A solid oxide electrolytic cell that self-enriches carbon dioxide and its preparation method

By designing a solid oxide electrolytic cell that can self-enrich carbon dioxide, and utilizing specific materials and nanocatalysts, the efficient conversion of fossil fuels into hydrogen and carbon dioxide has been achieved. This solves the problems of low efficiency in hydrogen production from fossil fuels and high cost of carbon dioxide capture in existing technologies, and reduces the energy consumption and cost of clean hydrogen production.

CN119663311BActive Publication Date: 2026-11-17CERAMIC CELLS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411770150.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-12-04
Publication Date
2026-11-17
Estimated Expiration
2044-12-04

AI Technical Summary

Technical Problem

Existing technologies for producing hydrogen from fossil fuels are characterized by low efficiency, high energy consumption, and high costs for carbon dioxide capture. Electrolysis of water for hydrogen production consumes a large amount of electricity, making it difficult to achieve efficient and low-cost hydrogen production and carbon dioxide enrichment.

Method used

A solid oxide electrolytic cell for self-enriching carbon dioxide is designed. By introducing water vapor and hydrocarbon fuel into the negative and positive electrodes respectively, and using nanocatalysts to accelerate the electrolysis of water and the oxidation reaction of hydrocarbon fuel, a specific combination of materials and microstructure design are employed to achieve efficient hydrogen production and carbon dioxide enrichment.

Benefits of technology

It improves the efficiency of hydrogen production from fossil fuels, reduces the electricity consumption for hydrogen production, achieves efficient self-enrichment and convenient capture of carbon dioxide, and reduces the cost of clean hydrogen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119663311B_ABST
    Figure CN119663311B_ABST
Patent Text Reader

Abstract

This invention discloses a solid oxide electrolytic battery with self-enriched carbon dioxide and its preparation method. The battery includes a negative electrode current collector layer, on the surface of which a negative electrode active layer, an electrolyte membrane, and a positive electrode active layer are sequentially disposed. The negative electrode current collector layer is one or more of an electronically conductive phase and an ionicly conductive phase. The negative electrode active layer and the positive electrode active layer are composite ceramics composed of the electronically conductive phase and the ionicly conductive phase, with the volume fraction of the electronically conductive phase not less than 40%. The porosity of the negative electrode current collector layer is 10-70%, the porosity of the negative electrode active layer is 20-35%, and the porosity of the positive electrode active layer is 20-35%. This invention can efficiently convert fossil fuels into hydrogen. Taking natural gas as an example, one standard cubic meter of natural gas can produce four standard cubic meters of hydrogen. Simultaneously, it self-enriches carbon dioxide for easy capture, reducing the cost of CCUS in traditional fossil fuel hydrogen production and lowering the cost of clean hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention pertains to electrolytic batteries and their manufacturing methods, specifically a solid oxide electrolytic battery that self-enriches carbon dioxide and its preparation method. Background Technology

[0002] Hydrogen energy is a readily available, green, low-carbon, and widely applicable secondary energy source, and it is gradually becoming one of the important carriers for global energy transition and development. Currently, most of the hydrogen demand is met through the production of hydrogen from fossil fuels, namely through natural gas steam reforming and coal gasification. However, traditional fossil fuel hydrogen production produces high carbon dioxide emissions, and the cost of carbon dioxide capture is very high. The water electrolysis hydrogen production process has no carbon dioxide emissions and is an important source of hydrogen in the future. However, the current electricity consumption for water electrolysis hydrogen production is too high, and the high cost of electricity is a major barrier to the rapid large-scale promotion and application of water electrolysis hydrogen production.

[0003] In existing technology, US6051125 couples natural gas into a high-temperature electrolyzer. However, CO readily undergoes disproportionation at high temperatures and in the presence of a Ni cermet catalyst, leading to carbon deposition. Furthermore, the Ni in the Ni cermet catalyst is easily oxidized under an oxidizing atmosphere, resulting in failure. Chinese patent CN101103140A uses metallic Ni as the anode, where methane easily decomposes and deposits carbon under the influence of Ni at high temperatures, covering the electrode and causing blockage. To prevent carbon deposition, water vapor or carbon dioxide needs to be mixed into the methane during operation, which complicates the operation of the electrolyzer.

[0004] In summary, current fossil fuel reforming for hydrogen production involves steam reforming, a highly endothermic reaction. Therefore, traditional hydrogen production processes require the combustion of some fossil fuels to sustain the reforming reaction in the thermochemical reactor. This results in low hydrogen production efficiency (for example, natural gas reforming produces only 2.2-2.4 standard cubic meters of hydrogen per cubic meter of natural gas). Furthermore, the carbon dioxide concentration produced by fossil fuel combustion is low during carbon dioxide capture, making capture extremely difficult and energy-intensive. In traditional water electrolysis for hydrogen production, the electrolysis reaction is also highly endothermic, with the entire reaction powered by electricity. This leads to significant electricity consumption (3-5 kWh per standard cubic meter of hydrogen) and high production costs. Summary of the Invention

[0005] Purpose of the invention: In order to overcome the shortcomings of the prior art, the purpose of this invention is to provide a solid oxide electrolytic battery that self-enriches carbon dioxide with high hydrogen production efficiency and reduced hydrogen production energy consumption. Another purpose of this invention is to provide a convenient and controllable method for preparing a solid oxide electrolytic battery that self-enriches carbon dioxide.

[0006] Technical Solution: The present invention discloses a solid oxide electrolytic battery for self-enriching carbon dioxide, comprising a negative electrode current collector layer, wherein a negative electrode active layer, an electrolyte separator, and a positive electrode active layer are sequentially disposed on the surface of the negative electrode current collector layer; the negative electrode current collector layer is one or more of an electronically conductive phase and an ionicly conductive phase; the negative electrode active layer and the positive electrode active layer are composite ceramics composed of an electronically conductive phase and an ionicly conductive phase, wherein the volume fraction of the electronically conductive phase is not less than 40%; the porosity of the negative electrode current collector layer is 10-70%, the porosity of the negative electrode active layer is 20-35%, and the porosity of the positive electrode active layer is 20-35%.

[0007] A solid oxide electrolytic cell for carbon dioxide self-enrichment, wherein water vapor or a mixture of water vapor and hydrogen, with water vapor as the main component, is introduced into the negative electrode of the cell, and an electrolytic reduction reaction of water vapor occurs to obtain hydrogen or a mixture of hydrogen and water vapor, with hydrogen as the main component; a combustible gas or a mixture containing combustible gas is introduced into the positive electrode of the cell, and a deep or complete oxidation reaction of the combustible gas occurs to obtain carbon dioxide or a mixture containing a high concentration of carbon dioxide; the combustible gas includes, but is not limited to, hydrogen, carbon monoxide, methane, ethane, propane, gasoline, diesel, kerosene, methanol, ethanol, and mixtures thereof.

[0008] Furthermore, the electronically conductive phases in the negative electrode current collector layer and the negative electrode active layer are all Ni, Fe, Cu, Co, FeNi3, 430L, SUS445, SUS446, (La 1-x Sr x (Cr) 1-y Fe y )O 3-δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3-δ 、(La 1-x Sr x TiO 3-δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, wherein 0 < x < 1, 0 < y < 1, 0 < δ < 1; the ionic conductive phase in the negative electrode current collector layer and the negative electrode active layer is one or more of the following: doped zirconium oxide, doped cerium oxide, doped lanthanum gallate, doped barium zirconate, and doped barium cerate.

[0009] Furthermore, the electronically conductive phase in the positive electrode active layer is 430L, SUS445, SUS446, NiO, CuO, Fe3O4, Co3O4, (La) 1-x Sr x(Cr) 1-y Fe y )O 3-δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3-δ 、(La 1-x Sr x TiO 3-δ La 2-x Sr x Fe 2-y- z Ni y Mo z O 6-δ One or more of the following, wherein 0 < x < 1, 0 < y < 1, 0 < δ < 1; the ionic conductive phase in the positive electrode active layer is one or more of the following: doped zirconium oxide, doped cerium oxide, doped lanthanum gallate, doped barium zirconate, and doped barium cerate.

[0010] To accelerate the electrolysis of water and the oxidation of hydrocarbon fuels, the inner surfaces of both the negative electrode current collector and the negative electrode active layer are covered with nano-sized negative electrode catalysts with a particle size of 1–500 nm. These nano-sized negative electrode catalysts are composed of Fe, Ni, Cu, Co, FeNi3, and Ce. 1-x La x O 2-δ Ce 1- x Y x O 2-δ Ce 1-x Sm x O 2-δ Ce 1-x Gd x O 2-δ Ce 1-x Pr x O 2-δ Ce 1-x Nd x O 2-δ Ce 1-x Ca x O 2-δ Ce 1-x Mg x O 2-δ 、(La 1- x Sr x (Cr) 1-y Fe y )O 3-δ 、(La 1-x Sr x (Cr) 1-y Mn y )O3-δ 、(La 1-x Sr x TiO 3-δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, wherein 0 < x < 1, 0 < δ < 1. Preferably, the nano-anode catalyst is NiO-Ce. 0.9 Gd 0.1 O 2-δ Nanocatalysts. Nanocatalysts can reduce reaction overpotential and improve efficiency.

[0011] Preferably, the thickness of the electrolyte membrane is 5 to 10 micrometers, the porosity of the negative electrode current collector is 30 to 45%, and the thickness is 50 to 2000 micrometers.

[0012] The negative electrode active layer is the region where the water electrolysis reaction occurs. The water electrolysis reaction takes place at the interface of the oxygen ion conductive phase, the electronic conductive phase, and the gas phase. Therefore, it is necessary to have both oxygen ion conductive phase and electronic conductive phase, which form a permeation network with each other. The gas phase is formed by a porous structure. The lower or higher the porosity and thickness, the fewer the number of reaction sites will be. The negative electrode active layer has the most reaction sites in the range of 20-35% porosity and 5-20 micrometers.

[0013] The electrolyte membrane provides a channel for oxygen ion transport, so it must be an oxygen ion conductive phase. The thickness of the electrolyte membrane is related to the resistance to oxygen ion transport. The thicker the membrane, the greater the resistance to oxygen ion transport, and the greater the ohmic impedance. The thinner the membrane, the more difficult it is to prepare. The range of 5 to 300 micrometers can ensure both the preparation yield and the low resistance to oxygen ion transport.

[0014] The positive electrode active layer is mainly the region where the oxidation reaction of hydrocarbon fuels occurs. The reaction takes place at the interface of the oxygen ion conductive phase, the electronic conductive phase, and the gas phase. Therefore, the material needs to have both oxygen ion conductive and electronic conductive phases that form a permeation network. The gas phase is formed by a porous structure. Lower or higher porosity and thickness will lead to a decrease in the number of reaction sites. The selected porosity range of 20-35% and 5-20 micrometers has the highest number of reaction sites. Furthermore, the atmosphere before the reaction of the positive electrode active layer is a reducing atmosphere for hydrocarbon fuels, and the atmosphere after the reaction is an oxidizing atmosphere of water vapor and carbon dioxide. Therefore, the material of the positive electrode active layer needs to be able to exist stably under both oxidizing and reducing conditions. This configuration can enable 100% conversion of hydrocarbon fuels.

[0015] Furthermore, a positive current collector layer is also provided on the surface of the positive active layer, which is one or more of an electronically conductive phase and an ionically conductive phase.

[0016] Furthermore, the electronically conductive phases in the positive current collector layer are 430L, SUS445, SUS446, and (La). 1-x Sr x (Cr) 1- y Fe y )O 3-δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3-δ 、(La 1-x Sr x TiO 3-δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, 0 < x < 1, 0 < y < 1, 0 < δ < 1.

[0017] Furthermore, the ion-conducting phase in the positive electrode current collector layer is one or more of doped zirconium oxide, doped cerium oxide, and doped lanthanum gallate, with a porosity of 10–70%.

[0018] To accelerate the electrolysis of water and the oxidation of hydrocarbon fuels, nano-sized cathode catalysts with a particle size of 1–500 nm are coated on the inner surface of the cathode current collector and the cathode active layer. The nano-sized cathode catalyst is Ce. 1-x La x O 2-δ Ce 1-x Y x O 2-δ Ce 1-x Sm x O 2-δ Ce 1- x Gd x O 2-δ Ce 1-x Pr x O 2-δ Ce 1-x Nd x O 2-δ Ce 1-x Ca x O 2-δ Ce 1-x Mg x O 2-δ One or more of the following, wherein 0 < x < 1, 0 < δ < 1. Preferably, the nano-cathode catalyst is Ce. 0.9 Gd 0.1 O2-δ Catalysts. Nanocatalysts can reduce reaction overpotential and improve efficiency.

[0019] Furthermore, the thickness of the negative electrode current collector layer is 50–2000 micrometers, the thickness of the negative electrode active layer is 5–20 micrometers, the thickness of the electrolyte membrane is 1–1000 micrometers, the thickness of the positive electrode active layer is 5–20 micrometers, and the thickness of the positive electrode current collector layer is 50–2000 micrometers.

[0020] Efficient hydrogen production via coupled water electrolysis using positive and negative electrode nanocatalysts, as well as positive and negative electrode active layer materials and microstructures, is achieved.

[0021] The preparation method of the above-mentioned solid oxide electrolytic cell that self-enriches carbon dioxide includes the following steps:

[0022] Step 1: Prepare negative electrode current collector green body, negative electrode active layer green body, electrolyte membrane green body, positive electrode active layer green body and positive electrode current collector green body on the mylar membrane respectively;

[0023] Step 2: After stacking the negative electrode current collector green sheet, negative electrode active layer green sheet, electrolyte membrane green sheet, positive electrode active layer green sheet, and positive electrode current collector green sheet in the manner of green sheet, the whole sheet is statically pressed to obtain a solid oxide electrolytic cell green sheet.

[0024] Step 3: The product obtained in Step 2 is subjected to gradient sintering to make the electrolyte membrane layer dense, and then cooled to obtain a solid oxide electrolytic cell that enriches carbon dioxide.

[0025] The working principle of a solid oxide electrolytic cell: A mixture of hydrogen and water vapor is introduced at the negative electrode, and hydrocarbon fuel is introduced at the positive electrode. Water vapor dissociates at the negative electrode to generate hydrogen and oxygen ions. The oxygen ions are transported through the electrolyte membrane to the positive electrode, where they undergo a complete oxidation reaction with the hydrocarbon fuel to produce water and carbon dioxide. The gas exiting the negative electrode is hydrogen and water vapor, which, after condensation, yields high-purity hydrogen. The gas exiting the positive electrode is carbon dioxide and water vapor, which, after condensation, yields high-purity carbon dioxide, which can be directly captured. Coupling fossil fuels into the water electrolysis hydrogen production process releases the energy contained in the fossil fuels in an electrochemical form, compensating for the energy required for water electrolysis, reducing hydrogen production power consumption, and simultaneously improving the efficiency of hydrogen production from fossil fuels. It also achieves self-enrichment of carbon dioxide for easy capture. In terms of material selection, carbon-resistant electrode materials are chosen to simplify actual operating conditions and reduce the energy consumption of hydrogen production.

[0026] Beneficial effects: Compared with the prior art, the present invention has the following significant features:

[0027] 1. It can efficiently convert fossil fuels into hydrogen. Taking natural gas as an example, one standard cubic meter of natural gas can produce four standard cubic meters of hydrogen. At the same time, it can enrich carbon dioxide for easy capture, reducing the cost of CCUS in traditional fossil fuel hydrogen production.

[0028] 2. Compared with traditional water electrolysis for hydrogen production, it can greatly reduce the power consumption for hydrogen production (1 kWh per standard cubic meter of hydrogen), thereby reducing the cost of clean hydrogen;

[0029] 3. By loading nano-catalysts onto the positive and negative electrodes respectively, the electrolysis of water and the oxidation of hydrocarbon fuels can be accelerated, the reaction overpotential can be reduced, and the efficiency can be improved. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the structure of Embodiment 1 of the present invention;

[0031] Figure 2 This is a cross-sectional view of Embodiment 1 of the present invention;

[0032] Figure 3 This is a schematic diagram of the structure of Embodiment 2 of the present invention;

[0033] Figure 4 This is a cross-sectional view of Embodiment 2 of the present invention;

[0034] Figure 5 This is a schematic diagram of the operation of the solid oxide electrolytic cell that self-enriches carbon dioxide according to the present invention;

[0035] Figure 6 This is a bar chart (dry) of the anode product gas composition of the solid oxide electrolytic cell obtained in Example 4 of the present invention under different currents;

[0036] Figure 7 These are the electrolysis and power consumption curves of the solid oxide electrolytic battery obtained in Example 4 of this invention. Detailed Implementation

[0037] Unless otherwise specified, all materials, reagents, and instruments used in the following examples are commercially available. Experimental methods not specifically described in the examples are generally performed under standard conditions or as recommended by the manufacturer. In the following examples, 0 < δ < 1, and both the binder and plasticizer are polyvinyl butyral.

[0038] Example 1

[0039] A method for preparing a solid oxide electrolytic cell with self-enriched carbon dioxide includes the following steps:

[0040] (1) Preparation of negative electrode current collector green blank: NiO, Zr 0.97 Y 0.06 O 2-δThe mixture is made with graphite powder in a ratio of 48:32:20, then xylene and butyl acetate are added as a two-component solvent and acrylic resin dispersant. After ball milling, polyvinyl butyral is added as a binder and plasticizer, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode current collector.

[0041] (2) Preparation of negative electrode active layer green blank: NiO, Zr 0.97 Y 0.06 O 2-δ The mixture is mixed with graphite powder in a ratio of 54:36:10, and then xylene and butyl acetate, a two-component solvent and an acrylic resin dispersant are added. After ball milling, polyvinyl butyral is added as a binder and plasticizer, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode active layer.

[0042] (3) Preparation of electrolyte membrane green body: In Zr 0.97 Y 0.06 O 2-δ Xylene and butyl acetate, a two-component solvent, and an acrylic resin dispersant are added to the powder. After ball milling, polyvinyl butyral is added as a binder and plasticizer, and the powder is ball milled again to obtain a uniformly dispersed cast slurry. The slurry is filtered, degassed, cast on a Mylar membrane, and dried to obtain an electrolyte diaphragm green body.

[0043] (4) Preparation of the positive electrode active layer green body: (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ Zr 0.97 Y 0.06 O 2-δ The mixture is made with graphite powder in a ratio of 54:36:10, and then xylene and butyl acetate are added as a two-component solvent and acrylic resin dispersant. After ball milling, polyvinyl butyral is added as a binder and plasticizer, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green blank of the positive electrode active layer.

[0044] (5) After stacking the negative current collector green sheet, negative active layer green sheet, electrolyte membrane green sheet and positive active layer green sheet, the whole is statically pressed to obtain a solid oxide electrolytic cell green sheet.

[0045] (6) The solid oxide electrolytic cell blank is heated to 730°C at 0.5°C / min, and held at 180°C, 250°C, 350°C and 730°C for 2 hours each. Then, the temperature is increased to 1400°C at 1°C / min and held for 4 hours to make the electrolyte membrane layer dense. After sintering, the temperature is reduced to 800°C at 3°C / min and allowed to cool naturally to room temperature in the furnace to obtain a solid oxide electrolytic cell with carbon dioxide self-enrichment.

[0046] like Figures 1-2 The solid oxide electrolytic cell for carbon dioxide self-enrichment obtained in this embodiment comprises, from top to bottom: 20 μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.92 Y 0.16 O 2-δ Positive electrode active layer 4, porosity 20%; 10μm Zr 0.92 Y 0.16 O 2-δ Electrolyte membrane layer 3, 20 μm NiO-Zr 0.92 Y 0.16 O 2-δ Negative electrode active layer 2, with a porosity of 20%; 400μm NiO-Zr 0.97 Y 0.06 O 2-δ Negative electrode current collector layer 1 has a porosity of 45%.

[0047] Example 2

[0048] A method for preparing a solid oxide electrolytic cell with self-enriched carbon dioxide includes the following steps:

[0049] (1) Preparation of negative electrode current collector green blank: (La 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ Zr 0.97 Y 0.06 O 2-δ The mixture is made with graphite powder in a ratio of 51:34:15, then xylene and butyl acetate are added as a two-component solvent and an acrylic resin dispersant. After ball milling, binder and plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode current collector.

[0050] (2) Preparation of negative electrode active layer green body: (La 0.8 Sr 0.2 (Cr) 0.5 Fe0.5 )O 3-δ Zr 0.92 Y 0.16 O 2-δ The mixture is made with graphite powder in a ratio of 54:36:10, then xylene and butyl acetate two-component solvent and acrylic resin dispersant are added. After ball milling, binder and plasticizer are added, and ball milling is performed again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode active layer.

[0051] (3) Preparation of electrolyte membrane green body: In Zr 0.92 Y 0.16 O 2-δ Xylene and butyl acetate, a two-component solvent, and an acrylic resin dispersant are added to the powder. After ball milling, a binder and a plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. The slurry is filtered, degassed, cast on a Mylar membrane, and dried to obtain an electrolyte diaphragm green body.

[0052] (4) Preparation of the positive electrode active layer green body: (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ Zr 0.92 Y 0.16 O 2-δ The mixture is made with graphite powder in a ratio of 54:36:10, then xylene and butyl acetate are added as a two-component solvent and an acrylic resin dispersant. After ball milling, binder and plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green cathode active layer.

[0053] (5) Preparation of positive electrode current collector green blank: (La 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ Zr 0.97 Y 0.06 O 2-δ The mixture is mixed with graphite powder in a ratio of 51:34:15, and then xylene and butyl acetate two-component solvent and acrylic resin dispersant are added. After ball milling, binder and plasticizer are added, and ball milling is performed again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green blank of the positive electrode current collector.

[0054] (6) After stacking the negative current collector green sheet, negative active layer green sheet, electrolyte membrane layer green sheet, positive active layer green sheet, and positive current collector green sheet in the manner of green sheet, the whole sheet is statically pressed to obtain a solid oxide electrolytic cell green sheet.

[0055] (7) The solid oxide electrolytic cell blank is heated to 730°C at 0.5°C / min, and held at 180°C, 250°C, 350°C and 730°C for 2 hours each. Then, the temperature is increased to 1400°C at 1°C / min and held for 4 hours to make the electrolyte membrane layer dense. After sintering, the temperature is reduced to 800°C at 3°C / min and then naturally cooled to room temperature with the furnace to obtain a solid oxide electrolytic cell with carbon dioxide self-enrichment.

[0056] like Figures 3-4 The solid oxide electrolytic cell for carbon dioxide self-enrichment obtained in this embodiment comprises, from top to bottom: 200 μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.97 Y 0.06 O 2-δ Positive electrode current collector layer 5, porosity 30%; 5μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.92 Y 0.16 O 2-δ Positive electrode active layer 4, porosity 20%; 5μm Zr 0.92 Y 0.16 O 2-δ Electrolyte membrane layer 3.5 μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.92 Y 0.16 O 2-δ Negative electrode active layer 2, porosity 20%; 200μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.97 Y 0.06 O 2-δ Negative electrode current collector layer 1 has a porosity of 30%.

[0057] Example 3

[0058] A method for preparing a solid oxide electrolytic cell with self-enriched carbon dioxide includes the following steps:

[0059] 1) Preparation of negative electrode current collector green blank: (La0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ Zr 0.97 Y 0.06 O 2-δ The mixture is made with graphite powder in a ratio of 51:34:15, then xylene and butyl acetate are added as a two-component solvent and an acrylic resin dispersant. After ball milling, binder and plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode current collector.

[0060] (2) Preparation of negative electrode active layer green body: (La 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 The mixture is made with graphite powder in a ratio of 54:36:10, then xylene and butyl acetate two-component solvent and acrylic resin dispersant are added. After ball milling, binder and plasticizer are added, and ball milling is performed again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode active layer.

[0061] (3) Preparation of electrolyte membrane green body: In La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 Xylene and butyl acetate, a two-component solvent, and an acrylic resin dispersant are added to the powder. After ball milling, a binder and a plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. The slurry is filtered, degassed, cast on a Mylar membrane, and dried to obtain an electrolyte diaphragm green body.

[0062] (4) Preparation of the positive electrode active layer green body: (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85The mixture is made with graphite powder in a ratio of 54:36:10, then xylene and butyl acetate are added as a two-component solvent and an acrylic resin dispersant. After ball milling, binder and plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green cathode active layer.

[0063] (5) Preparation of positive electrode current collector green blank: (La 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ Zr 0.97 Y 0.06 O 2-δ The mixture is mixed with graphite powder in a ratio of 51:34:15, and then xylene and butyl acetate two-component solvent and acrylic resin dispersant are added. After ball milling, binder and plasticizer are added, and ball milling is performed again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green blank of the positive electrode current collector.

[0064] (6) After stacking the negative current collector green sheet, negative active layer green sheet, electrolyte membrane layer green sheet, positive active layer green sheet, and positive current collector green sheet in the manner of green sheet, the whole sheet is statically pressed to obtain a solid oxide electrolytic cell green sheet.

[0065] (7) The solid oxide electrolytic cell blank is heated to 730°C at 0.5°C / min, and held at 180°C, 250°C, 350°C and 730°C for 2 hours each. Then, the temperature is increased to 1400°C at 1°C / min and held for 4 hours to make the electrolyte membrane layer dense. After sintering, the temperature is reduced to 800°C at 3°C / min and then naturally cooled to room temperature with the furnace to obtain a solid oxide electrolytic cell with carbon dioxide self-enrichment.

[0066] The solid oxide electrolytic cell for carbon dioxide self-enrichment obtained in this embodiment includes, from top to bottom: 50 μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.97 Y 0.06 O 2-δ Positive electrode current collector layer 5, porosity 30%; 5μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85Positive electrode active layer 4, porosity 20%; 200μm La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 Electrolyte membrane layer 3.5 μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -La 0.9 Sr 0.1 Ga 0.8 Mg 0.2 O 2.85 Negative electrode active layer 2, porosity 20%; 50μm (La) 0.8 Sr 0.2 (Cr) 0.5 Fe 0.5 )O 3-δ -Zr 0.97 Y 0.06 O 2-δ Negative electrode current collector layer 1 has a porosity of 30%.

[0067] Example 4

[0068] A method for preparing a solid oxide electrolytic cell with self-enriched carbon dioxide includes the following steps:

[0069] (1) Preparation of negative electrode current collector green blank: 430L, Zr 0.97 Y 0.06 O 2-δ The mixture is mixed with graphite powder in a ratio of 48:32:20, and then xylene and butyl acetate two-component solvent and acrylic resin dispersant are added. After ball milling, binder and plasticizer are added, and ball milling is performed again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a negative electrode current collector green body.

[0070] (2) The steps for preparing the negative electrode active layer green body include: mixing 430L and Zr 0.92 Y 0.16 O 2-δ The mixture is made with graphite powder in a ratio of 51:34:15, then xylene and butyl acetate are added as a two-component solvent and an acrylic resin dispersant. After ball milling, binder and plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green negative electrode active layer.

[0071] (3) Preparation of electrolyte membrane green body: In Zr 0.92 Y 0.16 O 2-δXylene and butyl acetate, a two-component solvent, and an acrylic resin dispersant are added to the powder. After ball milling, a binder and a plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. The slurry is filtered, degassed, cast on a Mylar membrane, and dried to obtain an electrolyte diaphragm green body.

[0072] (4) Preparation of positive electrode active layer green body: 430L, Zr 0.92 Y 0.16 O 2-δ The mixture is prepared by mixing graphite powder in a ratio of 51:35:15, then adding a two-component solvent of xylene and butyl acetate, as well as an acrylic resin dispersant. After ball milling, a binder and plasticizer are added, and the mixture is ball milled again to obtain a uniformly dispersed cast slurry. The slurry is filtered, degassed, cast onto a Mylar membrane, and dried to obtain a green cathode active layer.

[0073] (5) Preparation of positive electrode current collector green blank: 430L, Zr 0.97 Y 0.06 O 2-δ The mixture is mixed with graphite powder in a ratio of 48:32:20, and then xylene and butyl acetate two-component solvent and acrylic resin dispersant are added. After ball milling, binder and plasticizer are added, and ball milling is performed again to obtain a uniformly dispersed cast slurry. After filtration and degassing, the slurry is cast and dried on a Mylar membrane to obtain a green blank of the positive electrode current collector.

[0074] (6) After stacking the negative current collector green sheet, negative active layer green sheet, electrolyte membrane layer green sheet, positive active layer green sheet, and positive current collector green sheet in the manner of green sheet, the whole is statically pressed to obtain a solid oxide electrolytic cell green sheet.

[0075] (7) The solid oxide electrolytic cell blank is heated to 730°C at 0.5°C / min in a 4% H2-96% N2 atmosphere, and held at 180, 250, 350 and 730°C for 2 hours each. Then, the temperature is increased to 1400°C at 1°C / min and held for 4 hours to make the electrolyte membrane layer dense. After sintering, the temperature is reduced to 800°C at 3°C / min and then naturally cooled to room temperature with the furnace to obtain the solid oxide electrolytic cell frame.

[0076] (8) According to NiO-Ce 0.9 Gd 0.1 O 2-δ Ni(NO3)2·6H2O, Ce(NO3)3·6H2O, and Gd(NO3)3·6H2O were dissolved in deionized water according to a stoichiometric ratio. Citric acid was added at a molar ratio of citric acid to total cations of 1:1. The solution was then heated and concentrated at 80°C to obtain NiO-CeO with a total cation concentration of 1 mol / L. 0.9 Gd 0.1 O 2-δPrecursor solution, NiO-Ce 0.9 Gd 0.1 O 2-δ The precursor solution was impregnated into the negative electrode active layer 2 and the negative electrode current collector layer 1, and calcined in air at 850°C for 2 hours. The impregnation-calcination step was repeated to make NiO-Ce 0.9 Gd 0.1 O 2-δ The catalyst loading is approximately 10.wt% relative to the cathode framework.

[0077] (9) According to Ce 0.9 Gd 0.1 O 2-δ The stoichiometric ratio of Ce(NO3)3·6H2O and Gd(NO3)3·6H2O was determined by dissolving them in deionized water. Citric acid was added at a molar ratio of citric acid to total cations of 1:1. The solution was then concentrated at 80°C to obtain Ce(NO3)3·6H2O with a total cation concentration of 1 mol / L. 0.9 Gd 0.1 O 2-δ Precursor solution, Ce 0.9 Gd 0.1 O 2-δ The precursor solution was impregnated into the positive electrode active layer 4 and the positive electrode current collector layer 5, and calcined in air at 850°C for 2 hours. The impregnation-calcination step was repeated to make Ce... 0.9 Gd 0.1 O 2-δ The catalyst loading relative to the cathode framework is approximately 10 wt.%.

[0078] The carbon dioxide self-enriched solid oxide electrolytic cell obtained in this embodiment comprises, from top to bottom: a 200 μm 430L positive electrode current collector layer 5 with a porosity of 45%; and a 5 μm 430L-Zr... 0.92 Y 0.16 O 2-δ Positive electrode active layer 4, with a porosity of 35%; 5μm Zr 0.92 Y 0.16 O 2-δ Electrolyte membrane layer 3.5 μm 430L-Zr 0.92 Y 0.16 O 2-δ The negative electrode active layer 2 has a porosity of 35%; the 200μm 430L negative electrode current collector layer 1 has a porosity of 45%. The porous 430L positive electrode current collector layer 5 and 430L-Zr... 0.92 Y 0.16 O 2-δ Ce is loaded inside the positive electrode active layer 4 0.9 Gd 0.1 O 2-δNanocatalysts with an average particle size of 1–500 nm were loaded at 10 wt.% of the positive electrode framework. These catalysts were used in the porous 430L negative electrode current collector layer 1 and 430L-Zr. 0.92 Y 0.16 O 2-δ NiO-Ce is loaded inside the negative electrode active layer 2. 0.9 Gd 0.1 O 2-δ The nanocatalyst has an average particle size of 1–500 nm and a loading of 10 wt.% of the negative electrode framework.

[0079] Example 5

[0080] Using the solid oxide electrolytic cell from Example 1, it was sealed in a test fixture, such as... Figure 5 The test fixture was divided into a positive electrode chamber and a negative electrode chamber by the solid oxide electrolytic cell. 80% H₂O-20% H₂ (560 ml / min H₂O-140 ml / min H₂) was introduced into the negative electrode chamber, and 105 ml / min CH₄ was introduced into the positive electrode chamber. The temperature was raised to 700℃. Figure 6 As the electrolysis current increases, water vapor in the negative electrode chamber is gradually electrolyzed to produce hydrogen and oxygen ions, while natural gas in the positive electrode chamber is oxidized by oxygen ions to produce CO2 and H2O. When the electrolysis current increases to 60A, CH4 in the positive electrode chamber is completely oxidized to CO2 and H2O, and the tail gas in the negative electrode chamber is 80% H2 - 20% H2O (560ml / min H2 - 140ml / min H2O). At this point, the electrolysis power consumption is 0.87 kWh per standard cubic meter of hydrogen. Figure 7 The exhaust gas from the positive electrode chamber is condensed to obtain pure CO2, and the exhaust gas from the negative electrode chamber is condensed to obtain pure H2.

[0081] Example 6

[0082] Using the solid oxide electrolytic cell from Example 2, it was sealed in a test fixture, which was divided into a positive electrode chamber and a negative electrode chamber by the solid oxide electrolytic cell. 80% H₂O - 20% H₂ (560 ml / min H₂O - 140 ml / min) was introduced into the negative electrode chamber. Coke oven gas (composition: 60% H2, 25% CH4, 3% CO2, 5% CO, 5% H2O, 2% N2) is introduced into the positive electrode chamber at a rate of 255 ml / min and heated to 700℃. As the electrolysis current increases, water vapor in the negative electrode chamber is gradually electrolyzed to produce hydrogen and oxygen ions, while the coke oven gas in the positive electrode chamber is oxidized by oxygen ions to produce CO2 and H2O. When the electrolysis current increases to 60A, the coke oven gas in the positive electrode chamber is completely oxidized to CO2 and H2O. The tail gas in the positive electrode chamber is 76.67% H2O - 22% CO2 - 1.33% N2 (293.25 ml / min H2O - 91.8 ml / min CO2 - 5.1 ml / min N2), and the tail gas in the negative electrode chamber is 80% H2 - 20% H2O (560 ml / min H2 - 140 ml / min N2). H2O); the tail gas from the positive electrode chamber is condensed to obtain 94.7% CO2 and 5.3% N2, and the tail gas from the negative electrode chamber is condensed to obtain pure H2.

[0083] Example 7

[0084] This embodiment aims to explore the relationship between the thickness and porosity of each layer and the electrolytic hydrogen production performance of a carbon dioxide self-enriched solid oxide electrolysis battery.

[0085] The remaining preparation steps are the same as in Example 4, except that: the porosity of the negative electrode current collector 1 is set to 10%, 20%, 30%, 35%, 40%, 45%, 50%, 60%, and 70%, respectively; the thickness of the negative electrode current collector 1 is set to 50 μm, 100 μm, 500 μm, 1000 μm, 1500 μm, and 2000 μm, respectively; the porosity of the negative electrode active layer 2 is set to 20%, 25%, 30%, and 35%, respectively; and the thickness of the negative electrode active layer 2 is set to 5 μm, 10 μm, 15 μm, and 20 μm, respectively; and the thickness of the electrolyte 3 is set to... The porosity of the positive electrode active layer 4 is set to 50μm, 100μm, 300μm, and 500μm respectively, the porosity of the positive electrode active layer 4 is set to 20%, 25%, 30%, and 35% respectively, the thickness of the positive electrode active layer 4 is set to 5μm, 10μm, 15μm, and 20μm respectively, the porosity of the positive electrode current collector layer 5 is set to 10%, 20%, 30%, 35%, 40%, 45%, 50%, 60%, and 70% respectively, and the thickness of the positive electrode current collector layer 5 is set to 50μm, 100μm, 500μm, 1000μm, 1500μm, and 2000μm respectively. Electrolytic hydrogen production tests were conducted, and the results showed that the optimal performance was achieved when the porosity of the negative electrode active layer 2 was between 20% and 35%, and the thickness of the negative electrode active layer 2 was between 5 and 20 μm. Similarly, the optimal performance was also achieved when the porosity of the positive electrode active layer 4 was between 20% and 35%, and the thickness of the positive electrode active layer 2 was between 5 and 20 μm. Finally, the optimal performance was achieved when the porosity of the negative electrode current collector layer 1 was between 45% and 50%. Porosities below these ranges resulted in lower water vapor conversion rates and reduced electrolytic hydrogen production performance. The electrolytic hydrogen production performance is poor when the porosity is above a certain value. The positive electrode current collector 5 has the best electrolytic hydrogen production performance when the porosity is between 45% and 50%. When the porosity is below this value, the water vapor conversion rate is low, resulting in poor electrolytic hydrogen production performance. When the porosity is above this value, the electrolytic hydrogen production performance is good. When the total thickness of the solid oxide electrolytic cell is less than 300 μm, the electrolytic hydrogen production performance cannot be measured due to cell failure. The thickness of electrolyte 3 is between 5 and 300 μm, resulting in good electrolytic hydrogen production performance. When the thickness is above 300 μm, the electrolytic hydrogen production performance is poor due to the large ohmic resistance, as shown in Table 1.

[0086] Table 1. Electrolytic hydrogen production performance of solid oxide electrolytic cells with different layer thicknesses and porosities.

[0087]

[0088] Comparative Example 1

[0089] The remaining steps of this comparative example are the same as those in Example 4, except that 430L in the positive electrode active layer 4 and the positive electrode current collector layer 5 is replaced with Ni. Electrolysis hydrogen production tests were conducted, and the results showed that rapid carbon buildup in the pores of the positive electrode active layer 4 and the positive electrode current collector layer 5 led to the failure of the electrolysis battery, and the electrolysis voltage increased rapidly when the hydrocarbon fuel conversion rate was above 80%.

[0090] Of the above embodiments, the preferred embodiment is Embodiment 4.

Claims

1. A solid oxide electrolytic cell that self-enriches carbon dioxide, characterized in that: The device includes a negative current collector layer (1), on which a negative active layer (2), an electrolyte membrane (3), and a positive active layer (4) are sequentially disposed; the negative current collector layer (1) is one or more of an electronically conductive phase and an ionicly conductive phase; the negative active layer (2) and the positive active layer (4) are composite ceramics composed of an electronically conductive phase and an ionicly conductive phase, wherein the volume fraction of the electronically conductive phase is not less than 40%; the porosity of the negative current collector layer (1) is 10~70%, the porosity of the negative active layer (2) is 20~35%, and the porosity of the positive active layer (4) is 20~35%; The electron-conducting phase in the positive electrode active layer (4) is 430L, SUS445, SUS446, (La 1-x Sr x (Cr) 1-y Fe y )O 3−δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3−δ 、(La 1-x Sr x TiO 3−δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, wherein 0 < x < 1, 0 < y < 1, 0 < δ < 1; the ionic conductive phase in the positive electrode active layer (4) is one or more of the following: doped zirconium oxide, doped cerium oxide, doped lanthanum gallate, doped barium zirconate, and doped barium cerate. The electrolyte membrane (3) is a dense oxygen ion conductor electrolyte membrane; The inner surface of the positive electrode active layer (4) is covered with a nano-positive electrode catalyst with a particle size of 1~500nm, and the nano-positive electrode catalyst is Ce. 1-x La x O 2−δ Ce 1-x Y x O 2−δ Ce 1-x Sm x O 2−δ Ce 1-x Gd x O 2−δ Ce 1-x Pr x O 2−δ Ce 1-x Nd x O 2−δ Ce 1- x Ca x O 2−δ Ce 1-x Mg x O 2−δ 、(La 1-x Sr x (Cr) 1-y Fe y )O 3−δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3−δ 、(La 1-x Sr x TiO 3−δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, where 0 < x < 1, 0 < δ < 1; The negative electrode of the carbon dioxide self-enriched solid oxide electrolytic battery is fed with water vapor or a mixture of water vapor and hydrogen, which is mainly composed of water vapor, and an electrolytic reduction reaction of water vapor occurs to obtain hydrogen or a mixture of hydrogen and water vapor, which is mainly composed of hydrogen; the positive electrode is fed with combustible gas or a mixture of combustible gas, and a deep or complete oxidation reaction of combustible gas occurs to obtain carbon dioxide or a mixture of gas containing a high concentration of carbon dioxide; the material of the positive electrode active layer (4) can exist stably under both oxidation and reduction conditions.

2. A solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 1, characterized in that: The electron-conducting phases in the negative electrode current collector layer (1) and the negative electrode active layer (2) are all Ni, Fe, Cu, Co, FeNi3, 430L, SUS445, SUS446, NiO, CuO, Fe3O4, Co3O4, (La 1-x Sr x (Cr) 1-y Fe y )O 3−δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3−δ 、(La 1-x Sr x TiO 3−δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, wherein 0 < x < 1, 0 < y < 1, 0 < δ < 1; the ionic conductive phase in the negative electrode current collector layer (1) and the negative electrode active layer (2) is one or more of the following: doped zirconium oxide, doped cerium oxide, doped lanthanum gallate, doped barium zirconate, and doped barium cerate.

3. A solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 1, characterized in that: The inner surfaces of both the negative electrode current collector layer (1) and the negative electrode active layer (2) are covered with nano-negative electrode catalysts with a particle size of 1~500nm. The nano-negative electrode catalysts are Fe, Ni, Cu, Co, FeNi3, Ce. 1-x La x O 2−δ Ce 1-x Y x O 2−δ Ce 1-x Sm x O 2−δ Ce 1-x Gd x O 2−δ Ce 1-x Pr x O 2−δ Ce 1-x Nd x O 2−δ Ce 1-x Ca x O 2−δ Ce 1-x Mg x O 2−δ 、(La 1-x Sr x (Cr) 1-y Fe y )O 3−δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3−δ 、(La 1-x Sr x TiO 3−δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, where 0 < x < 1 and 0 < δ < 1.

4. A solid oxide electrolytic cell with self-enriched carbon dioxide according to any one of claims 1 to 3, characterized in that: The surface of the positive electrode active layer (4) is further provided with a positive electrode current collector layer (5), which is one or more of an electronically conductive phase and an ionicly conductive phase.

5. A solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 4, characterized in that: The electron-conducting phase in the positive current collector layer (5) is 430L, SUS445, SUS446, (La 1-x Sr x (Cr) 1-y Fe y )O 3−δ 、(La 1- x Sr x (Cr) 1-y Mn y )O 3−δ 、(La 1-x Sr x TiO 3−δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, 0 < x < 1, 0 < y < 1, 0 < δ < 1.

6. A solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 4, characterized in that: The ionic conductive phase in the positive electrode current collector layer (5) is one or more of the following: doped zirconium oxide, doped cerium oxide, doped lanthanum gallate, doped barium zirconate, and doped barium cerate, with a porosity of 10-70%.

7. A solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 4, characterized in that: The inner surface of the positive electrode current collector layer (5) is covered with a nano-positive electrode catalyst with a particle size of 1~500nm. The nano-positive electrode catalyst is Fe, Ni, Cu, Co, FeNi3, Ce. 1-x La x O 2−δ Ce 1-x Y x O 2−δ Ce 1-x Sm x O 2−δ Ce 1-x Gd x O 2−δ Ce 1-x Pr x O 2−δ Ce 1- x Nd x O 2−δ Ce 1-x Ca x O 2−δ Ce 1-x Mg x O 2−δ 、(La 1-x Sr x (Cr) 1-y Fe y )O 3−δ 、(La 1-x Sr x (Cr) 1-y Mn y )O 3−δ 、(La 1- x Sr x TiO 3−δ La 2-x Sr x Fe 2-y-z Ni y Mo z O 6-δ One or more of the following, where 0 < x < 1 and 0 < δ < 1.

8. A solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 1 or 2, characterized in that: The thickness of the negative electrode current collector layer (1) is 50~2000 micrometers, the thickness of the negative electrode active layer (2) is 5~20 micrometers, the thickness of the electrolyte membrane (3) is 1~1000 micrometers, the thickness of the positive electrode active layer (4) is 50~2000 micrometers, the thickness of the positive electrode current collector layer (5) is 50~2000 micrometers, and the total thickness of the self-enriched carbon dioxide solid oxide electrolytic battery is not less than 300 micrometers.

9. The method for preparing a solid oxide electrolytic cell with self-enriched carbon dioxide according to claim 1, characterized in that, Includes the following steps: Step 1: Prepare negative electrode current collector green body, negative electrode active layer green body, electrolyte membrane green body, positive electrode active layer green body and positive electrode current collector green body on the mylar membrane respectively; Step 2: After stacking the negative electrode current collector green sheet, negative electrode active layer green sheet, electrolyte membrane green sheet, positive electrode active layer green sheet, and positive electrode current collector green sheet in the manner of green sheet, the whole sheet is statically pressed to obtain a solid oxide electrolytic cell green sheet. Step 3: The product obtained in Step 2 is subjected to gradient sintering to make the electrolyte membrane layer dense, and then cooled to obtain a solid oxide electrolytic cell that enriches carbon dioxide.

Citation Information

Patent Citations

  • Method and apparatus for producing hydrogen

    CN101103140A

  • Natural gas-assisted steam electrolyzer

    US6051125A

  • Proton conductor solid oxide battery with negative electrode barrier layer

    CN114628753A

  • Electrode, solid -state oxide fuel cell and solid -state oxidation thing electrolytic bath

    CN207459069U