A flame-retardant composite fiber fabric and its preparation method

By using a layered structure design and a gradient hot-pressing composite process, the problems of high combustion temperature, non-dense structure, and flame retardant shedding in flame-retardant composite fiber fabrics have been solved, resulting in reduced combustion temperature, improved tear resistance, and increased production efficiency.

CN120245550BActive Publication Date: 2026-11-17江苏合源纺织科技有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202510643929.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-05-19
Publication Date
2026-11-17
Estimated Expiration
2045-05-19

AI Technical Summary

Technical Problem

Existing flame-retardant composite fiber fabrics cannot reduce the burning temperature, have a loose structure, low production efficiency, are prone to flame retardant shedding, have poor washability, and feel stiff.

Method used

It adopts a layered structure design, with a microcapsule coating on the surface, a graphene-reinforced ceramic barrier in the middle layer, and flame retardants chemically bonded to the inner layer through plasma grafting technology, combined with a gradient hot-pressing composite process to form an integrated material.

Benefits of technology

It achieves a reduction in combustion temperature, prevents flame retardant from falling off, improves tear resistance and provides a soft, skin-friendly feel, and increases production efficiency by 30%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120245550B_ABST
    Figure CN120245550B_ABST
Patent Text Reader

Abstract

This invention discloses a flame-retardant composite fiber fabric and its preparation method. The invention relates to the field of flame-retardant composite fiber fabric technology and includes the following layered structure: A surface flame-retardant protective layer: prepared as a double-strand blended yarn using eddy spinning technology from aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber at a mass ratio of 4:1. The double-strand blended yarn density is 18-22 tex. The double-strand blended yarn is plain woven to form a base fabric. The surface of the base fabric is coated with a microcapsule coating containing a nitrogen-phosphorus-graphene composite flame retardant. The microcapsule coating thickness is 50-80 μm, and the microcapsule particle size distribution is 2-8 μm. This invention inhibits the combustion chain reaction by installing an outer layer of microcapsules that rupture upon contact with fire to release gaseous flame retardants. The middle layer of silicate colloids undergoes high-temperature carbonization to form a heat insulation barrier, combined with graphene to enhance thermal conductivity and dispersion. The inner layer of aluminum hydroxide particles decomposes upon heating, absorbing heat and releasing water vapor, thus reducing the combustion temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of flame-retardant composite fiber fabric technology, specifically to a flame-retardant composite fiber fabric and its preparation method. Background Technology

[0002] While natural fibers such as cotton and linen offer comfort, their limiting oxygen index (LOI) is typically below 21, making them highly flammable and fast-burning, thus failing to meet safety protection requirements. Synthetic fibers such as polyester and nylon are prone to melting and dripping at high temperatures, potentially causing secondary injuries. Flame-retardant composite fiber fabrics have been widely used in protective clothing, vehicle interiors, and public space decorations, but existing flame-retardant composite fiber fabrics cannot reduce the combustion temperature.

[0003] The existing defects of flame-retardant composite fiber fabrics are: 1. Patent document CN109338538A discloses a composite flame-retardant fabric fiber, "made of a blend of a first flame-retardant fabric fiber and a second flame-retardant fabric fiber, wherein the first flame-retardant fabric fiber is a blend of poly(terephthalamide) oxalate bis(imidazolium) metal-bonded fiber, polyamide fiber and calcium alginate fiber, and the second flame-retardant fabric fiber is a blend of phenolic fiber, polyester fiber and poly(isophthalamide) m-phenylenediamine fiber. This invention improves the flame-retardant performance of the fabric and also improves the durability of the flame-retardant performance." However, existing flame-retardant composite fiber fabrics cannot reduce the combustion temperature. 2. Patent document CN105274687A discloses a composite flame-retardant fabric fiber, "woven from a blend of a first flame-retardant fabric fiber and a second flame-retardant fabric fiber. The first flame-retardant fabric fiber is woven from a blend of poly(terephthalic acid) bis(imidazolium) metal-bonded fiber, kapok fiber, and polyamide fiber, while the second flame-retardant fabric fiber is woven from a blend of phenolic fiber, polyacrylonitrile fiber, and polyester fiber. This invention uses a blend of multiple fibers to create a fabric with good flame-retardant effect, high strength, suitability for wear, and good safety." However, the existing flame-retardant composite fiber fabrics are prone to detachment of the flame retardant accelerant. 3. Patent document CN103122517A discloses a flame-retardant and antibacterial composite fiber fabric. "This composite fiber is made by blending polyacrylonitrile carbon fiber, cotton fiber, corn fiber, aloe vera fiber, and hydroxyapatite. The weight percentage of each raw material is 20-30% polyacrylonitrile carbon fiber, 10-40% cotton fiber, 20-50% corn fiber, 5-15% aloe vera fiber, and 1-5% hydroxyapatite. This invention uses polyacrylonitrile carbon fiber with added hydroxyapatite, environmentally friendly cotton fiber, corn fiber, and a small amount of aloe vera fiber as raw materials to prepare the composite fiber fabric. Hydroxyapatite contains phosphorus atoms and has a certain flame-retardant ability. The resulting fiber fabric not only has the ability to adsorb metals but also increases the flame-retardant performance of the fabric. The fabric of this invention combines the advantages of each fiber, with a soft and comfortable texture, good breathability, high strength, good elasticity, and no skin irritation." However, existing flame-retardant composite fiber fabric processes suffer from poor washability and a stiff feel. 4. Patent document CN109130359A discloses a novel flame-retardant composite fiber fabric, "comprising: a fabric substrate layer (1), the fabric substrate layer (1) being made of modified aramid fiber and polylactic acid fiber blend, a flame-retardant fiber fabric layer (2) being disposed on the upper surface of the fabric substrate layer (1), a fireproof layer (3) being disposed on the upper surface of the flame-retardant fiber fabric layer (2), the fabric substrate layer (1), the flame-retardant fiber fabric layer (2), and the fireproof layer (3) being bonded together by an adhesive, a protective layer (4) being disposed on the lower surface of the fabric substrate layer (1), and a heat insulation layer being disposed on the lower surface of the protective layer (4). Through the above method, the present invention adopts an optimized structural design, using a flame-retardant fiber fabric as the outer layer, which has a long-lasting flame-retardant effect, and a fireproof layer as the inner layer, which has good high-temperature resistance, which can greatly improve the long-term flame-retardant performance of the fiber fabric." However, the existing flame-retardant composite fiber fabric has a non-dense structure and low production efficiency. Summary of the Invention

[0004] The purpose of this invention is to provide a flame-retardant composite fiber fabric and its preparation method, so as to solve the technical problem mentioned in the background art that the existing flame-retardant composite fiber fabrics cannot reduce the combustion temperature.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a flame-retardant composite fiber fabric, comprising the following layered structure: Surface flame-retardant protective layer: A double-strand blended yarn is prepared by eddy spinning technology using aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1. The density of the double-strand blended yarn is 18-22 tex. The double-strand blended yarn is woven into a base fabric through plain weave. The surface of the base fabric is coated with a microcapsule coating containing nitrogen, phosphorus and graphene composite flame retardant. The thickness of the microcapsule coating is 50-80 μm, and the microcapsule particle size distribution is 2-8 μm. Intermediate gradient barrier layer: a hexagonal honeycomb mesh structure is formed by interweaving basalt fibers and polyimide fibers through a three-dimensional warp knitting process. The mesh pore size of the hexagonal honeycomb mesh structure is 0.5-1.2mm. The pores of the mesh are filled with a zinc silicate borate composite flame retardant colloid. The solid content of the zinc silicate borate composite flame retardant colloid is ≥85%. The zinc silicate borate composite flame retardant colloid contains 0.8%-1.5% graphene oxide nanosheets and 2%-3% silicon carbide whiskers by mass. Inner functional composite layer: The double-sided mesh structure is formed by the circular knitting process of modified acrylonitrile fiber and viscose-based chitosan fiber with a mass ratio of 3:2. The fiber surface is grafted with nano-sized aluminum hydroxide and silica composite flame retardant particles through low temperature plasma treatment. The grafting density is 1200-1500 particles / μm², and the particle size is 50-150nm. The surface flame-retardant protective layer, the intermediate gradient barrier layer, and the inner functional composite layer are formed into an integrated material through a gradient hot-pressing composite process. The hot-pressing parameters are: temperature 185-195℃, pressure 8-12MPa, and holding time 30-45s.

[0006] Preferably, the nitrogen-phosphorus graphene composite flame retardant in the microcapsule coating is a composite of melamine polyphosphate and aluminum hypophosphite in a mass ratio of 7:3, and the graphene doping amount is 1.2%-1.8% of the total mass of the flame retardant. The microcapsule wall material adopts a polyurethane-polyurea-chitosan three-layer coating structure with a wall thickness of 0.5-1.2μm.

[0007] Preferably, the basalt fiber monofilament diameter of the intermediate gradient barrier layer is 9-12 μm, the polyimide fiber adopts a core-sheath structure, the sheath is a bromine-containing epoxy resin modified layer, the core is a polyimide bulk material, and the fiber breaking strength is ≥4.5 cN / dtex.

[0008] Preferably, the modification method of the modified acrylonitrile fiber includes: immersing the acrylonitrile precursor in an ethanol solution containing 2%-3% vinyltriethoxysilane for 30-45 minutes, pre-drying at 80°C, and then heat-curing at 160-180°C under nitrogen protection, resulting in a fiber limiting oxygen index (LOI) ≥ 32%.

[0009] Preferably, the low-temperature plasma treatment parameters are: power 400-600W, treatment time 3-5 minutes, working gas is a mixture of argon and oxygen with a volume ratio of 8:2, and vacuum degree is maintained at 50-80Pa.

[0010] Preferably, the preparation includes the following steps: Step 1: Preparation of the surface flame-retardant protective layer; Aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber are processed into 18.5 tex double-ply yarn through opening, carding, drawing, and vortex spinning processes, and then treated with a composite process of padding and spraying. Impregnated with a 15% nitrogen-phosphorus flame retardant, which is an emulsion of melamine polyphosphate and aluminum hypophosphite in a 7:3 ratio, with a roll-off rate of 75%-80%; After impregnation and pre-baking at 80℃, the microcapsule coating is loaded using electrostatic spraying technology with a spraying voltage of 45-50kV, and the coating weight gain rate is 8%-10%. After spraying, cure with hot air at 120-130℃ for 10-15 minutes to form a flame-retardant protective layer on the surface; Step 2: Forming the intermediate gradient barrier layer; Basalt fiber and polyimide fiber are three-dimensionally warp-knitted with a warp density of 58 yarns / cm and a weft density of 42 yarns / cm. The zinc silicate borate composite colloid has a solid content of 85%. The zinc silicate borate composite colloid is dispersed and mixed with graphene oxide and silicon carbide whiskers at high speed. The mesh pores are filled using a vacuum dispensing device, and the dispensing pressure is 0.3-0.5 MPa. Segmented curing at 135-145℃: first stage 40℃ / 20min, second stage 80℃ / 30min, third stage 120℃ / 45min to form an intermediate gradient barrier layer. Step 3: Inner functional composite layer processing; Modified acrylic fiber and viscose-based chitosan fiber are knitted on a 24-needle circular knitting machine to form a double-sided mesh fabric with an areal density of 180-220 g / m². A low-temperature plasma treatment system was used, in which aluminum hydroxide and silica suspension were introduced into the grafting cavity. The concentration of aluminum hydroxide and silica suspension was 8%-12%, and the particle deposition rate was controlled at 2-3 μm / min during the treatment.

[0011] Preferably, in step one, the pH value of the nitrogen-phosphorus flame retardant emulsion is adjusted to 4.8-5.2 by citric acid, and the emulsion viscosity is controlled at 120-150 mPa·s.

[0012] Preferably, in step two, the vacuum degree of the vacuum dispensing equipment is maintained at -0.08 to -0.1 MPa, and the colloid flowability index is: rotational viscometer value at 25°C ≤ 5000 cP.

[0013] Preferably, in the water-cooling and shaping process of step four, a gradient cooling mode is adopted: the temperature drops to 80°C within 5 seconds in the first stage, to 40°C within 10 seconds in the second stage, and then naturally cools to room temperature in the third stage.

[0014] Compared with the prior art, the beneficial effects of the present invention are: 1. This invention utilizes an outer layer of microcapsules that rupture upon contact with fire to release gaseous flame retardants, thereby inhibiting the combustion chain reaction. The middle layer of silicate colloid undergoes high-temperature carbonization to form a heat insulation barrier, which is combined with graphene to enhance thermal conductivity and dispersion. The inner layer of aluminum hydroxide particles decomposes upon heating, absorbing heat and releasing water vapor, thus reducing the combustion temperature.

[0015] 2. This invention achieves a rapid response mechanism that is triggered upon contact with a fire source by installing surface microcapsules, releasing flame-retardant gas within the first 3 seconds. The middle layer forms a graphene-reinforced ceramic barrier with a thermal conductivity of ≤0.15W / m·K at 800℃. The inner layer nanoparticle grafting technology ensures that the flame retardant shedding rate is <3% / 50 washes.

[0016] 3. This invention enhances tear resistance by installing a three-dimensional mesh intermediate layer, imparts antibacterial properties with the inner chitin fiber, and provides a soft, skin-friendly feel with the modified acrylonitrile fiber.

[0017] 4. This invention achieves chemical bonding between flame retardant and fiber by installing plasma grafting technology, avoiding the problem of detachment. The hot-pressing composite process simultaneously completes interlayer bonding and structural densification, improving production efficiency by 30%. Attached Figure Description

[0018] Figure 1 This is a front view structural diagram of the present invention; Figure 2 This is a cross-sectional structural diagram of the present invention.

[0019] In the diagram: 1. Surface flame-retardant protective layer; 2. Middle gradient barrier layer; 3. Inner functional composite layer. Detailed Implementation

[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] In the description of this invention, it should be noted that the terms "upper," "lower," "inner," "outer," "front end," "rear end," "both ends," "one end," and "the other end," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention. Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0022] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installed," "equipped with," "connected," etc., should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. Those skilled in the art can understand this according to the specific circumstances.

[0023] Example 1: An embodiment of the present invention: a flame-retardant composite fiber fabric comprising the following layered structure: a surface flame-retardant protective layer: a double-strand blended yarn prepared by eddy spinning technology from aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1, with a double-strand blended yarn density of 18-22 tex; the double-strand blended yarn is plain woven to form a base fabric; the surface of the base fabric is coated with a microcapsule coating containing a nitrogen-phosphorus-graphene composite flame retardant, the microcapsule coating thickness being 50 μm and the microcapsule particle size distribution being 2 μm; and an intermediate gradient barrier layer: a hexagonal honeycomb mesh structure formed by interlacing basalt fiber and polyimide fiber through a three-dimensional warp knitting process. The structure has a mesh size of 0.5-1.2 mm, and the pores are filled with a zinc silicate borate composite flame retardant colloid. The solid content of the zinc silicate borate composite flame retardant colloid is ≥85%, and 0.8%-1.5% (by mass) of graphene oxide nanosheets and 2%-3% (by mass) of silicon carbide whiskers are dispersed in the zinc silicate borate composite flame retardant colloid. The inner functional composite layer is formed by a circular knitting process using modified acrylonitrile fiber and viscose-based chitin fiber in a 3:2 mass ratio to form a double-sided mesh structure. The fiber surface is grafted with nano-sized aluminum hydroxide and silica composite flame retardant particles through low-temperature plasma treatment, with a grafting density of 1200-1500 particles / μm² and a particle size of 50-1 μm. 50nm; the surface flame-retardant protective layer, the intermediate gradient barrier layer, and the inner functional composite layer are formed into an integrated material through a gradient hot-pressing composite process. The hot-pressing parameters are: temperature 185-195℃, pressure 8-12MPa, and holding time 30-45s. The nitrogen-phosphorus graphene composite flame retardant in the microcapsule coating is a composite of melamine polyphosphate and aluminum hypophosphite, with a mass ratio of 7:3. The graphene doping amount is 1.2%-1.8% of the total mass of the flame retardant. The microcapsule wall material adopts a polyurethane-polyurea-chitosan three-layer coating structure with a wall thickness of 0.5-1.2μm. The basalt fiber monofilament diameter of the intermediate gradient barrier layer is 9-12μm, and the polyimide fiber is... The modified acrylonitrile fiber has a core-sheath structure, with the sheath being a bromine-containing epoxy resin modified layer and the core being a polyimide bulk material. The fiber breaking strength is ≥4.5cN / dtex. The modification method of the modified acrylonitrile fiber includes: immersing the acrylonitrile precursor in an ethanol solution containing 2%-3% vinyltriethoxysilane for 30-45 minutes, pre-drying at 80℃, and then heat-curing at 160-180℃ under nitrogen protection. The fiber limiting oxygen index (LOI) is ≥32. The low-temperature plasma treatment parameters are: power 400-600W, treatment time 3-5 minutes, working gas is a mixture of argon and oxygen with a volume ratio of 8:2, and vacuum degree maintained at 50-80Pa. The preparation steps include the following: Step 1: Preparation of the surface flame-retardant protective layer; Aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber are processed into 18.5 tex double-ply yarn through opening, carding, drawing, and vortex spinning processes, and then treated with a composite process of padding and spraying. Impregnated with a 15% nitrogen-phosphorus flame retardant, which is an emulsion of melamine polyphosphate and aluminum hypophosphite in a 7:3 ratio, with a roll-off rate of 75%-80%; After impregnation and pre-baking at 80℃, the microcapsule coating is loaded using electrostatic spraying technology with a spraying voltage of 45-50kV, and the coating weight gain rate is 8%-10%. After spraying, cure with hot air at 120-130℃ for 10-15 minutes to form a flame-retardant protective layer on the surface; Step 2: Forming the intermediate gradient barrier layer; Basalt fiber and polyimide fiber are three-dimensionally warp-knitted with a warp density of 58 yarns / cm and a weft density of 42 yarns / cm. The zinc silicate borate composite colloid has a solid content of 85%. The zinc silicate borate composite colloid is dispersed and mixed with graphene oxide and silicon carbide whiskers at high speed. The mesh pores are filled using a vacuum dispensing device, and the dispensing pressure is 0.3-0.5 MPa. Segmented curing at 135-145℃: first stage 40℃ / 20min, second stage 80℃ / 30min, third stage 120℃ / 45min to form an intermediate gradient barrier layer. Step 3: Inner functional composite layer processing; Modified acrylic fiber and viscose-based chitosan fiber are knitted on a 24-needle circular knitting machine to form a double-sided mesh fabric with an areal density of 180-220 g / m². A low-temperature plasma treatment system was used, in which aluminum hydroxide and silica suspension were introduced into the grafting cavity. The concentration of aluminum hydroxide and silica suspension was 8%-12%, and the particle deposition rate was controlled at 2-3 μm / min during the treatment process. In step one, the pH value of the nitrogen-phosphorus flame retardant emulsion is adjusted to 4.8-5.2 using citric acid, and the emulsion viscosity is controlled at 120-150 mPa·s. In step two, the vacuum degree of the vacuum dispensing equipment is maintained at -0.08 to -0.1 MPa, and the colloid flowability index is: rotational viscometer value at 25°C ≤ 5000 cP; In the water-cooling and shaping process described in step four, a gradient cooling mode is adopted: the temperature drops to 80°C within 5 seconds in the first stage, to 40°C within 10 seconds in the second stage, and then naturally cools to room temperature in the third stage.

[0024] Example 2: An embodiment of the present invention: a flame-retardant composite fiber fabric comprising the following layered structure: a surface flame-retardant protective layer: a double-strand blended yarn prepared by eddy spinning technology from aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1, with a double-strand blended yarn density of 18-22 tex; the double-strand blended yarn is plain woven to form a base fabric; the surface of the base fabric is coated with a microcapsule coating containing a nitrogen-phosphorus-graphene composite flame retardant, the microcapsule coating thickness being 60 μm and the microcapsule particle size distribution being 4 μm; and an intermediate gradient barrier layer: a hexagonal honeycomb mesh structure formed by interlacing basalt fiber and polyimide fiber through a three-dimensional warp knitting process. The structure has a mesh size of 0.5-1.2 mm, and the pores are filled with a zinc silicate borate composite flame retardant colloid. The solid content of the zinc silicate borate composite flame retardant colloid is ≥85%, and 0.8%-1.5% (by mass) of graphene oxide nanosheets and 2%-3% (by mass) of silicon carbide whiskers are dispersed in the zinc silicate borate composite flame retardant colloid. The inner functional composite layer is formed by a circular knitting process using modified acrylonitrile fiber and viscose-based chitin fiber in a 3:2 mass ratio to form a double-sided mesh structure. The fiber surface is grafted with nano-sized aluminum hydroxide and silica composite flame retardant particles through low-temperature plasma treatment, with a grafting density of 1200-1500 particles / μm² and a particle size of 50-1 μm. 50nm; the surface flame-retardant protective layer, the intermediate gradient barrier layer, and the inner functional composite layer are formed into an integrated material through a gradient hot-pressing composite process. The hot-pressing parameters are: temperature 185-195℃, pressure 8-12MPa, and holding time 30-45s. The nitrogen-phosphorus graphene composite flame retardant in the microcapsule coating is a composite of melamine polyphosphate and aluminum hypophosphite, with a mass ratio of 7:3. The graphene doping amount is 1.2%-1.8% of the total mass of the flame retardant. The microcapsule wall material adopts a polyurethane-polyurea-chitosan three-layer coating structure with a wall thickness of 0.5-1.2μm. The basalt fiber monofilament diameter of the intermediate gradient barrier layer is 9-12μm, and the polyimide fiber is... The modified acrylonitrile fiber has a core-sheath structure, with the sheath being a bromine-containing epoxy resin modified layer and the core being a polyimide bulk material. The fiber breaking strength is ≥4.5cN / dtex. The modification method of the modified acrylonitrile fiber includes: immersing the acrylonitrile precursor in an ethanol solution containing 2%-3% vinyltriethoxysilane for 30-45 minutes, pre-drying at 80℃, and then heat-curing at 160-180℃ under nitrogen protection. The fiber limiting oxygen index (LOI) is ≥32. The low-temperature plasma treatment parameters are: power 400-600W, treatment time 3-5 minutes, working gas is a mixture of argon and oxygen with a volume ratio of 8:2, and vacuum degree maintained at 50-80Pa. The preparation steps include the following: Step 1: Preparation of the surface flame-retardant protective layer; Aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber are processed into 18.5 tex double-ply yarn through opening, carding, drawing, and vortex spinning processes, and then treated with a composite process of padding and spraying. Impregnated with a 15% nitrogen-phosphorus flame retardant, which is an emulsion of melamine polyphosphate and aluminum hypophosphite in a 7:3 ratio, with a roll-off rate of 75%-80%; After impregnation and pre-baking at 80℃, the microcapsule coating is loaded using electrostatic spraying technology with a spraying voltage of 45-50kV, and the coating weight gain rate is 8%-10%. After spraying, cure with hot air at 120-130℃ for 10-15 minutes to form a flame-retardant protective layer on the surface; Step 2: Forming the intermediate gradient barrier layer; Basalt fiber and polyimide fiber are three-dimensionally warp-knitted with a warp density of 58 yarns / cm and a weft density of 42 yarns / cm. The zinc silicate borate composite colloid has a solid content of 85%. The zinc silicate borate composite colloid is dispersed and mixed with graphene oxide and silicon carbide whiskers at high speed. The mesh pores are filled using a vacuum dispensing device, and the dispensing pressure is 0.3-0.5 MPa. Segmented curing at 135-145℃: first stage 40℃ / 20min, second stage 80℃ / 30min, third stage 120℃ / 45min to form an intermediate gradient barrier layer. Step 3: Inner functional composite layer processing; Modified acrylic fiber and viscose-based chitosan fiber are knitted on a 24-needle circular knitting machine to form a double-sided mesh fabric with an areal density of 180-220 g / m². A low-temperature plasma treatment system was used, in which aluminum hydroxide and silica suspension were introduced into the grafting cavity. The concentration of aluminum hydroxide and silica suspension was 8%-12%, and the particle deposition rate was controlled at 2-3 μm / min during the treatment process. In step one, the pH value of the nitrogen-phosphorus flame retardant emulsion is adjusted to 4.8-5.2 using citric acid, and the emulsion viscosity is controlled at 120-150 mPa·s. In step two, the vacuum degree of the vacuum dispensing equipment is maintained at -0.08 to -0.1 MPa, and the colloid flowability index is: rotational viscometer value at 25°C ≤ 5000 cP; In the water-cooling and shaping process described in step four, a gradient cooling mode is adopted: the temperature drops to 80°C within 5 seconds in the first stage, to 40°C within 10 seconds in the second stage, and then naturally cools to room temperature in the third stage.

[0025] Example 3: An embodiment of the present invention: a flame-retardant composite fiber fabric comprising the following layered structure: a surface flame-retardant protective layer: a double-strand blended yarn prepared by eddy spinning technology from aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1, with a double-strand blended yarn density of 18-22 tex; the double-strand blended yarn is plain woven to form a base fabric; the surface of the base fabric is coated with a microcapsule coating containing a nitrogen-phosphorus-graphene composite flame retardant, the microcapsule coating thickness being 70 μm and the microcapsule particle size distribution being 6 μm; and an intermediate gradient barrier layer: a hexagonal honeycomb mesh structure formed by interlacing basalt fiber and polyimide fiber through a three-dimensional warp knitting process. The structure has a mesh size of 0.5-1.2 mm, and the pores are filled with a zinc silicate borate composite flame retardant colloid. The solid content of the zinc silicate borate composite flame retardant colloid is ≥85%, and 0.8%-1.5% (by mass) of graphene oxide nanosheets and 2%-3% (by mass) of silicon carbide whiskers are dispersed in the zinc silicate borate composite flame retardant colloid. The inner functional composite layer is formed by a circular knitting process using modified acrylonitrile fiber and viscose-based chitin fiber in a 3:2 mass ratio to form a double-sided mesh structure. The fiber surface is grafted with nano-sized aluminum hydroxide and silica composite flame retardant particles through low-temperature plasma treatment, with a grafting density of 1200-1500 particles / μm² and a particle size of 50-1 μm. 50nm; the surface flame-retardant protective layer, the intermediate gradient barrier layer, and the inner functional composite layer are formed into an integrated material through a gradient hot-pressing composite process. The hot-pressing parameters are: temperature 185-195℃, pressure 8-12MPa, and holding time 30-45s. The nitrogen-phosphorus graphene composite flame retardant in the microcapsule coating is a composite of melamine polyphosphate and aluminum hypophosphite, with a mass ratio of 7:3. The graphene doping amount is 1.2%-1.8% of the total mass of the flame retardant. The microcapsule wall material adopts a polyurethane-polyurea-chitosan three-layer coating structure with a wall thickness of 0.5-1.2μm. The basalt fiber monofilament diameter of the intermediate gradient barrier layer is 9-12μm, and the polyimide fiber is... The modified acrylonitrile fiber has a core-sheath structure, with the sheath being a bromine-containing epoxy resin modified layer and the core being a polyimide bulk material. The fiber breaking strength is ≥4.5cN / dtex. The modification method of the modified acrylonitrile fiber includes: immersing the acrylonitrile precursor in an ethanol solution containing 2%-3% vinyltriethoxysilane for 30-45 minutes, pre-drying at 80℃, and then heat-curing at 160-180℃ under nitrogen protection. The fiber limiting oxygen index (LOI) is ≥32. The low-temperature plasma treatment parameters are: power 400-600W, treatment time 3-5 minutes, working gas is a mixture of argon and oxygen with a volume ratio of 8:2, and vacuum degree maintained at 50-80Pa. The preparation steps include the following: Step 1: Preparation of the surface flame-retardant protective layer; Aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber are processed into 18.5 tex double-ply yarn through opening, carding, drawing, and vortex spinning processes, and then treated with a composite process of padding and spraying. Impregnated with a 15% nitrogen-phosphorus flame retardant, which is an emulsion of melamine polyphosphate and aluminum hypophosphite in a 7:3 ratio, with a roll-off rate of 75%-80%; After impregnation and pre-baking at 80℃, the microcapsule coating is loaded using electrostatic spraying technology with a spraying voltage of 45-50kV, and the coating weight gain rate is 8%-10%. After spraying, cure with hot air at 120-130℃ for 10-15 minutes to form a flame-retardant protective layer on the surface; Step 2: Forming the intermediate gradient barrier layer; Basalt fiber and polyimide fiber are three-dimensionally warp-knitted with a warp density of 58 yarns / cm and a weft density of 42 yarns / cm. The zinc silicate borate composite colloid has a solid content of 85%. The zinc silicate borate composite colloid is dispersed and mixed with graphene oxide and silicon carbide whiskers at high speed. The mesh pores are filled using a vacuum dispensing device, and the dispensing pressure is 0.3-0.5 MPa. Segmented curing at 135-145℃: first stage 40℃ / 20min, second stage 80℃ / 30min, third stage 120℃ / 45min to form an intermediate gradient barrier layer. Step 3: Inner functional composite layer processing; Modified acrylic fiber and viscose-based chitosan fiber are knitted on a 24-needle circular knitting machine to form a double-sided mesh fabric with an areal density of 180-220 g / m². A low-temperature plasma treatment system was used, in which aluminum hydroxide and silica suspension were introduced into the grafting cavity. The concentration of aluminum hydroxide and silica suspension was 8%-12%, and the particle deposition rate was controlled at 2-3 μm / min during the treatment process. In step one, the pH value of the nitrogen-phosphorus flame retardant emulsion is adjusted to 4.8-5.2 using citric acid, and the emulsion viscosity is controlled at 120-150 mPa·s. In step two, the vacuum degree of the vacuum dispensing equipment is maintained at -0.08 to -0.1 MPa, and the colloid flowability index is: rotational viscometer value at 25°C ≤ 5000 cP; In the water-cooling and shaping process described in step four, a gradient cooling mode is adopted: the temperature drops to 80°C within 5 seconds in the first stage, to 40°C within 10 seconds in the second stage, and then naturally cools to room temperature in the third stage.

[0026] Example 4: An embodiment of the present invention: a flame-retardant composite fiber fabric, comprising the following layered structure: a surface flame-retardant protective layer: a double-strand blended yarn prepared by eddy spinning technology from aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1, with a double-strand blended yarn density of 18-22 tex; the double-strand blended yarn is plain woven to form a base fabric; the surface of the base fabric is coated with a microcapsule coating containing a nitrogen-phosphorus-graphene composite flame retardant, the microcapsule coating thickness is 80 μm, and the microcapsule particle size distribution is 8 μm; an intermediate gradient barrier layer: a hexagonal honeycomb grid structure formed by interweaving basalt fiber and polyimide fiber through a three-dimensional warp knitting process. The structure has a mesh size of 0.5-1.2 mm, and the pores are filled with a zinc silicate borate composite flame retardant colloid. The solid content of the zinc silicate borate composite flame retardant colloid is ≥85%, and 0.8%-1.5% (by mass) of graphene oxide nanosheets and 2%-3% (by mass) of silicon carbide whiskers are dispersed in the zinc silicate borate composite flame retardant colloid. The inner functional composite layer is formed by a circular knitting process using modified acrylonitrile fiber and viscose-based chitin fiber in a 3:2 mass ratio to form a double-sided mesh structure. The fiber surface is grafted with nano-sized aluminum hydroxide and silica composite flame retardant particles through low-temperature plasma treatment, with a grafting density of 1200-1500 particles / μm² and a particle size of 50-1 μm. 50nm; the surface flame-retardant protective layer, the intermediate gradient barrier layer, and the inner functional composite layer are formed into an integrated material through a gradient hot-pressing composite process. The hot-pressing parameters are: temperature 185-195℃, pressure 8-12MPa, and holding time 30-45s. The nitrogen-phosphorus graphene composite flame retardant in the microcapsule coating is a composite of melamine polyphosphate and aluminum hypophosphite, with a mass ratio of 7:3. The graphene doping amount is 1.2%-1.8% of the total mass of the flame retardant. The microcapsule wall material adopts a polyurethane-polyurea-chitosan three-layer coating structure with a wall thickness of 0.5-1.2μm. The basalt fiber monofilament diameter of the intermediate gradient barrier layer is 9-12μm, and the polyimide fiber is... The modified acrylonitrile fiber has a core-sheath structure, with the sheath being a bromine-containing epoxy resin modified layer and the core being a polyimide bulk material. The fiber breaking strength is ≥4.5cN / dtex. The modification method of the modified acrylonitrile fiber includes: immersing the acrylonitrile precursor in an ethanol solution containing 2%-3% vinyltriethoxysilane for 30-45 minutes, pre-drying at 80℃, and then heat-curing at 160-180℃ under nitrogen protection. The fiber limiting oxygen index (LOI) is ≥32. The low-temperature plasma treatment parameters are: power 400-600W, treatment time 3-5 minutes, working gas is a mixture of argon and oxygen with a volume ratio of 8:2, and vacuum degree maintained at 50-80Pa. The preparation steps include the following: Step 1: Preparation of the surface flame-retardant protective layer; Aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber are processed into 18.5 tex double-ply yarn through opening, carding, drawing, and vortex spinning processes, and then treated with a composite process of padding and spraying. Impregnated with a 15% nitrogen-phosphorus flame retardant, which is an emulsion of melamine polyphosphate and aluminum hypophosphite in a 7:3 ratio, with a roll-off rate of 75%-80%; After impregnation and pre-baking at 80℃, the microcapsule coating is loaded using electrostatic spraying technology with a spraying voltage of 45-50kV, and the coating weight gain rate is 8%-10%. After spraying, cure with hot air at 120-130℃ for 10-15 minutes to form a flame-retardant protective layer on the surface; Step 2: Forming the intermediate gradient barrier layer; Basalt fiber and polyimide fiber are three-dimensionally warp-knitted with a warp density of 58 yarns / cm and a weft density of 42 yarns / cm. The zinc silicate borate composite colloid has a solid content of 85%. The zinc silicate borate composite colloid is dispersed and mixed with graphene oxide and silicon carbide whiskers at high speed. The mesh pores are filled using a vacuum dispensing device, and the dispensing pressure is 0.3-0.5 MPa. Segmented curing at 135-145℃: first stage 40℃ / 20min, second stage 80℃ / 30min, third stage 120℃ / 45min to form an intermediate gradient barrier layer. Step 3: Inner functional composite layer processing; Modified acrylic fiber and viscose-based chitosan fiber are knitted on a 24-needle circular knitting machine to form a double-sided mesh fabric with an areal density of 180-220 g / m². A low-temperature plasma treatment system was used, in which aluminum hydroxide and silica suspension were introduced into the grafting cavity. The concentration of aluminum hydroxide and silica suspension was 8%-12%, and the particle deposition rate was controlled at 2-3 μm / min during the treatment process. In step one, the pH value of the nitrogen-phosphorus flame retardant emulsion is adjusted to 4.8-5.2 using citric acid, and the emulsion viscosity is controlled at 120-150 mPa·s. In step two, the vacuum degree of the vacuum dispensing equipment is maintained at -0.08 to -0.1 MPa, and the colloid flowability index is: rotational viscometer value at 25°C ≤ 5000 cP; In the water-cooling and shaping process described in step four, a gradient cooling mode is adopted: the temperature drops to 80°C within 5 seconds in the first stage, to 40°C within 10 seconds in the second stage, and then naturally cools to room temperature in the third stage.

[0027] Comparative experiment: The difference between Comparative Example 1 and Example 1 is that; Surface flame-retardant protective layer: A double-strand blended yarn is prepared by eddy spinning technology using aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1. The density of the double-strand blended yarn is 18-22 tex. The double-strand blended yarn is woven into a base fabric through plain weave. The surface of the base fabric is coated with a microcapsule coating containing nitrogen-phosphorus-graphene composite flame retardant. The thickness of the microcapsule coating is 50 μm, and the microcapsule particle size distribution is 2 μm.

[0028] The difference between Comparative Example 1 and Example 2 is that; Surface flame-retardant protective layer: A double-strand blended yarn is prepared by eddy spinning technology using aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1. The density of the double-strand blended yarn is 18-22 tex. The double-strand blended yarn is woven into a base fabric through plain weave. The surface of the base fabric is coated with a microcapsule coating containing nitrogen-phosphorus-graphene composite flame retardant. The thickness of the microcapsule coating is 60 μm, and the microcapsule particle size distribution is 4 μm.

[0029] The difference between Comparative Example 1 and Example 3 is that; Surface flame-retardant protective layer: A double-strand blended yarn is prepared by eddy spinning technology using aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1. The density of the double-strand blended yarn is 18-22 tex. The double-strand blended yarn is woven into a base fabric through plain weave. The surface of the base fabric is coated with a microcapsule coating containing nitrogen-phosphorus-graphene composite flame retardant. The thickness of the microcapsule coating is 70 μm, and the microcapsule particle size distribution is 6 μm.

[0030] The difference between Comparative Example 1 and Example 4 is that; Surface flame-retardant protective layer: A double-strand blended yarn is prepared by eddy spinning technology using aramid 1414 fiber and phosphorus-based copolymer flame-retardant polyester fiber in a mass ratio of 4:1. The density of the double-strand blended yarn is 18-22 tex. The double-strand blended yarn is woven into a base fabric through plain weave. The surface of the base fabric is coated with a microcapsule coating containing nitrogen-phosphorus-graphene composite flame retardant. The thickness of the microcapsule coating is 80 μm, and the microcapsule particle size distribution is 8 μm.

[0031] The flame-retardant composite fiber fabrics of Examples 1, 2, 3, and 4 of this invention were compared with traditional flame-retardant composite fiber fabrics (Comparative Example 1). According to GB / T 5455-2014 standard, a vertical burning test chamber was used to record the afterflame time and smoldering time. According to GB / T 3923.1-2013 standard, an electronic universal testing machine was used to stretch the specimens at a speed of (500±10) mm / min, and the breaking strength was recorded. The protective values ​​were calculated and statistically analyzed. The results are shown in Table 1.

[0032] As can be seen from the data in Table 1, the breaking strength coefficients of the flame-retardant composite fiber fabrics used in Examples 1, 2, 3, and 4 of this invention are 850 N / 5 cm, 980 N / 5 cm, 1020 N / 5 cm, 1060 N / 5 cm, and 1080 N / 5 cm, respectively, which are significantly higher than the breaking strength coefficient of the flame-retardant composite fiber fabric in Comparative Example 1. Therefore, it is shown that the toughness of the flame-retardant composite fiber fabric of this invention is significantly improved.

[0033] As can be seen from the data in Table 1, the afterflame time of the flame-retardant composite fiber fabrics in Examples 1, 2, 3, and 4 of the present invention is 10s, 6s, 4s, 3s, and 2s, respectively, which is significantly lower than the afterflame time of the flame-retardant composite fiber fabric in Comparative Example 1. Therefore, it is shown that the afterflame time of the flame-retardant composite fiber fabric of the present invention is significantly reduced.

[0034] As can be seen from the data in Table 1, the smoldering times of the flame-retardant composite fiber fabrics in Examples 1, 2, 3, and 4 of the present invention are 12s, 10s, 9s, 7s, and 5s, respectively, which are significantly lower than the smoldering time of the flame-retardant composite fiber fabric in Comparative Example 1. Therefore, it is shown that the smoldering time of the flame-retardant composite fiber fabric of the present invention is significantly reduced.

[0035] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A flame-retardant composite fiber fabric, characterized in that: It includes the following layered structures: Surface flame retardant protective layer (1): A double-strand blended yarn is prepared by eddy spinning technology from aramid 1414 fiber and phosphorus-based copolymer flame retardant polyester fiber with a mass ratio of 4:

1. The density of the double-strand blended yarn is 18-22 tex. The double-strand blended yarn is woven into a base fabric by plain weave. The surface of the base fabric is coated with a microcapsule coating containing nitrogen, phosphorus and graphene composite flame retardant. The thickness of the microcapsule coating is 50-80 μm and the microcapsule particle size distribution is 2-8 μm. Intermediate gradient barrier layer (2): a hexagonal honeycomb grid structure is formed by interweaving basalt fiber and polyimide fiber through three-dimensional warp knitting process. The mesh size of the hexagonal honeycomb grid structure is 0.5-1.2 mm. The pores of the grid are filled with zinc silicate borate composite flame retardant colloid. The solid content of the zinc silicate borate composite flame retardant colloid is ≥85%. The zinc silicate borate composite flame retardant colloid contains 0.8%-1.5% graphene oxide nanosheets and 2%-3% silicon carbide whiskers by mass. Inner functional composite layer (3): A double-sided mesh structure is formed by a circular knitting process of modified acrylonitrile fiber and viscose chitosan fiber with a mass ratio of 3:

2. The fiber surface is grafted with nano-sized aluminum hydroxide and silicon dioxide composite flame retardant particles through low temperature plasma treatment. The grafting density is 1200-1500 particles / μm², and the particle size is 50-150nm. The surface flame-retardant protective layer (1), the intermediate gradient barrier layer (2) and the inner functional composite layer (3) are formed into an integrated material through a gradient hot-pressing composite process. The hot-pressing parameters are temperature 185-195℃, pressure 8-12MPa and holding time 30-45s. The nitrogen-phosphorus graphene composite flame retardant in the microcapsule coating is a composite of melamine polyphosphate and aluminum hypophosphite in a mass ratio of 7:

3. The graphene doping amount is 1.2%-1.8% of the total mass of the flame retardant. The microcapsule wall material adopts a polyurethane-polyurea-chitosan three-layer coating structure with a wall thickness of 0.5-1.2μm. The basalt fiber monofilament diameter of the intermediate gradient barrier layer (2) is 9-12μm, the polyimide fiber adopts a core-sheath structure, the sheath is a bromine-containing epoxy resin modified layer, the core is a polyimide body material, and the fiber breaking strength is ≥4.5cN / dtex. The modification method of the modified acrylonitrile fiber includes: immersing the acrylonitrile precursor in an ethanol solution containing 2%-3% vinyltriethoxysilane by mass for 30-45 minutes, pre-drying at 80°C, and then heat-curing at 160-180°C under nitrogen protection, resulting in a fiber limiting oxygen index (LOI) ≥ 32%.

2. The flame-retardant composite fiber fabric according to claim 1, characterized in that: The parameters for low-temperature plasma treatment are: power 400-600W, treatment time 3-5 minutes, working gas is a mixture of argon and oxygen with a volume ratio of argon to oxygen of 8:2, and vacuum degree maintained at 50-80Pa.

Citation Information

Patent Citations

  • Inflaming-retardant and antimicrobial composite fiber fabric

    CN103122517A

  • Composite flame-retardant fabric fiber

    CN105274687A

  • Novel flame-retardant composite fiber fabric

    CN109130359A

  • Composite flame-retardant fabric fiber

    CN109338538A

  • Flame retardant anti-dripping blended fabric and preparation method thereof

    CN102634896A