A method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition (ALD) technology

By adjusting the initial atomic layer deposition cycle ratio of indium gallium oxide (IoO) films, the interface quality of IoO films was optimized, the film defect problem was solved, and high mobility and low cost IoO film deposition were achieved, which is suitable for 3D nanostructure semiconductor devices.

CN120026306BActive Publication Date: 2026-11-17SHANGHAI UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510394564.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-03-31
Publication Date
2026-11-17
Estimated Expiration
2045-03-31

AI Technical Summary

Technical Problem

In atomic layer deposition (ALD) technology, there are many film defects at the interface of indium gallium oxide (IGaO) films, resulting in poor mobility. Traditional processes cannot meet the requirements for uniform coverage and thickness control of 3D nanostructures.

Method used

By adjusting the precursor ratio in the initial atomic layer deposition cycle, the pulse ratio of indium source to gallium source was changed from the traditional 3:1 to 13:1, and the subsequent cycle ratio was adjusted to 3:1. This optimized the interface quality of the indium gallium oxide film, formed a dense indium-enriched seed layer, and reduced the random aggregation of gallium atoms.

Benefits of technology

It significantly improves the interface quality and mobility of indium gallium oxide thin films, increasing carrier mobility by 56.7% and reducing interface roughness by 22%, while maintaining compatibility with existing ALD production lines and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120026306B_ABST
    Figure CN120026306B_ABST
Patent Text Reader

Abstract

This invention provides a method for improving the interface quality of indium gallium oxide (IGO) thin films in atomic layer deposition (ALD) technology. By optimizing the precursor ratio in the initial cycle, the mobility of IGO thin-film transistors is significantly improved. Traditional experimental IGO deposition uses a fixed cycle ratio (e.g., In:Ga = 3:1), which suffers from numerous interface defects and low carrier mobility. This invention proposes adjusting the precursor ratio to 13:1 (e.g., In:Ga = 13:1) in the first ALD cycle. This enhances the uniformity of the initial nucleation stage, reduces interface defects, and maintains the conventional ratio (3:1) in subsequent cycles. Compared with existing technologies, the IGO thin film prepared by this invention has a 22% lower roughness and an approximately 56.7% higher transistor mobility. Furthermore, it exhibits strong process compatibility, requires no additional equipment investment, and is suitable for manufacturing high-performance semiconductor devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor thin film preparation technology, and in particular to a method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology. Background Technology

[0002] Indium (In)-based oxides have achieved great success in display applications due to their excellent mobility, uniformity, and superior optical transparency. Indium oxide thin films exhibit high mobility and high electron density due to the overlapping of isotopically diffused In orbitals, providing efficient electron penetration pathways and high oxygen vacancy defects. However, this also leads to incomplete channel shut-off and device instability. Studies have shown that these problems with indium oxide can be effectively addressed by doping with metal cations with high oxygen collection energies. Among these cation dopants, gallium (Ga) is considered a powerful In₂O₃ binder and carrier suppressor due to its small radius, high ionic potential, and high bonding energy with oxygen. Recently, oxides have attracted significant attention as next-generation channel materials for 3D DRAM, 3D NAND, and M3D (Mirauge3D) to meet the ever-growing demands of semiconductor chips under Moore's Law. For semiconductor applications, conventional physical vapor deposition (PVD) processes cannot meet the stringent requirements of 3D nanostructures, such as uniform coverage and controllable thickness in conformal deposition. Atomic layer deposition (ALD) technology, due to its unique self-limiting growth behavior, offers excellent uniformity and precise thickness control, enabling the embedding of oxide thin films in complex three-dimensional device structures. For example, CN112877674A discloses a method for growing Sn-doped Ga2O3 films with precisely controllable Sn content. The steps include: growing n1 cycles of Ga2O3 film; growing 1 cycle of SnO2 film; and growing n2 cycles of Ga2O3 film. Repeating this step multiple times yields a Sn-doped Ga2O3 film of a predetermined thickness. ALD deposition of the Sn-doped Ga2O3 film achieves atomic-level doping of Sn within the Ga2O3 film.

[0003] However, actual ALD deposition involves a process from nucleation to film formation, and is not self-limiting growth from the beginning, which leads to more film defects at the interface compared to the stable growth stage. Summary of the Invention

[0004] The purpose of this invention is to provide a method for improving the interface quality of indium gallium oxide (IGO) thin films in atomic layer deposition (ALD) technology in order to solve the above-mentioned problems. By adjusting the ratio of the first cycle, the problem of more thin film defects at the interface can be effectively solved. By adjusting the precursor ratio of the initial ALD cycle, the interface quality of indium gallium oxide (IGO) thin films can be improved and the mobility can be increased.

[0005] The objective of this invention is achieved through the following technical solution:

[0006] The purpose of this invention is to provide a method for improving the interface quality of indium gallium oxide (IGO) thin films in atomic layer deposition (ALD) technology. This method improves both the interface quality and mobility of IGO thin films, and includes the following steps:

[0007] Step 1: Perform the first atomic layer deposition (ALD) cycle on the substrate surface, with the pulse ratio of precursor A to precursor B being 13:1;

[0008] Step 2: Perform subsequent atomic layer deposition (ALD) cycles. In the subsequent ALD cycles, the pulse ratio of precursor A to precursor B is adjusted to 3:1.

[0009] Step 3: Repeat step 2 until the target film thickness is achieved to complete the indium gallium oxide film deposition;

[0010] Precursor A is an indium source, and precursor B is a gallium source.

[0011] Furthermore, a large cycle refers to N indium cycles (N=13 or 3) and one gallium cycle, which together constitute one large cycle.

[0012] Furthermore, the precursor A is dimethyl indium (DADI), and the precursor B is trimethyl gallium (TMGa).

[0013] Furthermore, in step one, the number of pulses for precursor A is 13, the number of pulses for precursor B is 1, and the single pulse duration for precursor A is 0.1 seconds, the pulse interval for precursor A is 10 seconds, the single pulse duration for precursor B is 0.05 seconds, and the pulse interval for precursor B is 10 seconds.

[0014] Furthermore, in step two, precursor A is pulsed 3 times, precursor B is pulsed 1 time, and the duration of a single pulse of precursor A is 0.1 seconds, with a pulse interval of 10 seconds. The duration of a single pulse of precursor B is 0.05 seconds, with a pulse interval of 10 seconds.

[0015] Furthermore, in step one, the deposition temperature of atomic layer deposition is 250°C, and the pressure in the reaction chamber is 0.1–10 Torr.

[0016] Furthermore, in step two, the deposition temperature of atomic layer deposition is 250°C, and the pressure in the reaction chamber is 0.1–10 Torr.

[0017] Furthermore, the substrate is a silicon wafer.

[0018] Furthermore, the substrate is cleaned before the first atomic layer deposition cycle is performed on the substrate surface.

[0019] Furthermore, after the first atomic layer deposition cycle, the root mean square roughness of the interface is 0.8–1.0 nm.

[0020] More preferably, after the first atomic layer deposition cycle, the root mean square roughness of the interface is 0.874 nm.

[0021] Furthermore, in step three, the target film thickness is 10–20 nm, and after the indium gallium oxide (IO) film deposition is completed, the carrier mobility of the IO film is 21–24 cm⁻¹. 2 / (V·s).

[0022] Compared with the prior art, the present invention has the following characteristics:

[0023] 1) In traditional ALD processes, a fixed precursor ratio (e.g., In:Ga = 3:1) easily leads to competitive adsorption of indium and gallium atoms during the initial nucleation stage, forming an uneven island-like growth structure, which in turn causes interface defects (such as voids or grain boundary dislocations). This invention adjusts the precursor ratio (In:Ga) of the first atomic layer deposition cycle to 13:1 (In:Ga), significantly increasing the pulse frequency of indium atoms (e.g., 13 pulses for TMI and 1 pulse for TMGa), allowing indium atoms to preferentially cover the substrate surface, forming a continuous and dense indium-enriched seed layer. This seed layer not only provides uniform nucleation sites for subsequent deposition but also suppresses the random aggregation of gallium atoms by reducing surface energy differences. Experiments show that the adjusted initial cycle can reduce the interface roughness (RMS) from 1.12 nm in the traditional process to 0.874 nm, a reduction of 22%. Atomic force microscopy (AFM) analysis shows that the optimized interface exhibits a highly smooth three-dimensional growth pattern, effectively reducing the density of interface traps caused by carrier scattering.

[0024] 2) The improved atomic layer deposition (ALD) method for indium gallium oxide (IGO) thin film interface quality directly enhances the electrical performance of the IGO film. The dense seed layer reduces the grain boundary barrier height, while the uniform indium distribution reduces the localized electronic state density, significantly improving the continuity of carrier migration paths. Hall effect testing shows that using the 13:1 / 3:1 cycling ratio of this invention, the carrier mobility of the IGO film increases from 10.3 cm⁻¹ in conventional processes. 2 / (V·s) increased to 23.84cm 2 / (V·s), an increase of 56.7%. This improvement is particularly significant in high-frequency devices.

[0025] 2) The core advantage of the improved indium gallium oxide (IGO) thin film interface quality method in this invention lies in its seamless compatibility with existing ALD production lines. Adjusting the cycle ratio requires no hardware modification; only software programming is needed to modify the precursor pulse sequence parameters (such as pulse count and timing). Mainstream ALD equipment (such as the Cambridge NanoTech Savannah series) fully supports 13:1 and 3:1 cycle switching in terms of pulse control accuracy (±0.01 seconds) and temperature control stability (±1℃). In practical verification, this method was used to continuously deposit 100 batches of IGO thin films on commercial ALD equipment, with a process repeatability deviation of less than 2% (mobility fluctuation range: 23.36~24.32cm). 2 The equipment maintenance cycle is consistent with traditional processes. Furthermore, since no new precursors or vacuum chamber modifications are required, the production cost increases by only about 1.5% (mainly due to minor adjustments in the indium source dosage), far lower than the 10%–20% cost increase of other interface optimization technologies (such as plasma processing or intercalation layer deposition). This allows the invention to be rapidly applied to large-scale mass production scenarios such as flexible display driver ICs and high-resolution OLED backplanes. Attached Figure Description

[0026] Figure 1 The diagrams show a comparison of the ALD loop of the present invention and the conventional method, where (a): Comparative Example 1, (b): Example 1;

[0027] Figure 2 The curves show the thin film mobility comparison between Example 1 and Comparative Example 1.

[0028] Figure 3 Here are the AFM topography diagrams of the interface, where (a): Comparative Example 1, (b): Example 1. Detailed Implementation

[0029] The present invention will now be described in detail with reference to specific embodiments, but this is by no means a limitation thereof. Any preparation methods, materials, structures, or compositional ratios not explicitly described in this technical solution are considered common technical features disclosed in the prior art.

[0030] Unless otherwise specified, the reagents, methods, instruments, and equipment used in this invention are conventional in the art. Unless otherwise specified, the reagents and materials used in the following examples are all commercially available.

[0031] In the following examples, atomic layer deposition was performed using an ALD device, specifically the Cambridge NanoTech Savannah series.

[0032] Example 1

[0033] like Figure 1 As shown, this embodiment provides a method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology, including the following steps:

[0034] 1. Clean the silicon wafer substrate using the RCA standard cleaning process, and place the cleaned silicon wafer substrate in the ALD reaction chamber;

[0035] 2. First cycle: Perform the first ALD large cycle on the substrate surface. The pulse ratio of precursor A (DADI) to precursor B (TMGa) is 13:1. TMI pulses 13 times (0.1 seconds / pulse, 10-second interval), followed by TMGa pulses once (0.05 seconds / pulse, 10-second interval).

[0036] 3. Subsequent Cycles: Perform subsequent atomic layer deposition cycles. In the subsequent atomic layer deposition cycle, the pulse ratio of precursor A (DADI) to precursor B (TMGa) is adjusted to 3:1, and the pulse ratio of TMI to TMGa is adjusted to 3:1. TMI pulses are performed 3 times (0.1 seconds / pulse, 10-second interval), followed by TMGa pulses once (0.05 seconds / pulse, 10-second interval), and this process is repeated 74 times.

[0037] Deposition parameters for the first and subsequent cycles: temperature 250℃, pressure 5 Torr, film thickness 15 nm; as shown in Table 1. Figure 2 , Figure 3 As shown, the test results are: mobility 23.89 cm. 2 / (V·s), interface RMS 0.87nm.

[0038] Comparative Example 1

[0039] like Figure 1 As shown, this comparative example provides a method for improving the interface quality of indium gallium oxide thin films using conventional atomic layer deposition technology. The difference between this method and the previous example lies in step 2; the other steps are the same as in Example 1. In this comparative example, step 2 is as follows:

[0040] 2. First cycle: Traditional 3:1 fixed cycle ratio, pulsed under the same parameters, the pulse ratio of precursor A (DADI) to precursor B (TMGa) is 3:1, DADI pulses 3 times (0.1 seconds / pulse, 10-second interval), followed by TMGa pulses 1 time (0.05 seconds / pulse, 10-second interval).

[0041] As shown in Table 1, Figure 2 , Figure 3 As shown, the test results are: mobility 10.8 cm. 2 / (V·s), interface RMS 1.18nm.

[0042] Table 1 shows the mobility and root mean square roughness (RMS) of the interface for Example 1 and Comparative Example 1.

[0043]

[0044] As shown in Table 1, in the traditional ALD process, a fixed precursor ratio of In:Ga = 3:1 easily leads to competitive adsorption of indium and gallium atoms in the initial nucleation stage, forming an uneven island-like growth structure, which in turn causes interface defects (such as voids or grain boundary dislocations). This invention adjusts the precursor ratio (In:Ga) of the first atomic layer deposition cycle to 13:1 (In:Ga), significantly increasing the pulse frequency of indium atoms (e.g., 13 pulses for TMI and 1 pulse for TMGa), allowing indium atoms to preferentially cover the substrate surface, forming a continuous and dense indium-enriched seed layer. This seed layer not only provides uniform nucleation sites for subsequent deposition but also suppresses the random aggregation of gallium atoms by reducing surface energy differences. Experiments show that the adjusted initial cycle can reduce the interface roughness (RMS) from 1.12 nm in the traditional process to 0.874 nm, a reduction of 22%. Atomic force microscopy (AFM) analysis shows that the optimized interface exhibits a highly smooth three-dimensional growth pattern, effectively reducing the density of interface traps caused by carrier scattering. This invention provides an improved method for improving the interface quality of indium gallium oxide (IGO) thin films in atomic layer deposition (ALD) technology. Optimized interface quality directly enhances the electrical properties of IGO films. A dense seed layer reduces the grain boundary barrier height, while a uniform indium distribution reduces the localized electronic state density, significantly enhancing the continuity of carrier migration paths. Hall effect measurements show that, using the 13:1 / 3:1 cycling ratio of this invention, the carrier mobility of the IGO film increases from 10.3 cm⁻¹ in conventional processes. 2 / (V·s) increased to 23.84cm 2 / (V·s), an increase of 56.7%.

[0045] Mainstream ALD equipment (such as the Cambridge NanoTech Savannah series) fully supports cyclic switching between 13:1 and 3:1 pulse control accuracy (±0.01 seconds) and temperature control stability (±1℃). In actual verification, this method was used to continuously deposit 100 batches of IGO films on commercial ALD equipment, with a process repeatability deviation of less than 2% (mobility fluctuation range: 23.36~24.32cm). 2 The equipment maintenance cycle is consistent with traditional processes. In addition, since there is no need to introduce new precursors or modify the vacuum chamber, the production cost increases by only about 1.5% (mainly due to fine-tuning of the indium source usage), which is far lower than the 10% to 20% cost increase of other interface optimization technologies (such as plasma treatment or intercalation layer deposition).

[0046] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition (ALD) technology, characterized in that, The method includes the following steps: Step 1: Perform the first atomic layer deposition cycle on the substrate surface, with the pulse ratio of precursor A to precursor B being 13:1; after the first atomic layer deposition cycle, the root mean square roughness of the interface is 0.8~1.0 nm. Step 2: Perform subsequent atomic layer deposition cycles. In the subsequent atomic layer deposition cycles, the pulse ratio of precursor A to precursor B is adjusted to 3:

1. Step 3: Repeat step 2 until the target film thickness is achieved to complete the indium gallium oxide film deposition; In step three, the target film thickness is 10–20 nm. After the indium gallium oxide (IoO) film deposition is completed, the carrier mobility of the IoO film is 21–24 cm⁻¹. 2 / (V·s); Precursor A is an indium source, and precursor B is a gallium source; The method adjusts the precursor ratio of the first atomic layer deposition cycle to 13:1, increases the pulse count of indium atoms, and enables indium atoms to preferentially cover the substrate surface, forming a continuous and dense indium-enriched seed layer.

2. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, The precursor A is dimethylindium, and the precursor B is trimethylgallium.

3. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, In step one, precursor A has 13 pulses and precursor B has 1 pulse. The duration of a single pulse of precursor A is 0.1 seconds and the pulse interval of precursor A is 10 seconds. The duration of a single pulse of precursor B is 0.05 seconds and the pulse interval of precursor B is 10 seconds.

4. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, In step two, precursor A is pulsed 3 times, precursor B is pulsed 1 time, and the pulse duration of precursor A is 0.1 seconds, with a pulse interval of 10 seconds. The pulse duration of precursor B is 0.05 seconds, with a pulse interval of 10 seconds.

5. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, In step one, the deposition temperature of atomic layer deposition is 250℃, and the pressure in the reaction chamber is 0.1~10 Torr.

6. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, In step two, the deposition temperature for atomic layer deposition is 250°C, and the pressure in the reaction chamber is 0.1~10 Torr.

7. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, The substrate is a silicon wafer.

8. The method for improving the interface quality of indium gallium oxide thin films in atomic layer deposition technology according to claim 1, characterized in that, The substrate is cleaned before the first atomic layer deposition cycle is performed on the substrate surface.

Citation Information

Patent Citations

  • Growth method of Sn-doped Ga2O3 film material with accurately controllable content

    CN112877674A

  • Thin film transistor channel layer preparation method and thin film transistor

    CN117198861A