A method for harmless resource utilization of fly ash from waste incineration
By adding heavy metal stabilizers, fluxes, and diagenetic agents to fly ash from waste incineration, followed by molding, granulation, and low-temperature heat treatment, combined with leaching and desalination, the problems of heavy metal fixation and dioxin decomposition in fly ash resource utilization have been solved, achieving efficient, low-cost, and harmless resource utilization.
Patent Information
- Application Number
- CN202411969762.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-12-30
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-12-30
AI Technical Summary
Existing methods for the resource-based treatment of fly ash from waste incineration suffer from problems such as low fly ash content, high sintering temperature, and high cost, making it difficult to achieve efficient and low-cost heavy metal fixation and dioxin decomposition.
The mixture of fly ash, heavy metal stabilizer, flux, rock-forming agent and metal-based auxiliary materials is granulated and then heat-treated at low temperature. Combined with leaching and desalination, a high-strength new phase is formed, which stabilizes heavy metals and decomposes dioxins, resulting in a harmless resource-based product.
It achieves the fixation of heavy metals and the decomposition of dioxins at low temperatures. The resulting harmless resource-based products have long-lasting heavy metal stability, low dioxin content, low heavy metal leaching concentration and low soluble chlorine content, and high treatment efficiency and low energy consumption.
Smart Images

Figure CN119747349B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of fly ash harmless treatment technology, and in particular to a method for harmless resource utilization of fly ash from waste incineration. Background Technology
[0002] Fly ash from municipal solid waste incineration is a substance produced during the incineration of municipal solid waste and enters the flue gas purification system along with the flue gas, ultimately being collected by a dust collector. For grate-type waste incinerators, the output of fly ash is approximately 2-5% of the total waste fed into the furnace. Because fly ash is enriched with heavy metals such as Hg, Pb, Cd, Cu, Cr, and Zn, and also contains carcinogenic substances such as dioxins, it is classified as hazardous waste. Currently, the disposal methods for fly ash in domestic waste-to-energy plants are still limited to adding cement and stabilizers for solidification and landfilling, with resource utilization not yet on a large scale. Fly ash also contains abundant calcium and silicon resources, making its resource utilization significant. Fly ash washing in cement kilns is a relatively mature method for fly ash resource utilization, but the entire process is complex and costly. Sintering heat treatment of fly ash can achieve dioxin detoxification and is an effective means of fly ash resource utilization. However, current fly ash sintering heat treatment processes generally suffer from problems such as low fly ash content and high sintering temperature, resulting in disposal costs that are still far higher than landfill disposal costs. Therefore, developing efficient and cost-effective fly ash resource utilization technologies is of great value and significance. Summary of the Invention
[0003] To address one or more technical problems existing in the prior art, this invention provides a method for the harmless resource utilization of fly ash from waste incineration. The method provided by this invention can achieve the fixation of heavy metals and the decomposition of dioxins at low temperatures. The harmless resource utilization process is highly efficient and energy-saving. The harmless resource utilization products obtained have a long-lasting effect of heavy metal stability, low dioxin content, and low heavy metal leaching concentration and soluble chlorine content.
[0004] This invention provides a method for the harmless resource utilization of fly ash from waste incineration, the method comprising the following steps: Fly ash and auxiliary materials are mixed to obtain a mixture; the auxiliary materials include heavy metal stabilizers, fluxes, rock-forming agents, and metal-based auxiliary materials; the heavy metal stabilizers are phosphates; the rock-forming agents are silicon-based compounds; and the metal-based auxiliary materials are one or more of magnesium compounds and aluminum compounds. The mixture is shaped into granules, heat-treated, washed to remove salt, and dried to obtain a harmless resource-based product.
[0005] Preferably, the amount of phosphate used is 1-3% of the fly ash mass; and / or The phosphate is one or more of potassium dihydrogen phosphate, potassium monohydrogen phosphate, and potassium phosphate.
[0006] Preferably, the amount of flux used is 2-10% of the fly ash mass; and / or The flux is at least one of glass powder and fluorite powder.
[0007] Preferably, the amount of the silicon-based compound is 10-60% of the fly ash mass; and / or The silicon-based compound is one or more of the following: fly ash, steel slag powder, silica gel, tailings powder, silica fume, and fumed silica.
[0008] Preferably, the amount of the metal-based auxiliary material is 1-5% of the fly ash mass; and / or The metal-based auxiliary material is one or more of magnesium hydroxide, magnesium oxide, magnesium carbonate, and aluminum hydroxide.
[0009] Preferably, the pressure of the granulation process is not less than 20 MPa; and / or The size of the granulated particles is 2~8mm.
[0010] Preferably, the heat treatment is carried out under an inert atmosphere, wherein the concentration of the inert gas in the inert atmosphere is not less than 99.2 vol%; and / or The heat treatment temperature is 500~900℃ and the time is 20~60min.
[0011] Preferably, the rinsing and desalination is achieved by a rinsing device, which includes: a porous conveyor belt for conveying materials, multiple spraying areas and draining areas arranged alternately above the porous conveyor belt, and multiple liquid tanks located below the porous conveyor belt for containing rinsing liquid. The spraying area is equipped with a liquid atomizing component, which is used to evenly spray the rinsing liquid onto the surface of the material for rinsing. The draining area is equipped with a high-pressure gas spray gun for blowing away liquid from the surface of the material.
[0012] Preferably, the width of the spraying area is 8 to 12 times the width of the draining area; and / or The number of liquid tanks 24 is 3 to 10.
[0013] Preferably, the amount of rinsing solution used in the rinsing and desalination process is 1.5 to 2.5 times the mass of fly ash, and the rinsing time is 10 to 40 minutes.
[0014] Compared with the prior art, the present invention has at least the following beneficial effects: This invention first mixes fly ash and auxiliary materials, and then granulates the mixed material to obtain particles of a certain size. Then, under the action of the auxiliary materials, a low-temperature heat treatment is carried out to form a new phase with high strength, which effectively stabilizes the heavy metals in the fly ash and decomposes dioxins. Finally, soluble chloride salts are removed by rinsing and desalination to obtain a harmless resource product with higher added value.
[0015] The fly ash harmless resource utilization method provided by this invention can realize the fixation of heavy metals and the decomposition of dioxins at low temperatures. The harmless resource utilization process is highly efficient and energy-saving. The harmless resource utilization products obtained have high strength, long-lasting heavy metal stabilization effect, low dioxin content, and low heavy metal leaching concentration and soluble chlorine content. Attached Figure Description
[0016] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0017] Figure 1 A schematic diagram of the structure of a heat treatment device provided by the present invention; Figure 2 A schematic diagram of a rinsing device provided by the present invention.
[0018] Reference numerals: 11-Cylinder body, 12-Cylinder body support; 13-Heating medium; 111-Material inlet; 112-Material inlet cover; 113-Material outlet; 114-Material outlet cover; 115-Gas inlet; 116-Gas outlet; 14-Material conveying component; 21-Perforated conveyor belt; 22-Spraying area; 221-Liquid atomizing component; 23-Draining area; 231-High-pressure gas spray gun; 24-Liquid tank; 3-Material. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0020] This invention provides a method for the harmless resource utilization of fly ash from waste incineration, the method comprising the following steps: Fly ash and auxiliary materials are mixed to obtain a mixture; the auxiliary materials include heavy metal stabilizers, fluxes, rock-forming agents, and metal-based auxiliary materials; the heavy metal stabilizers are phosphates; the rock-forming agents are silicon-based compounds; and the metal-based auxiliary materials are one or more of magnesium compounds and aluminum compounds. The mixture is shaped into granules, heat-treated, washed to remove salt, and dried to obtain a harmless resource-based product.
[0021] This invention first mixes fly ash and auxiliary materials, and then granulates the mixed material to obtain particles of a certain size. Then, under the action of the auxiliary materials, a low-temperature heat treatment is carried out to form a new phase with high strength, which effectively stabilizes the heavy metals in the fly ash and decomposes dioxins. Finally, soluble chloride salts are removed by rinsing and desalination to obtain a harmless resource product with higher added value.
[0022] The fly ash harmless resource utilization method provided by this invention can realize the fixation of heavy metals and the decomposition of dioxins at low temperatures. The harmless resource utilization process is highly efficient and energy-saving. The harmless resource utilization products obtained have high strength, long-lasting heavy metal stabilization effect, low dioxin content, and low heavy metal leaching concentration and soluble chlorine content.
[0023] According to some preferred embodiments, the amount of phosphate used is 1 to 3% of the fly ash mass.
[0024] According to some preferred embodiments, the phosphate is one or more of potassium dihydrogen phosphate, potassium monohydrogen phosphate, and potassium phosphate.
[0025] According to some preferred embodiments, the amount of flux used is 2 to 10% of the fly ash mass.
[0026] According to some preferred embodiments, the flux is at least one of glass powder and fluorite powder.
[0027] According to some preferred embodiments, the amount of the silicon-based compound is 10-60% of the fly ash mass.
[0028] According to some preferred embodiments, the silicon-based compound is one or more of fly ash, steel slag powder, silica gel, tailings powder, silica fume, and fumed silica.
[0029] According to some preferred embodiments, the amount of the metal-based auxiliary material is 1 to 5% of the fly ash mass.
[0030] According to some preferred embodiments, the metal-based auxiliary material is one or more of magnesium hydroxide, magnesium oxide, magnesium carbonate, and aluminum hydroxide.
[0031] This invention achieves localized melting by adding flux to fly ash, thereby lowering the heat treatment temperature. It also synergistically enhances the strength of the new phase after heat treatment in conjunction with diagenetic agents and metal-based additives. Without the addition of flux, diagenetic agents, and metal-based additives, the new phase after heat treatment has low strength and is easily dispersed during subsequent rinsing.
[0032] According to some preferred embodiments, the pressure of the molding and granulation is not less than 20 MPa.
[0033] According to some preferred embodiments, the size of the granulated particles is 2~8mm.
[0034] According to some preferred embodiments, the heat treatment is carried out in an inert atmosphere, wherein the concentration of inert gas in the inert atmosphere is not less than 99.2 vol; the present invention ensures efficient decomposition of dioxins by performing heat treatment in an inert atmosphere. If the content of inert gas is too low, it will affect the decomposition efficiency of dioxins.
[0035] According to some preferred embodiments, the heat treatment temperature is 500~900℃ and the time is 20~60min.
[0036] According to some preferred embodiments, heat treatment is achieved by a heat treatment apparatus, which includes: a cylinder 11, a cylinder support 12, and a heating medium 13 for heating the cylinder; a material inlet 111 and a material outlet 113 are respectively provided at both ends of the cylinder 11; a material inlet cover 112 and a material outlet cover 114 are respectively provided at the material inlet 111 and the material outlet 113; a gas inlet 115 and a gas outlet 116 communicating with the cylinder 11 are provided on the side wall of the cylinder 11; the gas inlet 115 is close to the material outlet 113 and its opening faces downward; the gas outlet 116 is close to the material inlet 111 and its opening faces upward; the height of the cylinder support 12 is adjustable to facilitate the removal of material after heat treatment; a material conveying component 14 for accommodating the heat-treated material is provided below the material outlet. The heating medium 13 is one of a resistance wire heating medium, an electromagnetic heating medium, a high-temperature gas heating medium, and a high-temperature liquid heating medium.
[0037] Before heat treatment, close the material outlet cover, introduce gas into the cylinder through the gas inlet, and expel the air from the cylinder through the gas outlet. Add material into the cylinder, close the material inlet cover, and heat the cylinder using a heating element for heat treatment. After heat treatment, open the material outlet cover, adjust the height of the cylinder support so that the height of the material inlet is greater than the material outlet, allowing the material to flow out of the cylinder and be conveyed to the rinsing device for rinsing and desalination via the material conveying component.
[0038] This invention, by adding heavy metal stabilizers, fluxes, rock-forming agents, and metal-based auxiliary materials to fly ash, reduces the stringent temperature requirements for heat treatment of the mixture, enabling harmless resource recovery under heat treatment conditions of 500-900℃. Therefore, the aforementioned heat treatment device can achieve a high filling volume of the mixture (the cylinder can be fully filled) with a small footprint, effectively solving the problems of low filling volume and large footprint associated with existing rotary kilns for fly ash treatment.
[0039] According to some preferred embodiments, rinsing desalination is achieved by a rinsing device, such as... Figure 2 As shown, the rinsing device includes: a porous conveyor belt 21 for conveying material 3, multiple spray zones 22 and draining zones 23 arranged alternately above the porous conveyor belt 21, and multiple liquid tanks 24 located below the porous conveyor belt 21 for containing rinsing liquid; the porous conveyor belt 21 is used to convey material 3; the spray zone 22 is provided with a liquid atomizing component 221 for uniformly spraying the rinsing liquid onto the surface of material 3 to rinse material 3; the draining zone 23 is provided with a high-pressure gas spray gun 231 for blowing away the liquid on the surface of material 3.
[0040] According to some preferred embodiments, the width of the spraying area 22 is 8 to 12 times the width of the draining area 23; the number of liquid tanks 24 is 3 to 10.
[0041] The rinsing device provided by this invention has multiple alternating spray zones and draining zones. In the rinsing zones, the rinsing liquid is atomized by a liquid atomizing component, allowing it to be evenly sprayed onto the material surface, ensuring thorough rinsing. The rinsing effect is significantly better than rinsing methods using ordinary nozzles. Then, a high-pressure gas spray gun blows the liquid off the material surface, effectively removing the salt solution after rinsing. Repeating the rinsing-draining process multiple times can effectively improve the efficiency of rinsing and desalination.
[0042] According to some preferred embodiments, the material conveying component 14 in the heat treatment apparatus is connected to the porous conveyor belt 21 of the rinsing apparatus; the material conveying component 14 is used to convey the heat-treated material to the rinsing apparatus.
[0043] According to some preferred embodiments, the amount of rinsing solution used in the rinsing and desalination process is 1.5 to 2.5 times the mass of fly ash, and the rinsing time is 10 to 40 minutes.
[0044] According to some preferred embodiments, after rinsing and desalination, a step of removing heavy metals from the brine is further included, specifically comprising: introducing a carbon dioxide-containing gas into the brine after rinsing and desalination, and then adding a heavy metal treatment agent; the heavy metal treatment agent is at least one of phosphate and sulfide. The phosphate is one or a mixture of more than one of sodium phosphate, sodium pyrophosphate, and sodium phytate; the sulfide is one or a mixture of more than one of sodium sulfide and potassium sulfide. The amount of phosphate used is 0.01~0.1% of the mass of the brine after rinsing and desalination. The amount of sulfide used is 0.05~0.2% of the mass of the brine after rinsing and desalination. This invention uses a heavy metal treatment agent to remove heavy metals from the brine after rinsing and desalination to ensure that the treated brine meets discharge standards and is discharged from the system.
[0045] To more clearly illustrate the technical solution and advantages of the present invention, the present invention will be further described below with reference to embodiments. The present invention does not specifically limit the source of the reagents used in the embodiments and comparative examples; they can be directly purchased or synthesized in-house.
[0046] Example 1 The fly ash, heavy metal stabilizer (potassium phosphate, 2% of the fly ash mass), flux (glass powder, 8% of the fly ash mass), rock-forming agent (fly ash, 40% of the fly ash mass), and metal-based auxiliary material (magnesium hydroxide, 3% of the fly ash mass) are mixed to obtain a mixture. The mixture is subjected to molding, granulation, and heat treatment (using...) Figure 1 The heat treatment is carried out in an inert atmosphere with an inert gas concentration of not less than 99.2 vol%. The heat treatment temperature is 800℃ and the time is 40 min. The process involves rinsing and desalination (using...). Figure 2 The rinsing device is used for rinsing and desalination, with the amount of water being twice the mass of the ash and the rinsing time being 30 minutes. After drying, a harmless resource-based product is obtained.
[0047] Example 2 The fly ash, heavy metal stabilizer (potassium monohydrogen phosphate, 1% of the fly ash mass), flux (fluorite powder, 2% of the fly ash mass), rock-forming agent (steel slag powder, 60% of the fly ash mass), and metal-based auxiliary material (aluminum hydroxide, 1% of the fly ash mass) are mixed to obtain a mixture. The mixture is subjected to molding, granulation, and heat treatment (using...) Figure 1 The heat treatment is carried out in an inert atmosphere with an inert gas concentration of not less than 99.2 vol%. The heat treatment temperature is 500℃ and the time is 60 min. The process also includes rinsing and desalination. Figure 2The rinsing device is used for rinsing and desalination, with the amount of water being 2.5 times the mass of the ash and the rinsing time being 40 minutes. After drying, a harmless resource-based product is obtained.
[0048] Example 3 The fly ash, heavy metal stabilizer (potassium dihydrogen phosphate, 3% of the fly ash mass), flux (glass powder, 10% of the fly ash mass), rock-forming agent (silica fume, 40% of the fly ash mass), and metal-based auxiliary material (magnesium oxide, 5% of the fly ash mass) are mixed to obtain a mixture. The mixture is then subjected to molding and granulation, heat treatment (conducted under an inert atmosphere with an inert gas concentration of not less than 99.2 vol%, at a temperature of 900°C for 20 minutes), and rinsing for desalination (using...). Figure 2 The rinsing device is used for rinsing and desalination, with the amount of water being 1.5 times the mass of the ash and the rinsing time being 10 minutes. After drying, a harmless resource-based product is obtained.
[0049] Example 4 The fly ash, heavy metal stabilizer (potassium phosphate, 2% of fly ash mass), flux (glass powder, 6% of fly ash mass), rock-forming agent (fumed silica, 10% of fly ash mass), and metal-based auxiliary material (magnesium carbonate, 5% of fly ash mass) are mixed to obtain a mixture. The mixture is then subjected to molding and granulation, heat treatment (conducted under an inert atmosphere with an inert gas concentration of not less than 99.2 vol%, at a temperature of 900°C for 40 minutes), and rinsing for desalination (using...). Figure 2 The rinsing device is used for rinsing and desalination, with the amount of water being 2.5 times the mass of the ash and the rinsing time being 40 minutes. After drying, a harmless resource-based product is obtained.
[0050] Example 5 The process is basically the same as in Example 1, except that a conventional rotary kiln is used for heat treatment, which is carried out in an inert atmosphere with an inert gas concentration of not less than 99.2 vol%, a heat treatment temperature of 800°C, and a time of 40 min.
[0051] Comparative Example 1 It is basically the same as Example 1, except that no flux is added.
[0052] Comparative Example 2 It is basically the same as Example 1, except that no rock-forming agent is added.
[0053] Comparative Example 3 It is basically the same as Example 1, except that no metal-based auxiliary materials are added.
[0054] Comparative Example 4 It is basically the same as Example 1, except that the rinsing device does not include a draining area.
[0055] Comparative Example 5 It is basically the same as Example 1, except that the rinsing device is a conventional liquid nozzle.
[0056] The performance data of the harmless resource-based products of the embodiments and comparative examples of the present invention are shown in Table 1. The test methods for each performance are as follows: Dioxin content testing: The test shall be conducted in accordance with the HJ 77.3-2008 standard; Heavy metal leaching concentration: Tested according to HJ / T 300-2007 standard; Soluble chlorine content test: silver nitrate titration method; the soluble chlorine content refers to the mass fraction of soluble chlorine in harmless resource products.
[0057] Compressive strength: Tested in accordance with GB / T 17431.2-1998 standard.
[0058] Table 1. Performance data of the harmless resource-based products of the embodiments and comparative examples of the present invention.
[0059] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for the harmless resource utilization of fly ash from waste incineration, characterized in that, The method includes the following steps: Fly ash and auxiliary materials are mixed to obtain a mixture; the auxiliary materials include heavy metal stabilizers, fluxes, rock-forming agents, and metal-based auxiliary materials; the heavy metal stabilizer is a phosphate; the rock-forming agent is a silicon-based compound; the metal-based auxiliary materials are one or more of magnesium compounds and aluminum compounds; the amount of phosphate is 1-3% of the fly ash mass; the amount of flux is 2-10% of the fly ash mass; the amount of silicon-based compound is 10-60% of the fly ash mass; and the amount of metal-based auxiliary materials is 1-5% of the fly ash mass. The mixture is subjected to molding and granulation, heat treatment, rinsing and desalination, and drying to obtain a harmless resource-based product. The heat treatment is carried out under an inert atmosphere, wherein the concentration of inert gas in the inert atmosphere is not less than 99.2 vol%. The heat treatment temperature is 500~900℃, and the time is 20~60min; The rinsing and desalination is achieved by a rinsing device, which includes: a porous conveyor belt for conveying materials, multiple spraying areas and draining areas arranged alternately above the porous conveyor belt, and multiple liquid tanks located below the porous conveyor belt for containing rinsing liquid. The spraying area is equipped with a liquid atomizing component, which is used to evenly spray the rinsing liquid onto the surface of the material for rinsing. The draining area is equipped with a high-pressure gas spray gun for blowing away liquid from the surface of the material.
2. The method according to claim 1, characterized in that, The phosphate is one or more of potassium dihydrogen phosphate, potassium monohydrogen phosphate, and potassium phosphate.
3. The method according to claim 1, characterized in that, The flux is at least one of glass powder and fluorite powder.
4. The method according to claim 1, characterized in that, The silicon-based compound is one or more of the following: fly ash, steel slag powder, silica gel, tailings powder, silica fume, and fumed silica.
5. The method according to claim 1, characterized in that, The metal-based auxiliary material is one or more of magnesium hydroxide, magnesium oxide, magnesium carbonate, and aluminum hydroxide.
6. The method according to claim 1, characterized in that, The pressure for granulation is not less than 20 MPa; and / or The size of the granulated particles is 2~8mm.
7. The method according to claim 1, characterized in that, The width of the spraying area is 8 to 12 times the width of the draining area; and / or The number of liquid tanks is 3 to 10.
8. The method according to claim 1, characterized in that, The amount of rinsing solution used in the rinsing and desalination process is 1.5 to 2.5 times the mass of fly ash, and the rinsing time is 10 to 40 minutes.
Citation Information
Patent Citations
Flying ash desalination and water washing device
CN105753345A
Technology for preparing ultra-light filler from solid waste incineration fly ash
CN106187268A
Method for preparing salt by dechlorinating waste incineration fly ash
CN114538472A