin film (e.g., at least one of polyethylene, polypropylene, and polyvinylidene fluoride), a porous glass fiber, and a porous non-woven fabric. The porous substrate can be a single-layer film or a multi-layer composite film. When the porous substrate is a multi-layer composite film, the materials of each layer can be the same or different.
[0218] In some embodiments of the present application, the longitudinal thermal shrinkage of the isolation film at 150° C. for 1 hour is less than or equal to 3%.
[0219] In some embodiments of the present application, the transverse thermal shrinkage of the isolation film at 150° C. for 1 hour is less than or equal to 2%.
[0220] In the above embodiments, the separator of the present application has low thermal shrinkage in both the transverse and longitudinal directions, thereby further improving the thermal safety performance of the secondary battery.
[0221] In some embodiments of the present application, the separator has an air permeability of less than or equal to 200 s / 100 mL. Alternatively, the separator has an air permeability of 150 s / 100 mL to 200 s / 100 mL. The separator of the present application has good air permeability, thereby improving ion transport properties, reducing the resistance of the secondary battery, and thus improving the cycle performance of the secondary battery.
[0222] In some embodiments of the present application, the longitudinal tensile strength of the separator is greater than or equal to 2700 kg / cm 2 .
[0223] In some embodiments of the present application, the transverse tensile strength of the separator is greater than or equal to 2500 kg / cm 2 .
[0224] In the above embodiments, the separator of the present application has high tensile strength in both the transverse and longitudinal directions. Therefore, when the secondary battery expands, the separator is less likely to be damaged, thereby further improving the safety performance of the secondary battery.
[0225] In this application, the thermal shrinkage, tensile strength, and air permeability of the separator have meanings commonly known in the art and can be measured using methods known in the art. For example, they can all be tested in accordance with standard GB / T 36363-2018.
[0226] In some embodiments of the present application, the wetted length of the separator is 20 mm to 100 mm, and optionally 40 mm to 70 mm. The separator of the present application has good electrolyte wetting properties, thereby improving ion transport properties and secondary battery capacity.
[0227] In this application, the wetting length of the isolation membrane has a meaning well known in the art and can be measured using methods known in the art. An exemplary test method is as follows: cut the isolation membrane into samples with a width of 5 mm and a length of 100 mm, fix the two ends of the sample and place it horizontally; take 0.5 mg of electrolyte and drop it in the center of the sample. After 1 minute, take a picture and measure the length of the electrolyte diffusion to obtain the wetting length of the isolation membrane. In order to ensure the accuracy of the test results, multiple (for example, 5 to 10) samples can be taken for testing, and the test results are obtained by calculating the average value. The electrolyte can be prepared as follows: ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of 30:50:20 to obtain an organic solvent, and fully dried LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0228] It should be noted that the coating parameters of the above-mentioned isolation membrane are all coating parameters of a single side of the substrate.
[0229] When the coating is provided on both sides of the substrate, the coating parameters on either side satisfy the present application and are considered to fall within the protection scope of the present application.
[0230] Isolation film preparation method
[0231] The second aspect of the present application provides a method for preparing the isolation film of the first aspect of the present application, comprising the following steps: S1, providing a substrate; S2, mixing first particles and second particles in a solvent to prepare a coating slurry; S3, applying the coating slurry to at least one side of the substrate to form a slurry film layer, and drying the slurry film layer to form a coating to obtain an isolation film; wherein the first particles are organic particles, the average particle size of the first particles is denoted as D1, the average particle size of the second particles is denoted as D2, and 1 <D1 / D2≤10。
[0232] In some embodiments of the present application, in S2, the solvent may be water, such as deionized water. The binder may be an aqueous solution binder, which has the advantages of good thermodynamic stability and environmental protection, thereby facilitating the preparation and application of the coating slurry. As an example, the aqueous solution binder may include at least one of an aqueous solution acrylic resin (e.g., acrylic acid, methacrylic acid, sodium acrylate monomer homopolymer or a copolymer with other comonomers), polyvinyl alcohol (PVA), isobutylene-maleic anhydride copolymer, and polyacrylamide. In addition, the coating slurry may further include other components, for example, a dispersant, a wetting agent, etc.
[0233] In some embodiments of the present application, in S3, coating is performed using a coating machine. The present application does not particularly limit the model of the coating machine, for example, a commercially available coating machine can be used. Optionally, the coating machine includes a gravure roller, which is used to transfer the coating slurry to the substrate. Optionally, the line count of the gravure roller is 150LPI-250LPI, and more preferably 180LPI-200LPI. In addition, the coating method can be transfer coating, spin spray coating, dip coating, etc.
[0234] In some embodiments of the present application, in S3, the coating speed can be controlled between 40 m / min and 150 m / min, for example, between 60 m / min and 100 m / min. When the coating speed is within the above range, it can effectively reduce film surface problems of the coating and reduce the probability of uneven coating, thereby further improving the energy density and safety performance of the secondary battery.
[0235] By controlling the above process parameters within the given ranges, the performance of the isolation membrane of the present application can be further improved. Those skilled in the art can selectively adjust one or more of the above process parameters according to actual production conditions.
[0236] The parameters of some raw materials and their contents used in the preparation method of the isolation membrane of the present application can be referred to the isolation membrane of the first embodiment of the present application, and will not be repeated here. Unless otherwise specified, the raw materials used in the preparation method of the isolation membrane of the present application can be obtained commercially.
[0237] secondary batteries
[0238] A third aspect of the present application provides a secondary battery. A secondary battery, also known as a rechargeable battery or storage battery, refers to a battery that can be recharged after discharge to activate its active materials for continued use. Typically, a secondary battery includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode sheet, a negative electrode sheet, and a separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet, primarily preventing a short circuit between the positive and negative electrodes while allowing active ions to pass through.
[0239] The present application has no particular limitation on the type of secondary battery. For example, the secondary battery may be a lithium-ion battery, a sodium-ion battery, etc. In particular, the secondary battery may be a lithium-ion secondary battery.
[0240] The secondary battery of the present application includes the separator of the first aspect of the present application or the separator obtained by the preparation method of the second aspect of the present application, the separator being interposed between the positive electrode sheet and the negative electrode sheet. Optionally, at least the side of the separator proximal to the negative electrode sheet is coated with the coating of the present application. As a result, the secondary battery of the present application exhibits excellent thermal safety and cycling performance.
[0241] [Positive electrode]
[0242] In some embodiments of the present application, a positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one side of the positive electrode current collector and comprising a positive electrode active material. For example, the positive electrode current collector has two opposing sides in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0243] When the secondary battery of the present application is a lithium-ion secondary battery, the positive electrode active material may include, but is not limited to, at least one of a lithium-containing transition metal oxide, a lithium-containing phosphate, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their respective modified compounds. Examples of lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon, and their respective modified compounds.
[0244] In some embodiments of the present application, in order to further improve the energy density of the secondary battery, the positive electrode active material for the lithium ion secondary battery may include a general formula of Li a Ni b Co c M d O e A f At least one of lithium transition metal oxides and modified compounds thereof. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M is selected from at least one of Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A is selected from at least one of N, F, S and Cl.
[0245] As an example, the positive electrode active material for lithium ion secondary batteries may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333),LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622),LiNi 0.8 Co 0.1 Mn 0.1O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 At least one of O2, LiFePO4, and LiMnPO4.
[0246] When the secondary battery of the present application is a sodium ion secondary battery, the positive electrode active material may include but is not limited to at least one of sodium-containing transition metal oxides, polyanion materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.
[0247] As an example, the positive active material for a sodium ion secondary battery may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, NaNi 1 / 2 Ti 1 / 2 O2、NaNi 1 / 2 Mn 1 / 2 O2、Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2、NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials, general formula X p M' q (PO4) r O x Y 3-x At least one of the materials. p M' q (PO4) r O x Y 3-x , 0<p≤4, 0<q≤2, 1≤r≤3, 0≤x≤2, X is selected from H + 、Li + 、Na + , K + and NH4 + At least one of , M' is a transition metal cation, optionally at least one of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halogen anion, optionally at least one of F, Cl and Br.
[0248] In the present application, the modified compounds of the above-mentioned positive electrode active materials may be the ones subjected to doping modification and / or surface coating modification on the positive electrode active materials.
[0249] In some embodiments of the present application, the positive electrode film layer may further optionally include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. By way of example, the positive electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments of the present application, the mass percentage of the positive electrode conductive agent is ≤6 wt % based on the total weight of the positive electrode film layer.
[0250] In some embodiments of the present application, the positive electrode film layer may further optionally include a positive electrode binder. The present application does not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylic resin. In some embodiments of the present application, the mass percentage of the positive electrode binder is ≤5wt% based on the total weight of the positive electrode film layer. In some embodiments of the present application, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one side of the polymer material base layer. As an example, the metal material may include at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0251] The positive electrode film is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying it, and cold pressing it. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP).
[0252] [Negative electrode]
[0253] In some embodiments of the present application, a negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one side of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector has two opposing sides in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0254] The negative electrode active material may be any negative electrode active material known in the art for use in secondary batteries. For example, the negative electrode active material may include, but is not limited to, at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate. Silicon-based materials may include at least one of elemental silicon, silicon oxide, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include at least one of elemental tin, tin oxide, and tin alloys.
[0255] In some embodiments of the present application, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of negative electrode conductive agent. By way of example, the negative electrode conductive agent may include at least one of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments of the present application, the mass percentage of the negative electrode conductive agent is ≤7 wt % based on the total weight of the negative electrode film layer.
[0256] In some embodiments of the present application, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of negative electrode binder. As an example, the negative electrode binder may include at least one of styrene-butadiene rubber (SBR), a water-soluble unsaturated resin SR-1B, a water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments of the present application, the mass percentage of the negative electrode binder is ≤6 wt% based on the total weight of the negative electrode film layer.
[0257] In some embodiments of the present application, the negative electrode film layer may optionally include other additives. For example, the other additives may include thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, etc. In some embodiments of the present application, the mass percentage of the other additives is ≤ 3 wt % based on the total weight of the negative electrode film layer.
[0258] In some embodiments of the present application, the negative electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one side of the polymer material base layer. As an example, the metal material may include at least one of copper, a copper alloy, nickel, a nickel alloy, titanium, a titanium alloy, silver, and a silver alloy. As an example, the polymer material base layer may include at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0259] The negative electrode film layer is typically formed by coating the negative electrode slurry onto the negative electrode current collector, drying it, and cold pressing it. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0260] The negative electrode sheet does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode sheet of the present application further includes a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector. In other embodiments, the negative electrode sheet of the present application further includes a protective layer covering the surface of the negative electrode film layer.
[0261] [Electrolyte]
[0262] During the charge and discharge process of a secondary battery, active ions are embedded and released back and forth between the positive and negative electrodes, and the electrolyte conducts the active ions between the positive and negative electrodes. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected according to actual needs.
[0263] The electrolyte solution includes an electrolyte salt and a solvent. The types of the electrolyte salt and the solvent are not particularly limited and can be selected according to actual needs.
[0264] When the secondary battery of the present application is a lithium ion secondary battery, as an example, the electrolyte salt may include but is not limited to at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobisoxalatophosphate (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).
[0265] When the secondary battery of the present application is a sodium ion secondary battery, as an example, the electrolyte salt may include but is not limited to sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalatoborate (NaDFOB), sodium dioxalatoborate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorodioxalatophosphate (NaDFOP) and sodium tetrafluorooxalatophosphate (NaTFOP). At least one of the group.
[0266] As an example, the solvent may include, but is not limited to, at least one of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS), and diethyl sulfone (ESE).
[0267] In some embodiments of the present application, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives capable of improving certain properties of the secondary battery, such as additives that improve the overcharge performance of the secondary battery, additives that improve the high-temperature performance of the secondary battery, and additives that improve the low-temperature power performance of the secondary battery.
[0268] In some embodiments of the present application, the positive electrode sheet, the separator, and the negative electrode sheet may be formed into an electrode assembly through a winding process and / or a lamination process.
[0269] In some embodiments of the present application, the secondary battery may further include an outer package that can be used to encapsulate the electrode assembly and the electrolyte.
[0270] In some embodiments of the present application, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as at least one of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0271] The present application has no particular limitation on the shape of the secondary battery, which can be cylindrical, square, or any other shape. FIG1 shows a secondary battery 5 with a square structure as an example.
[0272] In some embodiments of the present application, as shown in FIG2 , the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 is used to cover the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process and / or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is impregnated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, which can be adjusted according to demand.
[0273] The preparation method of the secondary battery of the present application is well known. In some embodiments of the present application, a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte can be assembled to form a secondary battery. As an example, the positive electrode sheet, the separator, and the negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process. The electrode assembly is placed in an outer packaging, dried, and then injected with an electrolyte. The secondary battery is obtained through vacuum packaging, static standing, formation, and shaping processes.
[0274] In some embodiments of the present application, the secondary batteries according to the present application can be assembled into a battery module. The battery module can contain multiple secondary batteries, and the specific number can be adjusted according to the application and capacity of the battery module.
[0275] Figure 3 is a schematic diagram of an example battery module. As shown in Figure 3 , within a battery module 4, multiple secondary batteries 5 may be arranged sequentially along the length of the battery module 4. Of course, any other arrangement is also possible. Furthermore, the multiple secondary batteries 5 may be secured using fasteners.
[0276] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0277] In some embodiments of the present application, the above-mentioned battery modules may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0278] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 covers the lower case 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0279] Electrical devices
[0280] A fourth aspect of the embodiments of the present application provides an electrical device, which includes at least one of the secondary battery, battery module or secondary battery pack of the third aspect of the present application. The secondary battery, battery module or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.
[0281] The electrical device can select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0282] Figure 6 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0283] As another example, the electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a secondary battery as a power source.
[0284] The following embodiments describe the present disclosure in more detail, and these embodiments are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are by mass, and all reagents used in the embodiments are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0285] Example 1
[0286] Preparation of silicone particles
[0287] Preparation of prepolymer: 1400 g of deionized water and 7 g of sodium lauryl sulfate were added to a 5L three-necked flask, and the mixture was stirred and emulsified at a speed of 1500 r / min for 30 min to obtain a uniform and stable emulsion. Then, 645.68 g of methyl acrylate, 79.59 g of acrylonitrile and 663.50 g of methacryloyloxypropyl cage polysilsesquioxane (the molar content ratio of methyl acrylate, acrylonitrile and methacryloyloxypropyl cage polysilsesquioxane was 15:3:2) were added in sequence, and stirring was continued at a speed of 1500 r / min for 30 min to obtain a uniform prepolymer.
[0288] Polymer preparation: In a dry three-necked flask, add 3g of sodium lauryl sulfate and 1000g of deionized water, stir at high speed and emulsify for 30 minutes to obtain a uniform and stable emulsion; then use a peristaltic pump to slowly add the prepolymer and initiator solution prepared in the previous step (dissolve 3g of potassium persulfate in 30g of deionized water to form a solution), after the addition is complete, heat to 90°C and keep warm for 0.5h, cool to 40°C, adjust the pH to 7-8 with ammonia water, filter, discharge, and obtain silicone particles with a number average molecular weight of 43676 through a drying process, which is recorded as M1.
[0289] The average particle size D1 of the organic silicon particles M1 is 1.5 μm, and the volume distribution particle size D 1 v90 is about 1.6μm, D 1 v50 is about 1.3 μm, D 1 V10 is about 0.3 μm, and the specific surface area is about 30 m 2 / g.
[0290] Preparation of isolation membrane
[0291] Provide PE substrate: thickness 4.5μm, porosity 40%.
[0292] Preparation of coating slurry: organic silicon particles M1, aluminum oxide particles and binder polyacrylamide were mixed in water in a ratio of 5:1:1 to prepare a coating slurry, wherein the average particle size D2 of the aluminum oxide particles was 0.75 μm and the volume distribution particle size D 1 v90 is about 0.8μm, D 1 v50 is about 0.73 μm, D 1 V10 is about 0.2μm, and the specific surface area is about 8m 2 / g.
[0293] Coating: The prepared coating slurry was coated on both sides of the PE substrate using a coating machine, and a separator was obtained through drying and slitting processes. The thickness of the coating was 4 μm, and the porosity of the coating was 40%.
[0294] Preparation of positive electrode
[0295] The active material LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 (NCM333), conductive agent acetylene black, and binder polyvinylidene fluoride are mixed evenly in an appropriate amount of solvent N-methylpyrrolidone (NMP) in a weight ratio of 94:3:3 to obtain a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector aluminum foil, and the positive electrode sheet is obtained through processes such as drying, cold pressing, slitting, and cutting.
[0296] Preparation of negative electrode sheet
[0297] The negative electrode active material artificial graphite, the conductive agent carbon black (Super P), the binder styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) are mixed evenly in an appropriate amount of solvent deionized water at a mass ratio of 95:2:2:1 to obtain a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector copper foil, and the negative electrode sheet is obtained through the processes of drying, cold pressing, slitting and cutting.
[0298] Preparation of electrolyte
[0299] Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 30:70 to obtain an organic solvent, and fully dried LiPF6 was dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0300] Preparation of secondary batteries
[0301] The positive electrode sheet, separator, and negative electrode sheet are stacked and wound in sequence to obtain an electrode assembly; the electrode assembly is placed in an outer package, dried, and then injected with electrolyte. After vacuum packaging, standing, formation, shaping and other processes, a secondary battery is obtained.
[0302] Example 2-10
[0303] The secondary battery was prepared using a method similar to that of Example 1, except for the relevant parameters of the coating of the isolation membrane. The specific parameters are shown in Table 1.
[0304] Comparative Example 1-2
[0305] The secondary battery was prepared using a method similar to that of Example 1, with the difference being the coating-related parameters of the isolation membrane. Specific parameters are shown in Table 1.
[0306] Examples 11-14
[0307] The secondary battery was prepared using a method similar to that of Example 4, except that the coating of the isolation membrane contained first particles and second particles at different mass contents. Specific parameters are shown in Table 2.
[0308] Comparative Example 3
[0309] The secondary battery was prepared using a method similar to that of Example 4, except that the coating of the isolation membrane contained first particles and second particles of different masses. Specific parameters are shown in Table 2.
[0310] Test section
[0311] (1) Thermal shrinkage test of isolation film
[0312] Sample preparation: Punch the prepared isolation film into samples with a width of 50 mm and a length of 100 mm using a punching machine. Place 5 parallel samples on A4 paper and fix them. Then place the A4 paper with the samples on corrugated paper with a thickness of 1 mm to 5 mm.
[0313] Sample test: Place A4 paper on corrugated paper into a blast oven, set the oven temperature to 150°C, and start timing after the temperature reaches the set temperature and stabilizes for 30 minutes. After the set time (1 hour in this application) is reached, measure the length and width of the isolation film, and mark the values as a and b respectively.
[0314] Calculation of thermal shrinkage: longitudinal (MD) thermal shrinkage = [(100-a) / 100] × 100%, transverse (TD) thermal shrinkage = [(50-b) / 50] × 100%, and the average value of 5 parallel samples is taken as the test result.
[0315] (2) Wetting length test
[0316] The isolation membrane is cut into samples with a width of 5 mm and a length of 100 mm. The two ends of the sample are fixed and placed horizontally; 0.5 mg of electrolyte is dropped in the center of the sample. After 1 minute, a photo is taken and the length of the electrolyte diffusion is measured to obtain the wetting length of the isolation membrane. In order to ensure the accuracy of the test results, multiple (for example, 5 to 10) samples can be taken for testing, and the test results are obtained by calculating the average value. The electrolyte can be prepared as follows: ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are mixed in a mass ratio of 30:50:20 to obtain an organic solvent, and fully dried LiPF6 is dissolved in the above organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0317] (3) Secondary battery capacity retention test
[0318] At 25°C, charge at a constant current of 1 / 3C to 4.3V, then charge at a constant voltage of 4.3V to a current of 0.05C, let it sit for 5 minutes, and then discharge at 1 / 3C to 2.8V. The resulting capacity is recorded as the initial capacity C0. Repeat the above steps and record the discharge capacity C0 of the secondary battery after the 1000th cycle. 1000 , then the secondary battery capacity retention rate P after 1000 cycles 1000 =C 1000 / C0*100%.
[0319] Table 1 lists the test results of the coatings in Examples 1-10 and Comparative Examples 1-2 under different parameters.
[0320] Table 1
[0321]
[0322] According to the test results of Examples 1-10 and Comparative Examples 1-2 in Table 1, the separators provided by the embodiments of the present application have organic first particles, and the average particle size D1 of the first particles and the average particle size D2 of the second particles in the coating satisfy the aforementioned relationship. This allows the first and second particles to alternately overlap within the coating. When the substrate contracts due to heat, the particles can rapidly squeeze each other, exerting a force opposite to the direction of contraction on the substrate, thereby improving the thermal safety performance of the secondary battery. Furthermore, the second particles filling the gaps between the organic particles creates more voids in the coating, thereby enhancing the electrolyte's wetting effect on the separator, facilitating ion transport within the separator, and thus improving the cycling performance of the secondary battery.
[0323] Table 2 lists the test results of the coatings in Examples 4, 11-14 and Comparative Example 3 containing different mass fractions of the first particles and the second particles.
[0324] Table 2
[0325]
[0326] According to the test results of Examples 4, 11-14 and Comparative Example 3 in Table 2, the weight of the silicone particles in the coating and the weight of the second particles satisfying a suitable ratio relationship can not only help reduce the shrinkage of the isolation membrane to improve the thermal safety performance of the secondary battery, but also enable the silicone particles to be better overlapped to form more gaps, further improving the wetting effect of the electrolyte to improve the cycle performance of the secondary battery.
[0327] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present application, embodiments having substantially the same structure as the technical idea and exerting the same effects are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be conceived by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A separator comprising: substrate, and A coating is provided on at least one side of the substrate, wherein the coating comprises first particles and second particles, the first particles are organic particles, the average particle size of the first particles is recorded as D1, and the average particle size of the second particles is recorded as D2, then the coating satisfies: 1 <D1 / D2≤10。 2. The isolation film according to claim 1, wherein 2≤D1 / D2≤8; optionally, 3≤D1 / D2≤7.
3. The separator according to claim 1 or 2, wherein: 0.02μm≤D1≤3.0μm, optionally, 0.5μm≤D1≤2μm.
4. The isolation film according to any one of claims 1 to 3, wherein 0.01μm≤D2≤2μm; optionally, 0.1μm≤D2≤1μm.
5. The isolation film according to any one of claims 1 to 4, wherein The first particles satisfy at least one of the following characteristics: (1) Volume distribution particle size D of the first particles 1 v90≤3.0μm, optional 0.1μm≤D 1 v90≤2.0μm; (2) Volume distribution particle size D of the first particles 1 v50≤2μm, optional 0.01≤D 1 v50≤1.5μm; (3) The specific surface area of the first particles is greater than or equal to 3m 2 / g, optional 10m 2 / g-100m 2 / g; (4) The particle size distribution of the first particles (D 1 v90-D 1 v10) / D 1 v50≤1.5, optional 0.5≤(D 1 v90-D 1 v10) / D 1 v50≤1.
0.
6. The isolation film according to any one of claims 1 to 5, wherein: The second particles satisfy at least one of the following characteristics: (1) Volume distribution particle size D of the second particles 2 v90≤2μm; optional 0.3μm≤D 2 v90≤1.5μm; (2) Volume distribution particle size D of the second particles 2 v50≤1.5μm; optional 0.2μm≤D 2 v50≤1μm; (3) The specific surface area of the second particles is greater than or equal to 10 m 2 / g; (4) The particle size distribution of the second particles (D 2 v90-D 2 v10) / D 2 v50≤1.0, optional 0.2≤(D 2 v90-D 2 v10) / D 2 v50≤0.
8.
7. The isolation film according to any one of claims 1 to 6, wherein: The weight proportion of the first particles in the coating is recorded as A, and the weight proportion of the second particles in the coating is recorded as B, then the coating satisfies:
1. The weight proportion of the first particles in the coating is recorded as A, and the weight proportion of the second particles in the coating is recorded as B, then the coating satisfies: A≥50%, optionally 70%≤A≤90%; and / or, the coating satisfies: B≤35%, optionally 5%≤B≤25%.
8. The isolation film according to any one of claims 1 to 7, wherein: The first particles include one or more of silicone particles, melamine formaldehyde resin particles, phenolic resin particles, polyester particles, polyimide particles, polyamideimide particles, polyaramid particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyetheretherketone particles and polyaryletherketone particles; optionally, the first particles include silicone particles.
9. The isolation film according to any one of claims 1 to 8, wherein The first particles include organosilicon particles, the organosilicon particles include a first polymer, and the first polymer includes a first structural unit, a second structural unit, and a third structural unit; 10. The isolation film according to any one of claims 1 to 9, wherein The first structural unit has a structure as shown in formula (I): In formula (I), R1 includes a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; alternatively, R1 is selected from one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group; R2 includes one or more of a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C3-C20 cycloalkyl group, or a substituted or unsubstituted C1-C20 hydroxyalkyl group; alternatively, R2 includes one or more of a C1-C12 alkyl group, a C3-C12 cycloalkyl group, or a C1-C12 hydroxyalkyl group; The second structural unit is shown in formula (II): In formula (II), R3 includes one or more of a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; alternatively, R3 includes one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group; The third structural unit is shown in formula (III): Based on the total molar amount of the first structural unit, the second structural unit and the third structural unit, the molar content of the first structural unit is recorded as a%, 65≤a≤95; optionally, 70≤a≤85; and / or In formula (III), R4 to R 11 Each independently comprises one or more selected from a substituted or unsubstituted C1-C10 alkyl group, or a structural unit as shown in formula (III-1), and R4 to R 11 At least one of them is a structural unit represented by formula (III-1), In formula (III-1), R 12 Including one or more of a hydrogen atom, or a substituted or unsubstituted C1-C5 alkyl group; Optionally, R 12 including one or more of a hydrogen atom, or a substituted or unsubstituted C1-C3 alkyl group; R 13 Including one or more substituted or unsubstituted C1-C10 alkyl groups; optionally, R 13 It includes one or more substituted or unsubstituted C3-C10 alkyl groups. The isolation film according to claim 10 , wherein: Based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the second structural unit is denoted as b%, where 0 < b ≤ 15; optionally, 5 ≤ b ≤ 10; and / or Based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the third structural unit is denoted as c%, where 0 < c ≤ 10; optionally, 5 ≤ c ≤ 9.
12. The isolation film according to claim 10 or 11, wherein: Based on the total molar amount of the first structural unit, the second structural unit, and the third structural unit, the molar content of the first structural unit is denoted as a%, the molar content of the second structural unit is denoted as b%, and the molar content of the third structural unit is denoted as c%; the organosilicon particles satisfy one or more of the conditions (1) to (3): (1) 7 ≤ a / b ≤ 14; (2) 8 ≤ a / c ≤ 16; (3) a:b:c is (13 - 15):(2 - 4):(2 - 4).
13. The isolation film according to any one of claims 1 to 12, wherein: The organic particles include organosilicon particles, the organosilicon particles include a second polymer, and the second polymer includes a structural unit represented by formula (a): In formula (a), R 14 and R 15 Each independently comprises one or more of substituted or unsubstituted C1-C10 alkyl, hydroxyl or amino; optionally, R 14 and R 15 Each independently selected from one or more of substituted or unsubstituted C1-C6 alkyl, hydroxyl or amino; Optionally, the second polymer includes one or more of polymethylsiloxane, polydimethylsiloxane, polydiethylsiloxane, polymethylhydroxysiloxane, and polymethylaminosiloxane.
14. The isolation film according to any one of claims 1 to 13, wherein: The number average molecular weight of the organic particles is 30,000 - 70,000, and optionally 40,000 - 50,000.
15. The isolation film according to any one of claims 1 to 14, wherein: Based on the mass of the organic particles, the moisture content of the organic particles is less than or equal to 3000 μg / g; optionally 600 μg / g - 2800 μg / g.
16. The isolation film according to any one of claims 1 to 15, wherein: The second particles include one or more of inorganic particles and polymer particles; optionally, the second particles include inorganic particles.
17. The isolation film according to claim 16, wherein The inorganic particles include one or more selected from inorganic particles having a dielectric constant of 5 or higher, inorganic particles having the ability to transport active ions, and inorganic particles capable of undergoing electrochemical oxidation and reduction; and / or, The polymer particles include one or more of organosilicon particles, melamine formaldehyde resin particles, phenolic resin particles, polyester particles, polyimide particles, polyamideimide particles, polyaramide particles, polyphenylene sulfide particles, polysulfone particles, polyethersulfone particles, polyether ether ketone particles, and polyarylether ketone particles.
18. The isolation film according to any one of claims 1 to 17, wherein: The substrate satisfies at least one of the following characteristics: (1) The thickness of the substrate is less than or equal to 16 μm; optionally 3 μm - 9 μm; (2) The porosity of the substrate is greater than or equal to 20%; optionally 25% - 45%.
19. The isolation film according to any one of claims 1 to 18, wherein: The coating satisfies at least one of the following characteristics: (1) The thickness of the coating is from 0.1 μm to 5 μm; optionally 0.5 μm to 3 μm; (2) The porosity of the coating is greater than or equal to 20%; optionally 25% - 50%.
20. The isolation film according to any one of claims 1 to 19, wherein The separator membrane satisfies at least one of the following characteristics: (1) The longitudinal thermal shrinkage rate of the separator membrane at 150 °C for 1 h is less than or equal to 3%; (2) The transverse thermal shrinkage rate of the separator membrane at 150 °C for 1 h is less than or equal to 2%; (3) The air permeability of the isolation membrane is less than or equal to 200s / 100mL, and can be selected from 150s / 100mL to 200s / 100mL; (4) The longitudinal tensile strength of the separator is greater than or equal to 2700 kgf / cm 2 ; (5) The transverse tensile strength of the separator is greater than or equal to 2500 kgf / cm 2 ; (6) The wetted length of the isolation film is 20 mm to 100 mm; optionally 40 mm to 70 mm.
21. A method for preparing the isolation film according to any one of claims 1 to 20, comprising the following steps: providing a substrate; mixing the first particles and the second particles in a solvent to prepare a coating slurry; Applying the coating slurry on at least one side of the substrate to form a slurry film layer, and drying the slurry film layer to form a coating layer to obtain a separator; The first particles are organic particles, the average particle size of the first particles is recorded as D1, the average particle size of the second particles is recorded as D2, and the average particle size of the second particles is recorded as D3. <D1 / D2≤10。 22. A secondary battery comprising the separator according to any one of claims 1 to 20 or the separator obtained by the preparation method according to claim 21.
23. An electric device comprising the secondary battery according to claim 22.
Citation Information
Cited By
Separator, and electrochemical device and electronic device comprising same
CN119481592A