Composite material pressure vessel suitable for liquid oxygen environment and preparation method of composite material pressure vessel

By setting a thin-walled metal lining layer, a transition layer and a fiber-wrapped composite material layer in the pressure vessel, the problem of insufficient mechanical properties and permeability resistance of the pressure vessel under a liquid oxygen environment in the prior art is solved, and higher impact resistance and compression resistance are achieved.

CN119687360AInactive Publication Date: 2025-03-25SHENYANG OUSHIDUN NEW MATERIAL TECH

Patent Information

Application Number
CN202510221756.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-02-27
Publication Date
2025-03-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, pressure vessels suitable for liquid oxygen environments have shortcomings in terms of mechanical properties and anti-permeability, especially when they are stimulated by ignition sources such as impact, friction, and vibration in the liquid oxygen environment, combustion reactions are prone to occur.

Method used

By providing a thin-walled metal lining layer, a transition layer and a fiber-wrapped composite material layer, each layer has good liquid oxygen compatibility. The transition layer contains fluoropolyarylether, and phthalate coupling agent and nanofiller are added to enhance the bonding capacity between layers.

Benefits of technology

It significantly improves the mechanical properties and permeability of the pressure vessel, ensures that there is no combustion reaction in the liquid oxygen environment, and improves the overall impact and compression resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a composite material pressure container suitable for a liquid oxygen environment and a preparation method of the composite material pressure container, and belongs to the technical field of composite materials. The composite material pressure container suitable for the liquid oxygen environment sequentially comprises a thin-wall metal lining layer, a transition layer and a fiber winding composite material layer from inside to outside, the transition layer comprises fluorine-containing polyarylether; the fiber winding composite material layer is formed by carbon fiber woven cloth dipped with composite epoxy resin and carbon fiber yarns on the lining layer in a continuous annular and spiral cross winding manner; matrix resin in the composite epoxy resin comprises bromine-containing epoxy resin and / or chlorine-containing epoxy resin. By arranging the thin-wall metal lining layer, the transition layer and the fiber winding composite material layer, each layer of structure has good liquid oxygen compatibility; and by arranging the transition layer, the combining capacity of the thin-wall metal lining layer and the fiber winding composite material layer is further improved, and then the overall mechanical property and anti-permeation performance of the pressure container are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a composite material pressure vessel suitable for a liquid oxygen environment and a preparation method thereof, belonging to the technical field of composite materials. Background Art

[0002] The new generation of non-toxic and pollution-free cryogenic launch vehicles in China use cryogenic propellants, and the subsequent new generation of manned rockets and heavy-lift launch vehicles will also use cryogenic propellants. The new generation of manned and heavy-lift launch vehicles have higher requirements for carrying capacity, so the structural system should have higher structural efficiency. The gas cylinder is a key component of the liquid launch vehicle pressurization system, which is used to store high-pressure gas medium to pressurize or replenish the propellant tank. Placing the gas cylinder in the liquid oxygen propellant tank and utilizing the low temperature environment of the propellant can greatly increase the gas density inside the gas cylinder and improve the gas storage capacity, thereby reducing the number of gas cylinders required and reducing the weight of the rocket body structure.

[0003] However, this places higher demands on the performance of pressure vessels for storing high-pressure gas. For pressure vessels suitable for liquid oxygen environments, not only the lightweight performance of the pressure vessels should be considered, but also the compatibility with liquid oxygen and the pressure bearing capacity should be emphasized. On the one hand, it needs to be able to avoid combustion reactions when stimulated by ignition sources such as impact, friction, and vibration in the liquid oxygen environment; on the other hand, it needs to have excellent mechanical properties and anti-permeability properties at low temperatures.

[0004] The prior art discloses a composite pressure vessel with a metal lining and a resin system wrapped around the outside, which solves the problem of liquid oxygen compatibility; however, there is a problem of bonding between the metal lining and the external composite material, which in turn affects the overall mechanical properties and anti-permeation properties of the pressure vessel. Therefore, how to provide a composite pressure vessel with excellent mechanical properties and anti-permeation properties that can be suitable for liquid oxygen environments is an issue that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above problems, the present application proposes a composite pressure vessel suitable for liquid oxygen environment and a preparation method thereof. By setting a thin-walled metal lining layer, a transition layer and a fiber-wound composite material layer, each layer structure has good liquid oxygen compatibility; by setting the transition layer, the bonding ability between the thin-walled metal lining layer and the fiber-wound composite material layer is further improved, thereby improving the overall mechanical properties and anti-permeation properties of the pressure vessel.

[0006] According to one aspect of the present application, there is provided a composite pressure vessel suitable for a liquid oxygen environment, which comprises, from the inside to the outside, a thin-walled metal liner layer, a transition layer, and a fiber-wound composite material layer; The transition layer includes fluorinated polyarylether; The fiber-wound composite material layer is formed by continuous hoop and spiral cross-wound carbon fiber woven cloth impregnated with composite epoxy resin and carbon fiber yarn on the inner lining layer; The matrix resin in the composite epoxy resin includes bromine-containing epoxy resin and / or chlorine-containing epoxy resin.

[0007] Specifically, the material of the thin-walled metal lining layer includes stainless steel or aluminum alloy; the thickness of the thin-walled metal lining layer is 0.005 to 0.01 times the inner diameter of the pressure vessel.

[0008] Optionally, the transition layer is prepared by comprising the following raw materials in parts by weight: 100-110 parts of solvent, 40-60 parts of fluorinated polyarylether, 2-7 parts of phthalate coupling agent and 10-15 parts of nanofiller.

[0009] Specifically, the present application makes specific restrictions on the component composition and ratio of the transition layer, and by adding phthalate coupling agents and nanofillers into the fluorinated polyarylether, the components have good compatibility, which can, on the one hand, improve the interfacial bonding strength between the transition layer and the thin-walled metal lining layer and the fiber-wound composite material layer; on the other hand, it helps to improve its mechanical properties and anti-penetration properties.

[0010] Optionally, the fluorinated polyarylether is a fluorinated phthalocyanine polyarylether, the phthalate coupling agent includes isopropoxy tri(dioctyl pyrophosphate) titanate or isopropoxy aluminum tristearate; the nanofiller includes nanographene and nanoaluminum oxide; and the solvent includes N,N-dimethylacetamide.

[0011] Specifically, the weight ratio of nano-graphene to nano-alumina is 1:(2~4).

[0012] Optionally, the preparation method of the fluorinated phthalazinone polyarylether comprises the following steps: S1 Take 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and toluene and place them in a flask; S2 is introduced with nitrogen and heated to react with water; After the water reaction in S3 is completed, the temperature is lowered, and the polyfluorinated monomer perfluorobiphenyl and N,N-dimethylacetamide are added, and the reaction is continued until the viscosity no longer changes; Fluorinated poly(phenylene ether) was separated by S4 precipitation method.

[0013] Optionally, the molar ratio of the 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and the polyfluorinated monomer perfluorobiphenyl is 1:(1-1.5):(1-1.2); the heating reaction temperature in S2 is 120-140°C, and the reaction time is 3-5h; and the temperature is lowered to 105-115°C in S3.

[0014] Specifically, the present application does not make specific limitations on the amount of toluene and N,N-dimethylacetamide added. Those skilled in the art will adjust the amount of toluene and N,N-dimethylacetamide added based on the moisture collection and viscosity conditions.

[0015] Optionally, the composite epoxy resin comprises 80-100 parts of compound epoxy resin, 5-10 parts of composite nanofiller, 10-20 parts of ether diluent, 5-15 parts of flame retardant and 30-50 parts of amine curing agent in parts by weight; Specifically, the composite epoxy resin is prepared by adding a flame retardant to the compounded epoxy resin, stirring evenly, and reacting at 50-60° C. for 1-2 hours; adding a composite nanofiller and an ether diluent and dispersing evenly, adding an amine curing agent and stirring evenly to obtain the composite epoxy resin.

[0016] The compound epoxy resin is aliphatic epoxy resin and bisphenol A epoxy resin; the bisphenol A epoxy resin includes tetrabromobisphenol A epoxy resin or tetrachlorobisphenol A epoxy resin.

[0017] Specifically, the weight ratio of the aliphatic epoxy resin to the bisphenol A epoxy resin is (0.5~0.8):1.

[0018] Specifically, aliphatic epoxy resin and bisphenol A epoxy resin are compounded in a specific ratio to obtain compound epoxy resin. Firstly, the two have good compatibility and the interface layer is very stable. The two are blended in a specific ratio to improve toughness.

[0019] Specifically, the aliphatic epoxy resin includes 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate.

[0020] Optionally, the compounded epoxy resin further comprises polyimide and m-phenylenediamine; the weight ratio of the compounded epoxy resin to polyimide and m-phenylenediamine is (2-4):1, and the amount of m-phenylenediamine used is 2-5% of the epoxy equivalent of the compounded epoxy resin.

[0021] Specifically, the preparation method of the compound epoxy resin is to mix and react aliphatic epoxy resin, bisphenol A epoxy resin, polyimide and meta-phenylenediamine, the reactant temperature is 60-80° C., and the reaction time is 1-2 hours.

[0022] Optionally, the composite nanofiller comprises modified montmorillonite and modified carbon nanotubes in a weight ratio of 1:(2-4); Specifically, the modified montmorillonite is modified with an aminosilane coupling agent.

[0023] Specifically, the preparation method of modified montmorillonite comprises the following steps: S1 Place montmorillonite powder in deionized water, stir evenly, and adjust the pH to 3-4 with hydrochloric acid; Dissolve S2 aminosilane coupling agent in ethanol, add pretreated montmorillonite, stir evenly, and react in a constant temperature water bath at 60-70℃ for 20-26h; S3 is centrifuged, washed and dried to obtain modified montmorillonite.

[0024] Specifically, the volume fraction of the aminosilane coupling agent is 1%~2%; the mass ratio of montmorillonite to deionized water is 1:(400~600).

[0025] Specifically, the aminosilane coupling agent is 3-aminopropyltriethoxysilane or N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.

[0026] Preferably, the aminosilane coupling agent is 3-aminopropyltriethoxysilane.

[0027] Specifically, the aminosilane coupling agent is used to modify the montmorillonite, and 3-aminopropyltriethoxysilane undergoes a condensation reaction with the hydroxyl groups on the surface of the montmorillonite to introduce amino groups.

[0028] Specifically, the modified carbon nanotubes are obtained by acid modification.

[0029] Specifically, the method for preparing modified carbon nanotubes comprises the following steps: S01 placing the carbon nanotubes in a container, adding a mixed solution of concentrated sulfuric acid and concentrated nitric acid to obtain a mixture; S02 cool the mixture in an ice water bath, then heat it to 80-90°C and reflux for 3-5h; S03 is cooled to room temperature, centrifuged, washed and dried to obtain modified carbon nanotubes.

[0030] During the modification process of carbon nanotubes, the surface of carbon nanotubes is oxidized and a large number of hydroxyl groups and carboxyl groups are introduced.

[0031] Specifically, the volume ratio of concentrated sulfuric acid to concentrated nitric acid is (2~4):1.

[0032] Specifically, amino groups are introduced into the surface of the modified montmorillonite, and carboxyl groups are introduced into the surface of the modified carbon nanotubes. The two can undergo a condensation reaction to form an amide bond, thereby effectively enhancing the interfacial bonding strength between the modified montmorillonite and the modified carbon nanotubes.

[0033] Specifically, modified montmorillonite and modified carbon nanotubes are compounded in a specific ratio. The addition of modified montmorillonite is beneficial to improving its dispersibility and its bonding with the composite epoxy resin, improving the size uniformity, and improving its mechanical properties. The addition of modified carbon nanotubes, on the one hand, can have a good interface bonding between the modified montmorillonite and the modified carbon nanotubes, which can effectively transfer stress, reduce the generation and expansion of cracks, and improve fatigue resistance. On the other hand, the modified carbon nanotubes have good compatibility with carbon fiber woven cloth and carbon fiber yarn, which is beneficial to improving the bonding of the lining layer and the fiber winding composite material layer. In addition, the addition of modified montmorillonite and modified carbon nanotubes in a specific ratio is also beneficial to improving its mechanical properties.

[0034] The flame retardant is a phosphoric acid acrylate monomer containing a double bond; The amine curing agent is one of m-phenylenediamine and 4,4'-diaminodiphenyl ether; The ether diluent includes one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, phenyl glycidyl ether and 4-tert-butylphenyl glycidyl ether.

[0035] According to another aspect of the present application, a method for preparing the composite pressure vessel is also provided, comprising the following steps: (1) Preparation of thin-walled metal lining; (2) Preparation of transition layer: dissolving fluorinated polyarylether in a solvent, adding phthalate coupling agent and nanofiller, stirring evenly and filtering, coating on the outer surface of the thin-walled metal lining layer, and drying naturally; (3) The thin-walled metal liner coated with the transition layer is installed on a winding machine, and 2-4 layers of carbon fiber woven cloth impregnated with composite epoxy resin are successively wound hoop-wise on the outer surface of the liner, and then 1-2 layers of carbon fiber yarn impregnated with composite epoxy resin are successively spirally wound on the surface of the carbon fiber woven cloth, and the process is repeated for 6-10 cycles; (4) After the winding is completed, high temperature curing is performed to obtain the composite material pressure vessel.

[0036] Specifically, the thin-walled metal lining layer prepared in step (1) is a prior art and will not be described in detail in this application, wherein the thin-walled metal lining layer can be stainless steel or aluminum alloy.

[0037] Specifically, the preparation of the transition layer in step (2) specifically includes: placing the fluorinated polyarylether in N,N-dimethylacetamide and stirring; adding a phthalate coupling agent, nanographene and nanoalumina, dispersing them evenly, filtering, and then coating them on the outer surface of the thin-walled metal lining layer and drying them naturally.

[0038] Optionally, the glue content of the winding layer formed in each cycle in step (3) is 25-35%, the hoop winding is 90° winding using carbon fiber woven cloth, and the thickness of a single layer is 0.2-0.5 mm; the winding angle of the spiral winding is 12-14°, and the thickness of a single layer is 0.1-0.3 mm; In step (4), the high temperature curing is firstly to uniformly increase the temperature from 30°C to 90°C within 60 minutes and keep it at this temperature for 2-3 hours; then to uniformly increase the temperature to 120°C within 60 minutes and keep it at this temperature for 2-4 hours; finally, to uniformly increase the temperature to 160°C within 60 minutes and keep it at this temperature for 2-4 hours.

[0039] The beneficial effects of this application include but are not limited to: 1. The composite pressure vessel suitable for liquid oxygen environment provided in the present application has good liquid oxygen compatibility by arranging a thin-walled metal liner layer, a transition layer and a fiber-wound composite material layer; by arranging the transition layer, the bonding ability between the thin-walled metal liner layer and the fiber-wound composite material layer is further improved, thereby improving the overall mechanical properties and anti-permeation performance of the pressure vessel.

[0040] 2. The composite pressure vessel suitable for liquid oxygen environment provided in the present application is prepared by compounding a fluorinated polyarylether, a phthalate coupling agent and a nanofiller in a specific ratio to obtain a transition layer. The transition layer has a strong bonding force with the thin-walled metal liner layer, and the transition layer also has a strong bonding force with the fiber-wound composite material layer, which is beneficial to improving the bonding force between the fiber-wound composite material layer and the thin-walled metal liner layer, and improving the overall impact resistance and compression resistance. On the other hand, the synergistic effect of nano-graphene and nano-alumina compounded in a specific ratio is beneficial to improving its mechanical properties and interface bonding strength.

[0041] 3. The composite pressure vessel suitable for liquid oxygen environment provided in the present application comprises a composite epoxy resin in which aliphatic epoxy resin and bisphenol A epoxy resin are compounded in a specific ratio to obtain a composite epoxy resin. Firstly, the two have good compatibility and the interface layer is very stable. The two are blended in a specific ratio to improve toughness. The addition of polyimide and m-phenylenediamine causes an addition reaction between the imide group and the epoxy group to cause chemical crosslinking, thereby improving the liquid oxygen compatibility of the resin system. The polyimide can also provide a tough segment to further improve the liquid oxygen impact resistance. The m-phenylenediamine can also be used as an auxiliary curing agent to promote the co-curing reaction and improve the crosslinking degree. The two are helpful to comprehensively improve the performance of the composite epoxy resin.

[0042] 4. The present application provides a composite pressure vessel suitable for liquid oxygen environment, wherein modified montmorillonite and modified carbon nanotubes are compounded in a specific ratio, and the addition of modified montmorillonite is beneficial to improving its dispersibility and its binding property with composite epoxy resin, improving dimensional uniformity, and improving its mechanical properties; the addition of modified carbon nanotubes, on the one hand, can have a good interface binding between the modified montmorillonite and the modified carbon nanotubes, can effectively transfer stress, reduce the generation and expansion of cracks, and improve fatigue resistance; on the other hand, the modified carbon nanotubes have good compatibility with carbon fiber woven cloth and carbon fiber yarn, which is beneficial to improving the binding property of the liner layer and the fiber winding composite material layer; in addition, the addition of modified montmorillonite and modified carbon nanotubes in a specific ratio is also beneficial to improving its mechanical properties.

[0043] 5. The present application provides a method for preparing a composite material pressure vessel suitable for liquid oxygen environment. On the one hand, the present application adopts a combination of hoop winding and spiral winding to carry out fiber winding, and limits the thickness, winding angle, curing parameters, etc., so as to improve its overall load-bearing performance and pressure resistance, and ensure its strength and stability. DETAILED DESCRIPTION

[0044] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0045] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any methods and materials similar to or equivalent to those described herein can be applied to the method of the present invention. The preferred implementation methods and materials described in this patent are for demonstration purposes only. In the following embodiments, (1) the preparation of a thin-walled metal lining layer in the preparation of a composite pressure vessel is prepared using existing technology. The diameter, length, and thickness of the thin-walled metal lining layer in the following embodiments are the same and will not be repeated in the embodiments.

[0046] Example 1 This embodiment relates to a composite pressure vessel suitable for a liquid oxygen environment, which specifically includes the following steps: Preparation of composite epoxy resin: Step 01: Preparation of compound epoxy resin: tetrabromobisphenol A epoxy resin, 3,4-epoxycyclohexyl methyl ester, polyimide and m-phenylenediamine are reacted at 60°C for 1 hour to obtain a compound epoxy resin; wherein the weight ratio of tetrabromobisphenol A epoxy resin to 3,4-epoxycyclohexyl methyl ester is 1:0.5, the weight ratio of compound epoxy resin to polyimide and m-phenylenediamine is 2:1, and the amount of m-phenylenediamine is 2% of the epoxy equivalent of the compound epoxy resin; Step 02: Preparation of composite epoxy resin: Add 5 parts of flame retardant to 80 parts of the obtained compound epoxy resin, react at 50°C for 1 hour, then add 5 parts of composite nanofiller and 10 parts of ether diluent, stir and disperse, finally add 30 parts of amine curing agent and stir evenly to obtain a composite epoxy resin; wherein the composite nanofiller includes modified montmorillonite and modified carbon nanotubes in a weight ratio of 1:2; the flame retardant is a phosphate acrylate monomer containing a double bond; the amine curing agent is meta-xylylenediamine; and the ether diluent is ethylene glycol dimethyl ether.

[0047] The preparation method of modified montmorillonite is as follows: Place montmorillonite powder in deionized water with a mass ratio of montmorillonite to deionized water of 1:400, stir evenly, and adjust pH 3 with hydrochloric acid; 3-aminopropyltriethoxysilane is dissolved in ethanol with a volume fraction of aminosilane coupling agent of 1%, add pretreated montmorillonite, stir evenly, and react in a constant temperature water bath at 60°C for 24 hours; centrifuge, wash, and dry to obtain modified montmorillonite.

[0048] The preparation method of modified carbon nanotubes is as follows: The carbon nanotubes are placed in a container, and a mixed solution of concentrated sulfuric acid and concentrated nitric acid is added, wherein the volume ratio of the concentrated sulfuric acid to the concentrated nitric acid is 2:1, to obtain a mixture; the mixture is placed in an ice water bath for cooling, and then the temperature is raised to 80°C and refluxed for reaction for 3 hours; the mixture is cooled to room temperature, centrifuged, washed, and dried to obtain modified carbon nanotubes.

[0049] Preparation of fluorinated naphthalene biphenyl polyarylether: S1 Take 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and toluene and place them in a flask; S2 is introduced with nitrogen and heated to 120°C for 3 hours to carry out water-containing reaction; After S3 reacts with water, the temperature is lowered to 105-115°C, and polyfluorinated monomers perfluorobiphenyl and N,N-dimethylacetamide are added, and the reaction is continued until the viscosity no longer changes; Fluorinated naphthalene biphenyl polyarylether was separated by S4 precipitation method; Wherein, the molar ratio of 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and polyfluorinated monomer perfluorobiphenyl is 1:1:1.

[0050] Preparation of composite pressure vessels: (1) Preparation of thin-walled metal lining; (2) Preparation of transition layer: dissolving 40 parts of fluorinated poly(phenylene fluoride) in 100 parts of N,N-dimethylacetamide solvent, adding 2 parts of phthalate coupling agent isopropoxy tris(dioctyl pyrophosphate acyloxy) titanate and 10 parts of nanofiller, wherein the nanofiller includes nanographene and nanoalumina; the weight ratio of nanographene to nanoalumina is 1:2, stirring evenly, filtering, coating on the outer surface of the thin-walled metal lining layer, and drying naturally; (3) The thin-walled metal lining layer coated with the transition layer is installed on the winding machine, and two layers of carbon fiber woven cloth impregnated with composite epoxy resin are wound around the outer surface of the lining layer in turn. The circumferential winding is to use the carbon fiber woven cloth for 90° winding, and the thickness of a single layer is 0.2 mm; then, a carbon fiber yarn impregnated with composite epoxy resin is spirally wound on the surface of the carbon fiber woven cloth in turn, and the winding angle of the spiral winding is 12°, and the thickness of a single layer is 0.1 mm; 6 cycles are repeated, and the glue content in the winding layer formed in each cycle is 25%; (4) After winding is completed, high temperature curing is performed, and the composite pressure vessel is obtained after high temperature curing; wherein, the high temperature curing is firstly to uniformly increase the temperature from 30°C to 90°C within 60 minutes, and keep the temperature for 2 hours; then to uniformly increase the temperature to 120°C within 60 minutes, and keep the temperature for 2 hours; finally, to uniformly increase the temperature to 160°C within 60 minutes, and keep the temperature for 2 hours.

[0051] Example 2 Preparation of composite epoxy resin: Step 01: Preparation of compound epoxy resin: tetrachlorobisphenol A epoxy resin, 3,4-epoxycyclohexyl methyl ester, polyimide and m-phenylenediamine are reacted at 80°C for 2 hours to obtain a compound epoxy resin; wherein the weight ratio of tetrachlorobisphenol A epoxy resin to 3,4-epoxycyclohexyl methyl ester is 1:0.8, the weight ratio of compound epoxy resin to polyimide and m-phenylenediamine is 4:1, and the amount of m-phenylenediamine is 5% of the epoxy equivalent of the compound epoxy resin; Step 02: Preparation of composite epoxy resin: Add 15 parts of flame retardant to 100 parts of the obtained compound epoxy resin, react at 60°C for 2h, then add 10 parts of composite nanofiller and 20 parts of ether diluent and stir to disperse, finally add 50 parts of amine curing agent and stir evenly to obtain composite epoxy resin; wherein, the composite nanofiller includes modified montmorillonite and modified carbon nanotubes in a weight ratio of 1:4; the flame retardant is a phosphate acrylate monomer containing a double bond; the amine curing agent is 4,4'-diaminodiphenyl ether; and the ether diluent is diethylene glycol dimethyl ether.

[0052] The preparation method of modified montmorillonite is as follows: Montmorillonite powder was placed in deionized water with a mass ratio of montmorillonite to deionized water of 1:600, stirred evenly, and the pH was adjusted to 4 with hydrochloric acid; 3-aminopropyltriethoxysilane was dissolved in ethanol with a volume fraction of 1% of aminosilane coupling agent, the pretreated montmorillonite was added, stirred evenly, and reacted in a constant temperature water bath at 70°C for 20 hours; centrifuged, washed, and dried to obtain modified montmorillonite.

[0053] The preparation method of modified carbon nanotubes is as follows: The carbon nanotubes are placed in a container, and a mixed solution of concentrated sulfuric acid and concentrated nitric acid is added, wherein the volume ratio of the concentrated sulfuric acid to the concentrated nitric acid is 4:1, to obtain a mixture; the mixture is placed in an ice water bath for cooling, and then the temperature is raised to 90° C. and refluxed for reaction for 5 hours; the mixture is cooled to room temperature, centrifuged, washed, and dried to obtain modified carbon nanotubes.

[0054] Preparation of fluorinated naphthalene biphenyl polyarylether: S1 Take 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and toluene and place them in a flask; S2 is introduced with nitrogen and heated to a temperature of 140°C for 3 to 5 hours to carry out a water-containing reaction; After the water reaction in S3 is completed, the temperature is lowered to 115°C, and polyfluorinated monomers perfluorobiphenyl and N,N-dimethylacetamide are added, and the reaction is continued until the viscosity no longer changes; Fluorinated naphthalene biphenyl polyarylether was separated by S4 precipitation method; Among them, the molar ratio of 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and polyfluorinated monomer perfluorobiphenyl is 1:1.5:1.2.

[0055] Preparation of composite pressure vessels: (1) Preparation of thin-walled metal lining; (2) Preparing a transition layer: dissolving 60 parts of fluorinated poly(phenylene fluoride) in 110 parts of N,N-dimethylacetamide as a solvent, adding 7 parts of isopropoxy aluminum tristearate as a phthalate coupling agent and 15 parts of a nanofiller, wherein the nanofiller comprises nanographene and nanoalumina; the weight ratio of the nanographene to the nanoalumina is 1:4, stirring evenly, filtering, coating on the outer surface of the thin-walled metal lining layer, and drying naturally; (3) The thin-walled metal lining layer coated with the transition layer is installed on the winding machine, and four layers of carbon fiber woven cloth impregnated with composite epoxy resin are wound around the outer surface of the lining layer in sequence, and the circumferential winding is performed by winding the carbon fiber woven cloth at 90°, and the thickness of a single layer is 0.5 mm; then, carbon fiber yarn impregnated with composite epoxy resin is spirally wound on the surface of the carbon fiber woven cloth for two layers, and the winding angle of the spiral winding is 14°, and the thickness of a single layer is 0.3 mm; 10 cycles are repeated, and the glue content in the winding layer formed in each cycle is 35%; (4) After winding is completed, high temperature curing is performed, and the composite pressure vessel is obtained after high temperature curing; wherein, the high temperature curing is firstly to uniformly increase the temperature from 30°C to 90°C within 60 minutes, and keep the temperature for 3 hours; then to uniformly increase the temperature to 120°C within 60 minutes, and keep the temperature for 4 hours; finally, to uniformly increase the temperature to 160°C within 60 minutes, and keep the temperature for 4 hours.

[0056] Example 3 Preparation of composite epoxy resin: (1) Preparation of compound epoxy resin: tetrabromobisphenol A epoxy resin, 3,4-epoxycyclohexyl methyl ester, polyimide and m-phenylenediamine are reacted at 70°C for 2 hours to obtain a compound epoxy resin; wherein the weight ratio of tetrabromobisphenol A epoxy resin to 3,4-epoxycyclohexyl methyl ester is 1:0.5, the weight ratio of compound epoxy resin to polyimide and m-phenylenediamine is 3:1, and the amount of m-phenylenediamine used is 3% of the epoxy equivalent of the compound epoxy resin; (2) Preparation of composite epoxy resin: 10 parts of flame retardant were added to 90 parts of the obtained composite epoxy resin, and the mixture was reacted at 55°C for 2 h. Then 6 parts of composite nanofiller and 10 parts of ether diluent were added and stirred and dispersed. Finally, 40 parts of amine curing agent were added and stirred evenly to obtain composite epoxy resin; wherein the composite nanofiller includes modified montmorillonite and modified carbon nanotubes in a weight ratio of 1:3; the flame retardant is a phosphoric acid acrylate monomer containing a double bond; the amine curing agent is meta-xylylenediamine; and the ether diluent is ethylene glycol dimethyl ether.

[0057] The preparation method of modified montmorillonite is as follows: Place montmorillonite powder in deionized water with a mass ratio of montmorillonite to deionized water of 1:500, stir evenly, and adjust pH 3 with hydrochloric acid; 3-aminopropyltriethoxysilane is dissolved in ethanol with a volume fraction of aminosilane coupling agent of 1%, add pretreated montmorillonite, stir evenly, and react in a constant temperature water bath at 60°C for 24 hours; centrifuge, wash, and dry to obtain modified montmorillonite.

[0058] The preparation method of modified carbon nanotubes is as follows: The carbon nanotubes are placed in a container, and a mixed solution of concentrated sulfuric acid and concentrated nitric acid is added, wherein the volume ratio of the concentrated sulfuric acid to the concentrated nitric acid is 3:1, to obtain a mixture; the mixture is placed in an ice water bath for cooling, and then the temperature is raised to 80°C and refluxed for reaction for 3 hours; the mixture is cooled to room temperature, centrifuged, washed, and dried to obtain modified carbon nanotubes.

[0059] Preparation of fluorinated naphthalene biphenyl polyarylether: S1 Take 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and toluene and place them in a flask; S2 is introduced with nitrogen and heated to a temperature of 130°C for 4 hours to carry out a water-containing reaction; After the water reaction in S3 is completed, the temperature is lowered to 110°C, and polyfluorinated monomers perfluorobiphenyl and N,N-dimethylacetamide are added, and the reaction is continued until the viscosity no longer changes; Fluorinated naphthalene biphenyl polyarylether was separated by S4 precipitation method; Among them, the molar ratio of 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and polyfluorinated monomer perfluorobiphenyl is 1:1:1.2.

[0060] Preparation of composite pressure vessels: (1) Preparation of thin-walled metal lining; (2) Preparation of transition layer: dissolving 50 parts of fluorinated poly(phenylene fluoride) in 100 parts of N,N-dimethylacetamide solvent, adding 5 parts of phthalate coupling agent isopropoxy tris(dioctyl pyrophosphate acyloxy) titanate and 10 parts of nanofiller, wherein the nanofiller includes nanographene and nanoalumina; the weight ratio of nanographene to nanoalumina is 1:2, stirring evenly, filtering, coating on the outer surface of the thin-walled metal lining layer, and drying naturally; (3) The thin-walled metal lining layer coated with the transition layer is installed on the winding machine, and three layers of carbon fiber woven cloth impregnated with composite epoxy resin are wound around the outer surface of the lining layer in sequence, and the circumferential winding is performed by winding the carbon fiber woven cloth at 90°, and the thickness of a single layer is 0.2 mm; then, carbon fiber yarn impregnated with composite epoxy resin is spirally wound on the surface of the carbon fiber woven cloth for two layers, and the winding angle of the spiral winding is 14°, and the thickness of a single layer is 0.2 mm; 7 cycles are repeated, and the glue content in the winding layer formed in each cycle is 30%; (4) After winding is completed, high temperature curing is performed, and the composite pressure vessel is obtained after high temperature curing; wherein, the high temperature curing is firstly to increase the temperature uniformly from 30°C to 90°C within 60 minutes, and keep the temperature for 3 hours; then to increase the temperature uniformly to 120°C within 60 minutes, and keep the temperature for 3 hours; finally, to increase the temperature uniformly to 160°C within 60 minutes, and keep the temperature for 2 hours.

[0061] Example 4 The difference between Example 4 and Example 3 is that the transition layer does not include nanofillers, and the rest are the same.

[0062] Example 5 The difference between Example 5 and Example 3 is that in the nanofiller in the transition layer, the weight ratio of nano-graphene to nano-alumina is 1:1, and the rest are the same.

[0063] Example 6 The difference between Example 6 and Example 3 is that the transition layer does not include a phthalate coupling agent, and the rest is the same.

[0064] Example 7 The difference between Example 7 and Example 3 is that the transition layer only includes fluorinated poly(aryl phthalocyanine) biphenyl ether, and the rest are the same.

[0065] Example 8 The difference between Example 8 and Example 3 is that the composite nanofiller is not included, and the rest is the same.

[0066] Example 9 The difference between Example 9 and Example 3 is that modified montmorillonite is not included, and the rest are the same.

[0067] Example 10 The difference between Example 10 and Example 3 is that the weight ratio of modified montmorillonite to modified carbon nanotubes is 1:1, and the rest are the same.

[0068] Embodiment 11 The difference between Example 11 and Example 3 is that the compounded epoxy resin does not include aliphatic epoxy resin, and the rest is the same.

[0069] Example 12 The difference between Example 12 and Example 3 is that the weight ratio of tetrabromobisphenol A epoxy resin to 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexylcarboxylate is 1:1, and the rest are the same.

[0070] Example 13 The difference between Example 13 and Example 3 is that first, three layers of carbon fiber woven cloth impregnated with composite epoxy resin are hoop-wound on the outer surface of the inner lining layer, the hoop-wrap is performed by using the carbon fiber woven cloth for 90° winding, the single layer thickness is 0.2 mm, and 7 cycles are performed, and then the carbon fiber yarn impregnated with composite epoxy resin is spirally wound on the surface of the carbon fiber woven cloth with two layers, the winding angle of the spiral winding is 14°, the single layer thickness is 0.2 mm, and 7 cycles are performed, and the rest are the same.

[0071] Embodiment 14 The difference between Example 14 and Example 3 is that, during the preparation of the modified montmorillonite, silane coupling agent KH560 is added to replace 3-aminopropyltriethoxysilane, and the rest are the same.

[0072] Embodiment 15 The difference between Example 15 and Example 3 is that, during the preparation of the modified carbon nanotubes, the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 1:1, and the rest are the same.

[0073] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that the transition layer is not included, and the rest is the same.

[0074] Comparative Example 2 The difference between Comparative Example 2 and Example 3 is that ordinary bisphenol A epoxy resin is used instead of tetrabromobisphenol A epoxy resin, and the rest are the same.

[0075] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that the fiber-wound composite material layer is not included, and the rest is the same.

[0076] Experimental Example 1 Liquid oxygen compatibility test The composite pressure vessels obtained in Examples 1 to 13 and Comparative Examples 1 to 3 were tested. Liquid oxygen impact tests were performed according to the liquid oxygen compatibility evaluation standard of QJ3177-2003 standard. Each group was subjected to 20 independent impacts. The maximum impact energy (J) that can be sustained was tested, and the energy was increased by 10J as a unit if it was greater than 100J. If no sensitivity reaction (such as sparks, charring, explosion, combustion, etc.) occurred in 20 impact tests, it means that the material is compatible with liquid oxygen. If a sensitivity reaction occurs once in 20 impact tests, 40 impact tests are performed again. If no sensitivity reaction occurs in 40 impact tests, it is also considered to be compatible with liquid oxygen.

[0077] The test results are shown in Table 1.

[0078] Table 1 Liquid oxygen compatibility test results

[0079] Experimental Example 2 Mechanical Properties Test The composite pressure vessels obtained in the above embodiments and comparative examples were subjected to mechanical property tests, including bending strength test according to GB / T2567-2008, fracture toughness test according to ASTMD5045-99, and low-temperature tensile test at liquid oxygen temperature according to GB / T1040-2006. The test results are shown in Table 2 below.

[0080] Table 2 Mechanical properties test results

[0081] Experimental Example 3: Anti-permeability test The composite pressure vessel obtained in the above embodiments and comparative examples was subjected to a permeation resistance test. The pressure vessel to be tested was evacuated to -0.05 to -0.1 MPa, and then helium was injected into the pressure vessel to be tested. When the pressure in the pressure vessel to be tested reached a gauge pressure of 0.2 MPa, the injection of helium into the pressure vessel to be tested was stopped. Then, liquid nitrogen was used to cool the composite pressure vessel to be tested, so that the temperature of the pressure vessel to be tested was at a temperature of -196 to -180°C. The leakage rate of the composite pressure vessel to be tested was detected by a helium mass spectrometer leak detector. The indication of the helium mass spectrometer leak detector was the leakage rate of the pressure vessel to be tested. The test results are shown in Table 3 below.

[0082] Table 3 Anti-permeability test results

[0083] It can be seen from Tables 1 to 3 that the liquid oxygen compatibility, mechanical properties and anti-permeation properties of the composite pressure vessels prepared in Examples 1 to 3 are all very superior, and the liquid oxygen compatibility of the composite pressure vessel prepared in Comparative Example 2 is reduced. The reason for this may be that ordinary bisphenol A epoxy resin is used instead of tetrabromobisphenol A epoxy resin, which affects its liquid oxygen compatibility; the mechanical properties of the composite pressure vessels prepared in Example 13 and Comparative Examples 1 to 3 are significantly reduced. The reason for this is that no matter the winding method or the presence of the transition layer or the fiber-wound composite material layer, they all have a great influence on the mechanical properties; the anti-permeation properties of Example 8 and Comparative Examples 1 to 3 are significantly reduced. The reason for this is that the composite epoxy resin and the transition layer and the fiber-wound composite material layer have an influence on the anti-permeation properties.

[0084] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.

[0085] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A composite pressure vessel suitable for liquid oxygen environment, characterized in that: From inside to outside, it includes a thin-walled metal lining layer, a transition layer and a fiber-wound composite material layer; The transition layer includes fluorinated polyarylether; The fiber-wound composite material layer is formed by continuous hoop and spiral cross-wound carbon fiber woven cloth impregnated with composite epoxy resin and carbon fiber yarn on the inner lining layer; The matrix resin in the composite epoxy resin includes bromine-containing epoxy resin and / or chlorine-containing epoxy resin; The transition layer is prepared from the following raw materials in parts by weight: 100-110 parts of solvent, 40-60 parts of fluorinated polyarylether, 2-7 parts of phthalate coupling agent and 10-15 parts of nanofiller.

2. A composite material pressure vessel suitable for liquid oxygen environment according to claim 1, characterized in that: The fluorinated polyarylether is fluorinated phthalocyanine polyarylether, the phthalate coupling agent includes isopropoxy tri(dioctyl pyrophosphate acyloxy) titanate or isopropoxy tristearate aluminum; the nanofiller includes nanographene and nanoaluminum oxide; and the solvent includes N,N-dimethylacetamide.

3. A composite material pressure vessel suitable for liquid oxygen environment according to claim 2, characterized in that: The preparation method of the fluorinated phthalazinone polyarylether comprises the following steps: S1 Take 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and toluene and place them in a flask; S2 is introduced with nitrogen and heated to react with water; After the water reaction in S3 is completed, the temperature is lowered, and the polyfluorinated monomer perfluorobiphenyl and N,N-dimethylacetamide are added, and the reaction is continued until the viscosity no longer changes; Fluorinated poly(phenylene ether) was separated by S4 precipitation method.

4. A composite pressure vessel suitable for liquid oxygen environment according to claim 3, characterized in that: The molar ratio of the 4-(4-hydroxyphenyl)-2,3-naphthylidene-1-one, anhydrous potassium carbonate and the polyfluorinated monomer perfluorobiphenyl is 1:(1-1.5):(1-1.2); the heating reaction temperature in S2 is 120-140°C and the reaction time is 3-5h; and the temperature is lowered to 105-115°C in S3.

5. The composite pressure vessel suitable for liquid oxygen environment according to claim 1, characterized in that: In terms of weight, the composite epoxy resin comprises 80-100 parts of compound epoxy resin, 5-10 parts of composite nanofiller, 10-20 parts of ether diluent, 5-15 parts of flame retardant and 30-50 parts of amine curing agent; The compound epoxy resin comprises aliphatic epoxy resin and bisphenol A epoxy resin; the bisphenol A epoxy resin comprises tetrabromobisphenol A epoxy resin or tetrachlorobisphenol A epoxy resin.

6. A composite material pressure vessel suitable for liquid oxygen environment according to claim 5, characterized in that: The compounded epoxy resin also includes polyimide and meta-phenylenediamine; the weight ratio of the compounded epoxy resin to polyimide and meta-phenylenediamine is (2-4):1, and the amount of meta-phenylenediamine used is 2-5% of the epoxy equivalent of the compounded epoxy resin.

7. The composite pressure vessel suitable for liquid oxygen environment according to claim 5, characterized in that: The composite nanofiller comprises modified montmorillonite and modified carbon nanotubes in a weight ratio of 1:(2-4); The flame retardant is a phosphoric acid acrylate monomer containing a double bond; The amine curing agent is one of m-phenylenediamine and 4,4'-diaminodiphenyl ether; The ether diluent includes one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, phenyl glycidyl ether and 4-tert-butylphenyl glycidyl ether.

8. A method for preparing a composite pressure vessel suitable for liquid oxygen environment according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Preparation of thin-walled metal lining; (2) Preparation of transition layer: dissolving fluorinated polyarylether in a solvent, adding phthalate coupling agent and nanofiller, stirring evenly and filtering, coating on the outer surface of the thin-walled metal lining layer, and drying naturally; (3) The thin-walled metal liner coated with the transition layer is installed on a winding machine, and 2-4 layers of carbon fiber woven cloth impregnated with composite epoxy resin are successively wound hoop-wise on the outer surface of the liner, and then 1-2 layers of carbon fiber yarn impregnated with composite epoxy resin are successively spirally wound on the surface of the carbon fiber woven cloth, and the process is repeated for 6-10 cycles; (4) After the winding is completed, high temperature curing is performed to obtain the composite material pressure vessel.

9. The preparation method according to claim 8, characterized in that: The glue content of the winding layer formed in each cycle in step (3) is 25-35%, the hoop winding is 90° winding using carbon fiber woven cloth, and the thickness of the single layer is 0.2-0.5 mm; the winding angle of the spiral winding is 12-14°, and the thickness of the single layer is 0.1-0.3 mm; In step (4), the high temperature curing is firstly to uniformly increase the temperature from 30°C to 90°C within 60 minutes and keep it at this temperature for 2-3 hours; then to uniformly increase the temperature to 120°C within 60 minutes and keep it at this temperature for 2-4 hours; finally, to uniformly increase the temperature to 160°C within 60 minutes and keep it at this temperature for 2-4 hours.

Citation Information

Patent Citations

  • Composite material gas cylinder and preparation method thereof

    CN113790387A

  • Coupling agent modified phthalazinone polyarylether resin-based composite material and preparation method thereof

    CN116265529A

  • Low-viscosity high-liquid oxygen compatibility resin system for ultralow-temperature liquid oxygen environment as well as preparation method and application of low-viscosity high-liquid oxygen compatibility resin system

    CN117551335A

  • Epoxy fluorine-containing polyaryletherketone as well as preparation method and application thereof

    CN118359805A

  • Graphene oxide-fiber hybrid material reinforced phthalazinone polyarylether resin-based composite material and preparation method thereof

    CN118406363A

Cited By

  • Steel lining polyurethane composite pipe and preparation method thereof

    CN120269882A