A method for processing TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes

By employing a single-fire forging process and continuous skew rolling piercing, hot continuous rolling, and sizing rolling, the problem of low-cost mass production of TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes has been solved, achieving efficient and low-cost pipe processing and improving yield and performance.

CN119281858BActive Publication Date: 2026-11-17NORTHWEST INSTITUTE FOR NONFERROUS METAL RESEARCH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411693252.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-25
Publication Date
2026-11-17
Estimated Expiration
2044-11-25

AI Technical Summary

Technical Problem

Existing technologies cannot effectively solve the problem of low-cost, mass production of TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes. Traditional processes are complex and have low yields, which cannot meet the needs of marine equipment and shipbuilding.

Method used

The billet is prepared by one-time forging, combined with continuous skew rolling, hot continuous rolling and sizing rolling, avoiding heat treatment. By controlling the temperature and deformation, TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes with excellent performance are produced.

Benefits of technology

It significantly improved the yield rate, shortened the production cycle, reduced costs, and enhanced the comprehensive mechanical properties of the pipes, meeting the application needs of marine equipment and shipbuilding.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a processing method for TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes. The method includes the following steps: Step 1, forging a TA24 titanium alloy ingot in a single firing to obtain a billet; Step 2, subjecting the billet to continuous skew rolling, hot rolling, and sizing rolling to obtain a tube; Step 3, annealing and machining the tube to obtain the TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube. This processing method, by using a single firing forging to prepare the billet, breaks down the coarse casting structure to a certain extent, improving the microstructure and plasticity. Then, through skew rolling, hot rolling, sizing rolling, annealing, and machining, the TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube is obtained. This effectively shortens the processing cycle, reduces production costs, and is applicable to the field of titanium alloy seamless tube processing technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of titanium alloy seamless tube processing technology, and in particular relates to a processing method for TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes. Background Technology

[0002] TA24 titanium alloy is a near-α type marine titanium alloy independently developed in my country. It features high specific strength, good weldability, resistance to seawater corrosion, and ease of hot and cold working. It exhibits significant advantages, particularly in high-pressure, high-flow-rate, and highly corrosive marine pipeline systems, significantly improving system reliability. Currently, marine resource development has been incorporated into the national development strategy, and TA24 titanium alloy has enormous market potential and development prospects in the manufacturing of military ships, large civilian vessels, and offshore drilling platforms. The application of TA24 titanium alloy in next-generation ships and seawater pipeline systems is inevitable due to its significant performance advantages, especially the huge demand for thin-walled, large-diameter pipes (Φ200mm~Φ325mm, diameter-to-thickness ratio D / t not less than 20), which are the main specifications for marine pipeline systems. The production of ultra-long pipes (length ≥10000mm) can efficiently improve pipe utilization and reduce manufacturing costs. Based on the current huge market demand, the development prospects of thin-walled, large-diameter, ultra-long titanium pipes are broad.

[0003] Currently, the main production methods for titanium tubes in China include spinning, machining, skew rolling and piercing, extrusion, hot rolling, and cold rolling. However, due to limitations in maturity or feasibility, these processes cannot achieve low-cost industrial production of thin-walled, large-diameter, ultra-long seamless titanium alloy tubes, severely restricting their application in marine equipment and shipbuilding. Traditional tube processing methods typically involve first preparing a tube blank, and then processing the blank into a tube. Due to the complexity and cumbersome procedures, the final tube yield is only 10%–30%. For large-diameter, thin-walled tubes, spinning is commonly used. The tube blank is first thinned by ring rolling to increase the diameter, and then the length is increased through spinning to further thin the wall, ultimately obtaining a large-diameter, thin-walled titanium tube. However, spinning is too costly for producing thin-walled seamless tubes, and it is generally only suitable for manufacturing ultra-thin titanium alloy seamless tubes with short lengths and very high diameter-to-thickness ratios. In addition, machining produces pipes with low yield and high cost; skew-rolled pierced pipes have poor microstructure and properties; hot-extruded pipes have low dimensional accuracy; and cold-rolled pipes require many rolling passes and have long production cycles. These methods are not suitable for producing thin-walled, large-diameter, ultra-long seamless pipes.

[0004] In recent years, many new methods for processing seamless titanium tubes have emerged due to practical application needs. However, most of these methods are combinations of one or more processes from traditional seamless tube processing methods, failing to specifically address the problems of low mass production efficiency and low yield of thin-walled, large-diameter, ultra-long seamless tubes. For example, the Chinese invention patent "Production Method of Large-Diameter Seamless Titanium Tubes" (Publication No. CN107199243B) proposes a method that utilizes ingot casting...β The above-mentioned method of directly piercing at temperatures between 5℃ and 50℃ to prepare tube blanks, followed by grinding and hot rolling, results in tube blanks with incomplete microstructure, making it difficult to guarantee the performance of the hot-rolled tubes. Chinese invention patent "A Production Method of Titanium Alloy Oil Well Tubes" (Announcement No. CN103128102B) uses a continuous processing method of piercing and rolling to obtain seamless titanium alloy tubes. However, the specifications and diameter-to-thickness ratios of the processed oil well tubes are relatively small, and the large diameter reduction during production can cause circumferential instability and folding of the tubes. Furthermore, the piercing temperature is too high, making it impossible to guarantee the microstructure and performance of the pierced tubes. Chinese invention patent "An Efficient and Low-Cost Preparation Method for High-Strength TC18 Titanium Alloy Seamless Tubes" (Announcement No. CN114101372B) addresses this by strictly controlling the tube processing temperature, with the skew rolling piercing process being carried out at a specific temperature. β After the above process is completed at 120℃~180℃, the billet needs to be rapidly air-cooled and its temperature controlled to T before entering the continuous rolling process. β ±20℃, the billet temperature needs to be reheated to T before sizing rolling. β The precise temperature control of ±10℃ in this continuous processing undoubtedly increases the difficulty of actual production and reduces the yield of pipe products. At the same time, the processing temperature of this method is too high, which is not conducive to the improvement of the structure and performance of titanium alloys. High-alloyed TC18 alloys can still improve their performance through subsequent heat treatment, but low-alloyed TA24 titanium alloys cannot be effectively strengthened through heat treatment.

[0005] In summary, there is currently no short-process, low-cost method in China for producing TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes. Therefore, actively developing new methods for producing TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes, while ensuring the excellent performance of TA24 thin-walled tubes, to shorten the tube processing flow, improve the tube yield, and reduce production costs, thereby solving the challenges of short-process, low-cost, and mass production of titanium alloy thin-walled, large-diameter, ultra-long seamless tubes, is of great significance for improving the modernization level of my country's marine equipment. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a processing method for TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes. This processing method involves preparing a billet through a single-fire forging process, which breaks down the coarse casting structure to a certain extent, improving the microstructure and enhancing plasticity. Then, through continuous uninterrupted skew rolling piercing + hot continuous rolling + sizing rolling, followed by annealing and machining, the TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube is obtained. This method effectively shortens the processing cycle, reduces production costs, and solves the problem of the inability to achieve short-process, low-cost, and mass production of TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is: a method for processing TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes, characterized in that the method includes the following steps:

[0008] Step 1: Forge the TA24 titanium alloy ingot in one pass to obtain a billet.

[0009] Step 2: The bar billet obtained in Step 1 is subjected to continuous skew rolling, hot continuous rolling and sizing rolling to obtain the tube.

[0010] Step 3: Anneal and machine the pipes obtained in Step 2 to obtain TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes.

[0011] The above-mentioned processing method for a thin-walled, large-diameter, ultra-long seamless TA24 titanium alloy tube is characterized in that the TA24 titanium alloy ingot in step one is an ingot prepared by VAR melting or EB melting.

[0012] The VAR melting described in this invention is melting in a consumable electrode melting furnace, and the EB melting is melting in an electron beam cold hearth furnace.

[0013] The above-mentioned processing method for TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube is characterized in that the forging temperature in step one is (T β +150℃~(T β +250℃), the T β The value is the β phase transformation temperature of TA24 titanium alloy, expressed in °C.

[0014] The above-mentioned processing method for TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube is characterized in that the deformation amount of the blank forging in step one is greater than 60%.

[0015] This invention, by controlling the deformation amount during billet forging to be greater than 60%, can effectively break up the casting structure, improve the plasticity of the bar stock, and facilitate subsequent processes.

[0016] The above-mentioned processing method for TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes is characterized in that the temperature of the billet during the skew rolling piercing in step two is (T β -50℃~T β .

[0017] The above-mentioned processing method for a thin-walled, large-diameter, ultra-long seamless TA24 titanium alloy tube is characterized in that no heat treatment is performed during the skew rolling piercing, hot continuous rolling, and sizing rolling processes in step two.

[0018] This invention employs continuous, uninterrupted skew rolling piercing, hot continuous rolling, and sizing rolling processes, and controls the temperature of the billet during skew rolling piercing. This allows the process to be completed smoothly without the need for reheating the tube, effectively reducing the number of times precise temperature control is required during processing, lowering the actual production difficulty, and shortening the production preparation cycle.

[0019] The above-mentioned processing method for a thin-walled, large-diameter, ultra-long seamless TA24 titanium alloy tube is characterized in that the dimensions of the TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube in step three are as follows: outer diameter D is 200mm to 325mm, diameter-to-thickness ratio D / t is not less than 20, and length is not less than 10000mm; where t is the wall thickness in mm.

[0020] The above-mentioned processing method for TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube is characterized in that the yield of the TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube in step three is not less than 70%.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1. This invention uses a single-fire forging process to prepare the billet, which breaks down the coarse casting structure to a certain extent, improves the structure and enhances plasticity, thus providing conditions for subsequent skew rolling and piercing. Compared with the existing technology that uses multi-fire forging to prepare the billet, this invention can effectively shorten the processing cycle and reduce production costs. Compared with the existing technology that uses direct piercing rolling of ingots to prepare the tube blank, this invention can initially break down the billet structure and enhance plasticity, which is conducive to the smooth progress of subsequent skew rolling and hot continuous rolling, and further improves the performance of TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes.

[0023] 2. This invention uses bar billets instead of tube billets as raw materials to produce TA24 titanium alloy thin-walled large-diameter ultra-long tubes. By completing the skew rolling piercing + hot continuous rolling + sizing rolling processes in one continuous operation, it is equivalent to completing two processes, tube billet preparation and tube preparation, in one operation. This effectively shortens the production process and reduces production costs while ensuring performance. Compared with the conventional seamless tube production process with a yield of less than 30%, the processing method of this invention significantly improves the yield.

[0024] 3. This invention, by employing a process of skew rolling piercing, hot continuous rolling, and sizing rolling with large deformation, can strongly break down grains, thereby improving the microstructure and properties of the billet by replacing upsetting and forging; simultaneously, by controlling the temperature during skew rolling piercing to (T... β -50℃~T β Below T β Large deformation at certain temperatures is beneficial for the formation of equiaxed primary α phase, which can effectively improve the comprehensive mechanical properties of the pipe.

[0025] The technical solution of the present invention will be further described in detail below through embodiments. Detailed Implementation

[0026] Example 1

[0027] The processing method in this embodiment includes the following steps:

[0028] Step 1: Cast 1080 kg of TA24 titanium alloy ingot (the nominal composition of TA24 titanium alloy is Ti-3.4Al-2Mo-2.2Zr-0.04O, T... β =943℃) is subjected to one-time forging and drawing at 1190℃ to obtain a billet with a diameter of 320mm. After cooling, it is machined to obtain a 1005kg plain billet with a diameter of 310mm; the TA24 titanium alloy ingot is an ingot prepared by VAR melting, and the deformation of the forging is 70%.

[0029] Step 2: Heat the 310mm diameter blank obtained in Step 1 at 940℃ for 2 hours, and then perform continuous skew rolling, hot continuous rolling and sizing rolling. The whole process is continuous and does not require reheating, to obtain a 328mm×18mm (diameter×wall thickness) tube.

[0030] Step 3: Anneal and machine the 328mm×18mm (diameter×wall thickness) pipe obtained in Step 2 to obtain a TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipe with a diameter of 325mm×15mm×12000mm (diameter×wall thickness×length) weighing 790kg.

[0031] The room temperature mechanical properties of the TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube prepared in this embodiment, as tested, are as follows: tensile strength R... m 713 MPa, yield strength R p0.2 With a strength of 621 MPa, an elongation A of 18.0%, and a pipe yield of 73.1%, the processing method of this embodiment not only shortens the production cycle of TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes and improves the utilization rate of raw materials, but also produces TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes with excellent comprehensive mechanical properties.

[0032] Example 2

[0033] The processing method in this embodiment includes the following steps:

[0034] Step 1: Cast 460kg of TA24 titanium alloy ingot (the nominal composition of TA24 titanium alloy is Ti-3.5Al-2.1Mo-2.4Zr-0.13O, T... β=969℃) is subjected to one-time forging and drawing at 1120℃ to obtain a billet with a diameter of 238mm. After cooling, it is machined to obtain a 430kg bright billet with a diameter of 230mm; the TA24 titanium alloy ingot is an ingot prepared by EB melting, and the deformation of the forging is 65%.

[0035] Step 2: Heat the 230mm diameter blank obtained in Step 1 at 920℃ for 2 hours, and then perform continuous skew rolling, hot continuous rolling and sizing rolling. The whole process is continuous and does not require reheating, to obtain a 202mm×10mm (diameter×wall thickness) tube.

[0036] Step 3: Anneal and machine the 202mm×10mm (diameter×wall thickness) tube obtained in Step 2 to obtain a TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube with a diameter of 200mm×8mm×15000mm (diameter×wall thickness×length) weighing 328kg.

[0037] The room temperature mechanical properties of the TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube prepared in this embodiment, as tested, are as follows: tensile strength R... m 747 MPa, yield strength R p0.2 With a strength of 656 MPa, an elongation A of 20.5%, and a pipe yield of 71.3%, the processing method of this embodiment not only shortens the production cycle of TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes and improves the utilization rate of raw materials, but also produces TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes with excellent comprehensive mechanical properties.

[0038] Example 3

[0039] The processing method in this embodiment includes the following steps:

[0040] Step 1: Cast 720 kg of TA24 titanium alloy ingot (TA24 titanium alloy nominal composition is Ti-3.4Al-2.1Mo-2.3Zr-0.12O, T... β =963℃) is subjected to one-time forging and drawing at 1150℃ to obtain a billet with a diameter of 278mm. After cooling, it is machined to obtain a 668kg plain billet with a diameter of 270mm; the TA24 titanium alloy ingot is an ingot prepared by EB melting, and the deformation of the forging is 65%.

[0041] Step 2: Heat the 270mm diameter blank obtained in Step 1 at 930℃ for 2 hours, and then perform continuous skew rolling, hot continuous rolling and sizing rolling. The whole process is continuous and does not require reheating, to obtain a tube with a diameter of 277mm×14mm (diameter×wall thickness).

[0042] Step 3: Anneal and machine the 277mm×14mm (diameter×wall thickness) tube obtained in Step 2 to obtain a TA24 titanium alloy thin-walled large-diameter ultra-long seamless tube with a diameter of 275mm×12mm×12000mm (diameter×wall thickness×length) weighing 540kg.

[0043] Testing revealed that the room temperature mechanical properties of the TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes prepared in this embodiment were as follows: tensile strength Rm = 727 MPa, yield strength Rp0.2 = 632 MPa, elongation A = 21.0%, and tube yield = 75.0%. This indicates that the processing method in this embodiment not only shortened the production cycle of TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes and improved the utilization rate of raw materials, but also produced TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes with excellent comprehensive mechanical properties.

[0044] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the present invention. Any simple modifications, alterations, or equivalent structural transformations made to the above embodiments based on the technical essence of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A method for processing TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tubes, characterized in that, The method includes the following steps: Step 1: Perform a single-pass forging of the TA24 titanium alloy ingot to obtain a billet; the deformation during the forging process is greater than 60%. Step 2: The billet obtained in Step 1 is subjected to continuous skew rolling, hot continuous rolling, and sizing rolling to obtain the tube; the temperature of the billet during skew rolling is (T). β -50℃~T β No heat treatment is performed during the skew rolling piercing, hot continuous rolling and sizing rolling processes; Step 3: Anneal and machine the tubes obtained in Step 2 to obtain TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes; the dimensional specifications of the TA24 titanium alloy thin-walled large-diameter ultra-long seamless tubes are: outer diameter D of 200mm~325mm, diameter-to-thickness ratio D / t of not less than 20, and length of not less than 10000mm; where t is the wall thickness in mm.

2. The processing method for a TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube according to claim 1, characterized in that, The TA24 titanium alloy ingot mentioned in step one is an ingot prepared by VAR melting or EB melting.

3. The processing method for a TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube according to claim 1, characterized in that, The temperature for forging the billet in step one is (T) β +150℃) ~ (T β +250℃), the T β The value is the β phase transformation temperature of TA24 titanium alloy, expressed in °C.

4. The processing method for a TA24 titanium alloy thin-walled, large-diameter, ultra-long seamless tube according to claim 1, characterized in that, The yield rate of the TA24 titanium alloy thin-walled large-diameter ultra-long seamless pipes mentioned in step three shall not be less than 70%.

Citation Information

Patent Citations

  • Production method of titanium alloy oil well pipe

    CN103128102B

  • Production method of large diameter titanium seamless pipe

    CN107199243B

  • A High-Efficiency and Low-Cost Preparation Method for High-Strength TC18 Titanium Alloy Seamless Tubes

    CN114101372B

  • Preparation method of titanium alloy seamless pipe in petroleum and natural gas industry

    CN109280787A

  • Preparation method of high-precision ultra-large-diameter thin-wall Ti35 titanium alloy pipe

    CN118437767A