Electrode plates, secondary batteries and electrical equipment
By setting a functional layer of insulation and adhesive at the edge of the electrode sheet, the problems of membrane pore blockage and electrode edge cracking caused by adhesive are solved, which improves the structural stability and safety of the battery, and enhances battery performance and assembly yield.
Patent Information
- Application Number
- CN202410931306.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-07-11
AI Technical Summary
In the prior art, the application of adhesives on the membrane surface causes blockage of the membrane pore structure, affecting the transport of active ions. Furthermore, it is difficult to apply to thick electrodes, which can easily lead to edge bursting and cracking of the electrode, increasing the risk of short circuits.
A functional layer is set in the edge area of the electrode sheet, including an insulating layer and an adhesive layer. The adhesive layer is designed with an intermittently arranged adhesive structure. The insulating layer prevents the positive and negative electrodes from direct contact. The adhesive layer is bonded to the separator during the cell shaping process, avoiding large-area coating of adhesive slurry and reducing the risk of interpenetration.
It improves the structural stability and safety performance of the battery, reduces the risk of short circuits, increases the assembly yield and performance of the battery, saves internal space of the cell, and enhances the volumetric energy density of the battery.
Smart Images

Figure CN119764319B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, specifically to electrode sheets, secondary batteries, and electrical devices. Background Technology
[0002] Stacked batteries typically consist of a positive electrode, a negative electrode, and a separator between the positive and negative electrodes. To prevent short circuits caused by misalignment of the positive and negative electrodes during assembly and subsequent processes, an adhesive is usually applied to the separator surface to fix it to the negative electrode. However, the adhesive can clog the pore structure of the separator, affecting the transport of active ions and increasing the battery's internal resistance; alternatively, it can cause edge chipping and cracking of the electrodes, and makes it difficult to use in thick electrodes. Summary of the Invention
[0003] In view of this, embodiments of this application provide an electrode sheet, a secondary battery, and an electrical device. The functional layer in the edge region of the electrode sheet enables bonding between the separator and the electrode sheet, and the bonding strength and stability are both high. It can also effectively reduce the risk of short circuit caused by contact between the positive and negative electrodes in the battery.
[0004] The first aspect of this application provides an electrode sheet, including a current collector, an active material layer disposed on at least one side of the surface of the current collector, and at least one functional layer; wherein the functional layer is disposed at the edge of the current collector, and the functional layer is disposed in the same layer as the active material layer;
[0005] The functional layer includes an insulating layer and an adhesive layer disposed on the insulating layer away from the surface of the current collector, the adhesive layer including a plurality of adhesive structures arranged at intervals.
[0006] The aforementioned functional layer located at the edge of the current collector serves both insulating and adhesive functions. During the cell shaping process, the adhesive layer contacts the separator and adheres to it under the pressure applied during cell shaping. Furthermore, the adhesive structures within the adhesive layer are spaced apart, leaving deformation buffer zones between them. Even if the adhesive structure deforms during bonding with the separator, the risk of deformation spreading between the active material layer and the separator is minimal, which is beneficial for the structural stability of the battery's internal structure and the battery's performance. The presence of the insulating layer prevents direct contact between the positive and negative electrode plates, improving the battery's assembly yield and safety performance.
[0007] In addition, the special structural design of the adhesive layer allows the electrode sheet to avoid large-area coating of adhesive slurry used in related technologies during the preparation process. This can fundamentally prevent the interpenetration between the adhesive slurry and the active material layer slurry, thereby reducing the risk of edge bursting and cracking of the electrode sheet and improving the structural stability of the electrode sheet itself.
[0008] In some embodiments of this application, in the stacking direction of the functional layer and the current collector, the size of the functional layer is x μm, and the size of the active material layer is y μm, where 10 μm ≤ yx ≤ 50 μm.
[0009] In some embodiments of this application, the thickness of the insulating layer is 50 μm to 300 μm; and / or,
[0010] The size of the insulating layer is 0.1 cm to 1 cm in the direction from the functional layer to the active material layer.
[0011] In some embodiments of this application, the distance between two adjacent adhesive structures is characterized by being 300 μm to 1000 μm; and / or,
[0012] In the stacking direction of the functional layer and the current collector, the size of the bonding structure is 2μm to 5μm, and the maximum size of the orthographic projection of the bonding structure is 100μm to 500μm.
[0013] In some embodiments of this application, the material of the bonding structure includes a polymer, and the glass transition temperature of the polymer is -20°C to 100°C;
[0014] The polymer includes one or more of methyl methacrylate, butyl methacrylate, and hexyl acrylate.
[0015] In some embodiments of this application, the insulating layer comprises inorganic particles and a binder, wherein the particle size of the inorganic particles is 0.5 μm to 5 μm; and / or, the inorganic particles account for 90% to 99% of the mass of the insulating layer.
[0016] In some embodiments of this application, the inorganic particles are made of one or more of alumina, boehmite, titanium dioxide, zirconium dioxide, magnesium hydroxide, and aluminum hydroxide.
[0017] And / or, the adhesive includes carboxymethyl cellulose.
[0018] In some embodiments of this application, a tab is also included, which is adjacent to the current collector and disposed close to the functional layer.
[0019] A second aspect of this application provides a secondary battery, including the electrode plates provided in this application.
[0020] A third aspect of this application provides an electrical device, including a secondary battery provided in this application embodiment.
[0021] In some embodiments of this application, the electrical device includes electronic components, and a secondary battery powers these electronic components. Because the electrical device uses the secondary battery provided in the embodiments of this application, it has good market prospects.
[0022] In some embodiments of this application, the aforementioned electrical equipment includes, but is not limited to, vehicles, or 3C electronic consumer products such as mobile phones, laptops, tablets, and smartwatches. Attached Figure Description
[0023] Figure 1 A simplified schematic diagram of the cross-section of an electrode sheet provided in an embodiment of this application;
[0024] Figure 2 This is a top view of the functional layer in an electrode sheet provided in an embodiment of this application;
[0025] Figure 3A A top view of an electrode sheet provided in another embodiment of this application;
[0026] Figure 3B A top view of an electrode sheet provided in yet another embodiment of this application;
[0027] Figure 3C A top view of an electrode sheet provided in yet another embodiment of this application;
[0028] Figure 3D A top view of an electrode sheet provided in another embodiment of this application.
[0029] Explanation of reference numerals: 1-Electrode sheet; 10-Current collector; 20-Active material layer; 30-Functional layer; 301-Insulating layer; 302-Adhesive layer; 321-Adhesive structure; 40-Taper. Detailed Implementation
[0030] Please see Figures 1-2 This application provides an electrode sheet 1, including a current collector 10, an active material layer 20 disposed on at least one side of the surface of the current collector 10, and at least one functional layer 30; wherein, the functional layer 30 is disposed on the edge of the current collector 10, and the functional layer 30 is disposed in the same layer as the active material layer 20.
[0031] The functional layer 30 includes an insulating layer 301 and an adhesive layer 302 disposed on the insulating layer 301 away from the surface of the current collector 10. The adhesive layer 302 includes a plurality of adhesive structures 321 arranged at intervals.
[0032] The functional layer 30, located at the edge of the current collector 10, serves both insulating and adhesive functions. During the cell shaping process, the adhesive layer 302 contacts the separator and adheres to it under the pressure applied during the cell shaping process. Furthermore, the adhesive structures 321 within the adhesive layer 302 are spaced apart, with deformation buffer areas between them. Even if the adhesive structures 321 deform during adhesion to the separator, the risk of deformation spreading between the active material layer 20 and the separator is minimal, which is beneficial for the structural stability of the battery's internal structure and the battery's performance. Considering that the dimensions of the positive and negative electrode plates in the battery may not be exactly the same, there is a risk of direct contact between the positive and negative electrodes during lamination, subsequent shaping, and extreme operating conditions. The presence of the insulating layer 301 can prevent direct contact between the positive and negative electrode plates, improving the battery's assembly yield and safety performance.
[0033] Furthermore, the special structural design of the adhesive layer 302 allows the electrode sheet 1 to avoid the large-area coating of adhesive slurry used in related technologies during the preparation process. This fundamentally avoids the interpenetration between the adhesive slurry and the active material layer 20 slurry, thereby reducing the risk of edge bursting and cracking of the electrode sheet and improving the structural stability of the electrode sheet 1 itself. Moreover, compared to solutions in related technologies, which require increasing the thickness of the adhesive coating to match the thick active material layer 20, leading to cracking of the adhesive coating, the electrode sheet 1 provided in this application embodiment can flexibly adjust the thickness of the functional layer 30 when matching the thick active material layer 20. Even if the thickness of the adhesive layer 302 is increased, cracking will not occur.
[0034] In this embodiment, the electrode 1 can be either a positive electrode or a negative electrode. In some specific embodiments, the electrode 1 is a negative electrode.
[0035] In this embodiment, the active material layer 20 and the functional layer 30 may be provided on one side surface of the electrode plate 1, or the active material layer 20 and the functional layer 30 may be provided on both opposite sides of the electrode plate 1. Both of these are considered to be within the scope of protection of this application.
[0036] In this embodiment, the insulating layer 301 and the active material layer 20 can be arranged adjacent to each other, or there can be a certain gap between them.
[0037] In this embodiment of the application, please refer to Figures 3A-3DTaking a rectangle as an example, the active material layer 20 can be described as follows: A functional layer 30 can be provided on one outer periphery of the active material layer 20; or functional layers 30 can be provided on both outer peripheries of the active material layer 20 (specifically, functional layers 30 can be provided on opposite outer peripheries of the active material layer 20, or functional layers 30 can be provided on adjacent outer peripheries of the active material layer 20); or functional layers 30 can be provided on three outer peripheries of the active material layer 20; or functional layers 30 can be provided around the periphery of the active material layer 20. This application does not limit this, and those skilled in the art can choose according to actual production needs.
[0038] Understandably, the electrode plate 1 may also be provided with tabs 40. In some embodiments of this application, the electrode plate 1 includes tabs 40, which are adjacent to the current collector 10 and are disposed close to the functional layer 30. For example... Figure 3A As shown, in some specific embodiments, an active material layer 20 and a functional layer 30 are disposed on one side surface of the current collector 10 in the same layer, with the functional layer 30 disposed close to the tab 40. The tab 40 may be welded to the current collector 10 or may be integrally formed with the current collector 10.
[0039] For ease of description, the stacking direction of the functional layer 30 and the current collector 10 is defined as the first direction. In some embodiments of this application, in the stacking direction of the functional layer 30 and the current collector 10 (i.e., the first direction), the size of the functional layer 30 is x μm, and the size of the active material layer 20 is y μm, where 10 μm ≤ yx ≤ 50 μm. In the embodiments of this application, the size of the functional layer 30 in the first direction refers to the distance from the highest point of the bonding structure 321 in the first direction to the surface of the current collector 10; the size of the active material layer 20 in the first direction is essentially the thickness of the active material layer 20. Controlling yx within the range of 10 μm-50 μm is beneficial for the bonding of the electrode sheet 1 and the separator in the cell shaping process, and also helps to save space inside the cell and improve the volumetric energy density of the battery. Specifically, yx can be, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, etc.
[0040] In some embodiments of this application, the thickness of the insulating layer 301 is 50 μm to 300 μm. The thickness of the insulating layer 301 can be adjusted according to the thickness of the active material layer 20 and the dimensions of the bonding structure 321. Controlling the thickness of the insulating layer 301 within the above range is also beneficial to the performance of insulation. Specifically, the thickness of the insulating layer 301 can be, for example, 50 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm, 200 μm, 220 μm, 250 μm, 280 μm, 300 μm, etc.
[0041] In some embodiments of this application, the dimension (L) of the insulating layer 301 along the direction from the functional layer 30 to the active material layer 20 is 0.1 cm to 1 cm. That is, the width of the insulating layer 301 is 0.1 cm to 1 cm. This allows it to support a sufficient amount of the bonding structure 321 to improve the peel strength between the electrode plate 1 and the separator, provides a sufficient buffer area for misalignment of the electrode plate 1, and helps to ensure the energy density of the battery. Specifically, the lateral dimension of the insulating layer 301 along the direction from the functional layer 30 to the active material layer 20 can be, for example, 0.1 cm, 0.2 cm, 0.3 cm, 0.4 cm, 0.5 cm, 0.6 cm, 0.7 cm, 0.8 cm, 0.9 cm, 1.0 cm, etc.
[0042] In some embodiments of this application, the insulating layer 301 comprises inorganic particles and a binder. The inorganic particles have good insulating properties, and the presence of the binder facilitates the molding of the insulating layer 301 and maintains its structural stability. In some specific embodiments, the inorganic particles are made of one or more of alumina, boehmite, titanium dioxide, zirconium dioxide, magnesium hydroxide, and aluminum hydroxide.
[0043] In some embodiments of this application, the particle size of the inorganic particles is 0.5 μm to 5 μm. This facilitates the control of the thickness of the insulating layer 301 and the preparation of the insulating layer 301. Specifically, the particle size of the inorganic particles can be, for example, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, or 5 μm.
[0044] In some embodiments of this application, the inorganic particles account for 90%-99% of the mass of the insulating layer 301, and the binder accounts for 1%-10% of the mass of the insulating layer 301. Specifically, the mass percentage of inorganic particles in the insulating layer 301 can be, for example, 90%, 92%, 95%, 98%, etc., and the mass percentage of binder in the insulating layer 301 can be, for example, 1%, 2%, 5%, 8%, 10%, etc.
[0045] In some embodiments of this application, the binder in the insulating layer 301 includes, but is not limited to, carboxymethyl cellulose. Carboxymethyl cellulose has a high surface tension, which can reduce the risk of interpenetration between the insulating layer 301 slurry and the active material layer 20 slurry during the preparation of the electrode sheet 1, thus benefiting the structural stability and electrochemical performance of the electrode sheet 1.
[0046] In some embodiments of this application, the dimensions of the bonding structure 321 are 2 μm to 5 μm along the stacking direction of the functional layer 30 and the current collector 10 (i.e., the first direction). In other words, the height of the bonding structure 321 is 2 μm to 5 μm. This results in better bonding performance of the bonding layer 302 and makes it easier to fabricate. Specifically, the dimensions of the bonding structure 321 in the first direction can be, for example, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, etc.
[0047] In some embodiments of this application, the maximum size of the orthographic projection of the adhesive structure 321 in the first direction is 100 μm to 500 μm. Similarly, the adhesive layer 302 exhibits superior bonding performance and is easy to fabricate. Specifically, the maximum lateral size of the orthographic projection of the adhesive structure 321 in the first direction can be, for example, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, etc. In the embodiments of this application, the orthographic projection of the adhesive structure 321 in the first direction can be circular, elliptical, polygonal, irregular, etc. For example, when the orthographic projection of the adhesive structure 321 in the first direction is circular, the aforementioned maximum size is the diameter of the circle.
[0048] In some embodiments of this application, the distance d between two adjacent adhesive structures 321 is 300 μm to 1000 μm. This results in superior adhesive performance and lower cost for the adhesive layer 302. In the embodiments of this application, the distance between any two adjacent adhesive structures 321 can be equal or unequal. Specifically, the distance between two adjacent adhesive structures 321 can be, for example, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1000 μm, etc.
[0049] In some embodiments of this application, the adhesive structure 321 is made of a polymer with a glass transition temperature of -20°C to 100°C. Thus, the adhesive structure 321 can be dried at room temperature using a blower, eliminating the need for oven baking, making it easy to manufacture. Furthermore, it can be bonded to the separator under conditions commonly used in battery cell shaping processes (room temperature, pressure 0.5 MPa-1 MPa), saving process time and energy. Specifically, the glass transition temperature of the polymer can be, for example, -20°C, -10°C, 0°C, 10°C, 20°C, 50°C, 80°C, 100°C, etc. In some embodiments of this application, the adhesive structure 321 is made of one or more polymers selected from methyl methacrylate, butyl methacrylate, and hexyl acrylate. The adhesive structure 321 containing the above materials can be bonded to any known separator and the surface of the aforementioned insulating layer 301. In the embodiments of this application, room temperature refers to 25±3°C.
[0050] In some embodiments of this application, the preparation of the electrode plate 1 may include:
[0051] An active material layer and an insulating layer are formed on the surface of the current collector, and an adhesive layer is formed on the surface of the insulating layer away from the current collector.
[0052] In this embodiment of the application, the formation of the insulating layer includes: applying an insulating paste to the surface of the current collector.
[0053] In some embodiments of this application, the solid content of the insulating slurry is 30wt%-60wt%. This allows the viscosity of the insulating slurry to be controlled within a suitable range, facilitating the preparation and molding of the insulating layer. Specifically, the solid content of the insulating slurry can be, for example, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, 55wt%, 60wt%, etc.
[0054] In some embodiments of this application, the room temperature viscosity of the insulating slurry is 2500 MPa·s to 4000 MPa·s. This facilitates the preparation and molding of the insulating layer. Specifically, the room temperature viscosity of the insulating slurry can be, for example, 2500 MPa·s, 2800 MPa·s, 3000 MPa·s, 3200 MPa·s, 3500 MPa·s, 3800 MPa·s, 4000 MPa·s, etc. In the embodiments of this application, the test method for the room temperature viscosity of the insulating slurry can refer to the national standard: GB / T1904-2005.
[0055] In some embodiments of this application, the active material layer and the insulating layer can be coated simultaneously or separately. The coating method can be extrusion coating. In some specific embodiments of this application, the insulating layer and the active material layer are formed simultaneously. Specifically, the insulating layer slurry and the active material layer slurry can be simultaneously coated on a predetermined area of the current collector, for example, using a dual coating head.
[0056] In some embodiments of this application, the bonding structure can be prepared using a piston-type dot coating method. The dot coating process can prevent interpenetration between the insulating layer slurry and the active material layer or the active material layer slurry, thereby effectively reducing the risk of edge bursting and cracking of the electrode sheet. Specifically, the bonding layer slurry is dotted onto a predetermined area of the insulating layer using a piston-type dot coating method, with the coating head installed at the oven outlet and equipped with a small blower.
[0057] In some embodiments of this application, the solid content of the adhesive layer slurry is 40wt%-60wt%. This allows the viscosity of the adhesive layer slurry to be controlled within a suitable range, facilitating the preparation and molding of the bonded structure. Specifically, the solid content of the adhesive layer slurry can be, for example, 40wt%, 42wt%, 45wt%, 48wt%, 50wt%, 52wt%, 55wt%, 58wt%, 60wt%, etc.
[0058] In some embodiments of this application, the room temperature viscosity of the adhesive layer slurry is 200 MPa·s to 300 MPa·s. This facilitates the preparation and molding of the bonded structure. Specifically, the room temperature viscosity of the adhesive layer slurry can be, for example, 200 MPa·s, 220 MPa·s, 250 MPa·s, 280 MPa·s, 300 MPa·s, etc. In the embodiments of this application, the test method for the room temperature viscosity of the adhesive layer slurry can refer to the national standard: GB / T1904-2005.
[0059] In this embodiment, the active material layer can be any known positive electrode active material layer or negative electrode active material layer suitable for the corresponding type of secondary battery.
[0060] In some embodiments of this application, the above-mentioned active material layer is a negative electrode active material layer. That is, the electrode sheet is a negative electrode sheet.
[0061] In this embodiment of the application, the current collector can be any current collector known in the art.
[0062] This application also provides a secondary battery, including the aforementioned electrode plates provided in this application embodiment.
[0063] In some embodiments of this application, at least a portion of the negative electrode in the secondary battery is provided in the embodiments of this application, while the positive electrode is any electrode known in the art. In other embodiments, at least a portion of the positive electrode in the secondary battery is provided in the embodiments of this application, while the negative electrode is any electrode known in the art. In still other embodiments, at least a portion of the positive electrode in the secondary battery and at least a portion of the negative electrode are provided in the embodiments of this application.
[0064] In this application embodiment, the aforementioned secondary battery includes, but is not limited to, any known secondary battery such as lithium-ion battery, sodium-ion battery, and magnesium-ion battery.
[0065] In some embodiments of this application, the secondary battery includes a positive electrode, a negative electrode, and a separator. The separator is located between the positive and negative electrode, and a portion of the separator is bonded to the positive and / or negative electrode via an adhesive layer. The separator can be any type of separator known in the industry, such as a single-layer polypropylene (PP) membrane, a single-layer polyethylene (PE) membrane, a double-layer PP / PE membrane, a double-layer PP / PP membrane, or a triple-layer PP / PE / PP membrane, or a non-woven fabric, etc.
[0066] In some embodiments of this application, an electrolyte is also included between the positive electrode and the negative electrode.
[0067] This application also provides an electrical device, including the secondary battery provided in this application embodiment. In some embodiments of this application, the electrical device includes electronic components, and the secondary battery powers the electronic components. Because it uses the secondary battery provided in this application embodiment for power supply, this electrical device has good market prospects.
[0068] In some embodiments of this application, the aforementioned electrical equipment includes, but is not limited to, vehicles, or 3C electronic consumer products such as mobile phones, laptops, tablets, and smartwatches.
[0069] The technical solution of this application is further described below with reference to several embodiments.
[0070] Example 1
[0071] A negative electrode sheet includes a current collector, a negative electrode active material layer with a thickness of 230 μm disposed on the surface of the current collector, and a functional layer disposed on one side of the negative electrode active material. The functional layer includes an insulating layer and an adhesive layer stacked together. The adhesive layer is disposed away from the current collector and includes multiple adhesive structures.
[0072] The insulating layer consists of alumina particles with a diameter of 0.8 μm and a binder (carboxymethyl cellulose). The alumina particles account for 9% and 91% of the total mass of the insulating layer. The size of the insulating layer is 0.5 cm in the direction from the functional layer to the negative electrode active material layer. The thickness of the insulating layer is 200 μm.
[0073] The bonding structure is made of polymethyl methacrylate with a glass transition temperature of -20℃. The distance between two adjacent bonding structures is 300μm. The orthographic projection of the bonding structure in the first direction is a circle with a diameter of 100μm. The height of the bonding structure is 2.5μm.
[0074] In this process, the insulating layer and the negative electrode active material layer are simultaneously extruded and coated on the current collector. In the insulating slurry, the mass ratio of carboxymethyl cellulose is 9%, the solid content of the insulating slurry is 42%, the solvent is water, and the viscosity at room temperature is 3000 mPa·s. The solid content of the adhesive layer slurry is 45%, and the viscosity at room temperature is 200 mPa·s.
[0075] Example 2
[0076] The difference from Example 1 is that the insulating layer consists of boehmite particles with a particle size of 0.5 μm and a binder (carboxymethyl cellulose). The mass percentage of alumina particles is 6%, and the mass percentage of boehmite particles is 94%. The size of the insulating layer is 0.5 cm in the direction from the functional layer to the negative electrode active material layer. The thickness of the insulating layer is 200 μm.
[0077] The bonding structure is made of polymethyl methacrylate particles with a glass transition temperature of -40℃. The distance between two adjacent bonding structures is 300μm. The orthographic projection of the bonding structure in the first direction is a circle with a diameter of 100μm, and the height of the bonding structure is 2.0μm. The insulating layer and the negative electrode active material layer are simultaneously extruded and coated on the current collector. In the insulating slurry, the mass percentage of carboxymethyl cellulose is 6%, the solid content of the insulating slurry is 40%, the solvent is water, and the viscosity at room temperature is 3500 mPa·s. The solid content of the bonding layer slurry is 45%, and the viscosity at room temperature is 200 mPa·s.
[0078] Example 3
[0079] The difference from Example 1 is that the distance between two adjacent adhesive structures in the adhesive layer is 1000 μm.
[0080] Example 4
[0081] The difference from Example 1 is that the distance between two adjacent adhesive structures in the adhesive layer is 750 μm.
[0082] Example 5
[0083] The difference from Example 1 is that the distance between two adjacent adhesive structures in the adhesive layer is 1100 μm.
[0084] Example 6
[0085] The difference from Example 1 is that in the adhesive layer, the orthographic projection of the adhesive structure in the first direction is a circle with a diameter of 500 μm.
[0086] Example 7
[0087] The difference from Example 1 is that the height of the adhesive structure in the adhesive layer is 5 μm.
[0088] Example 8
[0089] The difference from Example 1 is that the height of the adhesive structure in the adhesive layer is 1 μm.
[0090] To highlight the beneficial effects of the embodiments of this application, the following comparative examples are provided.
[0091] Comparative Example 1
[0092] The difference from Example 1 is that a negative electrode active material layer and an insulating adhesive layer are disposed on the surface of the current collector in the same layer; the insulating adhesive layer comprises 89% boehmite particles, 2% carboxymethyl cellulose, and 9% hot melt adhesive by mass. The thickness of the negative electrode active material layer is 230 μm, the thickness of the insulating adhesive layer is 200 μm, and the width is 0.5 cm.
[0093] Performance testing
[0094] The negative electrode sheet provided in each embodiment and comparative example is bonded to the separator, specifically:
[0095] Examples 1-8 show that the negative electrode sheet was bonded to the diaphragm at 25°C and 1 MPa pressure, and the peel strength was tested according to GB / T2792. The results are summarized in Table 1.
[0096] The negative electrode sheet of Comparative Example 1 could not be bonded to the diaphragm under the above conditions. It was necessary to hot press and bond the diaphragm to the negative electrode sheet under a pressure of 1 MPa for 5 minutes at 100℃. The peel strength was then tested according to GB / T2792. The results are summarized in Table 1.
[0097] Table 1
[0098] Case Peel strength Example 1 1.0 N / m Example 2 1.2N / m Example 3 0.6N / m Example 4 0.7N / m Example 5 0.5N / m Example 6 1.4 N / m Example 7 1.3 N / m Example 8 0.5N / m Comparative Example 1 0.4N / m
[0099] As can be seen from the above data, the electrode sheets provided in this application embodiment can be smoothly and stably bonded to the separator under conventional cell forming process conditions, and the peel strength is high. Furthermore, when the relevant parameters of the bonding structure are within the range further suggested in this application, the peel strength between the electrode sheets and the separator is relatively even higher.
[0100] The above description is an exemplary embodiment of this application. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of this application, and these improvements and modifications are also considered to be within the scope of protection of this application.
Claims
1. An electrode sheet, characterized in that, The device includes a current collector, an active material layer disposed on at least one surface of the current collector, and at least one functional layer; wherein the functional layer is disposed at the edge of the current collector, and the functional layer is disposed in the same layer as the active material layer. The functional layer includes an insulating layer and an adhesive layer disposed on the insulating layer away from the surface of the current collector. The adhesive layer includes a plurality of adhesive structures arranged at intervals. The insulating layer is disposed on at least one side of the active material layer and has a certain gap between it and the active material layer. The insulating layer comprises inorganic particles and a binder, wherein the inorganic particles are made of one or more of alumina, boehmite, titanium dioxide, zirconium dioxide, magnesium hydroxide, and aluminum hydroxide; and the binder comprises carboxymethyl cellulose. In the stacking direction of the functional layer and the current collector, the size of the functional layer is x μm, the size of the active material layer is y μm, 10 μm≤yx≤50 μm, and the thickness of the insulating layer is 50 μm~300 μm.
2. The electrode sheet according to claim 1, characterized in that, The size of the insulating layer is 0.1 cm to 1 cm along the direction from the functional layer to the active material layer.
3. The electrode sheet according to claim 1, characterized in that, The distance between two adjacent adhesive structures is 300 μm to 1000 μm; and / or, In the stacking direction of the functional layer and the current collector, the size of the bonding structure is 2 μm to 5 μm, and the maximum size of the orthographic projection of the bonding structure is 100 μm to 500 μm.
4. The electrode sheet according to claim 1, characterized in that, The adhesive structure is made of a polymer, and the glass transition temperature of the polymer is -20 ℃ to 100 ℃; The polymer includes one or more of methyl methacrylate, butyl methacrylate, and hexyl acrylate.
5. The electrode sheet according to claim 1, characterized in that, The inorganic particles have a particle size of 0.5 μm to 5 μm; and / or, the inorganic particles account for 90% to 99% of the mass of the insulating layer.
6. The electrode sheet according to claim 1, characterized in that, It also includes tabs, which are adjacent to the current collector and are disposed close to the functional layer.
7. A secondary battery, characterized in that, Includes the electrode sheet as described in any one of claims 1 to 6.
8. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 7.
Citation Information
Patent Citations
Battery and terminal equipment
CN113097611A
Electrode assembly, battery cell, battery and electric device
CN115084782A
Electrode plate, winding type battery cell and battery
CN214378500U