A sodium storage material based on anthracite hard carbon anode, its preparation method and application
By combining alkaline activation and chemical oxidation methods, the oxygen-containing functional groups of anthracite-based hard carbon anode materials are regulated to form a closed microporous structure, which solves the problems of low initial coulombic efficiency and low sodium storage capacity of anthracite-based hard carbon anode materials and achieves high-efficiency electrochemical performance.
Patent Information
- Application Number
- CN202410291632.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-03-14
AI Technical Summary
The existing anthracite-based hard carbon anode materials have low initial coulombic efficiency and sodium storage capacity, which affects the performance of sodium-ion batteries.
By combining alkaline activation and chemical oxidation methods, the electrochemical performance of the material is improved by regulating the oxygen-containing functional groups in the hard carbon precursor to form a closed microporous structure.
The prepared anthracite-based hard carbon anode material achieved an initial charge capacity of 325.2 mAh g⁻¹, an initial coulombic efficiency of 92.2%, and good cycle performance, with a capacity retention of 96.1% after 150 cycles.
Smart Images

Figure CN119430126B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrode materials technology, and in particular to anthracite-based hard carbon anode sodium storage material, its preparation method, and its application. Background Technology
[0002] Sodium-ion batteries possess advantages such as good low-temperature performance, high safety, and low cost, making them promising candidates for applications in power batteries and large-scale energy storage, complementing lithium-ion batteries in their development. Currently, the domestic production capacity of sodium-ion battery anode materials is relatively limited, a key factor restricting the large-scale commercial application of sodium-ion batteries. Sodium-ion battery anode materials typically include carbon materials, titanium-based compounds, metal oxide / sulfide organic compounds, and alloy materials. Among these, hard carbon materials are currently the most promising anode materials for sodium-ion batteries due to their low cost, wide availability, and ease of synthesis. Precursors for preparing hard carbon materials mainly include polymers, biomass, bitumen, and anthracite. Polymer-based hard carbon has higher costs and greater processing difficulty, while biomass hard carbon has lower processing difficulty but lower carbon yield and poor batch stability. Compared to other precursors, anthracite has advantages such as high carbon content, low ash content, and low cost. However, carbon materials obtained from the direct pyrolysis of anthracite have low sodium storage capacity and low initial coulombic efficiency, severely affecting battery performance. In the initial cycling of sodium-ion full cells, hard carbon with low initial coulombic efficiency consumes a large amount of sodium supplied by the cathode. To match this sodium consumption, the weight of the cathode needs to be increased, but this severely limits the energy density of the battery. Therefore, developing a method for preparing coal-based hard carbon sodium storage materials with high initial coulombic efficiency and high sodium storage capacity is crucial for the large-scale application of sodium-ion batteries. Summary of the Invention
[0003] The purpose of this invention is to address the aforementioned shortcomings of the prior art by proposing a high initial coulombic efficiency and high specific capacity anthracite-based hard carbon anode sodium storage material, its preparation method, and its application.
[0004] The present invention discloses a method for preparing an anthracite-based hard carbon anode sodium storage material, comprising the following steps:
[0005] S1. Using anthracite as a base material, a porous carbon intermediate was prepared by alkaline activation method;
[0006] S2. Oxidative modification of porous carbon intermediates;
[0007] S3. The oxidized porous carbon intermediate is carbonized at high temperature to obtain anthracite-based hard carbon anode sodium storage material.
[0008] Furthermore, the specific operation of step S1 is as follows: the anthracite is thoroughly mixed and ground with a strong alkali, and then the powder is transferred to air or nitrogen for preheating and decomposition. The preheating and decomposition product is ground, acid washed, water washed, filtered, and dried to obtain activated porous carbon intermediate.
[0009] Furthermore, the strong base includes one or more of sodium hydroxide and potassium hydroxide.
[0010] Furthermore, the prepyrolysis temperature is 200–800°C; and / or: the prepyrolysis temperature is 400°C.
[0011] Furthermore, pickling involves stirring and soaking in hydrochloric acid or sulfuric acid with a concentration of 1–6 mol / L.
[0012] Furthermore, the specific operation of step S2 is as follows: oxidation is carried out using an oxidant to introduce a large number of oxygen-containing functional groups, thereby obtaining an oxidized porous carbon intermediate.
[0013] Furthermore, the oxidant is one or more of potassium permanganate and concentrated nitric acid.
[0014] Furthermore, the temperature for high-temperature carbonization in step S3 is 1000–2000°C; and / or: the temperature for high-temperature carbonization is 1400°C.
[0015] A sodium storage material based on anthracite and hard carbon anode prepared by the above-described preparation method.
[0016] An application of the anthracite-based hard carbon anode sodium storage material as described above, used as an anode material for sodium-ion batteries.
[0017] This invention utilizes structural modification methods to regulate oxygen-containing functional groups in hard carbon precursors. Subsequently, the surface oxygen-containing functional groups decompose, are removed, or transformed during carbonization to form defects or closed micropores. These closed-pore structures can significantly improve the sodium storage capacity of the low-potential plateau, reduce irreversible losses in the first cycle, and thus improve the first coulombic efficiency.
[0018] This invention employs a combination of alkaline activation and chemical oxidation to prepare anthracite-based hard carbon. Alkaline activation effectively removes coal ash and activates porous carbon intermediates, with the large specific surface area significantly promoting the subsequent chemical oxidation process. Chemical oxidation can improve the initial coulombic efficiency and specific capacity of coal-based hard carbon. For example, in nitric acid oxidation, concentrated nitric acid introduces abundant oxygen-containing functional groups, such as carbonyl and carboxyl groups. These functional groups decompose, are removed, and transformed during high-temperature carbonization, leaving numerous defects or micropores. With further increases in temperature, the rearrangement of carbon atoms and the curling of graphite microcrystals cause open micropores to evolve into closed micropores. The closed-pore structure plays a crucial role in the initial coulombic efficiency and sodium storage capacity of hard carbon materials; therefore, chemical oxidation can significantly improve electrochemical performance.
[0019] The anthracite-based hard carbon anode sodium storage material prepared by this invention has a rich closed microporous structure, thus exhibiting excellent electrochemical performance, with an initial charge capacity reaching 325.2 mAh g⁻¹. -1 The initial coulombic efficiency can reach 92.2%, and the cycle performance is good, with a capacity retention of 96.1% after 150 cycles.
[0020] The chemical oxidation method provided by this invention can effectively regulate the oxygen-containing functional groups of coal-based carbon. During high-temperature calcination, the oxygen-containing functional groups on the surface decompose, are removed or transformed during carbonization to form defects or closed micropores. The oxygen-containing functional groups have a specific effect on the formation of closed micropores in hard carbon. These closed-pore structures can significantly improve the sodium storage capacity of the low potential plateau, reduce irreversible losses in the first cycle, and thus improve the first coulombic efficiency.
[0021] This invention combines alkali activation and chemical oxidation to prepare anthracite-based hard carbon anode sodium storage material with high initial coulombic efficiency and high specific capacity, meeting the requirements for commercial hard carbon. Attached Figure Description
[0022] Figure 1 This is a schematic flowchart of the preparation method of the anthracite-based hard carbon anode sodium storage material of the present invention;
[0023] Figure 2 XPS spectra of the porous carbon intermediate before and after oxidation in Example 1;
[0024] Figure 3 XRD pattern of anthracite-based hard carbon anode sodium storage material prepared in Example 1;
[0025] Figure 4 The first charge-discharge curve of the anthracite-based hard carbon anode sodium storage material prepared in Example 1 is shown.
[0026] Figure 5 The diagram shows the cycling performance of the anthracite-based hard carbon anode sodium storage material prepared in Example 1. Detailed Implementation
[0027] The following are specific embodiments of the present invention, which are described in conjunction with the accompanying drawings to further illustrate the technical solutions of the present invention. However, the present invention is not limited to these embodiments.
[0028] Example 1
[0029] Figure 1 This is a schematic flowchart of the preparation method of the anthracite-based hard carbon anode sodium storage material of the present invention, as shown below. Figure 1 As shown, the preparation method of the anthracite-based hard carbon anode sodium storage material of the present invention is as follows:
[0030] Step 1: Mix 1.5g of anthracite and 3.0g of potassium hydroxide thoroughly in an agate mortar. Then transfer the powder to a muffle furnace for preheating at 400℃ and a heating rate of 5℃ / min. Grind the preheated product into powder using an agate mortar. Soak and wash in 200mL of 3mol / L hydrochloric acid for 2 hours. Then wash with a large amount of deionized water until the pH is neutral. Finally, filter and dry to obtain the activated porous carbon intermediate.
[0031] Step 2: The porous carbon intermediate obtained in Step 1 is oxidized with 100 mL of 14 mol / L concentrated nitric acid. After being bathed in a water bath at 60°C for 3 hours, it is washed with deionized water, filtered, and dried to obtain the chemically oxidized porous carbon intermediate.
[0032] Step 3: Transfer the porous carbon intermediate obtained in step 2 to a high-temperature tube furnace and calcine it at 1400℃ with a heating rate of 2℃ / min to obtain the hard carbon anode material for sodium-ion batteries.
[0033] Figure 2 These are the XPS spectra of the porous carbon intermediate before and after oxidation in Example 1; from Figure 2 It can be seen that the content of carboxyl and carbonyl groups in the porous carbon intermediate increases significantly after oxidation with concentrated nitric acid, indicating that the chemical oxidation method effectively introduces oxygen-containing functional groups.
[0034] Figure 3 XRD pattern of anthracite-based hard carbon anode sodium storage material prepared in Example 1; from Figure 3 It can be seen that anthracite-based hard carbon has the characteristic of bulging peaks of amorphous carbon. The interplanar spacing of carbon layers is calculated to be 0.38 nm using the Bragg formula (2dSinθ=nλ), which is within the interplanar spacing range (0.36-0.40 nm) suitable for sodium ion transport and deintercalation.
[0035] Example 2
[0036] The implementation method differs from Example 1 in that the nitric acid concentration in step two is 6 mol / L. All other steps are the same as in Example 1.
[0037] Example 3
[0038] The implementation method differs from Example 1 in that the nitric acid concentration in step two is 10 mol / L. All other steps are the same as in Example 1.
[0039] Example 4
[0040] The implementation method differs from Example 1 in that the prepyrolysis temperature in step one is 300°C. All other steps are the same as in Example 1.
[0041] Example 5
[0042] The implementation method differs from Example 1 in that the prepyrolysis temperature in step one is 500°C. All other steps are the same as in Example 1.
[0043] Example 6
[0044] The implementation method differs from Example 1 in that the high-temperature calcination temperature in step two is 1200℃. All other steps are the same as in Example 1.
[0045] Example 7
[0046] The implementation method differs from Example 1 in that the high-temperature calcination temperature in step two is 1600℃. All other steps are the same as in Example 1.
[0047] Example 8
[0048] The implementation method differs from Example 1 in that the oxidation method in step two is potassium permanganate oxidation, that is, the porous carbon intermediate obtained in step one is added to a 3 mol / L KMnO4 solution and oxidized for 3 hours. The other steps are the same as in Example 1.
[0049] Comparative Example 1
[0050] Unlike Example 1, Comparative Example 1 did not use a chemical oxidation process to control the oxygen-containing functional groups in the porous carbon. The implementation steps are as follows:
[0051] Step 1: Thoroughly grind 1.5g of anthracite and 3.0g of potassium hydroxide in an agate mortar. Then transfer the powder to a muffle furnace and preheat it in air at 400℃ with a heating rate of 5℃ / min. Grind the preheated product into powder using an agate mortar. Soak and wash the powder in 200mL of 3mol / L hydrochloric acid for 2 hours. Then wash it with a large amount of deionized water until the pH is neutral. Finally, filter and dry to obtain the activated porous carbon intermediate.
[0052] Step 2: The porous carbon intermediate obtained in step 2 is transferred to a high-temperature tube furnace and calcined at 1400℃ with a heating rate of 2℃ / min to obtain the hard carbon anode material for sodium-ion batteries.
[0053] Comparative Example 2
[0054] The implementation method differs from Comparative Example 1 in that the coal-alkali ratio in step one is 1:0, while in Comparative Example 1 it is 1:2, meaning that the anthracite is directly carbonized without alkali activation.
[0055] Comparative Example 3
[0056] The implementation method differs from Comparative Example 1 in that the coal-alkali ratio in step one is 1:1, while in Comparative Example 1 it is 1:2, and the amount added is 1.5g of anthracite and 1.5g of potassium hydroxide. The other steps are the same as in Comparative Example 1.
[0057] Comparative Example 4
[0058] The implementation method differs from Example 1 in that the oxidation method in step two is air oxidation, that is, the porous carbon intermediate obtained in step one is oxidized in air at 400°C for 2 hours, with a heating rate of 5°C / min. The other steps are the same as in Example 1.
[0059] Comparative Example 5
[0060] The implementation method differs from Example 1 in that the oxidation method in step two is hydrogen peroxide oxidation, that is, the porous carbon intermediate obtained in step one is added to a 30% H2O2 solution and oxidized for 6 hours under an 80°C water bath. The other steps are the same as in Example 1.
[0061] Electrochemical performance testing
[0062] The electrochemical performance of anthracite-based hard carbon anode sodium storage material was tested by assembling a button half-cell.
[0063] Electrode slurry was prepared using sodium carboxymethyl cellulose (CMC) as a water-based binder and styrene-butadiene rubber (SBR). A mixture of hard carbon anode material, conductive carbon black, CMC, and SBR in a mass ratio of 91:2:2:5 was weighed, and an appropriate amount of ultrapure water was added. The mixture was then thoroughly mixed and uniformly coated onto copper foil. After drying in a forced-air drying oven at 60°C for 2 hours, it was transferred to a vacuum oven at 80°C for 10 hours. Circular electrode sheets with a diameter of 10 mm were then cut and assembled into coin cells. Sodium foil served as the counter electrode, the separator was glass fiber Whatman GF / D, and the electrolyte was 1M NaPF6 in DIGLYME = 100 Vol%. The oxygen and moisture content in the glove box were both below 0.1 ppm, and the test current was 0.3C (defined as 300 mAg). -1 =1C), the test voltage range is 0.001~3V, and charge-discharge cycle test is performed. Table 1 shows the charge-discharge cycle test results of the example and the comparative example.
[0064] Figure 4 The first charge-discharge curve of the anthracite-based hard carbon anode sodium storage material prepared in Example 1 is shown below. Figure 4 As shown, the initial charge capacity was 325.2 mAh g. -1 The initial Coulomb efficiency was 92.2%.
[0065] Figure 5 The cycling performance diagram of the anthracite-based hard carbon anode sodium storage material prepared in Example 1 is shown below. Figure 5 As shown, the initial coulombic efficiency is high and the cycling performance is excellent, with a capacity retention rate of 96.1% after 150 cycles.
[0066] Table 1. Charge-discharge cycle test results of the examples and comparative examples.
[0067]
[0068] The following conclusions can be drawn from the results in the table above.
[0069] (1) As can be seen from Examples 1, 2 and 3, the first effect gradually increases with the increase of nitric acid concentration. This is related to the number of oxygen-containing functional groups introduced. The higher the concentration of nitric acid, the more oxygen-containing functional groups are introduced, which is conducive to the evolution and formation of closed-pore structures.
[0070] (2) As can be seen from Examples 1, 4, and 5, the preheating temperature also affects the performance, because the preheating temperature mainly affects the degree of alkali activation. At 300°C, the activation is insufficient, the intermediate pore structure is not rich, and fewer closed pores are formed subsequently, resulting in a lower initial effect. At 500°C, the activation is sufficient, but the micropores formed in the intermediate may be too small, and the closed pores formed subsequently are also small.
[0071] (3) As can be seen from Examples 1, 6 and 7, it is necessary to select a suitable high-temperature calcination temperature. When the temperature is too low, the closed pore size formed is small, which is not conducive to sodium storage. However, if the temperature is too high, the degree of graphitization of hard carbon will increase and the carbon interlayer spacing will decrease, which is not conducive to the transport of sodium ions between layers, thus significantly reducing the performance.
[0072] (4) The product prepared in Comparative Example 1 has better performance than that prepared in Examples 6 and 7 because the high-temperature calcination temperature of Comparative Example 1 is more suitable.
[0073] (5) Comparative Examples 1, 2, and 3 show that the higher the coal-alkali ratio, the more complete the activation and the richer the pore structure of the intermediates, thus resulting in better performance. Furthermore, when the coal-alkali ratio is 1:2, the ash in the anthracite can be completely removed, improving the first-efficiency and recycling performance of the hard carbon.
[0074] (6) As can be seen from Examples 1 and 8, and Comparative Examples 4 and 5, not all oxidants improve the electrochemical performance of anthracite-based hard carbon; some may even reduce it. This may be related to the location of the introduced oxygen-containing functional groups. For example, air oxidation and hydrogen peroxide oxidation may be non-destructive oxidation, and the oxygen-containing functional groups may be generated at the edges of the carbon layer, having no effect on the formation of closed pores. In contrast, nitric acid and potassium permanganate oxidant solutions may be destructive oxidation, and the oxygen-containing functional groups may be generated on the basal surface of the carbon layer, significantly contributing to the formation of closed pores. Therefore, it is necessary to select appropriate chemical oxidation techniques.
[0075] For any points not covered above, existing technologies shall apply.
[0076] Although specific embodiments of the present invention have been described in detail by way of examples, those skilled in the art should understand that the above examples are for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art can make various modifications or additions to the described specific embodiments or use similar methods to replace them, without departing from the direction of the invention or exceeding the scope defined by the appended claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc., made to the above embodiments based on the technical essence of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing anthracite-based hard carbon anode sodium storage material, characterized in that: Includes the following steps: S1. Using anthracite as the base material, a porous carbon intermediate is prepared by alkali activation method. The specific operation of step S1 is as follows: the anthracite is thoroughly mixed with a strong alkali, and then the powder is transferred to air or nitrogen for preheating and decomposition. S2. Oxidation modification of porous carbon intermediate; specifically, oxidation is performed using an oxidizing agent to introduce a large number of oxygen-containing functional groups, thereby obtaining an oxidized porous carbon intermediate; the oxidizing agent is one or more of potassium permanganate and concentrated nitric acid; S3. The oxidized porous carbon intermediate is carbonized at high temperature to obtain anthracite-based hard carbon anode sodium storage material.
2. The preparation method of anthracite-based hard carbon anode sodium storage material as described in claim 1, characterized in that: In step S1, the prepyrolysis product is ground, acid-washed, water-washed, filtered, and dried to obtain an activated porous carbon intermediate.
3. The preparation method of anthracite-based hard carbon anode sodium storage material as described in claim 1, characterized in that: The strong base includes one or more of sodium hydroxide and potassium hydroxide.
4. The preparation method of anthracite-based hard carbon anode sodium storage material as described in claim 1, characterized in that: The preheating temperature is 200~800℃.
5. The preparation method of anthracite-based hard carbon anode sodium storage material as described in claim 1, characterized in that: The preheating temperature is 400℃.
6. The method for preparing anthracite-based hard carbon anode sodium storage material as described in claim 2, characterized in that: Pickling involves stirring and soaking in hydrochloric acid or sulfuric acid with a concentration of 1~6 mol / L.
7. The method for preparing anthracite-based hard carbon anode sodium storage material according to any one of claims 1-6, characterized in that: The temperature for high-temperature carbonization in step S3 is 1000~2000℃.
8. The method for preparing anthracite-based hard carbon anode sodium storage material according to any one of claims 1-6, characterized in that: The high-temperature carbonization temperature in step S3 is 1400℃.
Citation Information
Patent Citations
Low-alkali activated preparation method and application of pitch-based activated carbon
CN105174260A
Soft carbon negative electrode material with disordered layer micropore structure, preparation method of soft carbon negative electrode material and sodium battery
CN116119647A