Polyimide composite film and preparation method thereof

By embedding cyclodextrin and zwitterionic polymers in the reverse osmosis membrane, forming a dense hydration layer and a hydrophobic cavity, the problem of insufficient membrane pollution and permeability is solved, and more efficient anti-pollution and separation performance is achieved.

CN119488813AActive Publication Date: 2025-02-21ZHONGFU LIANZHONG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411971507.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-30
Publication Date
2025-02-21
Estimated Expiration
2044-12-30

AI Technical Summary

Technical Problem

The existing reverse osmosis membranes are susceptible to contamination during application, resulting in reduced filtrate quality and separation efficiency, and high sensitivity to chlorine, which shortens the service life of the membrane.

Method used

A polyimide composite film is used, which forms a dense hydration layer with zwitterionic polymer by hydrophilic groups embedded in the outside of the cyclodextrin molecule, inhibits the adsorption and deposition of pollutants, and improves permeability through a hydrophobic cavity.

Benefits of technology

It effectively inhibits the adsorption and deposition of pollutants on the membrane surface, improves the film's anti-pollution and permeability, and extends the membrane's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119488813A_ABST
    Figure CN119488813A_ABST
Patent Text Reader

Abstract

The invention provides a polyimide composite film and a preparation method thereof. The polyimide composite film comprises a base film and a polyimide functional layer arranged on one side of the base film, the polyimide functional layer is embedded into a cyclodextrin monomer modified by a zwitterionic polymer. The polyimide composite membrane effectively inhibits the adsorption of pollutants on the surface of the membrane, prevents the pollutants from depositing on the surface of the membrane, and further improves the permeability of the polyimide composite membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of membrane separation and relates to a polyimide composite membrane and a preparation method thereof. Background Art

[0002] As chemical separation technology continues to develop towards high efficiency, low cost, and energy saving, membrane separation technology has been widely studied and applied due to its advantages of low energy consumption and small footprint compared to traditional chemical separation technology. Polyamide membranes are usually composed of a non-woven fabric support layer, a polymer porous middle layer, and a polyamide separation layer. They are an economical and efficient separation method in the fields of water desalination, ultrapure water production, and wastewater treatment.

[0003] Although polyamide membranes have shown great advantages, their low surface hydrophilicity and negative charge make membrane fouling a major problem in the application process, which not only reduces the filtrate quality and separation efficiency, but also shortens the service life of the membrane due to the high sensitivity of the polyamide membrane layer to chlorine. Therefore, it is of great significance to invent a reverse osmosis membrane that can simultaneously enhance antifouling ability to reduce membrane fouling and slow down membrane degradation.

[0004] Cyclodextrin (CD) is a cyclic oligosaccharide with a hydrophilic shell and a hydrophobic inner cavity. Its special structure forms a stable host-guest inclusion complex, which can effectively adsorb and remove organic pollutants. The external hydrophilic groups of cyclodextrin can improve the hydrophilicity of the membrane, reduce the adsorption and deposition of pollutants, and optimize the overall permeability performance by regulating the membrane structure. 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt (SBMA) is a commonly used ionic polymer, and its monomer contains equal amounts of quaternary ammonium salt cations and sulfonate anions. Polymethacryloylethyl sulfobetaine (pSBMA) forms two hydration layers on its surface, and its hydrophilicity is stronger than that of polymers such as polyethylene glycol. The distance between its charge groups gives it balanced charge and strong hydration ability, and it is widely used in membrane separation, antifouling coatings and other fields. Summary of the invention

[0005] In order to solve the technical problems existing in the existing reverse osmosis membrane anti-pollution technology, the present invention provides a polyimide composite membrane and a preparation method thereof, which effectively inhibits the adsorption of pollutants on the membrane surface, prevents the pollutants from depositing on the membrane surface, and further improves the permeability of the polyimide composite membrane.

[0006] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0007] One of the purposes of the present invention is to provide a polyimide composite film, which comprises a base film and a polyimide functional layer disposed on one side of the base film;

[0008] The polyimide functional layer is embedded with zwitterionic polymer-modified cyclodextrin monomers.

[0009] As a preferred technical solution of the present invention, the base membrane includes a polysulfone porous ultrafiltration membrane.

[0010] As a preferred technical solution of the present invention, the zwitterionic polymer includes polymethacryloylethyl sulfobetaine.

[0011] And / or, the cyclodextrin includes any one of α-cyclodextrin, β-cyclodextrin or γ-cyclodextrin, or a combination of at least two of them.

[0012] The second object of the present invention is to provide a method for preparing the polyimide composite film provided by the first object, the preparation method comprising:

[0013] The zwitterionic compound monomer is copolymerized with the monomer containing epoxy group to obtain the zwitterionic copolymer;

[0014] reacting cyclodextrin with a first polyamine to obtain a cyclodextrin intermediate;

[0015] reacting the cyclodextrin intermediate with a zwitterionic copolymer to obtain a zwitterionic polymer-modified cyclodextrin monomer;

[0016] A solution containing a zwitterionic polymer-modified cyclodextrin monomer and a second polyamine is loaded on one side of the base film, and a polyacyl chloride solution is coated on the side to perform surface polymerization to obtain a polyimide composite membrane.

[0017] As a preferred technical solution of the present invention, methacryloylethyl sulfobetaine, glycidyl methacrylate and a solvent are mixed and dissolved, an initiator is added and a polymerization reaction is carried out under a protective atmosphere to obtain a zwitterionic copolymer.

[0018] As a preferred technical solution of the present invention, the mass ratio of methacryloylethyl sulfobetaine, glycidyl methacrylate and solvent is 2.5-3.0:0.05-0.07:18-23.

[0019] And / or, the polymerization reaction temperature is 50-80° C. and the reaction time is 4-8 hours.

[0020] As a preferred technical solution of the present invention, cyclodextrin and an alkaline solution are mixed, and a first polyamine is added to obtain a mixed solution; epichlorohydrin is added dropwise to the mixed solution to react and obtain the cyclodextrin monomer.

[0021] And / or, the molar ratio of the cyclodextrin to the polyamine is 0.005-0.01:0.3-0.4.

[0022] And / or, the molar ratio of cyclodextrin to epichlorohydrin is 0.005-0.01:0.06-0.12.

[0023] And / or, the first polyamine includes any one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine or 1,4-butylenediamine, or a combination of at least two thereof.

[0024] And / or, the base includes any one or a combination of at least two of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide.

[0025] And / or, the reaction temperature is 50-70° C. and the reaction time is 1-2 hours.

[0026] As a preferred technical solution of the present invention, the zwitterionic copolymer, cyclodextrin monomer and solvent are mixed and reacted to obtain the zwitterionic polymer-modified cyclodextrin monomer.

[0027] And / or, the solvent includes deionized water.

[0028] And / or, the reaction temperature is 50-80° C. and the reaction time is 8-16 hours.

[0029] As a preferred technical solution of the present invention, a zwitterionic polymer-modified cyclodextrin monomer is dispersed in a second polyamine aqueous solution to obtain a dispersion; a base film is immersed in the dispersion, and excess dispersion on the surface is removed after being taken out; a polyacyl chloride solution is coated on one side of the base film immersed in the dispersion, and a thermal cross-linking reaction is performed to obtain the polyimide composite film.

[0030] As a preferred technical solution of the present invention, the second polyamine includes any one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, polyetheramine or polyethyleneimine.

[0031] And / or, the mass fraction of the zwitterionic polymer-modified cyclodextrin monomer in the dispersion is 0.1-1.0 wt %.

[0032] And / or, the infiltration time is 60 to 300 seconds.

[0033] And / or, the polyacid chloride comprises 1,3,5-benzenetricarboxylic acid chloride.

[0034] And / or, the solvent of the polyacyl chloride solution includes any one of n-hexane, cyclohexane, n-heptane, n-decane, toluene, Isopar E or Isopar G, or a combination of at least two thereof.

[0035] And / or, the temperature of the thermal cross-linking reaction is 40-90° C., and the time is 60-600 s.

[0036] Compared with the prior art, the present invention has at least the following beneficial effects:

[0037] (1) The present invention provides a polyimide composite membrane and a preparation method thereof. The polyimide composite membrane forms a dense hydration layer through the hydrophilic groups on the outside of the embedded cyclodextrin molecules and the zwitterionic polymer, which can effectively inhibit the adsorption of pollutants on the membrane surface and prevent the pollutants from being deposited on the membrane surface;

[0038] (2) The present invention provides a polyimide composite membrane and a preparation method thereof. The hydrophobic cavity inside the polyimide composite membrane is embedded in the cyclodextrin molecules, thereby further improving the permeability of the polyimide composite membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The test results of water contact angle on the surface of polyimide reverse osmosis membrane provided in Examples 1-6 and Comparative Examples 1 and 2 of the present invention;

[0040] Figure 2 This is a test result diagram of the flux attenuation rate and flux recovery rate of the polyimide reverse osmosis membrane provided in Examples 1-6 of the present invention and Comparative Examples 1 and 2.

[0041] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0042] The technical solution of the present application is further described below through specific implementation methods.

[0043] A specific embodiment of the present invention provides a polyimide composite film, which includes a base film and a polyimide functional layer disposed on one side of the base film;

[0044] The polyimide functional layer is embedded with zwitterionic polymer-modified cyclodextrin monomers.

[0045] In the present invention, the cyclodextrin molecule has a hydrophilic group on the outside and a hydrophobic cavity on the inside. This special structure enables it to form a stable host-guest structure. The hydrophilic group on the outside can enhance the hydrophilicity of the membrane, effectively reduce the adsorption and deposition of pollutants on the membrane surface, and the hydrophobic cavity of the cyclodextrin can further optimize the permeability of the overall membrane. The two hydration layers formed on the surface of the zwitterionic polymer form a dense hydration layer on the surface of the polyimide composite membrane, effectively inhibiting the adsorption of pollutants on the membrane surface and preventing pollutants from depositing on the membrane surface.

[0046] In one embodiment of the present invention, the base membrane comprises a polysulfone porous ultrafiltration membrane.

[0047] In one embodiment of the present invention, the zwitterionic polymer comprises polymethacryloylethyl sulfobetaine.

[0048] In a specific embodiment of the present invention, the cyclodextrin includes any one of α-cyclodextrin, β-cyclodextrin or γ-cyclodextrin, or a combination of at least two of them.

[0049] In a specific embodiment of the present invention, the amount of zwitterionic polymer-modified cyclodextrin monomer embedded in the base film can be adjusted according to the use environment and transmittance requirements of the polyimide composite membrane, and is not specifically limited herein.

[0050] A specific embodiment of the present invention provides a method for preparing a polyimide composite film, the preparation method comprising:

[0051] The zwitterionic compound monomer is copolymerized with the monomer containing epoxy group to obtain the zwitterionic copolymer;

[0052] reacting cyclodextrin with a first polyamine to obtain a cyclodextrin intermediate;

[0053] reacting the cyclodextrin intermediate with a zwitterionic copolymer to obtain a zwitterionic polymer-modified cyclodextrin monomer;

[0054] A solution containing a zwitterionic polymer-modified cyclodextrin monomer and a second polyamine is loaded on one side of the base film, and a polyacyl chloride solution is coated on the side to perform surface polymerization to obtain a polyimide composite membrane.

[0055] In a specific embodiment of the present invention, methacryloylethyl sulfobetaine, glycidyl methacrylate and a solvent are mixed and dissolved, and an initiator is added to carry out a polymerization reaction under a protective atmosphere to obtain a zwitterionic copolymer.

[0056] In a specific embodiment of the present invention, the mass ratio of methacryloylethyl sulfobetaine, glycidyl methacrylate and solvent is 2.5-3.0:0.05-0.07:18-23, such as 2.5:0.05:18, 2.6:0.055:19, 2.7:0.06:20, 2.8:0.062:21, 2.9:0.065:22 or 3.0:0.07:23, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] In a specific embodiment of the present invention, the solvent is preferably a mixed solution of methanol and water, wherein the volume ratio of methanol to water is preferably 1:1.

[0058] In one embodiment of the present invention, the initiator is preferably 2,2'-azobisisobutyronitrile, but is not limited to this initiator. Other initiators suitable for olefin polymerization reactions are also suitable for the present invention. The amount of the initiator added can be adjusted according to the polymerization reaction, and is not further limited here. It is preferably 1% of the mass of the mixed solution.

[0059] In a specific embodiment of the present invention, the polymerization temperature is 50-80°C and the time is 4-8h. The temperature may be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and the time may be 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h or 8h, but are not limited to the listed values, and other values ​​not listed within the above numerical ranges are also applicable.

[0060] In a specific embodiment of the present invention, after the polymerization reaction is completed, an ice bath is used to terminate the reaction, and the cooling time may be 2 to 6 hours, preferably 3 hours.

[0061] In one specific embodiment of the present invention, the copolymerization reaction equation of methacryloylethyl sulfobetaine and glycidyl methacrylate can be shown as follows:

[0062]

[0063] In a specific embodiment of the present invention, after the reaction is terminated, solid-liquid separation is performed to obtain a white solid, the white solid is dissolved in water, the precipitate is washed with methanol solvent, and freeze-dried to obtain a zwitterionic copolymer.

[0064] In a specific embodiment of the present invention, cyclodextrin and an alkaline solution are mixed, and a first polyamine is added to obtain a mixed solution; epichlorohydrin is added dropwise to the mixed solution to react and obtain the cyclodextrin monomer.

[0065] In a specific embodiment of the present invention, the molar ratio of the cyclodextrin to the polyamine is 0.005-0.01:0.3-0.4, such as 0.005:0.3, 0.006:0.32, 0.007:0.35, 0.008:0.36, 0.009:0.38 or 0.01:0.4, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] In a specific embodiment of the present invention, the molar ratio of cyclodextrin to epichlorohydrin is 0.005-0.01:0.06-0.12, such as 0.005:0.06, 0.006:0.07, 0.007:0.08, 0.008:0.09, 0.009:0.10 or 0.01:0.12, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] In a specific embodiment of the present invention, the first polyamine includes any one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine or 1,4-butylenediamine, or a combination of at least two thereof, preferably ethylenediamine.

[0068] In a specific embodiment of the present invention, the base includes any one of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide, or a combination of at least two thereof, preferably potassium hydroxide.

[0069] In a specific embodiment of the present invention, the amount of alkali added and the concentration of the alkali solution can be adjusted according to the reaction conditions while maintaining the alkalinity of the reaction system, and are not specifically limited herein.

[0070] In a specific embodiment of the present invention, the reaction temperature is 50-70°C and the reaction time is 1-2h. The reaction temperature may be 50°C, 52°C, 55°C, 58°C, 60°C, 62°C, 65°C, 68°C or 70°C, and the reaction time may be 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h or 2h, but are not limited to the values ​​listed, and other values ​​not listed within the above numerical ranges are also applicable.

[0071] In a specific embodiment of the present invention, after the reaction is completed, the pH of the reaction solution is adjusted to neutral using an acid to obtain a cyclodextrin intermediate.

[0072] In one specific embodiment of the present invention, a zwitterionic copolymer, a cyclodextrin monomer and a solvent are mixed and reacted to obtain a zwitterionic polymer-modified cyclodextrin monomer.

[0073] In one embodiment of the present invention, the solvent comprises deionized water.

[0074] In a specific embodiment of the present invention, the mass ratio of the zwitterionic copolymer, the cyclodextrin monomer and water is 0.6-1.0:0.3-0.7:8-12, such as 0.6:0.3:8, 0.7:0.4:9, 0.8:0.5:10, 0.9:0.6:11 or 1.0:0.7:12, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0075] In a specific embodiment of the present invention, the reaction temperature is 50-80°C and the reaction time is 8-16h. The reaction temperature can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, and the reaction time can be 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h or 16h, but are not limited to the listed values, and other values ​​not listed within the above numerical ranges are also applicable.

[0076] In one embodiment of the present invention, after the reaction is completed, the reaction solution is dialyzed to obtain a zwitterionic polymer-modified cyclodextrin monomer. The dialysis time may be 48 hours, the molecular weight cut-off is 3500Da, and deionized water is used as the dialysate.

[0077] In one specific embodiment of the present invention, the structure of the zwitterionic polymer-modified cyclodextrin monomer is shown below:

[0078]

[0079] In a specific embodiment of the present invention, a zwitterionic polymer-modified cyclodextrin monomer is dispersed in a second polyamine aqueous solution to obtain a dispersion; a base film is immersed in the dispersion, and excess dispersion on the surface is removed after being taken out; a polyacyl chloride solution is coated on one side of the base film immersed in the dispersion, and a thermal cross-linking reaction is performed to obtain the polyimide composite film.

[0080] In one embodiment of the present invention, the zwitterionic polymer-modified cyclodextrin monomer is dispersed in the second polyamine aqueous solution by ultrasound. The ultrasonic dispersion time may be 20 to 30 minutes.

[0081] In one embodiment of the present invention, the second polyamine includes any one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, polyetheramine or polyethyleneimine.

[0082] In a specific embodiment of the present invention, the mass fraction of the zwitterionic polymer-modified cyclodextrin monomer in the dispersion is 0.1-1.0wt%, such as 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1.0wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0083] In a specific embodiment of the present invention, the immersion time is 60 to 300 seconds, such as 60 seconds, 120 seconds, 180 seconds, 240 seconds or 300 seconds, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0084] In a specific embodiment of the present invention, after the impregnation is completed, a rubber roller or a nitrogen air knife is used to remove the excess dispersion on the surface of the base film.

[0085] In one specific embodiment of the present invention, the polyacid chloride includes 1,3,5-benzenetricarboxylic acid chloride.

[0086] In a specific embodiment of the present invention, the solvent of the polyacyl chloride solution includes any one of n-hexane, cyclohexane, n-heptane, n-decane, toluene, Isopar E or Isopar G, or a combination of at least two thereof.

[0087] In a specific embodiment of the present invention, the concentration of the polyacid chloride solution can be 0.1-1.0wt%, such as 0.1wt%, 0.2wt%, 0.3wt%, 0.4wt%, 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt% or 1.0wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0088] In a specific embodiment of the present invention, the temperature of the thermal crosslinking reaction is 40 to 90°C, and the time is 60 to 600s. The thermal crosslinking temperature can be 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, and the time can be 60s, 120s, 180s, 240s, 300s, 360s, 420s, 480s, 540s or 600s, but are not limited to the listed values, and other values ​​not listed within the above numerical ranges are also applicable.

[0089] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0090] Example 1

[0091] This embodiment provides a method for preparing a polyimide composite film, the preparation method comprising:

[0092] Synthesis of p(SBMA-co-GMA) copolymers:

[0093] Methacryloylethyl sulfobetaine monomer (SBMA monomer) and glycidyl methacrylate (GMA monomer) were dissolved in a round-bottom flask filled with a methanol / water (volume ratio = 1:1) solution, wherein the mass ratio of 3-[N,N-dimethyl-[2-(2-methylprop-2-enoyloxy)ethyl]ammonium]propane-1-sulfonic acid inner salt (SBMA monomer), glycidyl methacrylate (GMA monomer) and methanol was 2.5:0.05:20. After adding 1% equivalent of initiator 2,2'-azobisisobutyronitrile AIBN, the homogeneous solution was degassed with a nitrogen gas stream for 10 minutes and then reacted at 60°C for 6 hours. The reaction was terminated by cooling in an ice-water bath for 3 hours, and the white precipitate product was collected. Subsequently, the white precipitate was redissolved in water and the precipitate was washed with a methanol solvent. Finally, the purified p(SBMA-co-GMA) product was obtained by freeze drying for 24 hours.

[0094] Synthesis of EDA-CD:

[0095] 0.01 mol of γ-cyclodextrin was added to a 50° C. potassium hydroxide aqueous solution, followed by 0.5 mol of ethylenediamine. 0.10 mol of epichlorohydrin (ECH) was added dropwise to the mixture, while slowly heating to 60° C., reacting for 1 h, and adjusting the pH to 7 with a hydrochloric acid solution to obtain EDA-CD.

[0096] Synthesis of pSBMA-CD:

[0097] p(SBMA-co-GMA) copolymer and EDA-CD were added to deionized water and reacted at 60°C for 12 hours. The mass ratio of p(SBMA-co-GMA) copolymer, EDA-CD and deionized water was 1.0:0.5:10, and the reaction product was obtained by dialyzing the solution for 48 hours (molecular weight cutoff 3500Da, using deionized water as the dialysate).

[0098] Preparation of polyimide composite membrane:

[0099] An aqueous solution containing 2.5 wt% of m-phenylenediamine, 3.0 wt% of camphorsulfonic acid and 1.5 wt% of triethylamine is prepared; 0.1 wt% of pSBMA-CD is added to the aqueous solution and the solution is evenly dispersed by ultrasonication for 20 min;

[0100] Using Isopar G isoparaffin as an organic solvent, an organic phase solution containing trimesoyl chloride at a concentration of 0.12 wt% was prepared;

[0101] The polysulfone PSF ultrafiltration base was fixed in a plexiglass frame, and the membrane surface was immersed in the aqueous solution for 120 seconds. Then, a nitrogen air knife was used to remove excess aqueous monomer solution on the surface of the ultrafiltration base membrane. It was then contacted with the organic solution for 60 seconds to remove excess organic solution, and then evenly purged until there was no residual solvent on the membrane surface. It was then placed in an 80°C oven for heat treatment for 5 minutes. After being taken out of the oven, it was rinsed with pure water.

[0102] Example 2

[0103] In this example, except that the concentration of pSBMA-CD in the aqueous phase is 0.2 wt % and the ultrasonic dispersion time is 25 min, the other conditions are the same as those in Example 1.

[0104] Example 3

[0105] In this example, except that the concentration of pSBMA-CD in the aqueous phase is 0.4 wt % and the ultrasonic dispersion time is 30 min, the other conditions are the same as those in Example 1.

[0106] Example 4

[0107] In this example, except that the concentration of pSBMA-CD in the aqueous phase is 0.6 wt % and the ultrasonic dispersion time is 35 min, the other conditions are the same as those in Example 1.

[0108] Example 5

[0109] In this example, except that the concentration of pSBMA-CD in the aqueous phase is 0.8 wt % and the ultrasonic dispersion time is 40 min, the other conditions are the same as those in Example 1.

[0110] Example 6

[0111] In this example, except that the concentration of pSBMA-CD in the aqueous phase was 1.0 wt % and the ultrasonic dispersion time was 45 min, the other conditions were the same as those in Example 1.

[0112] Comparative Example 1

[0113] This comparative example provides a method for preparing a polyamide reverse osmosis membrane, the preparation method comprising:

[0114] A casting solution containing 17 wt% polysulfone is prepared in N,N-dimethylformamide; after being stirred evenly, the casting solution is placed in a vacuum oven for 6 hours for degassing; then, the casting solution is poured and applied on a polyester non-woven fabric using an automatic film scraping machine, and immediately immersed in a 25°C deionized water coagulation bath to complete phase inversion, and then placed in pure water for soaking for standby use;

[0115] Prepare an aqueous solution containing 2.5 wt % of m-phenylenediamine, 3.0 wt % of camphorsulfonic acid and 1.5 wt % of triethylamine;

[0116] Using Isopar G isoparaffin as an organic solvent, an organic phase solution containing trimesoyl chloride at a concentration of 0.12 wt% was prepared;

[0117] The polysulfone PSF ultrafiltration base was fixed in a plexiglass frame, and the membrane surface was immersed in the aqueous solution for 120 seconds. Then, a nitrogen air knife was used to remove excess aqueous monomer solution on the surface of the ultrafiltration base membrane. It was then contacted with the organic solution for 60 seconds, and the excess organic solution was poured off. The membrane was then evenly purged until there was no residual solvent on the membrane surface. It was then placed in an 80°C oven for heat treatment for 5 minutes. After being taken out of the oven, it was rinsed with pure water.

[0118] Comparative Example 2

[0119] This comparative example provides a method for preparing a polyamide reverse osmosis membrane, the preparation method comprising:

[0120] An aqueous solution containing 2.5 wt% of m-phenylenediamine, 3.0 wt% of camphorsulfonic acid and 1.5 wt% of triethylamine is prepared; 0.4 wt% of γ-CD is added to the aqueous solution and the mixture is evenly dispersed by ultrasonication for 30 minutes;

[0121] Using Isopar G isoparaffin as an organic solvent, an organic phase solution containing trimesoyl chloride at a concentration of 0.12 wt% was prepared;

[0122] The polysulfone PSF ultrafiltration base was fixed in a plexiglass frame, and the membrane surface was immersed in the aqueous solution for 120 seconds. Then, a nitrogen air knife was used to remove excess aqueous monomer solution on the surface of the ultrafiltration base membrane. It was then contacted with the organic solution for 60 seconds, and the excess organic solution was poured off. The membrane was then evenly purged until there was no residual solvent on the membrane surface. It was then placed in an 80°C oven for heat treatment for 5 minutes. After being taken out of the oven, it was rinsed with pure water.

[0123] The performance of the polyamide reverse osmosis membranes prepared in Examples 1-6 and Comparative Examples 1 and 2 was tested, and the results are shown in Table 1.

[0124] Test method: The feed liquid is a 2000ppm sodium chloride aqueous solution, the solution pH is 7.0±0.5, the operating pressure is 225psi (1.55MPa), and the operating temperature is 25±1°C. For the anti-pollution performance test, protein is used as turbidity for anti-pollution test, and water flux test is carried out according to GB / T 32373-2015 reverse osmosis membrane test method.

[0125] Table 1

[0126] Experimental group name Flux (LMH) NaCl retention rate (%) Comparative Example 1 44.56 99.07 Comparative Example 2 49.51 98.43 Example 1 53.42 98.95 Example 2 55.97 99.30 Example 3 61.22 99.35 Example 4 62.38 99.21 Example 5 60.72 99.18 Example 6 58.93 99.04

[0127] The hydrophilicity of the surface of the polyamide reverse osmosis membranes prepared in Examples 1-6 and Comparative Examples 1 and 2 was tested using a contact angle tester. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that in Examples 1-6, as the loading amount of pSBMA-CD increases, the water contact angle on the surface of the polyamide reverse osmosis membrane becomes smaller and the hydrophilicity becomes better, indicating that the denser the surface hydration layer is, the better the anti-fouling performance is. The loading amount of pSBMA-CD in Example 3 is the same as the loading amount of γ-CD in Comparative Example 2, and the hydrophilicity of the surface of the polyamide reverse osmosis membrane in Example 3 is better than that in Comparative Example 2. Comparative Example 1 does not load pSBMA-CD or γ-CD, and its surface hydrophilicity is the worst.

[0128] The flux attenuation rate and flux recovery rate of the polyamide reverse osmosis membranes prepared in Examples 1-6 and Comparative Examples 1 and 2 were tested. The test method is: pre-press the reverse osmosis membrane with pure water for 30 minutes. The initial flux J at this time is recorded.0 Add model pollutant (BSA) to pure water solution at a concentration of 500ppm. Record the instantaneous flux after membrane surface contamination J t When the contamination reaches a stable state, stop the experiment and clean and resume the test: use pure water (without pressure) to rinse the membrane surface and record the flux after rinsing J c .

[0129] Flux decay rate: FDR (%) = (J 0 -J t ) / J 0* 100%

[0130] Flux recovery rate: FRR (%) = J c / J 0* 100%

[0131] The results are as follows Figure 2 As shown, from Figure 2 It can be seen that compared with the comparative example, as the loading amount of pSBMA-CD increases, the flux attenuation rate of the embodiment decreases and the recovery rate increases, and the flux recovery rate of Example 3 reaches 96%, indicating that its anti-fouling performance has been significantly improved. In the polyamide membrane, the incorporation of pSBMA-CD effectively inhibits the adsorption of pollutants on the membrane surface and prevents the deposition of pollutants on the membrane surface.

[0132] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0133] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0134] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0135] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A polyimide composite film, characterized in that: The polyimide composite film comprises a base film and a polyimide functional layer disposed on one side of the base film; The polyimide functional layer is embedded with zwitterionic polymer-modified cyclodextrin monomers.

2. The polyimide composite film according to claim 1, characterized in that: The base membrane includes a polysulfone porous ultrafiltration membrane.

3. The polyimide composite film according to claim 1, characterized in that: The zwitterionic polymer includes polymethacryloylethyl sulfobetaine; And / or, the cyclodextrin includes any one of α-cyclodextrin, β-cyclodextrin or γ-cyclodextrin, or a combination of at least two of them.

4. A method for preparing a polyimide thin composite film according to any one of claims 1 to 3, characterized in that: The preparation method comprises: The zwitterionic compound monomer is copolymerized with the monomer containing epoxy group to obtain the zwitterionic copolymer; reacting cyclodextrin with a first polyamine to obtain a cyclodextrin intermediate; reacting the cyclodextrin intermediate with the zwitterionic copolymer to obtain a zwitterionic polymer-modified cyclodextrin monomer; A solution containing a zwitterionic polymer-modified cyclodextrin monomer and a second polyamine is loaded on one side of the base film, and a polyacyl chloride solution is coated on the side to perform surface polymerization to obtain the polyimide composite film.

5. The preparation method according to claim 4, characterized in that: Methacryloylethyl sulfobetaine, glycidyl methacrylate and a solvent are mixed and dissolved, an initiator is added, and a polymerization reaction is carried out under a protective atmosphere to obtain a zwitterionic copolymer.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the methacryloylethyl sulfobetaine, glycidyl methacrylate and solvent is 2.5-3.0:0.05-0.07:18-23; And / or, the polymerization reaction temperature is 50-80° C. and the reaction time is 4-8 hours.

7. The preparation method according to claim 4, characterized in that: Mixing cyclodextrin and an alkaline solution, adding a first polyamine to obtain a mixed solution; dropping epichlorohydrin into the mixed solution to react and obtain the cyclodextrin monomer; and / or, the molar ratio of the cyclodextrin to the polyamine is 0.005-0.01:0.3-0.4; And / or, the molar ratio of cyclodextrin to epichlorohydrin is 0.005-0.01:0.06-0.12; and / or, the first polyamine includes any one of ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine or 1,4-butylenediamine, or a combination of at least two thereof; and / or, the base comprises any one or a combination of at least two of sodium carbonate, potassium carbonate, sodium hydroxide or potassium hydroxide; And / or, the reaction temperature is 50-70° C. and the reaction time is 1-2 hours.

8. The preparation method according to claim 4, characterized in that: The zwitterionic copolymer, cyclodextrin monomer and solvent are mixed to react to obtain the zwitterionic polymer-modified cyclodextrin monomer; and / or, the solvent comprises deionized water; And / or, the reaction temperature is 50-80° C. and the reaction time is 8-16 hours.

9. The preparation method according to claim 4, characterized in that: The zwitterionic polymer-modified cyclodextrin monomer is dispersed in a second polyamine aqueous solution to obtain a dispersion; the base film is immersed in the dispersion, and excess dispersion on the surface is removed after being taken out; a polyacyl chloride solution is applied to one side of the base film immersed in the dispersion, and a thermal crosslinking reaction is performed to obtain the polyimide composite film.

10. The preparation method according to claim 9, characterized in that: The second polyamine includes any one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, polyetheramine or polyethyleneimine; and / or, the mass fraction of the zwitterionic polymer-modified cyclodextrin monomer in the dispersion is 0.1 to 1.0 wt %; And / or, the infiltration time is 60 to 300 seconds; And / or, the polyacid chloride comprises 1,3,5-benzenetricarboxylic acid chloride; and / or, the solvent of the polyacyl chloride solution comprises any one of n-hexane, cyclohexane, n-heptane, n-decane, toluene, Isopar E or Isopar G, or a combination of at least two thereof; And / or, the temperature of the thermal cross-linking reaction is 40-90° C., and the time is 60-600 s.

Citation Information

Patent Citations

  • Micromolecular zwitterion modified surface polyamide composite membrane and preparation method thereof

    CN111558300A

  • Tannic acid-hydroxypropyl beta cyclodextrin composite nanofiltration membrane and preparation method thereof