A crystalline-amorphous composite Zr-Si-O barrier layer material, its preparation method, and its applications.
By preparing a crystalline-amorphous composite Zr-Si-O barrier layer material, the stability and adhesion problems of high-temperature infrared low emissivity coatings under high-temperature environments were solved, achieving a balance between high-temperature stability and low emissivity, making it suitable for barrier layers of high-temperature infrared low emissivity thin films.
Patent Information
- Application Number
- CN202510283963.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-11
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-03-11
AI Technical Summary
Existing high-temperature infrared low emissivity coatings with diffusion-blocking layers are prone to element diffusion, phase transition, and cracking under high-temperature conditions, leading to infrared function failure. Furthermore, the preparation process is complex and costly, making it difficult to meet the requirements of high-temperature stability and low emissivity.
A crystalline-amorphous composite Zr-Si-O barrier layer material is used to prepare zirconia grains and an amorphous SiO2 coating layer through electron beam evaporation, forming a regular crystal structure and Zr-O-Si bonds, which improves high-temperature stability and density, and has strong bonding force.
It achieves a balance between high-temperature stability and low emissivity. The surface of the barrier layer material is uniform and dense with good adhesion, which avoids element diffusion between the noble metal layer and the base metal and reduces the emissivity of the high-temperature infrared low emissivity film.
Smart Images

Figure CN120158710B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional coating materials technology, and specifically relates to a crystalline-amorphous composite Zr-Si-O barrier layer material, its preparation method, and its application. Background Technology
[0002] With the continuous upgrading of stealth fighters, the temperature resistance requirements for high-temperature infrared low-emissivity thin films on the rearward components of aircraft engines are constantly increasing, needing to reach temperatures above 900℃. Currently, high-temperature infrared low-emissivity thin films are typically coated on the surface of components made of Ni-based superalloys. To simultaneously meet the comprehensive performance requirements of high-temperature stability and ultra-low high-temperature infrared emissivity, noble metal thin films are usually used as the infrared stealth functional layer. Noble metals such as Pt / Pd possess high temperature, low emissivity, high melting point, and excellent oxidation resistance, which can meet the requirements of high temperature and low infrared emissivity. The commonly used preparation process is magnetron sputtering coating. However, when existing Pt / Pd and other noble metal coatings are used in the high-temperature environment above 900℃ of engines, element diffusion easily occurs between the noble metal layer and the base metal, leading to the disruption of infrared functional continuity and ultimately the loss of infrared stealth effect. Therefore, to prevent high-temperature diffusion between metals, a diffusion-blocking layer is needed.
[0003] The high-temperature infrared emissivity of noble metal thin films prepared by magnetron sputtering is closely related to the surface smoothness of the film and is mainly controlled by the surface smoothness of the substrate material. Therefore, to prepare high-performance low-emissivity coatings, a smooth and dense diffusion barrier layer is required. Furthermore, as an intermediate layer, the diffusion barrier layer needs to possess good high-temperature stability and high adhesion to both the substrate and the metal layer. Therefore, the composition design and fabrication process of the diffusion barrier layer are crucial for preparing high-temperature infrared low-emissivity coatings.
[0004] Depending on the composition of the diffusion barrier layer, current preparation processes for diffusion barrier layers in high-temperature infrared low-emissivity coatings include microcrystalline glass / ceramic coating sintering, magnetron sputtering, and plasma spraying. For example, patent CN201410173870.9 uses a microcrystalline glass sintering process to prepare a ZnO-Al2O3-SiO2 composite oxide as a diffusion barrier layer. The sintering temperature of this material is 850℃, but its actual temperature resistance only reaches 700℃. The sintering temperature is much higher than the operating temperature, making it unsuitable for high-temperature environments above 900℃, and its high-temperature stability is poor. For another example, patent CN201811422506.6 uses a plasma spraying process to prepare a YSZ ceramic diffusion barrier layer. The intermediate barrier layer prepared by plasma spraying is porous, has poor surface density, and typically has a high high-temperature emissivity (above 0.15), requiring additional surface treatment processes such as polishing. Furthermore, the high temperature of the plasma spraying coating process cannot meet the actual requirements of the parts. The preparation of composite oxide barrier layers using magnetron sputtering also has some drawbacks: First, magnetron sputtering is a low-temperature forming process, and the oxides prepared are usually amorphous or low-temperature stable crystalline forms, which are prone to phase transitions during high-temperature use, leading to film shrinkage and cracking. Furthermore, the oxide deposition rate using magnetron sputtering is low, and the process cycle is extremely long, which is not conducive to mass production.
[0005] In summary, the barrier layers prepared by existing processes suffer from poor long-term stability at high temperatures, poor surface density, high roughness, and are prone to cracking and phase transitions. This results in high emissivity of the high-temperature infrared low-emissivity thin film. Furthermore, the preparation process involves high temperatures, complex methods, long cycles, and high costs. Summary of the Invention
[0006] To address the technical problems raised in the background, the main objective of this invention is to provide a crystalline-amorphous composite Zr-Si-O barrier layer material, its preparation method, and its applications. The Zr-Si-O barrier layer material prepared by this invention has a uniform surface, a dense structure, good adhesion to the substrate and metal layer, and excellent high-temperature stability, which can overcome the shortcomings of existing barrier layer materials such as easy phase transformation and cracking at high temperatures.
[0007] To achieve the above objectives, the present invention provides a crystalline-amorphous composite Zr-Si-O barrier layer material, comprising zirconium oxide grains and amorphous SiO2, wherein the amorphous SiO2 covers the surface of the zirconium oxide grains to form a coating layer.
[0008] Furthermore, in the crystalline-amorphous composite Zr-Si-O barrier layer material, the atomic ratio of Zr to Si is 1 to 10:1.
[0009] Furthermore, the zirconium oxide grains are arranged in a tetragonal phase.
[0010] Furthermore, the zirconium oxide grains have a particle size of 10–200 nm.
[0011] Furthermore, the thickness of the crystalline-amorphous composite Zr-Si-O barrier layer material is 2–6 μm.
[0012] In another aspect, the present invention provides a method for preparing the aforementioned crystalline-amorphous composite Zr-Si-O barrier layer material, comprising the following steps:
[0013] Zirconia and quartz powder are mixed and pressed to obtain the target material;
[0014] When the electron beam evaporation system is evacuated to a preset vacuum level, the evaporation gun is turned on to preheat the target material.
[0015] The substrate is fed into the electron beam evaporation system for preheating. When the preset temperature is reached, the setting parameters of the electron beam evaporation system are adjusted to evaporate the target material to deposit a coating on the surface of the substrate. When the coating reaches the required thickness, the crystalline-amorphous composite Zr-Si-O barrier layer material is obtained.
[0016] Furthermore, in the target material, the atomic ratio of Zr to Si is 1 to 10:1.
[0017] Furthermore, during the target evaporation process, the electron beam bombardment current is 200–300 mA, and the ion source current is 3.5–4.5 mA.
[0018] Furthermore, the background vacuum of the electron beam evaporation system is ≤2×10⁻⁶. -3 Pa, working vacuum degree is 1×10 - 2 Pa ~ 5 × 10 -2 Pa.
[0019] Furthermore, the preset temperature of the substrate is 150-250℃.
[0020] In another aspect, the present invention provides the application of the above-mentioned crystalline-amorphous composite Zr-Si-O barrier layer material in high-temperature resistant, low-emissivity coatings.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention provides a crystalline-amorphous composite Zr-Si-O barrier layer material, prepared by electron beam evaporation. By controlling the process and component ratio, a crystalline-amorphous composite Zr-Si-O oxide thin film is prepared. Compared with existing technologies such as microcrystalline glass / ceramic coating sintering, magnetron sputtering, or plasma spraying, this method offers advantages such as fast oxide deposition rate, uniform and dense surface layer, low processing temperature, simple method, short cycle time, and low cost.
[0023] In the crystalline-amorphous composite Zr-Si-O barrier layer material of this invention, Zr-O forms regular grains arranged in a tetragonal phase. These zirconium oxide grains have a low thermal neutron absorption cross section, exhibiting superior resistance to high-temperature and high-pressure corrosion. Amorphous SiO2 covers the surface of the zirconium oxide grains, forming a coating layer that acts as a binder between the grains. Due to the presence of amorphous SiO2 filling the grain defects and interfaces, Zr-O-Si bonds are formed between the amorphous SiO2 and Zr elements. Through the interaction of the Zr-O-Si bonds and non-bridging siloxy groups (Si-O-), the interface energy is reduced, further improving the high-temperature stability of the crystalline-amorphous composite Zr-Si-O film. Furthermore, the presence of the amorphous SiO2 component improves the density of the composite oxide film and enhances its adhesion to the substrate and metal layer.
[0024] In summary, the Zr-Si-O barrier layer material of the present invention, which is a crystal-amorphous composite, can overcome the shortcomings of existing barrier layer materials such as high-temperature phase transition, cracking, and poor surface compactness, thus possessing both high-temperature stability and low emissivity performance. Attached Figure Description
[0025] Figure 1 The microstructure diagram of the crystalline-amorphous composite Zr-Si-O barrier layer material of Embodiment 1 of the present invention is shown;
[0026] Figure 2 The XRD analysis results of the crystalline-amorphous composite Zr-Si-O barrier layer material of Embodiment 1 of the present invention are shown.
[0027] Figure 3 The microstructure of the crystalline-amorphous composite Zr-Si-O barrier layer material of Embodiment 1 of the present invention after heat treatment at 900°C is shown.
[0028] Figure 4 A microstructure diagram of the ZrO2 barrier layer material of Comparative Example 1 of the present invention is shown;
[0029] Figure 5 The microstructure of the ZrO2 barrier layer material of Comparative Example 1 of the present invention after heat treatment at 900°C is shown. Detailed Implementation
[0030] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. Furthermore, regarding the numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included within this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range. The invention will now be described in detail with reference to embodiments.
[0031] To address the aforementioned problems, a first aspect of the present invention provides a crystalline-amorphous composite Zr-Si-O barrier layer material, comprising zirconium oxide grains and amorphous SiO2, wherein the amorphous SiO2 covers the surface of the zirconium oxide grains to form a coating layer.
[0032] In the crystalline-amorphous composite Zr-Si-O barrier layer material of the present invention, Zr-O forms regular grains. These zirconium oxide grains have a low thermal neutron absorption cross section, exhibiting superior resistance to high-temperature and high-pressure corrosion. Amorphous SiO2 covers the surface of the zirconium oxide grains, forming a coating layer that acts as a binder for the grains. Due to the presence of amorphous SiO2 filling the grain defects and interfaces, Zr-O-Si bonds are formed between the amorphous SiO2 and Zr elements. Through the interaction of Zr-O-Si bonds and non-bridging siloxy groups (Si-O-), the interface energy is reduced, further improving the high-temperature stability of the crystalline-amorphous composite Zr-Si-O film. Simultaneously, the presence of the amorphous Si-O component improves the density of the composite oxide film, resulting in good adhesion to the substrate and metal layer. Therefore, the barrier layer material of the present invention simultaneously possesses both high-temperature stability and low emissivity.
[0033] In a preferred embodiment of the present invention, the atomic ratio of Zr to Si in the crystalline-amorphous composite Zr-Si-O barrier layer material is 1 to 10:1. For example, it can be 1:1, 2:1, 3:1, 5:1, 6:1, 8:1, 9:1, or 10:1. More preferably, it is 1 to 3:1.
[0034] In a preferred embodiment of the present invention, the zirconia grains are arranged in a tetragonal phase; the grain size of the zirconia grains is 10–200 nm. For example, it can be 10 nm, 20 nm, 40 nm, 50 nm, 60 nm, 80 nm, 100 nm, 120 nm, 140 nm, 150 nm, 160 nm, 180 nm, or 200 nm.
[0035] To further improve the overall performance of the crystalline-amorphous composite Zr-Si-O barrier layer material, enabling it to simultaneously possess excellent high-temperature stability and low emissivity, in a preferred embodiment of the present invention, the thickness of the crystalline-amorphous composite Zr-Si-O barrier layer material is 2–6 μm. For example, it can be 2 μm, 3 μm, 4 μm, 5 μm, or 6 μm.
[0036] A second aspect of the present invention provides a method for preparing the aforementioned crystalline-amorphous composite Zr-Si-O barrier layer material, comprising the following steps:
[0037] Zirconia and quartz powder are mixed and pressed to obtain the target material;
[0038] When the electron beam evaporation system is evacuated to a preset vacuum level, the evaporation gun is turned on to preheat the target material.
[0039] The substrate is fed into the electron beam evaporation system for preheating. When the preset temperature is reached, the setting parameters of the electron beam evaporation system are adjusted to start evaporating the target material to deposit a coating on the surface of the substrate. When the coating reaches the required thickness, the crystalline-amorphous composite Zr-Si-O barrier layer material is obtained.
[0040] This invention employs electron beam physical vapor deposition to prepare a crystalline-amorphous composite Zr-Si-O barrier layer material. Compared with existing technologies such as microcrystalline glass / ceramic coating and sintering, magnetron sputtering, or plasma spraying, it has advantages such as fast oxide deposition rate, uniform and dense surface layer, low process temperature, simple method, short cycle, and low cost.
[0041] In a preferred embodiment of the present invention, the atomic ratio of Zr to Si in the target material is 1 to 10:1.
[0042] In some preferred embodiments of the present invention, during the target evaporation process, the electron beam bombardment current is 200–300 mA, and the ion source current is 3.5–4.5 mA; the background vacuum degree (preset vacuum degree) of the electron beam evaporation system is ≤2 × 10⁻⁶. -3 Pa, working vacuum degree is 1×10 -2 Pa ~ 5 × 10 -2 Pa; the preset temperature of the substrate is 150-250℃. By precisely controlling the process parameters of electron beam physical vapor deposition, the surface of the resulting crystalline-amorphous composite Zr-Si-O barrier layer material can be made denser and more uniform, and the amorphous-crystalline bonding force between materials can be higher, thereby further improving the high-temperature stability and low emissivity of the material.
[0043] In a third aspect of the invention, the application of the above-described crystalline-amorphous composite Zr-Si-O barrier layer material in a high-temperature resistant, low-emissivity coating is also provided.
[0044] For the reasons mentioned above, the crystalline-amorphous composite Zr-Si-O barrier layer material of the present invention is particularly suitable as a diffusion barrier layer in high-temperature resistant, low-emissivity coatings, to prevent elemental diffusion between the noble metal layer and the base metal at temperatures above 900°C, which would damage the infrared function.
[0045] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0046] Example 1
[0047] A crystalline-amorphous composite Zr-Si-O barrier layer material comprises zirconia grains and amorphous SiO2. The zirconia grains are dispersed within the amorphous SiO2, which covers the surface of the zirconia grains to form a coating layer. The zirconia grains are arranged in a tetragonal phase, with a zirconium to silicon ratio of 1:1. The grain size is 50 nm, and the barrier layer material has a thickness of 3 μm.
[0048] The material was prepared using electron beam physical vapor deposition, and the preparation process is as follows:
[0049] A columnar target is formed by uniformly mixing and pressing zirconium oxide and quartz powder, with an atomic ratio of Zr:Si of 1:1 in the target material;
[0050] The electron beam evaporation system was evacuated to a vacuum level of 1×10⁻⁶. -3 After Pa, turn on the evaporation gun to preheat the target material to 150°C; send the substrate into the electron beam evaporation system for preheating. When the workpiece reaches 150°C, adjust the system parameters (working vacuum 1×10⁻⁶). -2 (Pa, bombardment current 200mA, ion source current 4mA) to start evaporating the target material to deposit a coating on the substrate surface. When the coating reaches 3μm, the crystalline-amorphous composite Zr-Si-O barrier layer material is obtained.
[0051] The microstructure of the crystalline-amorphous composite Zr-Si-O barrier layer material prepared above was characterized and analyzed by XRD. Its microstructure is as follows: Figure 1 As shown, the grains are fine, uniformly distributed, and the surface is continuous, dense, and defect-free. XRD analysis results are as follows: Figure 2As shown, 30°, 35°, and 50° are characteristic peaks of tetragonal zirconia, while the 25° peak is a typical XRD characteristic peak of amorphous SiO2. Furthermore, the surface microstructure of the crystalline-amorphous composite Zr-Si-O barrier layer material was characterized after heat treatment at 900℃ for 30 hours, as shown in the figure. Figure 3 As shown, the results indicate that the zirconia grains increased in size after heat treatment, but the overall structure remained dense and continuous without any defects.
[0052] This invention further investigates the influence of the preparation process parameters on the performance of Zr-Si-O barrier layer materials, and provides crystalline-amorphous composite Zr-Si-O barrier layer materials in Examples 2 to 6. The process steps are the same as in Example 1, and the specific process parameters are shown in Table 1.
[0053] Table 1
[0054]
[0055]
[0056] The crystalline-amorphous composite Zr-Si-O barrier layer material prepared in Examples 1-6 above was used as the barrier layer for the high-temperature infrared low-emissivity thin film. The high-temperature infrared low-emissivity thin film consists of a substrate layer (Ni-based superalloy), a barrier layer, and a low-infrared emission surface layer (Pt noble metal) stacked sequentially from top to bottom. The high-temperature infrared low-emissivity thin film prepared above was subjected to performance testing and appearance observation; the test results are shown in Table 2.
[0057] Appearance: Observe the surface of the high-temperature infrared low emissivity thin film.
[0058] Tensile bond strength test method: GB / T 5210-2006- "Paints and varnishes pull-off adhesion test".
[0059] Blocking performance test method: After the high-temperature infrared low emissivity film is kept at 900℃ for 300h, the infrared emissivity is tested according to HB20540-2018- "Test method for infrared emissivity of stealth materials".
[0060] Thermal shock resistance test method: AETF 63A - Thermal shock test method for coatings. Specifically, the high-temperature infrared low emissivity film is heated from room temperature to 900°C and subjected to 300 cycles of air-cooling thermal shock. The appearance of the film is then observed. If no defects such as wrinkling, blistering, cracking, peeling, or detachment occur, it indicates that the film has excellent thermal shock resistance.
[0061] Heat resistance test method: After the film is kept at 900℃ for 300h, observe its appearance and test the tensile bond strength.
[0062] Table 2
[0063]
[0064] Visual inspection of the surface of the high-temperature infrared low-emissivity thin film of this embodiment revealed that the Pt-plated surface layer exhibited a silvery-white metallic luster, indicating good adhesion between the surface layer and the crystalline-amorphous Zr-Si-O barrier layer of this embodiment, with a smooth barrier layer material structure. Tensile bond strength testing showed excellent adhesion between the barrier layer and the surface layer, with a bond strength of 18–21 MPa, indicating superior mechanical properties of the high-temperature infrared low-emissivity thin film of this embodiment. When the high-temperature infrared low-emissivity thin film was heat-treated at 900℃ for 30 hours, the tensile bond strength between the barrier layer and the surface layer was tested, and no significant decrease in bond strength was observed. Simultaneously, no surface changes or cracking were observed. Thermal shock resistance testing showed no significant changes in the appearance of the high-temperature infrared low-emissivity thin film, with no wrinkling, blistering, or cracking observed. These performance tests demonstrate that the high-temperature infrared low-emissivity thin film of this embodiment exhibits excellent high-temperature stability, without cracking, blistering, or phase transitions occurring at high temperatures. In addition, according to the blocking performance test, the high-temperature infrared low emissivity film of this embodiment still has a low emissivity at high temperature, and its emissivity is ≤0.20.
[0065] Comparative Example 1
[0066] A ZrO2 barrier layer material was prepared using electron beam physical vapor deposition, and the preparation process is as follows:
[0067] Zirconia is fabricated into a cylindrical target;
[0068] The electron beam evaporation system was evacuated to a vacuum level of 1×10⁻⁶. -3 After Pa, turn on the evaporation gun to preheat the target material to 150°C; send the substrate into the electron beam evaporation system for preheating. When the workpiece reaches 150°C, adjust the system parameters (working vacuum 1×10⁻⁶). -2 (Pa, bombardment current 200mA, ion source current 4mA) to start evaporating the target material to deposit a coating on the substrate surface. When the coating reaches 3μm, the ZrO2 barrier layer material is obtained.
[0069] The microstructure of the ZrO2 barrier layer material prepared above was characterized as follows: Figure 4 As shown in the figure, the pure zirconium oxide crystals exhibit coarse grains and poor surface compactness. Furthermore, the surface microstructure of the ZrO2 barrier layer material after high-temperature treatment at 900℃ for 10 hours is characterized as follows: Figure 5As shown, the material cracks due to a significant phase change caused by heating. Consequently, when used as a barrier layer, it results in a high emissivity of the high-temperature infrared low-emissivity film, reaching 0.76.
[0070] In summary, the Zr-Si-O barrier layer material prepared by this invention exhibits a uniform surface, dense structure, good adhesion to the substrate and metal layer, and excellent high-temperature stability, thus overcoming the shortcomings of existing barrier layer materials such as susceptibility to phase transitions and cracking at high temperatures. When applied to high-temperature infrared low-emissivity thin films, this Zr-Si-O barrier layer material effectively prevents elemental diffusion between the metal layer and the substrate metal at high temperatures, effectively reducing the emissivity of the high-temperature infrared low-emissivity thin film at high temperatures.
[0071] The embodiments described above are merely illustrative of implementation methods of the present invention, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the present invention. The present invention can also be implemented in other specific ways or forms without departing from its spirit or essential characteristics. Therefore, the described embodiments should be considered illustrative rather than limiting in any respect. The scope of the present invention should be defined by the appended claims, and any variations equivalent to the intent and scope of the claims should also be included within the scope of the present invention.
Claims
1. A crystalline-amorphous composite Zr-Si-O barrier layer material, characterized in that, The material includes zirconium oxide grains and amorphous SiO2, wherein the amorphous SiO2 covers the surface of the zirconium oxide grains to form a coating layer; the atomic ratio of Zr to Si in the crystalline-amorphous composite Zr-Si-O barrier layer material is 1~10:
1. The crystalline-amorphous composite Zr-Si-O barrier layer material is prepared by the following method, including the following steps: Zirconia and quartz powder are mixed and pressed to obtain a target material; in the target material, the atomic ratio of Zr to Si is 1~10:1; When the electron beam evaporation system is evacuated to a preset vacuum level, the evaporation gun is turned on to preheat the target material. The substrate is fed into the electron beam evaporation system for preheating. When the preset temperature is reached, the setting parameters of the electron beam evaporation system are adjusted to start evaporating the target material to deposit a coating on the surface of the substrate. When the coating reaches the required thickness, the crystalline-amorphous composite Zr-Si-O barrier layer material is obtained.
2. The crystalline-amorphous composite Zr-Si-O barrier layer material according to claim 1, characterized in that, The zirconium oxide grains are arranged in a tetragonal phase, and the grain size of the zirconium oxide grains is 10~200nm.
3. The crystalline-amorphous composite Zr-Si-O barrier layer material according to claim 1, characterized in that, The thickness of the crystalline-amorphous composite Zr-Si-O barrier layer material is 2~6μm.
4. A method for preparing a crystalline-amorphous composite Zr-Si-O barrier layer material as described in any one of claims 1 to 3, characterized in that, Includes the following steps: Zirconia and quartz powder are mixed and pressed to obtain a target material; in the target material, the atomic ratio of Zr to Si is 1~10:1; When the electron beam evaporation system is evacuated to a preset vacuum level, the evaporation gun is turned on to preheat the target material. The substrate is fed into the electron beam evaporation system for preheating. When the preset temperature is reached, the setting parameters of the electron beam evaporation system are adjusted to start evaporating the target material to deposit a coating on the surface of the substrate. When the coating reaches the required thickness, the crystalline-amorphous composite Zr-Si-O barrier layer material is obtained.
5. The method for preparing the crystalline-amorphous composite Zr-Si-O barrier layer material according to claim 4, characterized in that, During the target material evaporation process, the electron beam bombardment current is 200~300mA, and the ion source current is 3.5~4.5mA.
6. The method for preparing the crystalline-amorphous composite Zr-Si-O barrier layer material according to claim 4, characterized in that, The background vacuum of the electron beam evaporation system is ≤2×10⁻⁶. -3 Pa, working vacuum degree is 1×10 -2 Pa~5×10 -2 Pa.
7. The method for preparing the crystalline-amorphous composite Zr-Si-O barrier layer material according to any one of claims 4 to 6, characterized in that, The preset temperature of the substrate is 150-250℃.
8. The application of a crystalline-amorphous composite Zr-Si-O barrier layer material as described in any one of claims 1 to 3 in high-temperature resistant, low-emissivity coatings.
Citation Information
Patent Citations
High-temperature-resisting, high-bonding-strength and low-infrared-emissivity composite coating and preparation method thereof
CN103963380A
High-temperature-resistant low-emissivity coating and preparation method thereof
CN109457210A
Preparation method for amorphous Al2O3 and superfine nanocrystalline-coated ZrO2 compound coating material
CN102912305A
Preparation method of Zr-Si-O amorphous protective coating for nuclear power
CN111206217A