A friction material, its preparation method, and a synthetic brake shoe

By using a specific ratio of friction material and manufacturing process, the problem of poor friction and wear performance of synthetic brake shoes in high-speed heavy-load trains has been solved, achieving stable friction performance and extended service life under high temperature and humid environments.

CN119899486BActive Publication Date: 2026-11-17SHENHUA RAIL & FREIGHT WAGONS TRANSPORT
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510003458.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-01-02
Publication Date
2026-11-17
Estimated Expiration
2045-01-02

AI Technical Summary

Technical Problem

Existing synthetic brake shoes have poor friction and wear performance, poor heat resistance, and short service life during high-speed heavy-haul train operation. They are also prone to damaging wheels in humid environments, leading to increased maintenance costs for railway freight cars.

Method used

The friction material is prepared by using a specific ratio of phenolic resin and powdered nitrile rubber as adhesives, sepiolite and steel fiber as reinforcing materials, and calcium carbonate as filler materials. The synthetic brake shoe is prepared by a specific stirring and mixing process to ensure the stability and friction performance of the material under high temperature conditions.

Benefits of technology

It improves the friction and wear resistance and mechanical properties of synthetic brake shoes, reduces noise, extends service life, meets the braking requirements of high-speed heavy-haul trains, and reduces maintenance frequency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005226147310000111
    Figure BDA0005226147310000111
  • Figure BDA0005226147310000121
    Figure BDA0005226147310000121
  • Figure BDA0005226147310000141
    Figure BDA0005226147310000141
Patent Text Reader

Abstract

This invention provides a friction material, its preparation method, and a synthetic brake shoe, relating to the technical field of synthetic brake shoes for heavy-duty railway freight cars. The friction material comprises or is made from raw materials comprising the following components: adhesive material: 46-68 parts by weight; reinforcing material: 48-88 parts by weight; filler material: 97-167 parts by weight; additives and auxiliaries: 1.5-9 parts by weight. The adhesive material comprises phenolic resin and powdered nitrile rubber, and the additives and auxiliaries comprise ethanol and octadecenoic acid. The friction material provided by this invention enables control over the hardness, impact strength, and other performance indicators of the synthetic brake shoe, obtaining an ideal coefficient of friction to meet the braking wear performance requirements of general-purpose railway freight cars with different axle loads and operating speeds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of synthetic brake shoes for heavy-duty freight cars, specifically to a friction material and its preparation method, as well as synthetic brake shoes. Background Technology

[0002] According to statistics from the National Railway Administration, the number of freight cars on the national railway in 2024 was 1.005 million, of which 854,000 were general-purpose freight cars, accounting for 85%. To ensure that general-purpose freight cars stop safely within the prescribed braking distance, the brake shoes typically grip the wheel tread during braking, using friction to stop the wheelset from rotating. From the 1940s to the present, the development of railway freight car brake shoes has evolved from cast iron brake shoes to powder metallurgy brake shoes, and then to synthetic brake shoes. After years of practical application, cast iron and powder metallurgy brake shoes have been gradually phased out due to their high manufacturing cost, unstable friction coefficient, significant environmental pollution, and severe wear on freight car wheels.

[0003] To overcome the aforementioned performance defects, many countries began research on synthetic brake shoes after the 1940s, and my country also began developing synthetic brake shoes in the 1950s. Compared with traditional brake shoes, synthetic brake shoes have advantages such as lower manufacturing costs, adjustable friction coefficients, environmental friendliness, and less wear on freight car wheels. In recent years, with the development of the national economy, in order to improve railway freight efficiency and reduce transportation costs, the technology of high-speed, heavy-haul general-purpose freight cars has developed rapidly. The braking friction and wear performance of synthetic brake shoes manufactured by traditional formulas and preparation methods cannot match the operating conditions of high-speed, heavy-haul trains. During use, they exhibit poor heat resistance, short service life, and are prone to metal embedding damage to freight car wheels under special braking conditions such as long slopes and humid environments. This increases the replacement frequency of railway freight car brake shoes and raises the maintenance costs of railway freight cars. Summary of the Invention

[0004] Based on the above analysis, the present invention aims to provide a friction material and its preparation method, as well as a synthetic brake shoe, to solve at least one of the following existing problems: improving the friction and wear performance of the synthetic brake shoe, and improving the mechanical properties of the synthetic brake shoe.

[0005] The objective of this invention is mainly achieved through the following technical solutions:

[0006] In a first aspect, the present invention provides a friction material comprising the following components or made from raw materials comprising the following components:

[0007] Adhesive material: 46-68 parts by weight;

[0008] Reinforcing material: 48-88 parts by weight;

[0009] Filler material: 97-167 parts by weight;

[0010] Additives and excipients: 1.5-9 parts by weight

[0011] The adhesive material includes phenolic resin and powdered nitrile rubber, and the additives include ethanol and octadecenoic acid.

[0012] Preferably, the amount of adhesive material used is 54-60 parts by weight.

[0013] Preferably, the amount of reinforcing material used is 62-76 parts by weight.

[0014] Preferably, the amount of filler material used is 118-147 parts by weight.

[0015] Preferably, the amount of additives and excipients used is 4-7.5 parts by weight.

[0016] Preferably, in the friction material, the amount of phenolic resin is 23-34 parts by weight, more preferably 27-30 parts by weight; and the amount of powdered nitrile rubber is 23-34 parts by weight, more preferably 27-30 parts by weight.

[0017] Preferably, the phenolic resin has a hexamethylenetetramine content of 7wt.%-8wt.%, a free phenol content of ≤1wt.%, a polymerization time of 40-70s at 150℃, and a particle size of 150-250 mesh.

[0018] Preferably, the powdered nitrile rubber has a bound acrylonitrile content of 36wt.%-40wt.% and a particle size of 35-45 mesh.

[0019] Preferably, in the friction material, the amount of ethanol is 1-6 parts by weight, more preferably 3-5 parts by weight; and the amount of octadecenoic acid is 0.5-3 parts by weight, more preferably 1-2.5 parts by weight.

[0020] Preferably, the reinforcing material includes at least one of sepiolite, steel fiber, mineral fiber, and acicular wollastonite.

[0021] Preferably, the reinforcing material comprises sepiolite, steel fiber, mineral fiber, and acicular wollastonite, wherein:

[0022] The amount of sepiolite used is 25-35 parts by weight, preferably 28-32 parts by weight;

[0023] The amount of steel fiber used is 10-20 parts by weight, preferably 14-17 parts by weight;

[0024] The amount of mineral fiber used is 6-16 parts by weight, preferably 10-13 parts by weight;

[0025] The amount of acicular wollastonite used is 7-17 parts by weight, preferably 10-14 parts by weight.

[0026] Preferably, the filler material includes at least one selected from calcium carbonate, barium sulfate, reduced iron powder, graphite, high alumina powder, potassium feldspar, molybdenum disulfide, and antimony trisulfide.

[0027] Preferably, the filler material includes calcium carbonate, barium sulfate, reduced iron powder, graphite, high alumina powder, potassium feldspar, molybdenum disulfide, and antimony trisulfide, wherein:

[0028] The amount of calcium carbonate used is 5-15 parts by weight, preferably 8-12 parts by weight;

[0029] The amount of barium sulfate used is 5-15 parts by weight, preferably 8-12 parts by weight;

[0030] The amount of reduced iron powder used is 21-31 parts by weight, preferably 24-28 parts by weight;

[0031] The amount of graphite used is 4-14 parts by weight, preferably 8-11 parts by weight;

[0032] The amount of high-alumina powder used is 11-21 parts by weight, preferably 14-18 parts by weight;

[0033] The amount of potassium feldspar used is 48-58 parts by weight, preferably 51-55 parts by weight;

[0034] The amount of molybdenum disulfide used is 2-8 parts by weight, preferably 3-7 parts by weight;

[0035] The amount of antimony trisulfide used is 1-5 parts by weight, preferably 2-4 parts by weight.

[0036] Secondly, the present invention provides a method for preparing the aforementioned friction material, comprising the following steps:

[0037] Step 1: The adhesive material, which includes phenolic resin and powdered nitrile rubber, is stirred for the first time, and then the reinforcing material and filler material are added, followed by a second stirring.

[0038] Step 2: Perform the first stage of intensive mixing, then add additives and excipients for the second stage of intensive mixing, and then discharge the material.

[0039] Preferably, in step 1, the duration of the first stirring and the second stirring may be the same or different, each independently being 2-5 minutes.

[0040] Preferably, in step 2, the conditions for the first stage of internal mixing include: a rotation speed of 20-30 rpm, preferably 24-27 rpm; a pressure of 0.2-0.4 MPa, preferably 0.25-0.35 MPa; and a mixing time of 120-180 s.

[0041] Preferably, in step 2, the conditions for the second stage of internal mixing include: a rotation speed of 20-30 rpm, preferably 24-27 rpm; and a pressure of 0.2-0.4 MPa, preferably 0.25-0.3 MPa.

[0042] Preferably, in step 2, the temperature of the discharged adhesive is 40-50℃, more preferably 42-45℃.

[0043] Thirdly, the present invention provides a synthetic brake shoe, comprising a friction material and a shoe back, wherein the friction material is fixed on the shoe back.

[0044] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0045] A) The friction material provided by this invention can control the performance indicators such as hardness and impact strength of the synthetic brake shoe, and obtain an ideal coefficient of friction to meet the requirements of general-purpose railway freight cars with different axle loads and running speeds for braking wear performance.

[0046] B) The method for preparing friction material provided by the present invention involves first stirring with adhesive material and fully coating cross-linked nitrile powder with thermoplastic phenolic resin, which can effectively prevent cross-linked nitrile powder from agglomerating during the mixing process and improve the quality of material mixing and vulcanization; the mixing process enables the synthetic brake shoe to have good heat resistance and adapt to the continuous high temperature generated during braking, and the performance of the brake shoe wheel tread will not drop sharply due to the increase in temperature.

[0047] C) The synthetic brake shoe provided by this invention is a brake shoe with friction material and backing solidified together. It is lightweight, has a stable coefficient of friction, low wear, low noise during braking, and high mechanical properties. It can be used for heavy-duty freight cars on railways, fully ensuring the braking friction and wear performance and mechanical properties of the synthetic brake shoe. Detailed Implementation

[0048] The following provides a detailed description of specific embodiments of the present invention. It should be understood that the specific embodiments described herein are for illustrative and explanatory purposes only and are not intended to limit the scope of the invention.

[0049] In a first aspect, the present invention provides a friction material comprising the following components or prepared from raw materials comprising the following components:

[0050] Adhesive material: 46-68 parts by weight, preferably 54-60 parts by weight;

[0051] Reinforcing material: 48-88 parts by weight, preferably 62-76 parts by weight;

[0052] Filler material: 97-167 parts by weight, preferably 118-147 parts by weight;

[0053] Additives and excipients: 1.5-9 parts by weight, preferably 4-7.5 parts by weight.

[0054] The adhesive material includes phenolic resin and powdered nitrile rubber, and the additives include ethanol and octadecenoic acid.

[0055] The friction material provided by this invention can control the performance indicators such as hardness and impact strength of the synthetic brake shoe, and obtain an ideal coefficient of friction to meet the requirements of general-purpose railway freight cars with different axle loads and operating speeds for braking wear performance.

[0056] It is believed that the adhesive material plays a role in bonding other components, making the friction material a whole and ensuring the structural integrity of the brake shoe. In existing technologies, liquid nitrile rubber is typically used as the adhesive material. Although the processing of friction materials using this system is relatively simple, it requires mixing and processing in a liquid state, usually requiring special equipment and processes to control its flowability. This invention uses powdered nitrile rubber and phenolic resin as the adhesive material, which is easily dispersed in the substrate during processing, providing a stable coefficient of friction, good impact resistance, and wear resistance.

[0057] Furthermore, ethanol and octadecenoic acid work synergistically to improve the performance of friction material. Octadecenoic acid, in particular, possesses excellent thermal stability. In high-friction synthetic brake shoes, octadecenoic acid can prevent lubrication failure and increased friction coefficient caused by high temperatures. This improved thermal stability helps ensure the normal operation of the braking system in high-temperature environments, improving braking efficiency and safety. During the mixing process, excessive octadecenoic acid can cause over-sulfurization, while insufficient octadecenoic acid can lead to inadequate sulfurization, both of which negatively impact material performance.

[0058] In a specific embodiment of the present invention, the amount of phenolic resin used is 23-34 parts by weight, such as 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 parts by weight, preferably 27-30 parts by weight.

[0059] In a specific embodiment of the present invention, the amount of powdered nitrile rubber is 23-34 parts by weight, such as 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34 parts by weight, preferably 27-30 parts by weight.

[0060] In a specific embodiment of the present invention, the phenolic resin has a flowability of 35-60 mm, a hexamethylenetetramine content of 7 wt.%-8 wt.%, a free phenol content of ≤1 wt.%, a polymerization time of 40-70 s at 150°C, and a particle size of 150-250 mesh, preferably 200 mesh ≥95 wt.%.

[0061] In a specific embodiment of the present invention, the acrylonitrile content of the powdered nitrile rubber is 36 wt.%-40 wt.%, and the Mooney viscosity is (ML). 100±0.5℃ 1+4)100-150, with a particle size of 35-45 mesh, preferably 40 mesh ≥95wt.%.

[0062] In a specific embodiment of the present invention, the amount of ethanol used is 1-6 parts by weight, such as 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6 parts by weight, preferably 3-5 parts by weight.

[0063] In a specific embodiment of the present invention, the amount of octadecenoic acid used is 0.5-3 parts by weight, such as 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3 parts by weight, preferably 1-2.5 parts by weight.

[0064] In a specific embodiment of the present invention, the ethanol is industrial alcohol with an alcohol content ≥95 wt.%.

[0065] In a specific embodiment of the present invention, octadecenoic acid is oleic acid with an acid value (mgKOH / g) of 180-195, a saponification value (mgKOH / g) of 190-202, and an iodine value (g / 100g) of 70-95.

[0066] In this invention, the additives and excipients can also accelerate the mixing speed of the friction body material, shorten the mixing time, and improve the mixing production efficiency.

[0067] In this invention, the reinforcing material can enhance the strength, hardness and wear resistance of the friction material, thereby improving the wear resistance of the brake shoe during braking.

[0068] In a specific embodiment of the present invention, the reinforcing material includes at least one selected from sepiolite, steel fiber, mineral fiber, and acicular wollastonite. Preferably, the reinforcing material includes sepiolite, steel fiber, mineral fiber, and acicular wollastonite, wherein:

[0069] The amount of sepiolite used is 25-35 parts by weight, such as 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35 parts by weight, preferably 28-32 parts by weight;

[0070] The amount of steel fiber used is 10-20 parts by weight, such as 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 parts by weight, preferably 14-17 parts by weight;

[0071] The amount of mineral fiber used is 6-16 parts by weight, such as 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16 parts by weight, preferably 10-13 parts by weight;

[0072] The amount of acicular wollastonite used is 7-17 parts by weight, such as 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 parts by weight, preferably 10-14 parts by weight.

[0073] In a specific embodiment of the present invention, the mineral fiber is selected from basalt fiber, and the fiber length of the mineral fiber is 0.3-0.5 mm and the fiber diameter is 0.03-0.08 mm.

[0074] In a specific embodiment of the present invention, the specifications of the steel fibers are: 14 mesh: 0-1.0 wt.%, 20 mesh: 0-1.5 wt.%, 40 mesh: 5-12 wt.%, 70 mesh: 5-25 wt.%, 100 mesh: 5-20 wt.%, and bottom of the tray: 55-75 wt.%.

[0075] In a specific embodiment of the present invention, the particle size of sepiolite is 4-6 mm.

[0076] In a specific embodiment of the present invention, the acicular wollastonite is needle-shaped, with a sieve pass rate of ≥95wt.% (60 mesh), an aspect ratio of 24:1, a SiO2 content of ≥48wt.%, a CaO content of ≥44wt.%, a Fe2O3 content of ≤1wt.%, and an Al2O3 content of ≤0.8wt.%.

[0077] In this invention, the filler material is used to adjust the braking friction and wear performance of the brake shoes, ensuring a suitable coefficient of friction under different operating conditions to achieve a stable braking effect. In a specific embodiment of this invention, the filler material includes at least one of calcium carbonate, barium sulfate, reduced iron powder, graphite, high alumina powder, potassium feldspar, molybdenum disulfide, and antimony trisulfide. Preferably, the filler material includes calcium carbonate, barium sulfate, reduced iron powder, graphite, high alumina powder, potassium feldspar, molybdenum disulfide, and antimony trisulfide, wherein:

[0078] The amount of calcium carbonate used is 5-15 parts by weight, such as 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 parts by weight, preferably 8-12 parts by weight;

[0079] The amount of barium sulfate used is 5-15 parts by weight, such as 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 parts by weight, preferably 8-12 parts by weight;

[0080] The amount of reduced iron powder used is 21-31 parts by weight, such as 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31 parts by weight, etc., preferably 24-28 parts by weight;

[0081] The amount of graphite used is 4-14 parts by weight, such as 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 parts by weight, preferably 8-11 parts by weight;

[0082] The amount of high-alumina powder used is 11-21 parts by weight, such as 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21 parts by weight, etc., preferably 14-18 parts by weight;

[0083] The amount of potassium feldspar used is 48-58 parts by weight, such as 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58 parts by weight, preferably 51-55 parts by weight.

[0084] The amount of molybdenum disulfide used is 2-8 parts by weight, such as 2, 3, 4, 5, 6, 7, 8 parts by weight, preferably 3-7 parts by weight;

[0085] The amount of antimony trisulfide used is 1-5 parts by weight, such as 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5 parts by weight, preferably 2-4 parts by weight.

[0086] In a specific embodiment of the present invention, the sieve passing rate of calcium carbonate is ≥95 wt.% for 325 mesh, and the calcium carbonate content is ≥97 wt.%.

[0087] In a specific embodiment of the present invention, the sieve pass rate of barium sulfate is ≥95 wt.% for 325 mesh and the barium content is ≥80 wt.%.

[0088] In a specific embodiment of the present invention, the sieving rate of the high-alumina powder is: 325 mesh ≥ 95 wt.%, Al2O3 content ≥ 75 wt.%, and Fe2O3 content ≤ 2 wt.%.

[0089] In a specific embodiment of the present invention, the sieve passing rate of potassium feldspar is: 325 mesh ≥ 95 wt.%, SiO2 content ≥ 70 wt.%, and Al2O3 content ≥ 10 wt.%.

[0090] In a specific embodiment of the present invention, the graphite is flake graphite with a carbon content ≥80 wt.%.

[0091] In a specific embodiment of the present invention, the molybdenum disulfide contains ≥98.5 wt.% molybdenum disulfide, ≤0.19 wt.% oil, ≤0.18 wt.% molybdic anhydride, and ≤0.15 wt.% moisture.

[0092] In a specific embodiment of the present invention, the sieve passing rate of antimony trisulfide is 200 mesh = 100%, and the antimony content is 69 wt.%-73 wt.%.

[0093] In this invention, the addition of molybdenum disulfide and antimony trisulfide can prevent the friction coefficient from being too high in the low-speed range and stabilize the friction coefficient in the high-speed range.

[0094] Although the types and functions of adhesive materials, reinforcing materials, fillers, and additives have been described above, in this invention, adhesive materials, reinforcing materials, fillers, and additives do not function individually, but rather work synergistically as a whole friction material to improve the friction and wear performance and mechanical properties of the friction material.

[0095] The friction material provided by this invention enables control over the performance indicators such as hardness and impact strength of the synthetic brake shoe, thereby obtaining an ideal coefficient of friction to meet the braking wear performance requirements of general-purpose railway freight cars with different axle loads and operating speeds.

[0096] Secondly, the present invention provides a method for preparing a friction material, comprising the following steps:

[0097] Step 1: The adhesive material, which includes phenolic resin and powdered nitrile rubber, is stirred for the first time, and then the reinforcing material and filler material are added, followed by a second stirring.

[0098] Step 2: Perform the first stage of intensive mixing, then add additives and excipients for the second stage of intensive mixing, and then discharge the material.

[0099] The method for preparing friction material provided by this invention involves initial stirring with an adhesive material, followed by thorough encapsulation of cross-linked nitrile butadiene powder with thermoplastic phenolic resin. This prevents the cross-linked nitrile butadiene powder from agglomerating during the internal mixing process, thus unaffected by the Mooney viscosity index of the cross-linked nitrile butadiene powder. This effectively prevents agglomeration and improves the quality of the material's internal mixing and vulcanization. Compared to traditional centrifugal mixing, the internal mixing process better improves the uniformity of the brake shoe material, ensuring the stability of the brake shoe's mechanical and tribological properties. It also fully utilizes the heat resistance of materials such as graphite and antimony trisulfide to withstand the continuous high temperatures generated during braking, preventing a sharp drop in the coefficient of friction due to temperature increases during braking. In the second stage of internal mixing, additives are added to accelerate the mixing speed, shorten the mixing time, improve mixing efficiency, and enhance the fusion effect of various friction material components.

[0100] It should be noted that in this invention, if no additives or auxiliaries are added, not only will the mixing speed be too slow, but the material will also be unable to form mixed particles, reducing the material fusion effect and thus deteriorating the mechanical properties of the friction material. Furthermore, additives and auxiliaries should not be added before mixing or during the first stage of mixing; otherwise, the material uniformity will deteriorate, and fibrous materials may agglomerate.

[0101] In the method for preparing the friction material provided by this invention, there is no limitation on the duration of the first and second stirring in step 1, as long as the stirring is uniform. For example, the duration of the first and second stirring can be the same or different, each independently ranging from 2 to 5 minutes. The temperature for the first and second stirring is room temperature.

[0102] In a specific embodiment of the present invention, the conditions for the first stage of intensive mixing in step 2 include:

[0103] The rotational speed is 20-30 rpm, such as 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 rpm, etc., preferably 24-27 rpm;

[0104] The pressure is 0.2-0.4 MPa, such as 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4 MPa, etc., preferably 0.25-0.35 MPa;

[0105] The mixing time is 120-180 seconds, such as 120, 130, 140, 150, 160, 170, 180 seconds, etc., at room temperature.

[0106] In a specific embodiment of the present invention, in step 2, the conditions for the second stage of intensive refining may be the same as or different from the conditions for the first stage of intensive refining. The conditions for the second stage of intensive refining include:

[0107] The rotational speed is 20-30 rpm, such as 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30 rpm, etc., preferably 24-27 rpm;

[0108] The pressure is 0.2-0.4 MPa, such as 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4 MPa, etc., preferably 0.25-0.35 MPa.

[0109] In a specific embodiment of the present invention, the rubber temperature in the second stage of the mixing process in step 2 is raised to 40-50°C for discharge, for example, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50°C, etc., preferably 42-45°C.

[0110] The method for preparing friction material provided by the present invention ensures that the synthetic brake shoe has a stable compressive modulus and compressive strength by setting standards for mixing time and mixing temperature, thereby improving the physical and mechanical properties of the brake shoe and ensuring that the synthetic brake shoe maintains stable braking friction and wear performance under extreme braking conditions such as high speed, heavy load, and humid conditions, thus improving the preparation quality of the synthetic brake shoe.

[0111] The friction material preparation method provided by this invention, in the mixing process, sets the rotation speed and pressure values ​​to make the raw material molecules more tightly bonded and the material distribution more uniform, which solves the problem of uneven wear rate caused by uneven material and thus extends the service life of the brake shoe.

[0112] In this invention, if the discharge temperature of the adhesive is too high, for example above 50°C, the compression modulus of the brake shoe will be too high, leading to cracks during operation. If the temperature is too low, for example below 40°C, the raw material cannot be molded, failing to achieve the desired mixing effect, resulting in a decline in the various properties of the friction material. It should be noted that in this invention, the mixing pressure is closely related to the adhesive temperature. If the mixing pressure is too high, for example above 0.4 MPa, the mixing temperature rises sharply, which is detrimental to adhesive dispersion and affects material properties. Excessive pressure also increases the power load on the mixer, potentially causing overload and power outage. If the mixing pressure is too low, for example below 0.2 MPa, the material will be mixed unevenly, affecting product quality.

[0113] In a specific embodiment of the present invention, the method for preparing the friction material further includes step 3, in which the friction material is obtained by crushing and drying in sequence.

[0114] In a specific embodiment of the present invention, step 3 includes the following steps:

[0115] Step 3a: Crushing: The raw materials after internal mixing are coarsely and finely crushed by a crusher and then set aside for use;

[0116] Step 3b: Drying: Place the crushed material into a curing oven for drying at a temperature of 60-80℃ for 4-6 hours to obtain the friction material.

[0117] It should be noted that the baking step in step 3b can reduce the moisture content of the friction material and prevent cracks in the brake shoe tread during curing.

[0118] Thirdly, the present invention provides a synthetic brake shoe, comprising the above-mentioned friction material and a shoe back, wherein the friction material is fixed on the shoe back.

[0119] Fourthly, the present invention provides a method for preparing a synthetic brake shoe, including a preforming and curing step of the friction material and the back of the shoe.

[0120] In a specific embodiment of the present invention, the preforming step is as follows: at room temperature, the baked friction material is pressed into a synthetic brake shoe blank by a press through a special mold and the back of the shoe. The press pressure is 100T and the holding time is 2s.

[0121] In a specific embodiment of the present invention, the curing step includes primary curing and secondary curing:

[0122] One-time curing: Place the pressed brake shoe blank into a hot press mold, set the frame press pressure to 220±10T, set the hot press mold heating temperature to 150±10℃, venting interval 18s, venting 2-6 times, and holding pressure for 600-1200s before demolding and taking out the shaped brake shoe.

[0123] Secondary curing: The shaped brake shoes are placed in a curing oven for secondary curing. The curing temperature is gradually increased from room temperature through 80℃—100℃—120℃—130℃—140℃—150℃ to 160℃, and then cooled down with the oven. The total time is 32-36 hours, which is used to improve the vulcanization effect of the brake shoes and stabilize the internal molecular structure of the friction material.

[0124] The synthetic brake shoe provided by this invention is prepared by mixing and kneading the components to produce a friction material, which is then pressed together with the back of the brake shoe to form a synthetic brake shoe. It is lightweight, has a stable coefficient of friction, low wear, low noise during braking, and high mechanical properties. It can be used for heavy-duty freight cars on railways, fully ensuring the braking friction and wear performance as well as the mechanical properties of the synthetic brake shoe.

[0125] The following detailed description of preferred embodiments of the present invention illustrates the principles of the invention and is not intended to limit the scope of the invention.

[0126] Unless otherwise specified, all materials used are commercially available products.

[0127] Example 1

[0128] (1) Preparation method of friction material, the raw materials of friction material are shown in Table 1:

[0129] Step 1: First, stir the phenolic resin and powdered nitrile for 2 minutes until they are evenly mixed. Then, add steel fiber, sepiolite, basalt fiber, acicular wollastonite, barium sulfate, calcium carbonate, iron powder, flake graphite, high alumina powder, potassium feldspar, molybdenum disulfide and antimony trisulfide, and stir for 2 minutes until they are evenly mixed.

[0130] Step 2: Put the mixed material into the internal mixer at a speed of 26 rpm and a top pressure of 0.31 MPa. After mixing for 120 seconds, add ethanol and octadecenoic acid. Keep the mixing conditions unchanged. When the rubber temperature reaches 45°C, open the bottom plug to discharge the material.

[0131] Step 3a: The raw materials after internal mixing are coarsely and finely crushed by a crusher and then set aside for use;

[0132] Step 3b: Drying in a drying oven at a set temperature of 60°C for 6 hours; to obtain the friction material.

[0133] (2) Preparation method of synthetic brake shoes:

[0134] Preforming: The back of the brake shoe and the friction material are pre-pressed into a brake shoe blank using a press and a mold. The press pressure is 100T and the holding time is 2s.

[0135] Curing: The brake shoe blank is placed in the heated mold cavity under the press for primary curing. The press pressure is 230T, the curing time is 600s, the venting interval is 18s, the number of venting times is 4, and the primary curing temperature is 150±10℃. After the brake shoe is initially vulcanized and shaped, it is demolded and the wear line is marked. The shaped brake shoe is placed in the curing oven for secondary curing. The curing temperature is gradually increased from 80℃ to 160℃.

[0136] Table 1. Composition of friction material raw materials in Example 1

[0137]

[0138]

[0139] Example 2

[0140] This embodiment is basically the same as Embodiment 1, except that the internal mixer speed is 30 rpm.

[0141] Example 3

[0142] This embodiment is basically the same as Embodiment 1, except that the internal mixer speed is 20 rpm.

[0143] Example 4

[0144] This embodiment is basically the same as Embodiment 1, except that the pressure value of the top bolt is 0.22 MPa.

[0145] Example 5

[0146] This embodiment is basically the same as Embodiment 1, except that the pressure value of the top bolt is 0.38MPa.

[0147] Example 6

[0148] This embodiment is basically the same as Embodiment 1, except that the bottom bolt is opened to discharge the material when the adhesive temperature rises to 49°C.

[0149] Example 7

[0150] This embodiment is basically the same as Embodiment 1, except that the bottom bolt is opened to discharge the material when the adhesive temperature rises to 40°C.

[0151] Example 8

[0152] This embodiment is basically the same as Embodiment 1, except that the amount of ethanol is 13g and the amount of octadecenoic acid is 35g.

[0153] Example 9

[0154] This embodiment is basically the same as Embodiment 1, except that the amount of ethanol is 43g and the amount of octadecenoic acid is 5g.

[0155] Example 10

[0156] This embodiment is basically the same as Embodiment 1, except that the amount of phenolic resin is 256g and the amount of powdered nitrile is 316g.

[0157] Comparative Example 1

[0158] This comparative example is basically the same as Example 1, except that it does not include ethanol and the amount of octadecenoic acid is 48g.

[0159] Comparative Example 2

[0160] This comparative example is basically the same as Example 1, except that it does not include octadecenoic acid and the amount of ethanol is 48g. When octadecenoic acid is not included, the material cannot be formed during the mixing process and subsequent steps cannot be continued.

[0161] Comparative Example 3

[0162] This comparative example is basically the same as Example 1, except that the first stirring is not performed, but the adhesive material, reinforcing composite material and filler material are stirred at the same time.

[0163] Test case

[0164] Friction and wear performance and mechanical properties were tested according to the content of "Part 1: Composite Brake Shoes" in TB / T 3104.1-2020 Locomotive and Rolling Stock Brake Shoes. Some performance parameters are shown in Table 2. Specifically, the average friction coefficient and wear amount tests were conducted using a 1:1 bench test according to the braking wear performance test requirements in Appendix F of TB / T 3104.1-2020 Locomotive and Rolling Stock Brake Shoes, "Part 1: Composite Brake Shoes". The test conditions for the average friction coefficient were a braking speed of 125 km / h and a braking pressure of 20 kN. After the test, the wear amount was calculated based on weight loss and braking energy. The performance parameter results of the examples and comparative examples are shown in Table 3.

[0165] Table 2 Performance Parameters

[0166]

[0167] Table 3. Friction and wear properties and mechanical property parameters of the examples and comparative examples.

[0168]

[0169]

[0170] As can be seen from Examples 1-10 and Comparative Examples 1-3, the friction material of the present invention has an ideal coefficient of friction, which can realize the control of performance indicators such as hardness and impact strength of the synthetic brake shoe, and can meet the requirements of general-purpose railway freight cars with different axle loads and running speeds for braking wear performance.

[0171] As can be seen from Example 1 and Comparative Examples 1-3, Comparative Example 1, without the addition of ethanol, showed a significant decrease in the coefficient of friction, a significant increase in wear, a significant decrease in impact strength, a significant decrease in hardness, and a significant deterioration in overall performance; Comparative Example 2, without the addition of octadecenoic acid, could not proceed to the subsequent steps; Comparative Example 3, without the first stirring of the adhesive material, showed a significant decrease in the coefficient of friction, a significant increase in wear, a decrease in impact strength, and a significant deterioration in overall performance.

[0172] As can be seen from Examples 1-3, when the internal mixer speeds in Examples 2 and 3 were adjusted to 30 rpm and 20 rpm respectively, the coefficient of friction decreased slightly, while the wear rate increased slightly. Compared to Example 1, the overall performance of Examples 2-3 declined.

[0173] As can be seen from Examples 1 and 4-5, the pressure values ​​of Examples 4 and 5 were adjusted to 0.22 MPa and 0.38 MPa, respectively. Although Example 4 had a higher coefficient of friction and lower wear, its hardness was too high (the optimal range for hardness is 80-90), exceeding 90. At this hardness, the risk of metal embedding in the friction material increased significantly, and metal embedding can lead to the formation of hard alloys in the friction material, thereby damaging the wheel. The brake shoe of Example 5 had a slightly lower coefficient of friction, a slightly increased wear, and a lower hardness. Compared to Example 1, the overall performance of Examples 4-5 was somewhat reduced.

[0174] As can be seen from Examples 1 and 6-7, when the discharge temperatures of the adhesive in Examples 6 and 7 were adjusted to 49℃ and 40℃ respectively, the compression modulus of Example 6 increased, increasing the risk of cracking in the brake shoe. Example 7 showed a slightly lower coefficient of friction, a slightly increased wear, lower impact strength, and lower pull-out force. Compared to Example 1, the overall performance of Examples 6-7 was somewhat reduced.

[0175] As can be seen from Examples 1 and 8-10, Examples 8 and 9 adjusted the amounts of ethanol and octadecenoic acid, respectively, while Example 10 adjusted the amounts of phenolic resin and powdered nitrile. The coefficient of friction and hardness of Example 8 decreased slightly; the coefficient of friction and pull-out force of Example 9 decreased slightly; and the coefficient of friction and flexural strength of Example 10 decreased slightly. Compared to Example 1, the overall performance of Examples 8-10 declined.

[0176] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

Claims

1. Use of synthetic brake shoes in railway heavy freight cars, characterized in that, The synthetic brake shoe includes a friction material and a backing. The friction material is fixed to the backing. The friction material includes the following components or is made from raw materials including the following components: Adhesive material: 46-68 parts by weight; Reinforcing material: 48-88 parts by weight; Filler material: 97-167 parts by weight; Additives and excipients: 4-7.5 parts by weight The adhesive material includes phenolic resin and powdered nitrile rubber, and the additives include ethanol and octadecenoic acid; in the friction material, the amount of ethanol is 3-5 parts by weight, and the amount of octadecenoic acid is 1-2.5 parts by weight. The method for preparing the friction material includes the following steps: Step 1: The adhesive material, which includes phenolic resin and powdered nitrile rubber, is stirred for the first time, and then the reinforcing material and filler material are added, followed by a second stirring. Step 2: Perform the first stage of intensive mixing, then add additives and excipients for the second stage of intensive mixing, and then discharge the material; In step 2, the conditions for the first stage of intensive mixing include: pressure of 0.25-0.35MPa, speed of 24-27rpm, and mixing time of 120-180s; in step 2, the conditions for the second stage of intensive mixing include: pressure of 0.25-0.35MPa and speed of 24-27rpm. In step 2, the temperature of the discharged adhesive is 42-45℃.

2. The application according to claim 1, characterized in that, The amount of adhesive material used is 54-60 parts by weight; And / or, the amount of reinforcing material used is 62-76 parts by weight; And / or, the amount of filler material used is 118-147 parts by weight.

3. The application according to claim 1 or 2, characterized in that, In the friction body material The amount of phenolic resin used is 23-34 parts by weight; The amount of powdered nitrile rubber used is 23-34 parts by weight. And / or, the phenolic resin has a hexamethylenetetramine content of 7wt.%-8wt.%, a free phenol content of ≤1wt.%, a polymerization time of 40-70s at 150℃, and a particle size of 150-250 mesh; And / or, the acrylonitrile content of the powdered nitrile rubber is 36wt.%-40wt.%, and the particle size is 35-45 mesh.

4. The application according to claim 3, characterized in that, In the friction body material The amount of phenolic resin used is 27-30 parts by weight; The amount of powdered nitrile rubber used is 27-30 parts by weight.

5. The application according to claim 1 or 2, characterized in that, The reinforcing material includes at least one of sepiolite, steel fiber, mineral fiber, and acicular wollastonite.

6. The application according to claim 5, characterized in that, The reinforcing material includes sepiolite, steel fiber, mineral fiber, and acicular wollastonite, wherein: The dosage of sepiolite is 25-35 parts by weight; The amount of steel fiber used is 10-20 parts by weight; The amount of mineral fiber used is 6-16 parts by weight; The amount of needle-shaped wollastonite used is 7-17 parts by weight.

7. The application according to claim 6, characterized in that, The dosage of sepiolite is 28-32 parts by weight; The amount of steel fiber used is 14-17 parts by weight; The amount of mineral fiber used is 10-13 parts by weight; The amount of needle-shaped wollastonite used is 10-14 parts by weight.

8. The application according to claim 1 or 2, characterized in that, The filler material includes at least one of calcium carbonate, barium sulfate, reduced iron powder, graphite, high alumina powder, potassium feldspar, molybdenum disulfide, and antimony trisulfide.

9. The application according to claim 8, characterized in that, The filler materials include calcium carbonate, barium sulfate, reduced iron powder, graphite, high alumina powder, potassium feldspar, molybdenum disulfide, and antimony trisulfide, among which: The amount of calcium carbonate used is 5-15 parts by weight; The amount of barium sulfate used is 5-15 parts by weight; The amount of reduced iron powder used is 21-31 parts by weight; The amount of graphite used is 4-14 parts by weight; The amount of high-alumina powder used is 11-21 parts by weight; The amount of potassium feldspar used is 48-58 parts by weight; The amount of molybdenum disulfide used is 2-8 parts by weight; The amount of antimony trisulfide used is 1-5 parts by weight.

10. The application according to claim 9, characterized in that, The amount of calcium carbonate used is 8-12 parts by weight; The amount of barium sulfate used is 8-12 parts by weight; The amount of reduced iron powder used is 24-28 parts by weight; The amount of graphite used is 8-11 parts by weight; The amount of high-alumina powder used is 14-18 parts by weight; The amount of potassium feldspar used is 51-55 parts by weight; The amount of molybdenum disulfide used is 3-7 parts by weight; The amount of antimony trisulfide used is 2-4 parts by weight.

11. The application according to claim 1, characterized in that, In step 1, the duration of the first and second stirring may be the same or different, each independently ranging from 2 to 5 minutes.

Citation Information

Patent Citations

  • High-friction synthetic brake shoe for high-power XHN5 locomotive, preparation method and application thereof

    CN102401052A

  • Rubber modified multielement resin material for disc brake pad and purposes

    CN107061574A

  • Preparation method of glass fiber reinforced ABS (Acrylonitrile Butadiene Styrene) composite material

    CN116535701A