A modified polyurethane sponge for efficient recovery of high-viscosity oil, its preparation and application
By introducing fluorinated polydimethylsiloxane, nano-silica, hydroxyl multi-walled carbon nanotubes and ammonium polyphosphate into polyurethane foam, a micro-nano rough layer is constructed, which solves the problems of low separation efficiency and low recycling rate of high viscosity oil, and achieves high efficiency recycling and multifunctionality, with high elasticity and high compressive strength.
Patent Information
- Application Number
- CN202411343620.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-09-25
Smart Images

Figure CN119219978B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polyurethane modification technology, specifically to a modified polyurethane sponge for efficient recovery of high-viscosity oil, its preparation and application. Background Technology
[0002] Frequent marine oil spills, along with the resulting oily wastewater and large-scale marine fires, have severely impacted human health and the ecological environment. Currently, superhydrophobic and oleophilic sponges modified with polyurethane (PU) or melamine (MS) sponges as a base are commonly used as oil-absorbing materials. These materials are characterized by high separation efficiency, good mechanical stability, low cost, and ease of operation, and are therefore widely used.
[0003] For example, patent CN117866281A discloses a method for preparing a novel superhydrophobic flame-retardant sponge and its application in oil-water separation, which can achieve complete oil-water separation. However, it can only handle low-viscosity oils such as carbon tetrachloride and cannot adsorb high-viscosity oils.
[0004] To address the aforementioned issues, CN117772148A discloses a superhydrophobic photothermal sponge for rapidly adsorbing high-viscosity petroleum, its preparation, and its application. The photothermal material used is Co-HHTP, which enables rapid adsorption under sunlight. However, its drawbacks include the inability to achieve extrusion-adsorption recycling, the inability to efficiently recover high-viscosity oil, and a low material recycling rate. Summary of the Invention
[0005] This invention provides a modified polyurethane sponge for efficient recovery of high-viscosity oils, its preparation, and its application. The modified polyurethane sponge achieves both high elasticity and high compressive strength, enabling extrusion-adsorption cycles for the recovery of high-viscosity oils. Furthermore, the obtained modified polyurethane sponge possesses multiple properties such as flame retardancy, hydrophobicity, and fire resistance, making it a versatile and widely applicable material.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] This invention provides a method for preparing a modified polyurethane sponge for efficient recovery of high-viscosity oil, comprising:
[0008] S1, polydimethylsiloxane, and trimethoxy(1H,1H,2H,2H-heptadecyl)silane are mixed in n-hexane at room temperature by stirring. After the polydimethylsiloxane is fluorinated, a curing agent is added to obtain mixture A.
[0009] S2, nano-silica, hydroxyl multi-walled carbon nanotubes, and ammonium polyphosphate are mixed in n-hexane at room temperature to obtain mixture B;
[0010] S3. Under room temperature stirring conditions, keep mixture B of S2 as a suspension dispersion for at least 30 minutes before immersing it in polyurethane sponge. Then add mixture A of S1, stir, and dry to obtain cross-linked and cured modified polyurethane sponge.
[0011] This application introduces low surface energy long chains and CF on the surface of polydimethylsiloxane through a fluorination reaction, and uses the cross-linking reaction between nano-silica and fluorinated polydimethylsiloxane to lock hydroxyl multi-walled carbon nanotube particles and ammonium polyphosphate particles onto the polyurethane sponge skeleton, thus jointly constructing a micro-nano rough layer, which improves the mechanical strength of the modified polyurethane sponge and significantly increases its compressive strength.
[0012] Furthermore, the hydroxyl groups on the hydroxyl-containing multi-walled carbon nanotubes enable high dispersion of the carbon nanotubes in hexane, allowing them to be uniformly dispersed on all surfaces of the polyurethane framework, resulting in a uniform reinforcement effect. When the modified polyurethane sponge containing uniformly dispersed hydroxyl-containing multi-walled carbon nanotubes is subjected to external forces (such as compression), these hydroxyl-containing multi-walled carbon nanotubes can act as bridges during stress transmission, distributing stress more evenly within the polyurethane sponge, thereby reducing stress concentration and improving the compressive strength of the polyurethane sponge.
[0013] Meanwhile, hydroxyl multi-walled carbon nanotubes can be used as photothermal materials, which can help modified polyurethane sponges heat up rapidly under light to reduce the viscosity of high-viscosity oils, thereby improving their adsorption capacity.
[0014] Therefore, the modified polyurethane sponge obtained according to the method of this application retains the high resilience of polyurethane sponge while effectively improving its compressive strength. Consequently, it performs excellently in the extrusion-adsorption cycle, which can help to efficiently recover high-viscosity oil.
[0015] Preferably, in S1, the mass ratio of polydimethylsiloxane to trimethoxy(1H,1H,2H,2H-heptadecylfluorodecyl)silane is (4-6):1.
[0016] Preferably, in S1, the concentration of trimethoxy(1H,1H,2H,2H-heptadecyl)silane in mixture A is 7-8 g / mL.
[0017] Preferably, in S1, the curing agent is any one of methyltrichlorosilane, benzoyl peroxide, dicumyl peroxide, and titanate.
[0018] Preferably, in S2, the particle size of the nano-silica is 100-200 nm.
[0019] Preferably, in S2, the hydroxyl content of the hydroxyl multi-walled carbon nanotubes is above 3 wt%, and the average diameter of the hydroxyl multi-walled carbon nanotubes is 8-15 nm and the length is 0.5-2 μm.
[0020] Preferably, in S3, the mass ratio of polydimethylsiloxane, nano-silica, hydroxyl multi-walled carbon nanotubes, and ammonium polyphosphate is 1:(0.15~0.25):(0.15~0.25):(0.25~0.35).
[0021] More preferably, in S3, the mass ratio of polydimethylsiloxane, nano-silica, hydroxyl multi-walled carbon nanotubes, and ammonium polyphosphate is 1:(0.17~0.22):(0.17~0.22):(0.28~0.33).
[0022] More preferably, in S3, the mass ratio of polydimethylsiloxane, nano-silica, hydroxyl multi-walled carbon nanotubes, and ammonium polyphosphate is 1:0.2:0.2:0.3.
[0023] Preferably, in step S3, the drying temperature is 80–100°C and the drying time is 1–5 hours.
[0024] Preferably, in step S3, after adding mixture A from step S1, the polyurethane foam is pressed and immersed again using external force.
[0025] Other methods that prevent the polyurethane foam from floating on the liquid and absorbing the liquid during impregnation are also acceptable.
[0026] The present invention also provides a modified polyurethane sponge for efficient recovery of high-viscosity oil prepared by the above preparation method.
[0027] This invention also provides the application of modified polyurethane sponge in the cyclic absorption of high-viscosity petroleum.
[0028] Therefore, the present invention has the following beneficial effects:
[0029] (1) The method provided in this application can obtain a multifunctional modified polyurethane sponge with high efficiency in recovering high viscosity oil, which can be used to treat marine crude oil spills.
[0030] (2) This application utilizes hydroxyl multiwalled carbon nanotubes with a specific hydroxyl content to help improve the strength of the polyurethane sponge skeleton, thereby significantly increasing the overall compressive strength of the modified polyurethane sponge.
[0031] (3) This application utilizes nano-silica with a specific particle size to crosslink with fluorinated polydimethylsiloxane to form a dense structure, which strengthens the polyurethane skeleton and helps to lock hydroxyl multi-walled carbon nanotubes and ammonium polyphosphate, preventing a large number of particles from falling off.
[0032] (4) The modified polyurethane sponge for efficient recovery of high viscosity oil provided in this application has multifunctional properties such as flame retardancy, superhydrophobicity, and fire resistance. Attached Figure Description
[0033] Figure 1 This is a schematic diagram illustrating the preparation of the FPMA-PU sponge in Example 1;
[0034] Figure 2 The images shown are SEM and EDS images of the PU sponge in Comparative Example 1. In the images, a to c are SEM images at different magnifications, d is the EDS energy spectrum formed at the target position in image c, and e is the elemental mapping distribution of C, N, O, F, Si, and P.
[0035] Figure 3 The images shown are SEM and EDS images of the FPMA-PU sponge in Example 1, where a to c are SEM images at different magnifications, d is the EDS energy spectrum formed at the target position in image c, and e is the elemental mapping distribution of C, N, O, F, Si, and P.
[0036] Figure 4 The figure shows the results of the carbon tetrachloride oil-water separation experiment of FPMA-PU sponge in Example 1;
[0037] Figure 5 The figure shows the experimental results of hexane oil-water separation of FPMA-PU sponge in Example 1;
[0038] Figure 6 The graph shows the adsorption capacity of the FPMA-PU sponge for different oils / organic solvents in Example 1.
[0039] Figure 7 The graph shows the adsorption capacity of the FPMA-PU sponge for different oils / organic solvents in Example 1.
[0040] Figure 8 This is a graph showing the adsorption-desorption cycle results of peanut oil on the FPMA-PU sponge in Example 1;
[0041] Figure 9 The graph shows the cycling results of the FPMA-PU sponge in Example 1 with different oils / organic solvents;
[0042] Figure 10 The following diagram shows the results of carbon tetrachloride separation by FPMA-PU sponge circulation in Example 1, where a is a schematic diagram of oil-water separation by gravity and b is a diagram of circulation separation efficiency.
[0043] Figure 11 This is a process diagram of the separation of carbon tetrachloride and n-hexane using FPMA-PU sponge in Example 1, where a is... Figure 9b is a process diagram of medium gravity separation of carbon tetrachloride, and b is a process diagram of continuous separation of n-hexane by combining FPMA-PU sponge and peristaltic pump.
[0044] Figure 12 The diagrams show the extrusion, torsion, and stretching processes of the FPMA-PU sponge in Example 1, where a is the extrusion process, b is the torsion process, and c is the stretching process.
[0045] Figure 13 The contact angle value corresponding to 100 friction tests of the FPMA-PU sponge in Example 1;
[0046] Figure 14 The cyclic compression process and corresponding stress-strain curves of the PU sponge in Comparative Example 1 are shown.
[0047] Figure 15 The cyclic compression process and corresponding stress-strain curves of the FPMA-PU sponge in Example 1 are shown.
[0048] Figure 16 The figures show the contact angle test results of the FPMA-PU sponge in Example 1 and the PU sponge in Comparative Example 1. In the figures, a is the contact angle diagram of the hydrophobic / oleophilic FPMA-PU sponge, b is the wetting condition of the surface and interior of the FPMA-PU sponge, c is the silver mirror phenomenon of the FPMA-PU sponge underwater, d is the wetting condition of different liquids on the surface of the FPMA-PU sponge, e is the rolling condition of water droplets on the surface of the PU sponge, and f is the rolling condition of water droplets on the surface of the FPMA-PU sponge.
[0049] Figure 17 The diagram shows the wetting of the FPMA-PU sponge in Example 1 when immersed at different pH values.
[0050] Figure 18 The graphs show the optical properties of the FPMA-PU sponge in Example 1 and the PU sponge in Comparative Example 1, where a is the absorbance and the full spectrum of sunlight, and b is the heating and cooling curve.
[0051] Figure 19 These are thermal images of the FPMA-PU sponge in Example 1 and the PU sponge in Comparative Example 1.
[0052] Figure 20 The diagram shows the process of FPMA-PU sponge in Example 1 and PU sponge in Comparative Example 1 absorbing butter;
[0053] Figure 21The diagram shows the photothermal properties of the FPMA-PU sponge in Example 1 and the PU sponge in Comparative Example 1. In example a, the diagram shows the melting and absorption process of petroleum by the FPMA-PU sponge in Example 1 and the PU sponge in Comparative Example 1 under light irradiation. In example b, the diagram shows the situation when a beaker containing petroleum and water is inverted at room temperature (FPMA-PU sponge in Example 1). In example c, the diagram shows the process of continuous separation of crude oil by combining the FPMA-PU sponge and the peristaltic pump in Example 1.
[0054] Figure 22 The image shows the flame retardant performance test results of the PU sponge in Comparative Example 1.
[0055] Figure 23 This is a test diagram of the flame retardant performance of the FPMA-PU sponge in Example 1;
[0056] Figure 24 The thermogravimetric curves are shown for the FPMA-PU sponge in Example 1 and the PU sponge in Comparative Example 1, where a is the TG curve and b is the DTG curve.
[0057] Figure 25 The fire resistance performance diagrams of FPMA-PU sponge in Example 1 and PU sponge in Comparative Example 1 are shown. In Example 1, a is the combustion process of PU sponge after hexane is added; b is the combustion process of FPMA-PU sponge in Example 1 after hexane is added; c is the oil absorption and fire extinguishing process of FPMA-PU sponge in Example 1 after simulating a small-scale oil spill fire; and d is the continuous oil absorption and fire extinguishing process of FPMA-PU sponge in Example 1 combined with a peristaltic pump after simulating a large-scale oil spill fire. Detailed Implementation
[0058] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0059] In this section, polyurethane foam (PU), density 35, hardness 80, was purchased from Xiangyang Mingfang store. Polydimethylsiloxane (PDMS) was purchased from Dow Corning in the form of Sylgard-184PDMS elastomer kit (including curing agent). Trimethoxy(1H,1H,2H,2H-heptadecyl)silane (FAS-17) was purchased from Aladdin Reagent (Shanghai) Co., Ltd. Unless otherwise specified, all other reagents were analytical grade and required no further purification. All experiments used ultrapure water (resistivity 18 MΩ·cm).
[0060] The crude oil was sourced from Huizhou Petrochemical. The seawater came from Baishamen Beach in Haikou City. The butter was sourced from Shenzhen Pin Yuepin Food Co., Ltd. Hexane, dichloromethane, cyclohexane, carbon tetrachloride, methanol, and epoxidized soybean oil were purchased from Xilong Reagent. The peanut oil was Luhua peanut oil (5S physical pressing, Grade 1), the olive oil was Oliolan extra virgin olive oil, and the tung oil was natural tung oil.
[0061]
Example
[0062] Example 1
[0063] S1, 2g of polydimethylsiloxane, and 0.4g of trimethoxy(1H,1H,2H,2H-heptadecyl)silane were mixed in 50mL of n-hexane at room temperature by stirring. After the polydimethylsiloxane was fluorinated, 0.2g of Dow Corning's own curing agent was added to obtain mixture A.
[0064] S2, 0.4 g of 180 nm nano-silica, 0.4 g of hydroxyl multi-walled carbon nanotubes (hydroxyl content 3.7 wt%, average diameter 8-15 nm, length 0.5-2 μm), and 0.6 g of ammonium polyphosphate were mixed in 10 mL of n-hexane at room temperature to obtain mixture B.
[0065] S3. Under room temperature stirring conditions, keep mixture B from S2 as a suspension dispersion for 60 minutes, then immerse it in a polyurethane sponge (2cm×2cm×3cm). Add mixture A from S1, and then repeatedly squeeze and release the polyurethane sponge with tweezers over 30 minutes. After impregnation, transfer the polyurethane sponge to a 100℃ oven and dry for 30 minutes.
[0066] S4. After removal, repeat the impregnation operation of S3 above, and then transfer the polyurethane sponge to a 100℃ oven to dry for 60 minutes. The difference is that the placement of the polyurethane sponge in S4 is reversed compared to S3. After drying, place the polyurethane sponge in anhydrous ethanol and repeatedly squeeze and wash away excess residue to obtain the modified polyurethane sponge, denoted as FPMA-PU.
[0067] Example 2
[0068] This embodiment is basically the same as Example 1, except that the amount of trimethoxy(1H,1H,2H,2H-heptadecyl)silane used in S1 is 0.35g.
[0069] Example 3
[0070] This embodiment is basically the same as embodiment 1, except that in S2, the amount of nano-silica is 0.35g, the amount of hydroxyl multi-walled carbon nanotubes is 0.35g, and the amount of ammonium polyphosphate is 0.65g.
[0071] Comparative Example 1
[0072] Untreated polyurethane foam is denoted as PU.
[0073] Comparative Example 2
[0074] This comparative example is basically the same as Example 1, except that in S2, the silica particle size used is 1 μm.
[0075] Comparative Example 3
[0076] This comparative example is basically the same as Example 1, except that in S2, the particle size of the nano-silica is 10nm.
[0077] Comparative Example 4
[0078] This comparative example is basically the same as Example 1, except that in S2, the hydroxyl multi-walled carbon nanotubes are replaced with multi-walled carbon nanotubes with similar average diameter and length.
[0079] Comparative Example 5
[0080] This comparative example is basically the same as Example 1, except that in S2, the hydroxyl content of the hydroxyl multi-walled carbon nanotubes is 1.06wt%, the average diameter is 30-50nm, and the length is 0.5-2μm.
[0081] Comparative Example 6
[0082] This comparative example is basically the same as Example 1, except that in S2, the hydroxyl content of the hydroxyl multi-walled carbon nanotubes is 1.76 wt%, the average diameter is 20-30 nm, and the length is 0.5-2 μm.
[0083] Comparative Example 7
[0084] This comparative example is basically the same as Example 1, except that: 2g of polydimethylsiloxane and 0.4g of trimethoxy(1H,1H,2H,2H-heptadecyl)silane are mixed in 50mL of n-hexane at room temperature to complete the fluorination of polydimethylsiloxane. Then, 0.2g of Dow Corning self-contained curing agent, 0.4g of 180nm nano-silica, 0.4g of hydroxyl multi-walled carbon nanotubes (hydroxyl content 3.7wt%, average diameter 8-15nm, length 0.5-2μm), and 0.6g of ammonium polyphosphate are added to obtain a mixture. The remaining impregnation and drying steps are the same as in Example 1.
[0085] [Performance Testing]
[0086] 1. Morphological composition
[0087] To determine the specific structural changes in the synthesized FPMA-PU sponge, SEM-EDS was used to analyze the untreated PU sponge and the treated FPMA-PU sponge. The results are as follows: Figures 2-3 As shown. Figure 2 In the study, the PU sponge's skeleton surface is observed to be smooth and has a three-dimensional porous spatial network structure. Figure 3 The SEM image of the FPMA-PU sponge shows that after loading the FPMA coating, the skeleton of the PU sponge becomes rougher; additionally, Figure 3 In image b, numerous micro- and nano-scale protrusions can be observed on the surface of the FPMA-PU sponge. These protrusions are condensates of varying sizes formed by the cross-linking of fluorinated PDMS and SiO2, and the adhesion of MWCNTs-OH and APP to the PU skeleton surface. Importantly, these protrusions increase the surface roughness of the FPMA-PU sponge skeleton, creating a solid-liquid-gas three-phase contact surface, resulting in the FPMA-PU sponge exhibiting superhydrophobic properties.
[0088] In addition, in comparison Figure 2 d and Figure 3 The EDS spectrum of d shows that after loading the FPMA coating onto the PU sponge, the proportions of C and N elements on the FPMA-PU sponge surface decreased, while the proportions of O, F, Si, and P elements increased. This result indicates the successful introduction of F, Si, and P elements. Figure 2 and Figure 3 The elemental mapping distribution diagram shows that C, N, O, F, Si and P elements are uniformly distributed on the surface of FPMA-PU sponge, indicating that the FPMA coating is uniformly loaded on the surface of FPMA-PU sponge.
[0089] 2. Elasticity and compressive strength
[0090] The elasticity and compressive strength of the sponges obtained in Examples 1-3 and Comparative Examples 1-7 were measured, and the results are shown in Table 1.
[0091] The specific testing method is as follows: the compression percentage of all sponges is fixed at 75%. That is, the compressive strength of the sponge is calculated by measuring the ratio of the compression length S to the compression length A of the sponge itself.
[0092] Table 1 Compressive strength of different polyurethane foams
[0093] Compression level (%) Compressive strength (kPa) Example 1 75 254.2738 Example 2 75 248.5401 Example 3 75 245.6521 Comparative Example 1 75 19.0631 Comparative Example 2 75 232.8754 Comparative Example 3 75 223.9357 Comparative Example 4 75 180.8283 Comparative Example 5 75 211.4357 Comparative Example 6 75 215.2352 Comparative Example 7 75 237.9019
[0094] Based on the results in section "2. Elasticity and Compressive Strength," the FPMA-PU sponge obtained in Example 1 exhibits the best elasticity and compressive strength. Theoretically, this ensures rapid rebound and repeated oil absorption during oil extrusion. Furthermore, the sponge's high elasticity and high compressive strength result in minimal wear during use, enabling long-term recycling. Therefore, the performance of the FPMA-PU sponge will be evaluated in sections "3-7" below to verify this hypothesis and explore other functionalities of the synthesized FPMA-PU sponge.
[0095] 3. Absorption and separation performance for dissolution in oils / organic solvents
[0096] ① Method for determining adsorption capacity: The multiple FPMA-PU sponges obtained in Example 1 were weighed to obtain m0. Subsequently, the multiple FPMA-PU sponges obtained in Example 1 were immersed in n-hexane, dichloromethane, cyclohexane, peanut oil, carbon tetrachloride, methanol, epoxidized soybean oil, olive oil, and tung oil, respectively. After the FPMA-PU sponges reached adsorption equilibrium, they were quickly removed and weighed to obtain M0.
[0097] The adsorption capacity Q of the FPMA-PU sponge is calculated according to equation (1). m :
[0098]
[0099] Where m0 represents the mass of the FPMA-PU sponge before adsorption equilibrium, in g; M0 represents the mass of the FPMA-PU sponge after adsorption equilibrium, in g; Q m This indicates the adsorption capacity of the FPMA-PU sponge, in g / g.
[0100] ② Methods for determining recyclability and recycling performance:
[0101] 1) Weigh the FPMA-PU sponge obtained in Example 1 to obtain m0. Then, completely immerse multiple FPMA-PU sponges obtained in Example 1 in non-volatile peanut oil. After adsorption equilibrium is reached, remove and weigh to obtain M0; calculate the adsorption amount Q according to formula (1). m .
[0102] 2) Squeeze out the peanut oil that was saturated with FPMA-PU sponge in step 1) and weigh it again to obtain m1; without drying, directly immerse it in the peanut oil in step 1) again, and after reaching the second adsorption equilibrium, take it out and weigh it to obtain M1; this process is recorded as the first extrusion-adsorption cycle.
[0103] 3) Repeat step 2) ten times, and calculate the adsorption amount Q for each cycle according to formula (2). an Calculate the residual oil amount Q after each cycle according to formula (3). b(n-1)The extrusion-adsorption cycle efficiency ε is calculated according to equation (4):
[0104]
[0105] Where n represents the total number of extrusion-adsorption cycles; m n M represents the mass of the FPMA-PU sponge after extrusion during the nth extrusion-adsorption cycle, in grams. n Q represents the mass of the FPMA-PU sponge after adsorption equilibrium at the nth extrusion-adsorption cycle, in grams. an Q represents the adsorption amount in the nth extrusion-adsorption cycle, in g / g; b(n-1) Q represents the residual oil content after the (n-1)th extrusion-adsorption cycle, in g / g; m ε represents the adsorption capacity of the FPMA-PU sponge, in g / g; ε represents the extrusion-adsorption cycle efficiency of the FPMA-PU sponge, in %.
[0106] ③ Method for determining the separation efficiency of heavy oil: Methylene blue-stained water (methylene blue 1 mg / L) and Sudan Red-stained carbon tetrachloride (Sudan Red 1 mg / L) were mixed at a mass ratio of 3:2 to obtain an oil-water mixture. The following separation experiment was then conducted. A 1cm × 1cm × 1cm FPMA-PU sponge obtained according to the operation method in Example 1 was placed in the neck of a long-necked funnel to form a gravity-driven one-way oil-water separation device (e.g., Figure 10 (as shown in a). Pour the oil-water mixture into a long-necked funnel and collect the separated oil. Calculate the separation efficiency η according to formula (5):
[0107]
[0108] Where C1 represents the weight of oil in the oil-water mixture before separation by the FPMA-PU sponge, in g; C0 represents the weight of oil in the oil-water mixture after separation by the FPMA-PU sponge, in g; and η represents the separation efficiency of the FPMA-PU sponge, in %.
[0109] ④ Determination method for the continuous oil-water separation capability of light oil: A mixture of methylene blue-stained water and Sudan Red-stained n-hexane at a mass ratio of 3:2 is obtained; Assemble an intelligent suction system based on a peristaltic pump (e.g. Figure 11 (as shown in b). Specifically, the rubber tube and FPMA-PU sponge are combined and immersed in the prepared oil-water mixture. A pressure difference is generated by the peristaltic pump, thereby causing the FPMA-PU sponge to separate the oil from the oil-water mixture.
[0110] To verify that the obtained FPMA-PU sponge has good oil-water separation performance, an oil-water separation experiment was conducted, and the results are as follows: Figure 4 and Figure 5 As shown. Observation Figures 4-5It can be seen that FPMA-PU sponge has a good separation effect on both heavy oils containing carbon tetrachloride and light oils containing n-hexane, and can adsorb oil and retain water to achieve a significant oil-water separation effect.
[0111] Furthermore, to test the oil absorption and separation capabilities of the FPMA-PU sponge, tests were conducted according to the methods described in ① to ④ above. The results are as follows:
[0112] Figure 6 The adsorption capacity of FPMA-PU sponge for n-hexane, dichloromethane, cyclohexane, peanut oil, carbon tetrachloride, methanol, epoxidized soybean oil, olive oil, and tung oil was observed. Figure 6 It can be seen that FPMA-PU sponge has a strong adsorption capacity for nine common oils, with an adsorption capacity of 6.37–21.99 g / g. (Observation) Figure 7 It can be seen that the adsorption capacity of FPMA-PU sponge is directly proportional to the density of the adsorbed object. And... Figure 8 The results of the cyclic adsorption capacity of FPMA-PU sponge show that after 10 repeated extrusion-adsorption cycles, the extrusion-adsorption cycle efficiency of the FPMA-PU sponge can still be maintained at around 80%. This indicates that FPMA-PU sponge has high resilience and stable adsorption-desorption capacity, and in practical applications, it can be recycled by extruding away oil / organic solvents, demonstrating its recyclability. Furthermore, observations... Figure 9 It can be seen that FPMA-PU sponge exhibits stable cyclic adsorption capacity for different oils / organic solvents.
[0113] Figure 10 a is a schematic diagram of the separation process of FPMA-PU sponge, according to the Young-Laplace theory of equation (6):
[0114]
[0115] Where ΔP is the Laplace pressure, γ SL θ represents the interfacial surface tension at the FPMA-PU sponge surface-liquid interface. L D is the contact angle between oil and water. p The pore size is the diameter of the FPMA-PU sponge surface.
[0116] Section 4.2 Wettability Figure 16 Data from a shows that the water contact angle on the FPMA-PU sponge surface is 156.55°, and the oil contact angle is 0°. Furthermore, γ... SL Greater than 0, D p The value is greater than 0. Therefore, the Laplace pressure of water is negative, i.e., ΔP. O A value less than 0 indicates that an external pressure is required for water to penetrate the FPMA-PU sponge. The Laplace pressure of oil, however, is positive, i.e., ΔP.O The value is greater than 0; therefore, oil can spontaneously penetrate into the FPMA-PU sponge. This driving force can effectively separate immiscible oil-water mixtures. Therefore, in Figure 11 In step a, it can be seen that carbon tetrachloride is completely separated from the oil-water mixture within 51 seconds, yielding clean water. Furthermore, after 51 seconds, it remains on the upper surface of the FPMA-PU sponge without further penetration, achieving complete oil-water separation. Moreover, in continuous carbon tetrachloride separation of the FPMA-PU sponge, the separation efficiency remained above 95% even after 29 cycles.
[0117] A continuous separation experiment was then conducted on n-hexane; however, n-hexane is a light oil with a density less than water, therefore, the following method was used... Figure 11 The separation capacity of the intelligent suction system of the peristaltic pump shown in b was measured, and the results are as follows: Figure 11 As shown. Observation Figure 11 b indicates that 20 mL of n-hexane can be completely separated from the oil-water mixture within 15 seconds without adsorbing any water.
[0118] 4. Mechanical properties and wettability tests
[0119] ① Test method for abrasion resistance: Place the FPMA-PU sponge on 400-grit sandpaper, press down with a 500g weight, and rub it at a constant speed along a ruler for 10cm, then return to the starting point. This is recorded as one abrasion cycle. Measure the contact angle on the worn surface of the FPMA-PU sponge every 10 cycles to evaluate its abrasion resistance.
[0120] ②Methods for determining mechanical properties: FPMA-PU foam was subjected to simple compression, torsion, and tension tests. The mechanical strength of PU foam and FPMA-PU foam was determined using an electronic universal testing machine (Shimadzu AGS-X-10kN, Japan). The parameters of the electronic universal testing machine were set as follows: maximum strain 75%, 5 cycles.
[0121] ③ Corrosion resistance test method: FPMA-PU sponge was placed in aqueous solutions with different pH values (pH = 1, 3, 7, 11, 13) for 24 hours for acid and alkali corrosion resistance test. The solutions with different pH values were prepared by mixing sodium hydroxide and hydrochloric acid; and food-grade pigments were used to distinguish the different pH values (compound coloring agents: bright red, fruit green, sky blue and lemon yellow).
[0122] 4.1 Mechanical properties
[0123] The mechanical properties of FPMA-PU foam play an important role in practical applications. To verify the mechanical properties of the obtained FPMA-PU foam, tests were conducted according to the methods described in ① to ② above. The results are as follows: Observation Figure 12 It can be seen that FPMA-PU sponge can quickly recover after compression and torsion, and it will not break even when stretched under a 500g load. Observation Figure 13 It can be seen that after 100 repeated wear tests, the contact angle is still higher than 150°, which confirms that the FPMA-PU sponge has superhydrophobicity. This is mainly due to the high adhesion of the FPMA coating. Even after wear, when some skeleton fractures occur on the worn surface of the FPMA-PU sponge, the FPMA coating remains firmly adhered to the FPMA-PU skeleton, thus ensuring the overall stability of the FPMA-PU sponge's performance.
[0124] To further verify the compression performance of FPMA-PU sponge, cyclic compression tests were conducted on FPMA-PU sponge and PU sponge. The results are as follows: Figures 14-15 As shown. Observation Figure 14 and Figure 15 It can be seen that, compared with PU foam, FPMA-PU foam exhibits a significant improvement in compressive strength, increasing from 18.3 kPa to 254.3 kPa when compressed to 75%; this phenomenon indicates that the FPMA-PU foam has a rigid molecular structure on its skeletal surface. (Observation) Figure 15 As shown in the cyclic compression process diagram, the FPMA-PU sponge can recover its original shape after five compression cycles from 0% to 75% to 0%. This phenomenon proves that the FPMA-PU sponge, while utilizing the inherent resilience of PU sponge, also possesses higher compressive strength, which is consistent with the results and conjectures in section "2. Elasticity and Compressive Strength".
[0125] 4.2 Wettability
[0126] The hydrophobicity of FPMA-PU sponge plays an important role in practical applications. To verify the hydrophobicity of the obtained FPMA-PU sponge, a contact angle experiment was conducted. The results are as follows: Figure 16 As shown. Observation Figure 16 As can be seen from this, PU sponge has hydrophobic and oleophilic properties, with contact angles of 94.79° and 0° for water and oil, respectively.
[0127] The FPMA-PU sponge exhibits a water contact angle of 156.55°, demonstrating superhydrophobicity; the oil contact angle remains at 0°. Furthermore, Figure 16 e and Figure 16The results in f show that when water droplets fall on the inclined surface of PU sponge, the droplets adhere to the PU sponge surface; however, when water droplets fall on the inclined surface of FPMA-PU sponge, the droplets slide off quickly and do not adhere to the FPMA-PU sponge. Furthermore, observations... Figure 16 As shown in b, water droplets can remain stably on both the surface and interior of the FPMA-PU sponge, maintaining an approximately spherical shape. Furthermore, the superhydrophobic effect inside the FPMA-PU sponge is better than on the surface, with a contact angle as high as 161.74°. Figure 16 In step c, when an FPMA-PU sponge is immersed in water using external force, the surface of the FPMA-PU sponge exhibits a silver mirror effect. This is because the micro-nano-scale protrusions form a gas layer, preventing water droplets from penetrating. Figure 16 The results show that drops of pure water, milk, coffee, and tea formed approximately spherical shapes on the surface of the FPMA-PU sponge, demonstrating the excellent liquid repellency of the FPMA-PU sponge.
[0128] Furthermore, to evaluate the stability of FPMA-PU sponge under acidic and alkaline conditions, tests were conducted according to the method described in ③ above, and the results are as follows. Figure 17 As shown. Observation Figure 17 It can be seen that after 24 hours, the FPMA-PU sponge still floats on aqueous solutions of different pH values, and its surface contact angle is still above 150°.
[0129] The above results demonstrate that FPMA-PU sponge has excellent oil-water recognition properties (superhydrophobic and oleophilic), exhibits good stability in different chemical environments, and meets the conditions for application in oil-water separation.
[0130] 5. Photothermal Assisted Adsorption and Separation of High-Viscosity Oil
[0131] ①Method for measuring photothermal capacity: A xenon lamp light source (CEL-HXF300-T3, China; 300~1100nm, 500w, 15A) was used to simulate a sun (1kW / m²). 2 The photothermal properties of FPMA-PU sponges were studied using the intensity of a light source. A mixture of 30 mL of water and 20 mL of crude oil was used as a simulant for marine oil spills. Under tilted xenon lamp illumination, FPMA-PU sponges / PU sponges were placed in beakers containing the prepared simulant, and the changes in oil absorption by the FPMA-PU sponges / PU sponges were observed.
[0132] ②Method for measuring photothermal performance: A xenon lamp light source (CEL-HXF300-T3, China; 300~1100nm, 500w, 15A) was used to simulate a sun (1kW / m²). 2 The photothermal properties of FPMA-PU sponge were determined by measuring the intensity of a light source. An intelligent suction system based on a peristaltic pump (such as...) was assembled. Figure 11(As shown in b): PU sponge and FPMA-PU sponge are connected to both ends of the peristaltic pump, respectively. The distance between the xenon lamp light source and the FPMA-PU / PU sponge is 10cm. PU sponge and FPMA-PU sponge are used as oil absorbents. The pump outlet is placed in a beaker to collect oil, and the pump connection end is immersed in castor oil. Before starting the xenon lamp light source, start the oil collection pump first, and check the oil quality after 1 minute. The PU / FPMA-PU sponge is preheated under the xenon lamp for 100s, and the mass of oil collected within 1 minute is measured during oil collection.
[0133] ③ Method for measuring photothermal conversion capacity: A xenon lamp light source (CEL-HXF300-T3, China; 300~1100nm, 500w, 15A) was used to simulate a sun (1kW / m²). 2 The photothermal conversion capability of FPMA-PU sponge was studied by measuring the light source intensity. To ensure the accuracy of the light intensity, an optical power meter (CEL-FZ-A, CEC Jin Yuan, China) was used for calibration. The temperature change of the material over time was measured using an infrared thermal imager, and the light source was turned off after 5 minutes, while the cooling rate of the sample was recorded.
[0134] ④ Method for determining absorption capacity: A xenon lamp light source (CEL-HXF300-T3, China; 300~1100nm, 500w, 15A) was used to simulate a sun (1kW / m²). 2 The absorption capacity of FPMA-PU sponges was studied using the intensity of a light source. A mixture of 250 mL of seawater and 60 mL of crude oil was used as a simulant for crude oil spills. Under xenon lamp irradiation, FPMA-PU sponges / PU sponges were placed into beakers containing the prepared simulant, and the mass change of the FPMA-PU sponges / PU sponges was observed. The absorption capacity was then analyzed based on the mass change.
[0135] Simulating a crude oil leak in a real-world application scenario, the corresponding simulation tests were completed using the measurement methods given in ① to ④ above, and the results are as follows:
[0136] observe Figure 18 As can be seen from this, the light absorption rate of FPMA-PU sponge is greater than 90%, which is significantly higher than that of PU sponge, proving that FPMA-PU sponge has better light absorption performance. Figure 18 b shows the heating and cooling curves. It can be seen that during the 240s heating process, the surface temperature of the FPMA-PU sponge rises faster than that of the PU sponge. Furthermore, after the lights are turned off (240–360s), the surface temperature of the FPMA-PU sponge decreases rapidly over time.
[0137] Figure 19 For the corresponding thermal imaging image of the temperature rise, observe Figure 19It can be observed that the surface temperature of the FPMA-PU sponge rapidly rises to 72.7℃ within 60s, increases to 89.3℃ after 120s, and reaches a maximum temperature of 98.1℃ after 232s; while the PU sponge only reaches 29.7℃ after 232s. This indicates that the photothermal conversion capability of the FPMA-PU sponge after being coated with FPMA is greatly improved.
[0138] Based on this, Figure 20 The absorption capacity of FPMA-PU sponges for high-viscosity oil was investigated, using high-viscosity butter as the test subject. Observation Figure 20 It can be seen that after 7 minutes, the butter on the PU sponge remained almost unchanged; while the butter on the FPMA-PU sponge was gradually absorbed within 7 minutes. This result indicates that the FPMA-PU sponge has excellent light absorption and photothermal conversion capabilities and can be applied to the adsorption of high viscosity oils.
[0139] To study the thermal conductivity of FPMA-PU sponge, FPMA-PU sponge and PU sponge were placed on solid crude oil and exposed to light. Both the FPMA-PU sponge and PU sponge were 1 cm thick. Results were obtained as follows: Figure 21 The results are shown in a. Observation Figure 21 As shown in Figure a, the PU sponge melted the crude oil through heat conduction after 4 minutes. However, after removing the PU sponge with tweezers, it was observed that the sponge had absorbed almost no crude oil. In contrast, the FPMA-PU sponge melted the crude oil beneath it after only 2 minutes of light exposure, and upon removal, some of the crude oil was observed to have been absorbed. These results indicate that the FPMA-PU sponge, after being coated with a PU coating, exhibits excellent thermal conductivity.
[0140] An FPMA-PU sponge and a peristaltic pump are assembled into an oil-water separator to separate a mixture of high-viscosity crude oil and water, yielding a product such as... Figure 21 The result shown in b. Observation. Figure 21 b indicates that even if the beaker is turned upside down, the crude oil and water will not flow out, which shows that the crude oil has a very high viscosity.
[0141] To separate a mixture of crude oil and water, a photothermal-assisted adsorption separation experiment was conducted under a xenon lamp. For example... Figure 21 As shown in Figure c, some crude oil melted and was extracted after 4 minutes; after 9 minutes, some crude oil had been collected in the left beaker; and after 13 minutes, most of the crude oil in the beaker had been extracted and separated. These results indicate that the FPMA-PU sponge coated with FPMA exhibits excellent photothermal effect and thermal conductivity, which is of great significance for handling marine oil spills and for subsequent crude oil recovery and reuse.
[0142] 6. Flame retardant
[0143] Test method: Place FPMA-PU sponge and PU sponge on a stainless steel mesh frame and ignite them with a lighter with a combustion temperature of about 1300℃.
[0144] Flame retardant performance results are as follows Figures 22-23 As shown: Due to the flammability of PU foam, it ignites within 1 second, the fire intensifies rapidly, and it cannot self-extinguish. After 23 seconds, the PU foam completely burns, generating molten droplets that drip from the stainless steel mesh and ignite the paper below. This property easily leads to secondary fires. In contrast, FPMA-PU foam requires 3 seconds to ignite, does not continue burning downwards, and self-extinguishes after 65 seconds. Furthermore, the burned portion of the FPMA-PU foam retains its complete rigid structure, and no molten droplets are generated. The results indicate that FPMA-PU foam can significantly prolong the burning time and prevent the generation of molten droplets during combustion, exhibiting excellent flame-retardant properties.
[0145] To investigate the mechanism of flame retardancy in FPMA-PU foam and PU foam, thermogravimetric analysis (TGA) was conducted under a nitrogen atmosphere. The results are as follows: Figure 24 As shown in Table 2. Table 2 gives the thermal decomposition parameters of PU sponge and FPMA-PU sponge, where T 5wt% and T 50wt% These are their initial thermal decomposition temperatures and the temperatures at which they lose half their mass, respectively. Both PU foam and FPMA-PU foam undergo a two-step thermal degradation process. The first stage mainly involves the breakage of the polyurethane polymer chains, and the second stage involves the further breakage of C-C and CO bonds in the polyurethane main chain. Figure 24 As shown, under nitrogen conditions, both PU sponge and FPMA-PU sponge exhibit similar second-order thermal decomposition behavior. It is noteworthy that, compared to PU sponge, the Tdecomposition... 5wt% (272.76℃) and T 50wt% (378.23℃), T of FPMA-PU sponge 5wt% (306.11℃) and T 50wt% The temperature (506.03℃) has increased.
[0146] Table 2. Thermal performance parameters of PU and FPMA-PU under nitrogen conditions.
[0147] <![CDATA[T 5wt% (℃)]]> <![CDATA[T 50wt% (℃)]]> High-temperature pyrolysis at 800℃ (wt%) PU 272.76 378.23 1.66 FPMA-PU 306.11 506.03 32.8
[0148] 7. Oil absorption and fire extinguishing
[0149] To test the fire resistance of FPMA-PU foam, hexane was dripped onto both FPMA-PU and PU foams, and then ignited with a lighter at a combustion temperature of approximately 1300℃. The results are as follows. Figure 25 As shown in a to b.
[0150] like Figure 25 a and Figure 25 As shown in b: After ignition of hexane, the PU sponge burns directly along with the hexane, completely burning after 18 seconds, leaving brownish-black ash. In contrast, the FPMA-PU sponge does not burn with the hexane within 10 seconds, begins to burn after 10 seconds, and self-extinguishes after 65 seconds. The results indicate that the FPMA-PU sponge possesses certain fire-resistant properties.
[0151] Since seawater itself can be used for fire extinguishing, FPMA-PU sponges can be used in conjunction with water for fire suppression. Simulating an oil spill fire at sea, FPMA-PU sponges were placed in petri dishes, and the results are as follows... Figure 25 As shown in c. Observe Figure 25 As can be seen from c, the FPMA-PU sponge rapidly absorbs oil within 2 seconds, reducing the fire intensity on the petri dish; and with the help of water isolating oxygen and cooling, the fire is extinguished after 4 seconds.
[0152] Furthermore, considering that FPMA-PU sponges can only absorb small areas of leaked oil for fire extinguishing, this application proposes the following... Figure 25 Figure d illustrates a method for continuous oil fire suppression using FPMA-PU sponge combined with a pump. By combining the FPMA-PU sponge with a peristaltic pump, the burning oil is rapidly and continuously absorbed, minimizing the amount of flammable oil in the beaker within 30 seconds. After 30 seconds, water is used to cool the burning FPMA-PU sponge and isolate it from oxygen to extinguish the fire. The FPMA-PU sponge remains undamaged throughout the entire combustion process. These results demonstrate that FPMA-PU sponge can be used for continuous oil fire suppression at sea, preventing the spread and diffusion of fires.
Claims
1. A method for preparing a modified polyurethane sponge for efficient recovery of high-viscosity oil, characterized in that, include: S1, polydimethylsiloxane, and trimethoxy(1H, 1H, 2H, 2H-heptadecyl)silane are mixed in n-hexane at room temperature by stirring. After the polydimethylsiloxane is fluorinated, a curing agent is added to obtain mixture A. The mass ratio of polydimethylsiloxane to trimethoxy(1H, 1H, 2H, 2H-heptadecyl)silane is (4~6):
1. S2, nano-silica with a particle size of 100~200 nm, hydroxyl multi-walled carbon nanotubes, and ammonium polyphosphate are mixed in n-hexane at room temperature to obtain mixture B; the hydroxyl content of the hydroxyl multi-walled carbon nanotubes is more than 3 wt%, and the average diameter of the hydroxyl multi-walled carbon nanotubes is 8~15 nm and the length is 0.5~2 μm; S3. Under room temperature stirring conditions, keep mixture B of S2 as a suspension dispersion for at least 30 min before immersing it in polyurethane sponge. Then add mixture A of S1, stir and dry to obtain cross-linked and cured modified polyurethane sponge. The mass ratio of polydimethylsiloxane, nano-silica, hydroxyl multi-walled carbon nanotubes, and ammonium polyphosphate is 1:(0.15~0.25):(0.15~0.25):(0.25~0.35).
2. The preparation method according to claim 1, characterized in that, In step S3, the drying temperature is 80~100℃ and the drying time is 1~5 h.
3. The preparation method according to claim 1, characterized in that, In step S3, after adding mixture A from step S1, the polyurethane foam is pressed and immersed again using external force.
4. The modified polyurethane sponge for efficient recovery of high-viscosity oil prepared by the preparation method according to any one of claims 1 to 3.
5. The application of the modified polyurethane sponge as described in claim 4 in the cyclic absorption of high-viscosity petroleum.
Citation Information
Patent Citations
Super-hydrophobic photo-thermal sponge capable of rapidly adsorbing high-viscosity petroleum as well as preparation and application of super-hydrophobic photo-thermal sponge
CN117772148A
Preparation method and oil-water separation application of novel super-hydrophobic flame-retardant sponge
CN117866281A
Superhydrophobic sponge body and preparation method thereof
CN107312198A
Super-oleophylic and super-hydrophobic sponge for oil-water separation, and preparation method and application of super-oleophylic and super-hydrophobic sponge
CN110387062A