A pipe fitting with shape memory function and its preparation method and application
By adding ethylene-octene copolymer, silica and other components to the PEXA pipe fittings to form a three-dimensional network structure, the problem of poor connection stability of PEXA pipe fittings is solved, and the shape memory function and aging resistance are improved.
Patent Information
- Application Number
- CN202510616350.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2025-08-29
- Estimated Expiration
- 2045-05-14
AI Technical Summary
The existing PEXA pipe fittings are complex in operation during the connection process, have poor connection stability, and are prone to loosening and leakage due to external forces or temperature changes.
Polyethylene is used as a matrix, combining ethylene-octene copolymer, silica, compatibilizer, vinyl compounds and polyethylene glycol diacrylate to form a three-dimensional network structure to improve shape memory function and aging resistance.
Pipe fittings are not prone to loosening and leaking when external forces or temperature changes, and the connection stability is improved, and are suitable for pipeline systems.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to a pipe fitting with shape memory function, a preparation method thereof and an application thereof. Background Art
[0002] In plastic piping systems, fittings are key components that connect pipes, and their performance directly affects the stability and reliability of the entire system. Currently, cross-linked polyethylene pipes are widely used in many fields due to their excellent heat resistance and corrosion resistance.
[0003] Pipe fittings are a crucial component of pipeline connections, and their connection methods often rely on a tight fit between the fitting and the pipe. However, existing PEXA fittings present several challenges during connection. For example, traditional connection methods are complex, require high technical skills, and are difficult to guarantee stability after connection. Furthermore, some fittings are susceptible to loosening and leakage when subjected to external forces or temperature fluctuations, impacting the normal operation of the pipeline system.
[0004] In view of this, this application is filed. Summary of the Invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a pipe fitting with shape memory function and its preparation method and application. The pipe fitting of the present invention has excellent shape recovery performance and aging resistance.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A pipe with shape memory function, comprising the following components in percentage by mass: 70-84% polyethylene, 5-15% ethylene-octene copolymer, 2-8% silicon dioxide, 2-5% compatibilizer, 1.5-2.5% vinyl compound, and 0.5-1.5% polyethylene glycol diacrylate;
[0008] The vinyl compound comprises a vinyl coupling agent and vinyl hydroxy silicone oil in a mass ratio of 1: (0.5-0.9).
[0009] The present invention combines the above-mentioned raw materials, takes polyethylene as the matrix, and, under the joint action of ethylene-octene copolymer, silicon dioxide, a compatibilizer, a vinyl compound, and polyethylene glycol diacrylate, significantly improves the shape memory function and aging resistance of the pipe fitting, so that the pipe fitting will not loosen or leak when subjected to external forces or temperature changes. The pipe fitting is very suitable for pipeline systems, especially for connecting various pipelines in the pipeline system.
[0010] Among them, the applicant of this application speculates that the present invention adds a vinyl coupling agent and vinyl hydroxy silicone oil in a mass ratio of 1: (0.5~0.9) to the formula system, and simultaneously adds polyethylene glycol diacrylate. The vinyl coupling agent improves the shape memory recovery ability of the material by enhancing the crosslinking degree and interfacial bonding strength of polyethylene, and makes the material have better aging resistance. The vinyl groups in the vinyl hydroxy silicone oil molecules cross-link with the vinyl groups in polyethylene or other chemical substances containing active hydrogen groups to form a three-dimensional network structure with the vinyl coupling agent and polyethylene glycol diacrylate. The double bonds of polyethylene glycol diacrylate may react when heated. Reversible breakage and recombination occur, and the hydroxyl groups of the vinyl hydroxy silicone oil can also form Si-O-Si bonds with the siloxane groups of the coupling agent through condensation reactions to enhance network stability. At the same time, the siloxane chains of the vinyl hydroxy silicone oil can reflect ultraviolet rays to a certain extent, and can adjust and improve the flexibility, thermal stability, ultraviolet resistance and aging resistance of polyethylene, so that the polyethylene can maintain good performance in complex environments, and the polyethylene can better maintain its shape when subjected to external forces, and restore its original shape after the external force is removed. It can also improve the stability of the polyethylene molecular chain and is not easily affected by aging factors, thereby improving its aging resistance.
[0011] The amount of polyethylene used is 70-84%, for example, it can be 70%, 72%, 73%, 75%, 76%, 78%, 80%, 82%, 84% or a range consisting of any two values therein.
[0012] The amount of the ethylene-octene copolymer is 5-15%, for example, 5%, 8%, 10%, 12%, 14%, 15% or a range consisting of any two of these values.
[0013] The amount of silicon dioxide is 2-8%, for example, 2%, 3%, 4%, 5%, 6%, 7%, 8% or a range consisting of any two of these values.
[0014] The amount of the compatibilizer is 2-5%, for example, 2%, 3%, 4%, 5% or a range consisting of any two of these values.
[0015] The amount of the vinyl compound is 1.5-2.5%, for example, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.5% or a range consisting of any two of these values.
[0016] The amount of polyethylene glycol diacrylate is 0.5-1.5%, for example, 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5% or a range consisting of any two of these values.
[0017] As an implementation scheme of the present application, it includes the following components in percentage by mass: 78~82% polyethylene, 8~10% ethylene-octene copolymer, 4~6% silica, 3~4% compatibilizer, 1.8~2.2% vinyl compound, and 0.8~1% polyethylene glycol diacrylate. In particular, when the amount of each raw material is within this range, the compatibility of each component is better, and the shape recovery performance and aging resistance can be more significantly improved.
[0018] As an embodiment of the present application, the polyethylene is high-density polyethylene (abbreviated as HDPE).
[0019] As an embodiment of the present application, the polyethylene has a melt index of 0.5~5g / 10min at 190°C and 2.16kg, for example, it can be 0.5g / 10min, 0.8g / 10min, 1g / 10min, 2g / 10min, 3g / 10min, 4g / 10min, 5g / 10min or a range consisting of any two values therein, and the test method is ISO1133-2011.
[0020] As an embodiment of the present application, the polyethylene has a melt index of 1-3 g / 10 min at 190° C. and 2.16 kg.
[0021] As an embodiment of the present application, the vinyl coupling agent includes at least one of vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, and vinyltrimethoxysilane.
[0022] As an embodiment of the present application, the vinyl content of the vinyl hydroxy silicone oil is 6-7 wt%, and the hydroxyl content is 5.5-6.5 wt%.
[0023] Among them, the vinyl content in vinyl hydroxy silicone oil can be tested according to the method in Appendix A of T / FSI 062-2021, and the hydroxyl content can be tested according to the method in Appendix A of T / FSI 062-2021.
[0024] As an embodiment of the present application, the ethylene-octene copolymer comprises a first ethylene-octene copolymer and a second ethylene-octene copolymer in a mass ratio of (3-7): (2-8);
[0025] The melt index of the first ethylene-octene copolymer at 190° C. and 2.16 kg is 0.5 to 2 g / 10 min, for example, 0.5 g / 10 min, 0.8 g / 10 min, 1 g / 10 min, 1.5 g / 10 min, 2 g / 10 min, or a range consisting of any two values thereof, and the test method is ISO1133-2011.
[0026] The melt index of the second ethylene-octene copolymer at 190° C. and 2.16 kg is 5 to 15 g / 10 min, for example, 5 g / 10 min, 6 g / 10 min, 8 g / 10 min, 10 g / 10 min, 12 g / 10 min, 15 g / 10 min, or a range consisting of any two values thereof, and the test method is ISO1133-2011.
[0027] The present invention utilizes two ethylene-octene copolymers (POE) with different melt indexes. The first POE has a lower melt index, promoting the formation of a more stable cross-linked network structure, while the second POE has a higher melt index, enhancing fluidity and improving processability. The combination of the two forms a microstructurally alternating "soft-hard" composite network. The high-melt index POE acts as the "soft segment," providing molecular chain sliding, while the low-melt index POE acts as the "hard segment," providing support for elastic recovery, significantly enhancing shape memory properties. Furthermore, the combination of the two facilitates more effective dispersion of other components and improves overall processability.
[0028] As an embodiment of the present application, the first ethylene-octene copolymer has a melt index of 0.5-1 g / 10 min at 190° C. and 2.16 kg.
[0029] As an embodiment of the present application, the second ethylene-octene copolymer has a melt index of 5 to 10 g / 10 min at 190° C. and 2.16 kg.
[0030] As an embodiment of the present application, the compatibilizer includes POE grafted glycidyl methacrylate.
[0031] As an embodiment of the present application, the POE grafted glycidyl methacrylate has a melt index of 3 to 5 g / 10 min at 190° C. and 2.16 kg, for example, it can be 3 g / 10 min, 3.5 g / 10 min, 4 g / 10 min, 4.5 g / 10 min, 5 g / 10 min or a range consisting of any two values therein, and the test method is ISO1133-2011.
[0032] As an embodiment of the present application, the average particle size of the silica is 0.5~20μm, for example, it can be 0.5μm, 1μm, 2μm, 4μm, 5μm, 6μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm or a range consisting of any two values therein.
[0033] As an embodiment of the present application, the average particle size of the silicon dioxide is 6 to 10 μm.
[0034] As an embodiment of the present application, it also includes an initiator with a mass percentage of 0.1 to 0.3%;
[0035] The initiator includes at least one of azobisisobutyronitrile, dibenzoyl peroxide, di-tert-amyl peroxide, dicumyl peroxide, and di-tert-butyl peroxide.
[0036] Preferably, the pipe fitting of the present invention may further include 0.1 to 10 parts of additives, wherein the additives include at least one of a lubricant, a colorant, an antioxidant, a weathering agent, a flame retardant, and an ultraviolet light absorber.
[0037] The pipe fittings of the present invention may include 0.1 to 2 parts of a colorant. Suitable colorants include, but are not limited to, carbon black, titanium dioxide, zinc sulfide, iron red, titanium yellow, and combinations thereof.
[0038] The pipe fitting of the present invention may include 0.1 to 2 parts of a lubricant. Suitable lubricants include, but are not limited to, polyethylene wax, fatty acid esters, hyperbranched amides, and combinations thereof.
[0039] The pipe fittings of the present invention may include 0.1 to 2 parts of an antioxidant, suitable antioxidants being thioester antioxidants, hindered phenol antioxidants, hydroxylamine antioxidants, phosphite antioxidants, phosphate antioxidants, and combinations thereof.
[0040] Preferably, the thioester antioxidant includes at least one of dialkyl thiodipropionate or pentaerythritol tetrakis (3-laurylthiopropionate).
[0041] Preferably, the hindered phenol antioxidant includes at least one of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 1,3,5-tris(4-tert-butyl-3-hydroxy-2,6-dimethylbenzyl)isocyanurate, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl ester, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate] or 3,9-bis[1,1-dimethyl-2-[(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl]-2,4,8,10-tetraoxaspiro[5.5]undecane.
[0042] Preferably, the hydroxylamine antioxidant includes bis(octadecyl)hydroxylamine.
[0043] Preferably, the phosphite antioxidant includes at least one of tris(2,4-di-tert-butylphenyl)phosphite and pentaerythritol bis(2,4-tert-butylphenyl)diphosphite.
[0044] Preferably, the phosphate antioxidant includes bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphate.
[0045] The pipe fittings of the present invention may include 0.1 to 2 parts of a weathering agent. Suitable weathering agents include, but are not limited to, hindered amine light stabilizers, benzotriazole ultraviolet light absorbers, and combinations thereof.
[0046] The pipe fittings of the present invention may include 0.1 to 10 parts of a flame retardant. Suitable flame retardants include, but are not limited to, brominated polymers (e.g., brominated polystyrene), metal dialkyl phosphites (e.g., aluminum tris(diethylphosphite)), metal hydroxides (e.g., magnesium hydroxide), aromatic phosphates (e.g., resorcinol di(diphenyl phosphate) and bisphenol A di(diphenyl phosphate), and combinations thereof.
[0047] The pipe of the present invention may include a UV absorber. Suitable UV absorbers include, but are not limited to, hydroxybenzophenones, hydroxybenzotriazoles, hydroxybenzotriazines, cyanoacrylates, nanoscale inorganic materials (eg, titanium oxide, cerium oxide, and zinc oxide), and combinations thereof.
[0048] The present invention also provides a method for preparing a pipe having a shape memory function, comprising the following steps:
[0049] Polyethylene, ethylene-octene copolymer, silicon dioxide, a compatibilizer, and polyethylene glycol diacrylate are uniformly mixed, and then other raw materials are added and extruded to obtain a pipe fitting with shape memory function.
[0050] The present invention also provides an application of a pipe fitting with shape memory function in the connection of a pipeline system.
[0051] The beneficial effects of the present invention are as follows: the present invention uses polyethylene as a matrix, and under the joint action of ethylene-octene copolymer, silicon dioxide, a compatibilizer, a vinyl compound, and polyethylene glycol diacrylate, significantly improves the shape memory function and aging resistance of the pipe fittings, so that the pipe fittings will not loosen or leak when subjected to external forces or temperature changes. The pipe fittings are very suitable for pipeline systems, especially for connecting various pipelines in the pipeline system. DETAILED DESCRIPTION
[0052] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments of this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0053] In this application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0054] In this application, when referring to numerical ranges, unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges subsumed therein.
[0055] In the present application, there is no particular limitation on the specific dispersion and stirring treatment methods.
[0056] Unless otherwise specified, the components, raw materials or instruments used in the embodiments and comparative examples of the present invention are all commercially available raw materials or instruments, and the components and raw materials used in each parallel experiment are all of the same kind.
[0057] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one such feature. In the description of the present invention, "plurality" means at least two, such as two, three, etc., unless otherwise specifically defined.
[0058] The raw materials used in the embodiments and comparative examples are described as follows:
[0059] Polyethylene: The melt index is 2.8 g / 10 min at 190°C and 21.6 kg. It is sourced from LG Chemical and is designated SL188.
[0060] POE-1 (ethylene-octene copolymer): melt index is 1.2 g / 10 min at 190°C and 2.16 kg. It is sourced from ExxonMobil and is designated Vistamaxx 3020FL.
[0061] POE-2 (ethylene-octene copolymer): melt index of 0.5 g / 10 min at 190°C and 2.16 kg. Source: DuPont, brand: Engage 8150.
[0062] POE-3 (ethylene-octene copolymer): melt index is 5 g / 10 min at 190°C and 2.16 kg. It is sourced from Dow and is designated Engage 8200.
[0063] POE-4 (ethylene-octene copolymer): melt index is 9.1 g / 10 min at 190°C and 2.16 kg. It is sourced from ExxonMobil and is designated Vistamaxx 6202.
[0064] POE-5 (ethylene-octene copolymer): melt index is 21 g / 10 min at 190°C and 2.16 kg. It is sourced from ExxonMobil and is designated Vistamaxx 6502.
[0065] POE-6 (ethylene-octene copolymer): melt index is 3.7 g / 10 min at 190°C and 2.16 kg. It is sourced from ExxonMobil and is designated Vistamaxx 3000.
[0066] POE grafted glycidyl methacrylate-1: The melt index is 3~5g / 10min at 190℃ and 2.16kg. It is sourced from Coase, brand W5A.
[0067] POE grafted glycidyl methacrylate-2: The melt index at 190°C / 2.16kg is 8~15g / 10min, sourced from Coase, brand W5D.
[0068] HDPE grafted maleic anhydride: from Coase, brand W1H.
[0069] Vinyltriethoxysilane: commonly available on the market.
[0070] Dibenzoyl peroxide: commonly available in the market.
[0071] Vinyl hydroxy silicone oil: vinyl content is 6~7wt%, hydroxyl content is 5.5~6.5wt%, sourced from Jipeng, brand GP-203.
[0072] Silica-1: average particle size 6 μm, derived from MacLean reagent, brand M757694.
[0073] Silica-2: average particle size 10 μm, derived from MacLean reagent, brand S817560.
[0074] Silica-3: average particle size 20 μm, derived from MacLean reagent, brand S757693.
[0075] Silica-4: average particle size 0.5 μm, derived from MacLean reagent, brand M964361.
[0076] Polyethylene glycol diacrylate: derived from MacLean reagent, brand P750153.
[0077] Unless otherwise specified, the components and raw materials used in the examples and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.
[0078] The following examples are provided to facilitate understanding of the present invention. These examples are not provided to limit the scope of the claims.
[0079] Example 1
[0080] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0081] The vinyl compound comprises vinyl triethoxysilane and vinyl hydroxy silicone oil in a mass ratio of 1:0.5.
[0082] The ethylene-octene copolymer comprises ethylene-octene copolymer-1 and ethylene-octene copolymer-3 in a mass ratio of 3:2.
[0083] The method for preparing the pipe with shape memory function comprises the following steps:
[0084] Polyethylene, ethylene-octene copolymer, silica, a compatibilizer, and polyethylene glycol diacrylate were mixed evenly, and the remaining raw materials were added. The mixture was extruded using an extruder to obtain a pipe fitting with a shape memory function (inner diameter of 16 mm, outer diameter of 19 mm). The temperatures of each section of the extruder were set to: 150°C for the first section, 160°C for the second section, 170°C for the third section, and 180°C for the fourth section. The die head temperature was 175°C, and the screw speed was 300 r / min.
[0085] Example 2
[0086] The difference between Example 2 and Example 1 is that the amounts of the raw materials are different, and the other aspects are the same.
[0087] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 80.78% polyethylene, 8% ethylene-octene copolymer, 4% silicon dioxide-1, 4% POE-grafted glycidyl methacrylate-1, 2.2% vinyl compound, 1% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0088] Example 3
[0089] The difference between Example 3 and Example 1 is that the amounts of the raw materials are different, and the other aspects are the same.
[0090] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 72.98% polyethylene, 15% ethylene-octene copolymer, 8% silicon dioxide-1, 2% POE-grafted glycidyl methacrylate-1, 1.5% vinyl compound, 0.5% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0091] Example 4
[0092] The difference between Example 4 and Example 1 is that the amounts of the raw materials are different, and everything else is the same.
[0093] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 83.98% polyethylene, 5% ethylene-octene copolymer, 2% silicon dioxide-1, 5% POE-grafted glycidyl methacrylate-1, 2.5% vinyl compound, 1.5% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0094] Example 5
[0095] The difference between Example 5 and Example 1 is that the mass ratio of vinyltriethoxysilane and vinylhydroxy silicone oil is different, and the other contents are the same.
[0096] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0097] Wherein, the vinyl compound includes vinyl triethoxysilane and vinyl hydroxy silicone oil in a mass ratio of 1:0.9.
[0098] Example 6
[0099] The difference between Example 6 and Example 1 is that the mass ratio of ethylene-octene copolymer-1 and ethylene-octene copolymer-3 is different, and the other contents are the same.
[0100] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0101] The ethylene-octene copolymer comprises ethylene-octene copolymer-1 and ethylene-octene copolymer-3 in a mass ratio of 7:8.
[0102] Example 7
[0103] The difference between Example 7 and Example 1 is that equal amounts of ethylene-octene copolymer-2 and ethylene-octene copolymer-4 are used to replace ethylene-octene copolymer-1 and ethylene-octene copolymer-3, respectively, and all other aspects are the same.
[0104] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0105] The ethylene-octene copolymer comprises ethylene-octene copolymer-2 and ethylene-octene copolymer-4 in a mass ratio of 3:2.
[0106] Example 8
[0107] The difference between Example 8 and Example 1 is that silica-2 is used instead of silica-1, and all other aspects are the same.
[0108] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-2, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0109] Example 9
[0110] The difference between Example 9 and Example 1 is that silica-3 is used instead of silica-1, and all other aspects are the same.
[0111] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-3, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0112] Example 10
[0113] The difference between Example 10 and Example 1 is that silica-4 is used instead of silica-1, and all other aspects are the same.
[0114] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silica-4, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0115] Example 11
[0116] The difference between Example 11 and Example 1 is that POE-grafted glycidyl methacrylate-2 is used instead of POE-grafted glycidyl methacrylate-1, and the other aspects are the same.
[0117] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-2, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0118] Example 12
[0119] The difference between Example 12 and Example 1 is that HDPE grafted maleic anhydride is used instead of POE grafted glycidyl methacrylate-1, and all other aspects are the same.
[0120] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% HDPE grafted maleic anhydride, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0121] Comparative Example 1
[0122] The difference between Comparative Example 1 and Example 1 is that the vinyl compound in Comparative Example 1 is a single vinyltriethoxysilane, and the other components are the same.
[0123] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl triethoxysilane, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0124] Comparative Example 2
[0125] The difference between Comparative Example 2 and Example 1 is that the vinyl compound in Comparative Example 2 is a single vinyl hydroxy silicone oil, and the other contents are the same.
[0126] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl hydroxy silicone oil, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0127] Comparative Example 3
[0128] The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 does not contain vinyl hydroxy silicone oil (the amount of vinyl hydroxy silicone oil is evenly distributed on polyethylene), and the other aspects are the same.
[0129] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.98% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.2% vinyl triethoxysilane, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0130] Comparative Example 4
[0131] The difference between Comparative Example 4 and Example 1 is that Comparative Example 4 does not contain vinyltriethoxysilane (the amount of vinyltriethoxysilane is evenly distributed on the polyethylene), and the other aspects are the same.
[0132] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 79.58% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 0.6% vinyl hydroxy silicone oil, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0133] Comparative Example 5
[0134] Comparative Example 5 differs from Example 1 in that the mass ratio of vinyltriethoxysilane to vinylhydroxysilicone oil is different, and all other aspects are the same.
[0135] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0136] The vinyl compound comprises vinyl triethoxysilane and vinyl hydroxy silicone oil in a mass ratio of 0.5:1.
[0137] Comparative Example 6
[0138] The difference between Comparative Example 6 and Example 1 is that the mass ratio of vinyltriethoxysilane and vinylhydroxy silicone oil is different, and the other contents are the same.
[0139] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0140] Wherein, the vinyl compound includes vinyl triethoxysilane and vinyl hydroxy silicone oil in a mass ratio of 1:0.2.
[0141] Comparative Example 7
[0142] The difference between Comparative Example 7 and Example 1 is that the ethylene-octene copolymer in Comparative Example 7 is a single ethylene-octene copolymer-1, and the other contents are the same.
[0143] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer-1, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0144] Comparative Example 8
[0145] The difference between Comparative Example 8 and Example 1 is that the ethylene-octene copolymer in Comparative Example 8 is a single ethylene-octene copolymer-3, and the other contents are the same.
[0146] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer-3, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0147] Comparative Example 9
[0148] The difference between Comparative Example 9 and Example 1 is that the ethylene-octene copolymer in Comparative Example 9 is a single ethylene-octene copolymer-5, and the other contents are the same.
[0149] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer-5, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0150] Comparative Example 10
[0151] The difference between Comparative Example 10 and Example 1 is that the ethylene-octene copolymer in Comparative Example 10 is a single ethylene-octene copolymer-6, and the other contents are the same.
[0152] A pipe fitting with a shape memory function comprises the following components in percentage by mass: 78.38% polyethylene, 10% ethylene-octene copolymer-6, 6% silicon dioxide-1, 3% POE-grafted glycidyl methacrylate-1, 1.8% vinyl compound, 0.8% polyethylene glycol diacrylate, and 0.02% dibenzoyl peroxide.
[0153] Test Case
[0154] Shape recovery rate: Place the pipe (initial inner diameter is D0) in a forced air oven and keep it at 120°C for 10 minutes. Use a mold to apply radial compression to the pipe to shrink the inner diameter to 80% of the original size (i.e., deformation D1 = 20% D0). Maintain the load for 5 minutes to fix the deformation. After removing the load, keep it at room temperature for 30 minutes, record the recovered size, and then heat it to 80°C and keep it for 15 minutes. Measure the final recovered size and record the inner diameter at this time as D2. Calculate the shape recovery rate.
[0155] Shape recovery rate = (D2-80%D0) / D1*100%.
[0156] Aging resistance: QUV accelerated aging test (UVB-313 lamp, 60℃ / 4h illumination + 50℃ / 4h condensation, cycle 500 hours).
[0157] The tensile strength before and after aging was tested, and the tensile strength retention was calculated. The tensile strength was tested according to ASTM-D638-10, with a tensile rate of 50 mm / min and room temperature (23±2°C).
[0158] Tensile strength retention rate = tensile strength before aging / tensile strength after aging × 100%.
[0159] Table 1
[0160]
[0161] It can be seen from Table 1 that the pipe fittings of the present invention have excellent shape recovery performance and aging resistance.
[0162] By comparing Example 1 with Comparative Examples 1 to 4, it can be seen that in the inventive system of the present invention, the vinyl coupling agent and vinyl hydroxy silicone oil described in the present invention have a significant synergistic effect in shape recovery performance and aging resistance. Under the synergy of the two, the shape recovery performance and aging resistance of the pipe fittings are significantly improved.
[0163] By comparing Example 1 with Comparative Examples 5 to 6, it can be seen that by controlling the mass ratio of the vinyl coupling agent to the vinyl hydroxy silicone oil to be 1:(0.5-0.9), the shape recovery performance and aging resistance are significantly improved.
[0164] By comparing Example 1 with Comparative Examples 7 to 10, it can be seen that the present invention uses the first ethylene-octene copolymer and the second ethylene-octene copolymer in a mass ratio of (3 to 7): (2 to 8), which significantly improves the shape recovery performance and aging resistance.
[0165] By comparing Examples 1-2 with Examples 3-4, it can be seen that the present invention improves the compatibility of the components by controlling the amount of each raw material to: 78-82% polyethylene, 8-10% ethylene-octene copolymer, 4-6% silica, 3-4% compatibilizer, 1.8-2.2% vinyl compound, and 0.8-1% polyethylene glycol diacrylate, which can further improve the shape recovery performance and aging resistance.
[0166] Comparison of Examples 1 and 8 to 10 shows that the shape recovery performance and aging resistance can be further improved by using silicon dioxide with an average particle size of 6 to 10 μm.
[0167] Comparing Example 1 with Example 12, it can be seen that the shape recovery performance and aging resistance can be further improved by using POE-grafted glycidyl methacrylate as a compatibilizer.
[0168] Comparing Example 1 with Example 11, it can be seen that controlling the melt index of POE-grafted glycidyl methacrylate to 3-5 g / 10 min at 190° C. and 2.16 kg can further improve the shape recovery performance and aging resistance.
[0169] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A pipe with shape memory function, characterized in that: The invention comprises the following components in percentage by mass: 70-84% polyethylene, 5-15% ethylene-octene copolymer, 2-8% silicon dioxide, 2-5% compatibilizer, 1.5-2.5% vinyl compound, 0.5-1.5% polyethylene glycol diacrylate, and 0.1-0.3% initiator; The vinyl compound includes a vinyl coupling agent and vinyl hydroxy silicone oil in a mass ratio of 1: (0.5-0.9); The vinyl content of the vinyl hydroxy silicone oil is 6-7 wt %, and the hydroxyl content is 5.5-6.5 wt %; The ethylene-octene copolymer comprises a first ethylene-octene copolymer and a second ethylene-octene copolymer in a mass ratio of (3-7): (2-8); The first ethylene-octene copolymer has a melt index of 0.5 to 2 g / 10 min at 190° C. and 2.16 kg; the second ethylene-octene copolymer has a melt index of 5 to 15 g / 10 min at 190° C. and 2.16 kg; The initiator includes at least one of azobisisobutyronitrile, dibenzoyl peroxide, di-tert-amyl peroxide, dicumyl peroxide, and di-tert-butyl peroxide.
2. The pipe with shape memory function according to claim 1, characterized in that: The vinyl coupling agent includes at least one of vinyltriethoxysilane, vinyltri(2-methoxyethoxy)silane, and vinyltrimethoxysilane.
3. The pipe with shape memory function according to claim 1, characterized in that: The first ethylene-octene copolymer has a melt index of 0.5 to 1.2 g / 10 min at 190° C. and 2.16 kg; and / or The second ethylene-octene copolymer has a melt index of 5-10 g / 10 min at 190° C. and 2.16 kg.
4. The pipe with shape memory function according to claim 1, characterized in that: The compatibilizer includes POE grafted glycidyl methacrylate.
5. The pipe with shape memory function according to claim 4, characterized in that: The POE grafted glycidyl methacrylate has a melt index of 3-5 g / 10 min at 190° C. and 2.16 kg.
6. The pipe with shape memory function according to claim 1, characterized in that: The average particle size of the silicon dioxide is 0.5-20 μm.
7. The method for preparing a pipe with shape memory function according to any one of claims 1 to 6, characterized in that: The following steps are involved: Polyethylene, ethylene-octene copolymer, silicon dioxide, a compatibilizer, and polyethylene glycol diacrylate are uniformly mixed, and then other raw materials are added and extruded to obtain a pipe fitting with shape memory function.
8. Use of the pipe fitting with shape memory function according to any one of claims 1 to 6 in connecting a pipeline system.
Citation Information
Patent Citations
PEXb pipe with high shape memory function
CN115490949A
Crosslinked polyolefin material as well as preparation method and application thereof
CN117362812A