An ethylene-α-olefin multi-component copolymer, its preparation method and application
By controlling the ratio of liquid to gaseous materials and the type of catalyst in a fluidized bed reactor, ethylene-α-olefin multi-component copolymers with low haze, high transmittance, and high volume resistivity are generated, solving the problems of high production cost and excessive solvent use in existing technologies and broadening their application in the field of photovoltaic films.
Patent Information
- Application Number
- CN202311035443.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-16
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-16
AI Technical Summary
Existing technologies are insufficient for the efficient production of ethylene-octene copolymers with low haze, high transmittance, and high volume resistivity. Furthermore, traditional processes suffer from high costs, excessive solvent usage, and poor environmental performance, which limits their application in the photovoltaic encapsulant film field.
The gas-phase fluidized bed process is adopted. By injecting liquid material into the fluidized bed reactor, a three-phase region of gas, liquid and solid is formed. By controlling the ratio of liquid material to gas material and the type of catalyst, the concentration of octene and the mass transfer rate are increased, and high molecular weight, high octene content ethylene-α-olefin multi-component copolymer is generated.
The production of ethylene-α-olefin multi-component copolymers with low haze, high light transmittance, and high volume resistivity reduces production costs, increases product density and crystallinity, and is suitable for photovoltaic films, thus reducing dependence on imported materials.
Smart Images

Figure CN119505057B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of olefin polymerization technology, specifically to an ethylene-α-olefin multi-component copolymer, its preparation method, and its application. Background Technology
[0002] Ethylene-octene copolymers have attracted significant attention from petrochemical companies both domestically and internationally due to their superior performance and broad application prospects. Particularly in the field of photovoltaic encapsulants, polyolefin materials, represented by ethylene-octene copolymer (POE), possess excellent light transmittance, electrical insulation, moisture barrier properties, and outstanding weather resistance and resistance to induced potential decay (PID). They are considered ideal materials to replace ethylene-vinyl acetate copolymer (EVA) encapsulation materials. The high branched content of POE enhances the light transmittance of photovoltaic encapsulants, while the saturation of its molecular chains gives them excellent heat aging resistance and UV resistance. Therefore, POE has immense application potential in the photovoltaic encapsulant field.
[0003] The main production processes for ethylene-octene copolymers include solution polymerization, dispersion polymerization, and slurry polymerization. Solution polymerization, currently the mainstream process for producing ethylene / 1-octene copolymers, although generally using lower polymer concentrations in the reaction system, allows for control over the molecular weight and distribution, comonomer content, and stereoregularity of the resulting polymer by selecting appropriate reactor conditions. In solution polymerization, the monomers and polymers dissolve in an inert solution, thus avoiding the adhesion problem caused by the adsorption of large amounts of octene on the surface of polyethylene particles, as seen in gas-phase polymerization. This allows for the production of ethylene-octene copolymers across the entire density range. However, solution polymerization involves reactions at relatively high temperatures (200°C or higher), and the commonly used Ziegler-Natta catalysts generally have low activity, necessitating the removal of residues from the polymer and requiring an additional slag removal process. Furthermore, solution polymerization suffers from high production costs, difficult solvent separation, high energy consumption, and expensive products, limiting the widespread application of ethylene-octene copolymers. Currently, solution polymerization technology is entirely owned by foreign companies, and original research and applications of ethylene / 1-octene copolymers in China are extremely rare. Dispersion polymerization is reported in patents such as CN103384686A. Although the patent claims that the polymer concentration can reach 40 wt%, this technology is still in the laboratory pilot stage and there are no reports of industrialization. As for the slurry method, due to the low melting point of ethylene / 1-octene copolymers, they swell easily in solvents, and the products are prone to melting and agglomeration, making stable and efficient production difficult.
[0004] Currently, the domestic ethylene-octene copolymer market is still characterized by structural overcapacity and weak production competitiveness. There is a shortage of high-performance and multi-functional specialty grades, failing to meet domestic market demand, including in the photovoltaic encapsulant film sector. Therefore, there is an urgent need to innovate the production processes and technologies for ethylene-octene copolymers to enhance their market competitiveness and reduce reliance on imports.
[0005] Gas-phase fluidized bed ethylene polymerization is the mainstream process, accounting for over 40% of global polyethylene production capacity. However, if gas-phase fluidized bed polymerization is directly used for the production of ethylene-octene copolymers, there are problems such as low octene partial pressure and low octene / ethylene ratio in the gas phase, making it difficult to increase the octene insertion rate in the product.
[0006] Industrial trials have shown that improvements to existing gas-phase fluidized bed production equipment and processes can produce linear low-density ethylene-α-olefin multi-component copolymers containing octene components, exhibiting low haze, high transmittance, and high volume resistivity. These copolymers are suitable for preparing photovoltaic films and are expected to significantly expand the high-end application market for linear low-density polyethylene (LLDPE) materials. Furthermore, the fluidized bed process offers advantages such as simple operation, solvent-free production, environmental friendliness, and low cost. Using LLDPE to replace POE in photovoltaic film preparation will significantly reduce production costs, which is of great significance for developing high-performance, domestically produced ethylene-octene copolymer-specific materials. Summary of the Invention
[0007] To address the aforementioned problems, this invention provides an ethylene-α-olefin multi-component copolymer, its preparation method, and its applications. The ethylene-α-olefin multi-component copolymer features low haze, high light transmittance, and high volume resistivity, making it suitable for photovoltaic film manufacturing. Furthermore, the production process is simple to operate, solvent-free, environmentally friendly, and low-cost.
[0008] To address the aforementioned technical problems, the first aspect of this invention provides an ethylene-α-olefin multi-component copolymer with a haze of 1%–7%, a light transmittance >87%, and a volume resistivity >5.0 × 10⁻⁶. 17 Ω·cm, weight-average molecular weight of 70,000–130,000, crystallinity of 15%–35%.
[0009] According to some embodiments of the present invention, based on the total molar amount of the ethylene-α-olefin multi-component copolymer, the molar content of the ethylene structural unit in the ethylene-α-olefin multi-component copolymer is 80 mol% to 96 mol%, the molar content of the 1-butene structural unit is 2.0 mol% to 10 mol%, the molar content of the 1-hexene structural unit is 0 mol% to 3.5 mol%, and the molar content of the 1-octene structural unit is 0.3 mol% to 15 mol%.
[0010] In this invention, the content of ethylene structural units, 1-butene structural units, 1-hexene structural units, and 1-octene structural units in the ethylene-α-olefin copolymer is determined using a Bruker Advance 2B 400MHz analyzer. 13 Measured by C-NMR. The ethylene structural unit is a vinyl group unit connected to the molecular chain via carbon-carbon covalent bonds; the 1-butene structural unit is a 1-butene group unit connected to the molecular chain via carbon-carbon covalent bonds; the 1-hexene structural unit is a 1-hexene group unit connected to the molecular chain via carbon-carbon covalent bonds; and the 1-octene structural unit is a 1-octene group unit connected to the molecular chain via carbon-carbon covalent bonds.
[0011] According to some embodiments of the present invention, the DSC melting curve of the ethylene-α-olefin multi-component copolymer includes a first melting peak T1 and a second melting peak T2; preferably, the temperature range of the first melting peak T1 is 105℃~135℃, and the temperature range of the second melting peak T2 is 90℃~110℃; more preferably, the ratio of the peak area of the second melting peak T2 to the peak area of the first melting peak T1 is 0.01~0.5.
[0012] In this invention, the temperature distribution of the first melting peak T1 refers to the distribution of the melting temperature Tm1 corresponding to the first melting peak T1 in the DSC melting curve of the copolymer; the temperature distribution of the second melting peak T2 refers to the distribution of the melting temperature Tm2 corresponding to the second melting peak T2 in the DSC melting curve of the copolymer.
[0013] In this invention, the area of the first melting peak ST1 and the area of the second melting peak ST2 are obtained by integrating the DSC melting curve of the copolymer.
[0014] According to some embodiments of the present invention, the molecular weight distribution index of the ethylene-α-olefin copolymer is 2 to 8, preferably 3 to 5.
[0015] According to some embodiments of the present invention, the density of the ethylene-α-olefin copolymer is 0.885 g / cm³. 3 ~0.930g / cm 3 0.89g / cm 3 ~0.92g / cm 3 Under conditions of 190℃ and 2.16kg load, the melt index of the ethylene-α-olefin copolymer is 0.5g / 10min to 15g / 10min, preferably 0.58g / 10min to 8g / 10min; the melting point of the ethylene-α-olefin copolymer is 80℃ to 130℃, preferably 100℃ to 125℃.
[0016] A second aspect of the present invention provides a method for preparing the above-mentioned ethylene-α-olefin multi-component copolymer, comprising, in the presence of a catalyst, contacting liquid phase material A from the sidewall of a fluidized bed reactor with liquid phase material B from the bottom of the fluidized bed reactor and a gaseous material containing ethylene to react and generate the ethylene-α-olefin multi-component copolymer.
[0017] According to some embodiments of the present invention, the α-olefin is selected from at least two of 1-butene, 1-hexene, and 1-octene; the liquid phase material A and the liquid phase material B may be the same or different, and each independently includes the α-olefin and an inert condenser; the mass flow rate ratio of the liquid phase material A to the liquid phase material B is 1:(2-50).
[0018] According to some embodiments of the present invention, the inert condenser is selected from saturated straight-chain or branched alkanes of C3 to C10 and cycloalkanes of C3 to C10; more preferably, the inert condenser is selected from saturated straight-chain or branched alkanes of C4 to C6 and cycloalkanes of C4 to C6; even more preferably, the inert condenser is selected from at least one of isopentane, n-pentane, n-hexane, cyclohexane, and n-heptane.
[0019] According to some embodiments of the present invention, the catalyst comprises a main catalyst and a co-catalyst; preferably, the main catalyst is selected from at least one of Ziegler-Natta catalysts, metallocene catalysts, chromium-based catalysts, and transition metal catalysts; the co-catalyst is selected from at least one of modified methylaluminoxane (commercially available), diethylaluminum chloride, diisobutylaluminum chloride, sesquiethylaluminum chloride, diisobutylaluminum, diethylaluminum chloride, trimethylaluminum, methylaluminoxane, triethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum hydrogen, and diisobutylaluminum hydrogen.
[0020] According to some embodiments of the present invention, the gaseous material further includes at least two of ethylene, 1-butene, 1-hexene, 1-octene, an inactive gas, and an optional molecular weight regulator; preferably, the inactive gas is selected from at least one of nitrogen, hexane, ethane, and propane.
[0021] According to some embodiments of the present invention, the preparation method further includes using unreacted reaction raw material gas as circulating gas to flow out from the top outlet of the fluidized bed reactor, and after compression, heat exchange, and gas-liquid separation, to obtain liquid phase material A, liquid phase material B, and gas phase material containing ethylene, which then enter the fluidized bed reactor.
[0022] According to some embodiments of the present invention, the unreacted reaction feed gas comes from unreacted liquid phase material A, unreacted liquid phase material B, and unreacted gaseous material containing ethylene; the unreacted reaction feed gas includes ethylene, 1-butene, 1-hexene, 1-octene, an inert condenser, and an optional molecular weight regulator; the molecular weight regulator is preferably hydrogen.
[0023] According to some embodiments of the present invention, the ratio of the mass flow rate of the liquid phase material A to the mass flow rate of the circulating gas is 0.005 to 0.2.
[0024] According to some embodiments of the present invention, in the circulating gas, the molar ratio of 1-butene to ethylene is 0.01 to 0.8; the molar ratio of 1-hexene to ethylene is 0 to 0.03; the molar ratio of 1-octene to ethylene is 0.001 to 0.05; the molar ratio of molecular weight regulator to ethylene is 0 to 0.8; and the molar content of inert condenser is 5% to 25%.
[0025] According to some embodiments of the present invention, the injection position of the liquid phase material A is 0.2D to 4D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor, and the injection position of the liquid phase material A includes at least one liquid injection pipeline.
[0026] According to some embodiments of the present invention, the reaction conditions include: a pressure of 1.8 MPa to 2.5 MPa, a reaction temperature of 40°C to 90°C, and an apparent fluidizing gas velocity of 0.55 m / s to 0.75 m / s.
[0027] A third aspect of the present invention provides a system for preparing the above-mentioned ethylene-α-olefin multi-component copolymer, comprising: a fluidized bed reactor, a compression unit, a heat exchange unit, a gas-liquid separation unit, a condensate storage unit, and a catalyst feeding unit;
[0028] The fluidized bed reactor is equipped with a distribution plate;
[0029] The top outlet of the fluidized bed reactor is connected to a compression unit via a pipeline, the compression unit being used to pressurize the circulating gas;
[0030] The outlet of the compression unit is connected to the heat exchange unit via a pipeline, and the heat exchange unit is used to cool the circulating gas compressed by the compression unit.
[0031] The outlet of the heat exchanger is connected to a gas-liquid separation unit via a pipeline. The gas-liquid separation unit is used to separate the circulating gas cooled by the heat exchanger.
[0032] The liquid phase outlet of the gas-liquid separation unit is connected to the condensate storage unit via a pipeline. The condensate storage unit introduces the stored liquid phase material into the fluidized bed reactor from different positions on the side wall above the distribution plate of the fluidized bed reactor via a feed pump. The gas phase outlet of the gas-liquid separation unit is connected to the bottom inlet of the fluidized bed reactor via a pipeline, and the gas phase material and the remaining liquid phase material are injected into it.
[0033] The catalyst is added to the fluidized bed reactor via the catalyst feed unit and the catalyst feed pipeline;
[0034] The ethylene-α-olefin copolymer is discharged from the fluidized bed reactor through the discharge pipeline.
[0035] The fourth aspect of the present invention provides an application of the above-mentioned ethylene-α-olefin multi-component copolymer in the preparation of photovoltaic films.
[0036] Beneficial effects:
[0037] This invention generates a gas-liquid-solid three-phase region containing atomized droplets and wet particles by spraying liquid materials into a fluidized bed reactor. This region exhibits high concentrations of 1-octene, 1-butene, and 1-hexene, low concentrations of ethylene and hydrogen, and a fast mass transfer rate of the comonomers. In contrast, traditional gas-phase polymerization methods have low concentrations of 1-octene, 1-butene, and 1-hexene, high concentrations of ethylene and hydrogen, and a relatively slow mass transfer rate of the comonomers. Therefore, this invention can generate a polyethylene component with high molecular weight, high 1-octene content, and high branching degree in the gas-liquid-solid three-phase region, resulting in reduced density, crystallinity, and haze, and increased light transmittance in the final product. Simultaneously, the high catalyst activity and low residual ash content reduce the product's volume resistivity. Based on this principle and method, this invention provides a low-haze, high-transmittance, and high-volume-resistivity ethylene-α-olefin multi-component copolymer, which, compared to an ethylene-octene copolymer POE (density 0.86–0.89 g / cm³) with equivalent haze or transmittance, is comparable to such a copolymer. 3 It has a higher density compared to other materials; and a lower crystallinity compared to ordinary linear low-density polyethylene (LLDPE) (35%–65% crystallinity).
[0038] This invention provides a method and system for producing ethylene-α-olefin multi-component copolymers in a fluidized bed reactor. By controlling the ratio of the mass flow rate of liquid material A entering the fluidized bed reactor to the mass flow rate of circulating gas, as well as the molar ratios of 1-butene / ethylene, 1-hexene / ethylene, 1-octene / ethylene, molecular weight regulator / ethylene, molar content of inert condenser, and injection position of liquid material A, ethylene-α-olefin multi-component copolymers with low haze, high transmittance, and high volume resistivity are obtained. Attached Figure Description
[0039] Figure 1 This is a schematic diagram of the production system for the ethylene-α-olefin multi-component copolymer described in this invention;
[0040] Figure 1 In the diagram, 1-fluidized bed reactor, 2-distribution plate, 3-compression unit, 4-heat exchange unit, 5-gas-liquid separation unit, 6-condensate storage unit, 7-feed pump, 8-catalyst feed unit, 9-circulation pipeline, 10-fluid pipeline, 11-bottom inlet of fluidized bed reactor, 12-catalyst feed pipeline, 13-ethylene and α-olefin multi-component copolymer discharge pipeline, 14-ethylene monomer feed pipeline, 15-molecular weight regulator feed pipeline, 16-1-butene, 1-hexene, 1-octene monomer feed pipeline, 17-inert condensate feed pipeline.
[0041] Figure 2 This is the DSC melting curve of the ethylene-α-olefin multi-component copolymer prepared in Example 1 of this invention. Detailed Implementation
[0042] The present invention will be further described below with reference to embodiments. However, the present invention is not limited to these embodiments.
[0043] The weight-average molecular weight and molecular weight distribution index of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention were determined by gel permeation chromatography (GPC) using a Polymer Laboratories PL-220 instrument; the column and rotating compartment were operated at 140℃; the solvent was 1,2,4-trichlorobenzene, and the concentration of the ethylene-α-olefin multi-component copolymer was 3‰; the injection volume was 100uL, and the flow rate was 1.0mL / min.
[0044] The haze of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention was determined according to GB / T2410.
[0045] The transmittance of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention was determined according to GB / T 2410.
[0046] The volume resistivity of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention was determined according to GB / T1410.
[0047] The tensile breaking strength of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention was determined according to GB / T1040.
[0048] The dart impact fracture quality of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention was determined according to GB / T9639.
[0049] The melt index of the ethylene-α-olefin multi-component copolymer prepared in the embodiments of the present invention was determined according to GB / T3682.
[0050] The density of the ethylene-α-olefin copolymer prepared in the embodiments of the present invention was determined according to the method of GB / T 1033.
[0051] The melting point and crystallinity of the ethylene-α-olefin multi-component copolymer prepared in this embodiment of the invention were determined by differential scanning calorimetry (DSC). The specific method was as follows: under a nitrogen atmosphere, the temperature was increased from room temperature to 160°C at a rate of 10°C / min and held at that temperature for 3 min to eliminate thermal history; then the temperature was decreased to 30°C at a rate of 10°C / min; then the temperature was increased from 30°C to 160°C at a rate of 10°C / min to obtain the melting curve, and the melting point and enthalpy of fusion were recorded to calculate the crystallinity.
[0052] Reference Figure 1 The fresh gaseous materials required for the reaction enter the gas circulation pipeline 9 through the ethylene monomer feed pipeline 14, the molecular weight regulator enters the gas circulation pipeline 9 through the molecular weight regulator feed pipeline 15, the comonomers enter the gas circulation pipeline 9 through the 1-butene, 1-hexene, and 1-octene monomer feed pipelines 16, the inert condenser enters the gas circulation pipeline 9 through the inert condenser feed pipeline 17, the catalyst enters the fluidized bed reactor 1 intermittently or continuously through the catalyst feed unit 8 and the catalyst feed pipeline 12, and the ethylene-α-olefin multi-component copolymer product flows out intermittently or continuously from the ethylene-α-olefin multi-component copolymer discharge pipeline 13.
[0053] In this process, the gaseous material after the reaction flows out from the top of the fluidized bed reactor 1 and enters the gas circulation pipeline 9. After passing through the compression unit 3 and the heat exchange unit 4, it enters the gas-liquid separation unit 5. The gas-liquid separation unit 5 separates all or part of the liquid phase material and then enters the condensate storage unit 6. The condensate is then introduced into the bed of the fluidized bed reactor 1 from different positions on the side wall above the distribution plate 2 of the fluidized bed reactor 1 by the feed pump 7. The unseparated material enters the fluidized bed reactor 1 through the bottom inlet 11 of the fluidized bed reactor 1.
[0054] Example 1
[0055] This embodiment provides a method for preparing an ethylene-α-olefin multi-component copolymer.
[0056] exist Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0057] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.07; in the circulating gas, the molar ratios of 1-butene / ethylene are 0.30, 1-hexene / ethylene, and 1-octene / ethylene are 0.008, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.12, and the molar content of inert condenser is 9%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point of liquid phase material A includes one liquid injection pipeline.
[0058] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.912 g / cm³. 3 The melt flow index is 0.70 g / 10 min, the crystallinity is 32%, the weight-average molecular weight is 80,000, the molecular weight distribution index is 3.5, the haze is 6.4%, the transmittance is 88%, and the volume resistivity is 5.8 × 10⁻⁶. 17 Ω·cm, tensile strength at break is 25MPa, and dart impact fracture mass is 215g; DSC melt curve is as follows. Figure 2 As shown, the temperature range of the first melting peak T1 is 110℃~128℃, and the temperature range of the second melting peak T2 is 90℃~110℃; the peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.1, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 122℃.
[0059] Example 2
[0060] This embodiment provides an ethylene-α-olefin multi-component copolymer.
[0061] exist Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0062] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.09; in the circulating gas, the molar ratio of 1-butene / ethylene is 0.32, the molar ratio of 1-hexene / ethylene is 0.010, the molar ratio of 1-octene / ethylene is 0.009, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.10, and the molar content of inert condenser is 9%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor, and the injection point of liquid phase material A includes one liquid injection pipeline.
[0063] The density of the ethylene-α-olefin copolymer obtained in Example 1 is 0.909 g / cm³. 3 The melt flow index is 0.60 g / 10 min, the crystallinity is 29%, the weight-average molecular weight is 95,000, the molecular weight distribution index is 3.3, the haze is 5.6%, the transmittance is 90%, and the volume resistivity is 6.0 × 10⁻⁶. 17 The tensile strength at break is 26 MPa, and the dart impact fracture mass is 219 g. In the DSC melting curve, the temperature range of the first melting peak T1 is 105℃~130℃, and the temperature range of the second melting peak T2 is 90℃~105℃. The peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.17, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 121℃.
[0064] Example 3
[0065] This embodiment provides an ethylene-α-olefin multi-component copolymer.
[0066] exist Figure 1The production system shown employs a catalytic system including a metallocene catalyst and a methylaluminoxane co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0067] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.09; in the circulating gas, the molar ratios of 1-butene / ethylene are 0.32, 1-hexene / ethylene, and 1-octene / ethylene are 0.009, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.10, and the molar content of inert condenser is 9%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point of liquid phase material A includes one liquid injection pipeline.
[0068] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.895 g / cm³. 3 The melt flow index is 0.66 g / 10 min, the crystallinity is 22%, the weight-average molecular weight is 88,000, the molecular weight distribution index is 3.0, the haze is 5.0%, the transmittance is 94%, and the volume resistivity is 9.0 × 10⁻⁶. 17 The tensile strength at break is 25 MPa, and the dart impact breakage mass is 230 g. In the DSC melting curve, the temperature range of the first melting peak T1 is 105℃~127℃, and the temperature range of the second melting peak T2 is 90℃~105℃. The peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.20, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 120.3℃.
[0069] Example 4
[0070] This embodiment provides an ethylene-α-olefin multi-component copolymer.
[0071] exist Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0072] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.09; in the circulating gas, the molar ratios of 1-butene / ethylene are 0.33, 1-hexene / ethylene are 0.014, 1-octene / ethylene are 0.012, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.09, and the molar content of inert condenser is 12%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point of liquid phase material A includes one liquid injection pipeline.
[0073] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.900 g / cm³. 3 The melt flow index is 0.58 g / 10 min, the crystallinity is 23%, the weight-average molecular weight is 96,000, the molecular weight distribution index is 4.0, the haze is 5.5%, the transmittance is 92%, and the volume resistivity is 6.5 × 10⁻⁶. 17 The tensile strength at break is 22 MPa, and the dart impact breakage mass is 218 g. In the DSC melting curve, the temperature range of the first melting peak T1 is 105℃~128℃, and the temperature range of the second melting peak T2 is 90℃~105℃. The peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.19, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 120.6℃.
[0074] Example 5
[0075] This embodiment provides an ethylene-α-olefin multi-component copolymer.
[0076] exist Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0077] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.09; in the circulating gas, the molar ratio of 1-butene / ethylene is 0.33, the molar ratio of 1-hexene / ethylene is 0.014, the molar ratio of 1-octene / ethylene is 0.012, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.09, and the molar content of inert condenser is 12%. Liquid phase material A is injected at a height of 3D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor, and the injection point of liquid phase material A includes one liquid injection pipeline.
[0078] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.910 g / cm³. 3 The melt flow index is 0.58 g / 10 min, the crystallinity is 35%, the weight-average molecular weight is 96,000, the molecular weight distribution index is 3.8, the haze is 7.0%, the transmittance is 89%, and the volume resistivity is 6.5 × 10⁻⁶. 17 The tensile strength at break is 27 MPa, and the dart impact breakage mass is 209 g. In the DSC melting curve, the temperature range of the first melting peak T1 is 110℃~130℃, and the temperature range of the second melting peak T2 is 100℃~110℃. The peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.12, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 122℃.
[0079] Example 6
[0080] This embodiment provides an ethylene-α-olefin multi-component copolymer.
[0081] exist Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0082] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.11; in the circulating gas, the molar ratios of 1-butene / ethylene are 0.40, 1-hexene / ethylene, and 1-octene / ethylene are 0.020, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.09, and the molar content of inert condenser is 12%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point for liquid phase material A includes two liquid injection pipelines.
[0083] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.895 g / cm³. 3 The melt flow index is 0.63 g / 10 min, the crystallinity is 21%, the weight-average molecular weight is 90,000, the molecular weight distribution index is 3.8, the haze is 4.6%, the transmittance is 94%, and the volume resistivity is 7.0 × 10⁻⁶. 17 The tensile strength at break is 24 MPa, and the dart impact breakage mass is 220 g. In the DSC melting curve, the temperature range of the first melting peak T1 is 105℃~126℃, and the temperature range of the second melting peak T2 is 90℃~105℃. The peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.13, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 120℃.
[0084] Example 7
[0085] This embodiment provides an ethylene-α-olefin multi-component copolymer.
[0086] exist Figure 1The production system shown employs a catalytic system including a metallocene catalyst and a methylaluminoxane co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0087] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:2.5; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.12; in the circulating gas, the molar ratios of 1-butene / ethylene are 0.40, 1-hexene / ethylene, and 1-octene / ethylene are 0.020, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.09, and the molar content of inert condenser is 12%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point for liquid phase material A includes two liquid injection pipelines.
[0088] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.890 g / cm³. 3 The melt flow index is 1.20 g / 10 min, the crystallinity is 19%, the weight-average molecular weight is 79,000, the molecular weight distribution index is 3.0, the haze is 3.5%, the transmittance is 96%, and the volume resistivity is 10.0 × 10⁻⁶. 17 The tensile strength at break is 22 MPa, and the dart impact breakage mass is 252 g. In the DSC melting curve, the temperature range of the first melting peak T1 is 105℃~126℃, and the temperature range of the second melting peak T2 is 90℃~105℃. The peak area ratio of the second melting peak T2 to the first melting peak T1 is 0.20, indicating that the melting point of the obtained ethylene-α-olefin multi-component copolymer is 119.5℃.
[0089] Comparative Example 1
[0090] This comparative example provides an ethylene-α-olefin multi-polymer.
[0091] The procedure is carried out according to the method described in Example 1, except that... Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a ternary copolymerization reaction of ethylene, 1-butene, and 1-hexene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, the copolymerization reaction of ethylene, 1-butene, and 1-hexene occurs.
[0092] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.07; in the circulating gas, the molar ratio of 1-butene / ethylene is 0.30, the molar ratio of 1-hexene / ethylene is 0.04, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.12, and the molar content of inert condenser is 9%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor, and the injection point of liquid phase material A includes one liquid injection pipeline.
[0093] The density of the ethylene-α-olefin copolymer obtained in this comparative example is 0.918 g / cm³. 3 The melt flow index is 1.0 g / 10 min, the crystallinity is 32%, the weight-average molecular weight is 85,000, the molecular weight distribution index is 3.4, the haze is 12%, the transmittance is 80%, and the volume resistivity is 6.0 × 10⁻⁶. 17 The tensile strength was 20 MPa, the dart impact fracture mass was 150 g, the DSC melting curve contained only the first melting peak T1, the temperature range was 90℃~135℃, and the melting point of the obtained ethylene-α-olefin multi-component copolymer was 126℃.
[0094] Comparative Example 2
[0095] This comparative example provides an ethylene-α-olefin multi-polymer.
[0096] The procedure is carried out according to the method described in Example 1, except that... Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the catalyst and co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0097] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:10; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.01; in the circulating gas, the molar ratio of 1-butene / ethylene is 0.30, the molar ratio of 1-hexene / ethylene is 0.009, the molar ratio of 1-octene / ethylene is 0.008, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.12, and the molar content of inert condenser is 9%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor; the injection point of liquid phase material A includes at least one liquid injection pipeline.
[0098] The density of the ethylene-α-olefin copolymer obtained in this comparative example is 0.925 g / cm³. 3 The melt flow index is 1.2 g / 10 min, the crystallinity is 40%, the weight-average molecular weight is 83,000, the molecular weight distribution index is 3.2, the haze is 15%, the transmittance is 80%, and the volume resistivity is 6.0 × 10⁻⁶. 17 The tensile strength was 25 MPa, the dart impact breakage mass was 180 g, the DSC melting curve contained only the first melting peak T1, the temperature range was 90℃~135℃, and the melting point of the obtained ethylene-α-olefin multi-component copolymer was 126℃.
[0099] Comparative Example 3
[0100] This comparative example provides an ethylene-α-olefin multi-polymer.
[0101] The procedure is carried out according to the method described in Example 1, except that... Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the catalyst and co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0102] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:1.7; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.13; in the circulating gas, the molar ratio of 1-butene / ethylene is 0.30, the molar ratio of 1-hexene / ethylene is 0.010, the molar ratio of 1-octene / ethylene is 0.008, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.10, and the molar content of inert condenser is 9%. Liquid phase material A is injected at a height of 1.5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point of liquid phase material A includes at least one liquid injection pipeline.
[0103] The density of the ethylene-α-olefin copolymer obtained in this comparative example is 0.895 g / cm³. 3 The melt flow index is 1.0 g / 10 min, the crystallinity is 25%, the weight-average molecular weight is 85,000, the molecular weight distribution index is 4.5, the haze is 10%, the transmittance is 87%, and the volume resistivity is 6.0 × 10⁻⁶. 17 The tensile strength was 20 MPa, the dart impact fracture mass was 175 g, the DSC melting curve contained only the first melting peak T1, the temperature range was 90℃~135℃, and the melting point of the obtained ethylene-α-olefin multi-component copolymer was 124℃.
[0104] Comparative Example 4
[0105] This comparative example provides an ethylene-α-olefin multi-polymer.
[0106] The procedure is carried out according to the method described in Example 1, except that... Figure 1The production system shown employs a catalytic system including a Ziegler-Natta catalyst and a triethylaluminum co-catalyst to carry out a multi-component copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene. The reaction temperature is 85℃, the reaction pressure is 2.3MPa, and the apparent fluidizing gas velocity is 0.66m / s. After passing through a compression unit, a heat exchange unit, and a gas-liquid separation unit, a portion of the liquid phase material (referred to as liquid phase material A), containing components such as 1-butene, 1-hexene, 1-octene, and isopentane, enters from the liquid inlet on the side wall of the fluidized bed reactor. The remaining liquid phase material (referred to as liquid phase material B) is mixed with the gas phase material containing components such as ethylene, nitrogen, hydrogen, 1-butene, 1-hexene, 1-octene, and isopentane, and enters from the bottom inlet of the fluidized bed reactor. In the fluidized bed reactor, after contacting with the main catalyst and the co-catalyst, a copolymerization reaction of ethylene, 1-butene, 1-hexene, and 1-octene occurs.
[0107] The mass flow rate ratio of liquid phase material A to liquid phase material B is 1:3; the mass flow rate ratio of liquid phase material A to the total mass flow rate of the circulating gas is 0.12; in the circulating gas, the molar ratios of 1-butene / ethylene are 0.40, 1-hexene / ethylene, and 1-octene / ethylene are 0.020, the molar ratio of molecular weight regulator (hydrogen) / ethylene is 0.09, and the molar content of inert condenser is 12%. Liquid phase material A is injected at a height of 5D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point of liquid phase material A includes two liquid injection pipelines.
[0108] The density of the ethylene-α-olefin copolymer obtained in this embodiment is 0.918 g / cm³. 3 The melt flow index is 0.63 g / 10 min, the crystallinity is 35%, the weight-average molecular weight is 90,000, the molecular weight distribution index is 3.8, the haze is 10%, the transmittance is 86%, and the volume resistivity is 4.0 × 10⁻⁶. 17 The tensile strength was 28 MPa, the dart impact fracture mass was 200 g, the DSC melting curve contained only the first melting peak T1, the temperature range was 100℃~135℃, and the melting point of the obtained ethylene-α-olefin multi-component copolymer was 123℃.
[0109] As can be seen from Examples 1-7 and Comparative Examples 1-4 above, the ethylene-α-olefin multi-component copolymer production method provided by the present invention can produce an ethylene-α-olefin multi-component copolymer product with low haze, high transmittance, and high volume resistivity in a fluidized bed reactor. Compared with POE products with the same haze or transmittance, it has a higher density. The ethylene-α-olefin multi-component copolymer product and its production method have important application value and wide application potential.
[0110] To further illustrate the present invention, the contents of ethylene structural units, 1-butene structural units, 1-hexene structural units, and 1-octene structural units in the ethylene-α-olefin multi-component copolymers prepared in Examples 1-7 and Comparative Examples 1-4 were analyzed using a Bruker Advance 2B 400MHz instrument. 13 The results were obtained by C-NMR and the statistics are shown in Table 1 below.
[0111] Table 1
[0112]
[0113]
[0114] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.
Claims
1. A copolymer of ethylene and α-olefin, characterized in that, The ethylene-α-olefin copolymer has a haze of 1%–7%, a light transmittance >87%, and a volume resistivity >5.0 × 10⁻⁶. 17 Ω·cm, weight-average molecular weight 70,000–130,000, crystallinity 15%–35%; Based on the total molar amount of the ethylene-α-olefin multi-component copolymer, the molar content of the ethylene structural unit in the ethylene-α-olefin multi-component copolymer is 80 mol% to 96 mol%, the molar content of the 1-butene structural unit is 2.0 mol% to 10 mol%, the molar content of the 1-hexene structural unit is 0.6 mol% to 3.5 mol%, and the molar content of the 1-octene structural unit is 0.3 mol% to 5.32 mol%. The DSC melting curve of the ethylene-α-olefin multi-component copolymer includes a first melting peak T1 and a second melting peak T2.
2. The ethylene-α-olefin multi-component copolymer according to claim 1, characterized in that, The ethylene-α-olefin copolymer contains at least ethylene structural units, 1-butene structural units, and 1-octene structural units.
3. The ethylene-α-olefin multi-component copolymer according to claim 1 or 2, characterized in that, The temperature range of the first melting peak T1 is 105℃~135℃, and the temperature range of the second melting peak T2 is 90℃~110℃.
4. The ethylene-α-olefin multi-component copolymer according to claim 3, characterized in that, The ratio of the peak area of the second melting peak T2 to that of the first melting peak T1 is 0.01 to 0.
5.
5. The ethylene-α-olefin multi-component copolymer according to claim 1 or 2, characterized in that, The molecular weight distribution index of the ethylene-α-olefin copolymer is 2 to 8; And / or, the density of the ethylene-α-olefin copolymer is 0.885 g / cm³. 3 ~0.930g / cm 3 ; And / or, under conditions of 190°C and 2.16 kg load, the melt index of the ethylene-α-olefin copolymer is 0.5 g / 10 min to 15 g / 10 min; And / or, the melting point of the ethylene-α-olefin copolymer is 80°C to 130°C.
6. The ethylene-α-olefin multi-component copolymer according to claim 5, characterized in that, The molecular weight distribution index of the ethylene-α-olefin copolymer is 3 to 5. And / or, the density of the ethylene-α-olefin copolymer is 0.89 g / cm³. 3 ~0.92g / cm 3 ; And / or, under conditions of 190°C and 2.16 kg load, the melt index of the ethylene-α-olefin copolymer is 0.58 g / 10 min to 8 g / 10 min; And / or, the melting point of the ethylene-α-olefin copolymer is 100°C to 125°C.
7. A method for preparing an ethylene-α-olefin multi-component copolymer as described in any one of claims 1-6, characterized in that, The reaction involves contacting liquid material A from the sidewall of a fluidized bed reactor with liquid material B from the bottom of the fluidized bed reactor and a gaseous material containing ethylene, in the presence of a catalyst, to generate the ethylene-α-olefin multi-component copolymer. The liquid phase material A and liquid phase material B may be the same or different, and each independently includes the α-olefin and the inert condenser.
8. The preparation method according to claim 7, characterized in that, The α-olefin is selected from at least two of 1-butene, 1-hexene, and 1-octene; And / or, the mass flow rate ratio of liquid phase material A to liquid phase material B is 1:(2~50); And / or, the inert condenser is selected from saturated straight-chain or branched alkanes of C3 to C10, and cycloalkanes of C3 to C10; And / or, the catalyst includes a main catalyst and a co-catalyst; And / or, the gaseous material includes at least two of ethylene, 1-butene, 1-hexene, 1-octene, inactive gas, and optionally a molecular weight regulator.
9. The preparation method according to claim 8, characterized in that, The inert condenser is selected from C4-C6 saturated straight-chain or branched alkanes and C4-C6 cycloalkanes; And / or, the main catalyst is selected from at least one of Ziegler-Natta catalysts, metallocene catalysts, and transition metal catalysts; And / or, the co-catalyst is selected from at least one of modified methylaluminoxane, diethylaluminum chloride, diisobutylaluminum chloride, sesquiethylaluminum chloride, diisobutylaluminum, diethylaluminum chloride, trimethylaluminum, methylaluminoxane, triethylaluminum, triisobutylaluminum, trioctylaluminum, diethylaluminum hydrogen, and diisobutylaluminum hydrogen. And / or, the inactive gas is selected from at least one of nitrogen, ethane, and propane.
10. The preparation method according to claim 9, characterized in that, The inert condenser is selected from at least one of isopentane, n-pentane, n-hexane, and cyclohexane; And / or, the transition metal catalyst is selected from chromium-based catalysts.
11. The preparation method according to any one of claims 8-10, characterized in that, The preparation method further includes using unreacted reaction raw material gas as circulating gas to flow out from the top outlet of the fluidized bed reactor, and after compression, heat exchange and gas-liquid separation, liquid phase material A, liquid phase material B and gas phase material containing ethylene are obtained again and enter the fluidized bed reactor. The unreacted reaction feed gas comes from unreacted liquid phase material A, unreacted liquid phase material B, and unreacted gaseous material containing ethylene; and / or, the unreacted reaction feed gas includes ethylene, 1-butene, 1-hexene, 1-octene, an inert condenser, and an optional molecular weight regulator; the molecular weight regulator is hydrogen.
12. The preparation method according to claim 11, characterized in that, In the circulating gas, the molar ratio of 1-butene to ethylene is 0.01 to 0.8; and / or, the molar ratio of 1-hexene to ethylene is 0 to 0.03; and / or, the molar ratio of 1-octene to ethylene is 0.001 to 0.05; and / or, the molar ratio of molecular weight regulator to ethylene is 0 to 0.8; and / or, the molar content of inert condenser is 5% to 25%.
13. The preparation method according to any one of claims 8-10, characterized in that, The liquid material A is injected at a height of 0.2D to 4D above the distribution plate of the fluidized bed reactor, where D is the inner diameter of the fluidized bed reactor. The injection point of the liquid material A includes at least one liquid injection pipeline. And / or, the reaction conditions include: a pressure of 1.8 MPa to 2.5 MPa, a reaction temperature of 40°C to 90°C, and an apparent fluidizing gas velocity of 0.55 m / s to 0.75 m / s.
14. The application of an ethylene-α-olefin copolymer as described in any one of claims 1-6 or an ethylene-α-olefin copolymer prepared by any one of claims 7-13 in the preparation of photovoltaic films.
Citation Information
Patent Citations
Olefin-based polymers and dispersion polymerizations
CN103384686A
Solar-cell sealant and solar-cell module using same
CN103222066A
Ethylene-butylene-octene terpolymer and preparation method and system thereof
CN115232239A