A PE gasket film, a composite film, its preparation method, and its application.

The PE gasket film prepared by the three-layer structure and composite process solves the problems of excessive crystal point impurities and poor die-cutting of existing PE gasket films, and meets the safe and hygienic packaging requirements of high-end bottled beverages and medicine bottles.

CN120287690BActive Publication Date: 2026-11-17JIANGMEN HUALONG MEMBRANE MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510452044.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-04-10
Publication Date
2026-11-17
Estimated Expiration
2045-04-10

AI Technical Summary

Technical Problem

Existing PE gasket films suffer from numerous crystal impurities, poor die-cutting, easy air leakage, and stringing, making it difficult to meet the requirements for use in high-end bottled beverages and pharmaceutical bottles.

Method used

The PE gasket film adopts a three-layer structure. The outer, middle and inner layers are made of low-density polyethylene, metallocene low-density polyethylene and processing aids. It is prepared by co-extrusion process and combined with composite film technology, including a printing layer, a barrier layer and a heat-sealing layer. It is cured with a specific adhesive.

Benefits of technology

The prepared PE gasket film and composite film have few crystal points and good die-cutting, avoiding heat sealing leakage and ensuring safety and hygiene. They are suitable for packaging high-end bottled beverages and pharmaceutical bottles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005354822880000071
    Figure BDA0005354822880000071
  • Figure BDA0005354822880000111
    Figure BDA0005354822880000111
  • Figure BDA0005354822880000121
    Figure BDA0005354822880000121
Patent Text Reader

Abstract

This invention relates to the field of composite film technology, providing a PE gasket film, a composite film, its preparation method, and its applications. The PE gasket film provided by this invention comprises an outer layer, a middle layer, and an inner layer. The outer layer is prepared from low-density polyethylene, metallocene low-density polyethylene, and processing aids. The middle layer is prepared from low-density polyethylene, high-density polyethylene, and processing aids. The inner layer is prepared from low-density polyethylene, metallocene low-density polyethylene, and processing aids. The PE gasket film provided by this invention has fewer crystal point impurities, making it safer and more hygienic. It can prevent deterioration of the contents due to heat sealing leakage, and it is easy to die-cut without stringing during slicing, meeting the requirements for high-end bottled beverages, pharmaceutical bottles, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of composite membrane technology, and more particularly to a PE gasket film, a composite film, its preparation method, and its application. Background Technology

[0002] Bottle cap gaskets are components used inside bottle caps to provide sealing and cushioning. Gasket film is a crucial part of bottle cap gaskets; currently, PE film is commonly used, as it possesses good heat-sealing properties, flexibility, and a certain degree of barrier properties, and is often used as a heat-sealing layer.

[0003] However, current gasket films contain many crystal impurities, which can easily lead to air leakage after sealing, reducing shelf life. Some gasket films are also difficult to die-cut, resulting in gasket stringing that can fall into the bottle during capping, posing a safety hazard. They cannot meet the requirements for use in high-end bottled beverages, medicine bottles, etc. Summary of the Invention

[0004] In view of this, the present invention provides a PE gasket film, a composite film, a preparation method, and applications. The PE gasket film provided by the present invention has few crystal points, is easy to die-cut, and when used in gaskets, it can prevent heat-sealing leakage, and the slices do not produce strings, thus meeting the requirements for use in high-end bottled beverages, pharmaceutical bottles, etc.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:

[0006] A PE gasket film includes an outer layer, a middle layer and an inner layer stacked sequentially;

[0007] The raw materials for preparing the outer layer, by mass parts, include: 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.3-0.8 parts of processing aids;

[0008] The raw materials for preparing the middle layer, by mass parts, include: 20-70 parts of low-density polyethylene, 10-50 parts of high-density polyethylene, and 0.5-1 parts of processing aids;

[0009] The raw materials for preparing the inner layer, by mass parts, include: 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.5-1 part of processing aids.

[0010] Preferably, the outer, middle, and inner layers are made of low-density polyethylene with a melt index of 1.5–2.5 g / 10 min and a density of 0.92–0.93 g / cm³. 3 .

[0011] Preferably, the outer and inner layers are made of metallocene low-density polyethylene with a melt index of 1.5–2.5 g / 10 min and a density of 0.908–0.92 g / cm³. 3.

[0012] Preferably, the high-density polyethylene used in the middle layer has a melt index of 6–8.5 g / 10 min and a density of 0.955–0.965 g / cm³. 3 The processing aids used in the outer, middle, and inner layers have a melt index of 1.5–3 g / 10 min and a density of 0.91–0.925 g / cm³. 3 .

[0013] Preferably, the low-density polyethylene used in the outer, middle, and inner layers is grade 2420H; the metallocene low-density polyethylene used in the outer and inner layers is grade SP1520 or SP2320; the high-density polyethylene used in the middle layer is grade H377C; and the processing aid used in the outer, middle, and inner layers is grade PA0895LD.

[0014] The present invention also provides a method for preparing the PE gasket film described above, comprising the following steps:

[0015] The raw materials for the outer, middle, and inner layers are co-extruded in three layers to obtain the PE gasket film.

[0016] The present invention also provides a composite film comprising a printed layer, a barrier layer and a heat-sealing layer stacked sequentially; wherein the heat-sealing layer is the PE gasket film described in the above scheme or the PE gasket film prepared by the preparation method described in the above scheme.

[0017] Preferably, the printed layer is a polyester film; the barrier layer is an aluminum foil.

[0018] The present invention also provides a method for preparing the composite membrane described above, comprising the following steps:

[0019] After laminating the printed layer and the barrier layer with an adhesive, a first curing process is performed to obtain a printed layer / barrier layer composite film.

[0020] The printed layer / barrier layer composite film and the PE gasket film are bonded together with an adhesive and then subjected to a second curing process to obtain the composite film.

[0021] The present invention also provides the application of the PE gasket film or the composite film described in the above-described scheme in bottle cap gaskets.

[0022] This invention provides a PE gasket film, comprising an outer layer, a middle layer, and an inner layer stacked sequentially. By weight, the outer layer comprises 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.3-0.8 parts of processing aids. By weight, the middle layer comprises 20-70 parts of low-density polyethylene, 10-50 parts of high-density polyethylene, and 0.5-1 part of processing aids. By weight, the inner layer comprises 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.5-1 part of processing aids. This invention, by controlling the types and proportions of raw materials for the outer, middle, and inner layers, obtains a PE gasket film with fewer crystal point impurities, better die-cutting properties, and superior mechanical properties. Furthermore, the raw materials used in this invention are all low-crystal point and easily die-cuttable, further ensuring the low-crystal point and easily die-cutting characteristics of the PE gasket film. The results of the embodiments show that the PE gasket film provided by the present invention has fewer crystal point impurities, is safer and more hygienic, can avoid the deterioration of contents caused by heat sealing leakage, and will not produce stringing when slicing, thus meeting the usage requirements of high-end bottled beverages, medicine bottles, etc.

[0023] This invention also provides a composite film comprising a printed layer, a barrier layer, and a heat-sealing layer stacked sequentially; the heat-sealing layer is the PE gasket film described in the above-described scheme or the PE gasket film prepared by the preparation method described in the above-described scheme. The composite film provided by this invention has the characteristics of few crystal points, easy die-cutting, low density, and good barrier properties, and has broad application prospects in bottle cap gaskets. Detailed Implementation

[0024] This invention provides a PE gasket film, comprising an outer layer, a middle layer, and an inner layer stacked sequentially;

[0025] The raw materials for preparing the outer layer, by mass parts, include: 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.3-0.8 parts of processing aids;

[0026] The raw materials for preparing the middle layer, by mass parts, include: 20-70 parts of low-density polyethylene, 10-50 parts of high-density polyethylene, and 0.5-1 parts of processing aids;

[0027] The raw materials for preparing the inner layer, by mass parts, include: 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.5-1 part of processing aids.

[0028] Unless otherwise specified, all raw materials used in this invention are commercially available.

[0029] The outer layer is prepared from 30 to 80 parts by weight, specifically 30, 45, 55, 60, 68, or 80 parts of low-density polyethylene. The melt index of the low-density polyethylene used in the outer layer is preferably 1.5 to 2.5 g / 10 min, more preferably 2 g / 10 min, and the density is preferably 0.92 to 0.93 g / cm³. 3 More preferably, it is 0.924–0.925 g / cm³. 3 The preferred grade of the low-density polyethylene is 2420H, manufactured by CNOOC Shell, Lanzhou Petrochemical, or Maoming Petrochemical. In a specific embodiment of the invention, the 2420H low-density polyethylene used is from CNOOC Shell, with a melt index of 2 g / 10 min and a density of 0.924 g / cm³. 3 The low-density polyethylene used in this invention has the characteristics of having few crystal points and being easy to process.

[0030] Based on the weight percentage of low-density polyethylene used in the outer layer, the raw materials for preparing the outer layer include 10 to 30 parts of metallocene low-density polyethylene, specifically 12, 18, 20, 25, 28, or 30 parts; the melt index of the metallocene low-density polyethylene used in the outer layer is preferably 1.5 to 2.5 g / 10 min, more preferably 1.9 to 2 g / 10 min, and the density is preferably 0.908 to 0.920 g / cm³. 3 More preferably, it is 0.913–0.915 g / cm³. 3 The metallocene low-density polyethylene is preferably SP1520 or SP2320, both manufactured by Mitsui Chemicals. In a specific embodiment of the invention, the metallocene low-density polyethylene used is SP1520, with a melt index of 1.9 g / 10 min and a density of 0.913 g / cm³. 3 The metallocene low-density polyethylene used in this invention has the characteristics of few crystal points and high composite strength.

[0031] Based on the weight percentage of low-density polyethylene used in the outer layer, the raw materials for preparing the outer layer include 0.3 to 0.8 parts of processing aids, specifically 0.3, 0.5, or 0.8 parts; the melt index of the processing aids is preferably 1.5 to 3 g / 10 min, more preferably 2 to 2.1 g / 10 min, and the density is preferably 0.91 to 0.925 g / cm³. 3 More preferably, it is 0.915–0.920 g / cm³. 3 In a specific embodiment of the present invention, the preferred grade of the processing aid is PA0895LD, with a melt index of 2.1 g / 10 min and a density of 0.915 g / cm³. 3The manufacturer is Suzhou Constance Engineering Plastics Co., Ltd. The processing aids used in this invention can effectively reduce crystal points, reduce die buildup, lower extrusion pressure, and improve production efficiency.

[0032] The raw materials for preparing the middle layer, by mass, include 20 to 70 parts of low-density polyethylene, specifically 20, 25, 35, 43, 45, or 70 parts; the melt index, density, and grade of the low-density polyethylene used in the middle layer are preferably the same as those of the outer layer, and will not be repeated here.

[0033] Based on the weight percentage of low-density polyethylene used in the middle layer, the raw materials for preparing the middle layer include 10 to 50 parts of high-density polyethylene, specifically 15, 22, 35, 42, 48, or 50 parts; the melt index of the high-density polyethylene is preferably 6 to 8.5 g / 10 min, more preferably 7.5 to 8 g / 10 min, and the density is preferably 0.955 to 0.965 g / cm³. 3 More preferably, it is 0.961–0.963 g / cm³. 3 In a specific embodiment of the present invention, the high-density polyethylene is preferably of grade H377C, with a melt index of 7.5 g / 10 min and a density of 0.961 g / cm³. 3 The manufacturer is SCG of Thailand. The high-density polyethylene used in this invention has the characteristics of few crystal points, high stiffness, good die-cutting, and good processability.

[0034] Based on the weight percentage of low-density polyethylene used in the middle layer, the raw materials for preparing the middle layer include 0.5 to 1 part of processing aids, specifically 0.5, 0.8, or 1 part; the melt index, density, and grade of the processing aids used in the middle layer are preferably the same as those of the outer layer, and will not be elaborated here.

[0035] The raw materials for preparing the inner layer include 30 to 80 parts of low-density polyethylene by mass, specifically 30, 45, 55, 70, 72, or 80 parts; the melt index, density, and grade of the low-density polyethylene used in the inner layer are preferably the same as those of the outer layer, and will not be repeated here.

[0036] Based on the weight percentage of low-density polyethylene used in the inner layer, the raw materials for preparing the inner layer include 10 to 30 parts of metallocene low-density polyethylene, specifically 12, 15, 18, 20, 25, or 28 parts; the melt index, density, and grade of the metallocene low-density polyethylene used in the inner layer are preferably the same as those of the outer layer, and will not be repeated here.

[0037] Based on the weight percentage of low-density polyethylene used in the inner layer, the raw materials for preparing the inner layer include 0.5 to 1 part of processing aids, specifically 0.5, 0.8, or 1 part; the melt index, density, and grade of the processing aids used in the middle layer are preferably the same as those in the outer layer, and will not be elaborated here.

[0038] In this invention, the total mass of the raw materials used in the outer layer, middle layer and inner layer is calculated as 100%. The mass fraction of the raw materials in the outer layer is preferably 20-30%, the mass fraction of the middle layer is preferably 45-55%, and the mass fraction of the inner layer is preferably 25-30%.

[0039] In this invention, the thickness of the PE gasket film is preferably 150-190 μm, more preferably 170 μm, and the thickness ratio of the outer layer, middle layer and inner layer is preferably 1-3:2-4:1-3, specifically 3:4:3, 1:2:1, 1:3:1 or 1:4:1.

[0040] In this invention, the longitudinal tensile strength of the PE gasket film is preferably 22-23.5 MPa, the transverse tensile strength is preferably 20-21.5 MPa, the longitudinal elongation is preferably 410%-435%, the transverse tensile strength is preferably 535%-555%, the longitudinal elastic modulus is preferably 330-350%, the transverse elastic modulus is preferably 335-365 MPa, the wetting tension is preferably 40-50 mN / 15 mm, more preferably 46 mN / 15 mm; the number of crystal points larger than 0.6 mm is 0 per 1000 m. 2 The number of crystal points with a size greater than or equal to 0.3 mm and less than 0.6 mm is less than 20 per 1000 m. 2 The number of crystal points with a size greater than or equal to 0.2 mm and less than 0.3 mm is less than 40 per 1000 m. 2 .

[0041] The present invention also provides a method for preparing the PE gasket film described above, comprising the following steps:

[0042] The raw materials for the outer, middle, and inner layers are co-extruded in three layers to obtain the PE gasket film.

[0043] In this invention, the three-layer co-extrusion process specifically includes: feeding the raw materials for the preparation of the outer layer, middle layer and inner layer into the outer layer, middle layer and inner layer extruders respectively for melt plasticization; conveying the obtained adhesive liquid to the die head; extruding and blowing film to obtain a film bubble; after the film bubble is cooled by air, it is traction-rotated by a stabilizing ring and herringbone pattern; after the film bubble is flattened, it is traction-measured by guide rollers; then it is corona treated and trimmed; and then it is wound into the front and rear winding device by the lower traction clamping rollers to obtain the PE gasket film.

[0044] In this invention, the outer extruder, the middle extruder, and the inner extruder are preferably each provided with 5 heating zones, which are numbered 1 to 5 according to the order in which the raw materials pass through; the die head is provided with 4 heating zones, which are numbered 1 to 4 according to the order in which the raw materials pass through.

[0045] In this invention, the temperature of zone 1 of the outer extruder is preferably 160-175°C, more preferably 165-170°C; the temperature of zone 2 is preferably 165-180°C, more preferably 170-175°C; the temperature of zone 3 is preferably 165-180°C, more preferably 170-175°C; the temperature of zone 4 is preferably 160-170°C, more preferably 165°C; and the temperature of zone 5 is preferably 155-165°C, more preferably 160°C. Similarly, the temperature of zone 1 of the middle extruder is preferably 160-180°C, more preferably 165-175°C; the temperature of zone 2 is preferably 165-185°C, more preferably 170-180°C; and the temperature of zone 3 is preferably 160-165°C. The temperature ranges from 0 to 180°C, more preferably from 165 to 175°C. The temperature in zone 4 is preferably from 157 to 175°C, more preferably from 162 to 170°C. The temperature in zone 5 is preferably from 155 to 170°C, more preferably from 160 to 165°C. The temperature in zone 1 of the inner extruder is preferably from 165 to 180°C, more preferably from 170 to 175°C. The temperature in zone 2 is preferably from 173 to 183°C, more preferably from 175 to 178°C. The temperature in zone 3 is preferably from 167 to 177°C, more preferably from 170 to 172°C. The temperature in zone 4 is preferably from 160 to 175°C, more preferably from 163 to 170°C. The temperature in zone 5 is preferably from 160 to 170°C, more preferably from 165°C.

[0046] In this invention, the die head preferably has four heating zones, which are numbered 1 to 4 according to the order in which the raw materials pass through. The temperature of zone 1 is preferably 180 to 190°C, more preferably 180 to 185°C; the temperature of zone 2 is preferably 185 to 195°C, more preferably 185 to 190°C; the temperature of zone 3 is preferably 180 to 190°C, more preferably 185 to 188°C; and the temperature of zone 4 is preferably 177 to 187°C, more preferably 182°C.

[0047] In this invention, the extrusion pressure of the outer extruder is preferably 205-265 bar, more preferably 208-245 bar; the extrusion pressure of the middle extruder is preferably 280-345 bar, more preferably 320-345 bar; and the extrusion pressure of the inner extruder is preferably 255-325 bar, more preferably 265-295 bar.

[0048] In this invention, the PE gasket film is preferably produced in a Class 10,000 cleanroom.

[0049] The present invention also provides a composite film comprising a printed layer, a barrier layer and a heat-sealing layer stacked sequentially; wherein the heat-sealing layer is the PE gasket film described in the above scheme or the PE gasket film prepared by the preparation method described in the above scheme.

[0050] In this invention, the printed layer is preferably a polyester (PET) film; the barrier layer is preferably an aluminum foil.

[0051] In this invention, the thickness of the polyester film is preferably 12 μm, and the thickness of the aluminum foil is preferably 15 to 40 μm, more preferably 25 μm.

[0052] The present invention also provides a method for preparing the composite membrane described above, comprising the following steps:

[0053] After laminating the printed layer and the barrier layer with an adhesive, a first curing process is performed to obtain a printed layer / barrier layer composite film.

[0054] The printed layer / barrier layer composite film and the PE gasket film are bonded together with an adhesive and then subjected to a second curing process to obtain the composite film.

[0055] This invention involves bonding a printed layer and a barrier layer with an adhesive (referred to as the first bonding) followed by a first curing process to obtain a printed layer / barrier layer composite film. In this invention, the printed layer is preferably printed before bonding with the barrier layer, according to requirements. This invention does not have special requirements for the printing method; gravure printing, a process well-known to those skilled in the art, is sufficient. In this invention, the first bonding is preferably a dry bonding process, and the adhesive used in the first bonding is preferably a low-solvent-residue dry bonding adhesive, specifically, the two-component aluminum foil adhesive YH3066 / YH3066B from Beijing Gaomeng New Materials Co., Ltd. During use, YH3066, YH3066B, and ethyl acetate are mixed, with the preferred mass ratio of YH3066, YH3066B, and ethyl acetate being 10:1:10.8. The preferred adhesive application amount for the first bonding is 3.0–3.8 g / m³. 2 The preferred temperature for the first curing process is 50±5℃, and the preferred time is 72h.

[0056] After obtaining the printed layer / barrier layer composite film, the present invention further composites the printed layer / barrier layer composite film and the PE gasket film with an adhesive (denoted as the second composite) and then performs a second curing to obtain the composite film. In the present invention, the adhesive used in the second composite is preferably a solvent-free adhesive, specifically a commercially available two-component solvent-free polyurethane composite adhesive SF10M(A+B). During use, SF10MA and SF10MB are mixed, and the preferred mass ratio of SF10MA to SF10MB is 100:50. The preferred operating conditions for the second composite include: mixing temperature: SF10MA: 40℃, SF10MB: 35℃ (i.e., heating SF10MA to 40℃ and SF10MB to 35℃, then mixing them); coating temperature: 42℃, specifically controlling the temperature of each steel roller in the coating system to 42℃; and adhesive application rate: 1.5~2.5g / m³. 2 .

[0057] In this invention, the temperature of the second curing is preferably 50±5℃ and the time is preferably 72h; after the second curing is completed, the resulting composite film is preferably placed at room temperature for 12h and then cut.

[0058] This invention also provides the application of the PE gasket film or composite film described above in bottle cap gaskets; the PE gasket film or composite film provided by this invention can be specifically used in bottle cap gaskets for packaging bottles of juice, wine, dairy products, water, liquid foods, health products, and pharmaceuticals. This invention does not have special requirements for the application; any application well-known to those skilled in the art can be used.

[0059] The technical solutions of this invention will be clearly and completely described below with reference to the embodiments thereof. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0060] The sources and indicators of the raw materials used in the following examples and comparative examples are shown in Table 1.

[0061] Table 1. Raw Material Sources and Indicators

[0062]

[0063] Example 1

[0064] 1. Preparation of PE gasket film

[0065] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 20%, middle layer 55%, and inner layer 25%.

[0066] The raw materials for each layer are as follows, by mass: outer layer: low-density polyethylene 2420H: 80 parts, metallocene low-density polyethylene SP1520: 12 parts, processing aid PA0895LD: 0.8 parts;

[0067] Middle layer: Low-density polyethylene 2420H: 25 parts, high-density polyethylene H377C: 50 parts, processing aid PA0895LD: 0.5 parts;

[0068] Inner layer: Low-density polyethylene 2420H: 80 parts, metallocene low-density polyethylene SP1520: 12 parts, processing aid PA0895LD: 0.8 parts.

[0069] The preparation method of PE gasket film is as follows: The raw materials for the outer, middle, and inner layers are mixed in proportion by an automatic batching system and then fed into the outer, middle, and inner layer extruders. Under the push of the screw, the barrel is heated to molten state, and the shearing force of the screw promotes full mixing and plasticization of the raw materials. The molten and plasticized raw materials are fed into the die head, and a tubular film preform is formed through the annular die head. Compressed air is introduced to inflate it into a tubular film bubble, which is then cooled by air to fix its shape and size. The cylinder is flattened by the stabilizing ring and herringbone arrangement and then pulled by the guide roller. The thickness is monitored in real time by an online thickness gauge, and the automatic air ring automatically adjusts the parameters to control the thickness. Then, it enters the corona treatment device for corona treatment, and the edges are separated and fed into the front and rear winding devices for front and rear winding to obtain a 170μm PE gasket film. The temperature and pressure of the outer, middle, and inner layer extruders, as well as the temperature of the die head, are shown in Table 2.

[0070] Table 2 Extruder temperature and pressure, die temperature

[0071] temperature Zone 1 / ℃ Zone 2 / ℃ Zone 3 / ℃ 4 zones / ℃ 5 zones / ℃ Pressure / bar outer layer 165 170 175 165 160 208 Middle layer 175 180 175 170 165 345 Inner layer 170 175 170 163 160 265 mold head 185 190 185 182 / /

[0072] 2. Preparation of composite membranes

[0073] The composite film in this embodiment consists of a polyester film (printed layer), an aluminum foil (barrier layer), and a PE gasket film (heat-sealing layer) stacked sequentially.

[0074] The polyester film (PET) used was purchased from Anhui Guofeng Plastics Co., Ltd., with a thickness of 12μm; the aluminum foil used was purchased from Shanghai Shenhuo Aluminum Foil Co., Ltd., with a thickness of 25μm.

[0075] The composite film is prepared as follows: After the polyester film is gravure-printed according to requirements, it is laminated with aluminum foil using a dry lamination process. The adhesive used is YH8950 / YH8950B low-solvent residual dry lamination adhesive from Beijing Gaomeng New Materials Co., Ltd., with a weight ratio of YH8950:YH8950B:ethyl acetate = 10:1:10.8, and the adhesive application amount is 3.5g / m³.2 After lamination, the PET / AL composite film is cured in a curing chamber at 50℃±5℃ for 72 hours to obtain the PET / AL composite film.

[0076] The cured PET / AL composite film was laminated with the PE gasket film prepared in the previous steps using a solvent-free adhesive. The adhesive used was a two-component solvent-free polyurethane composite adhesive SF10M(A+B), with an adhesive ratio of SF10MA / SF10MB of 100:50 (by mass). The mixing temperature was SF10MA: 40℃, SF10MB: 35℃. The temperature of each steel roller in the coating system was set to 42℃, and the adhesive application rate was 2g / m³. 2 After compounding, the mixture is placed in a curing room at 50℃±5℃ for 72 hours, then removed and left at room temperature for 12 hours before being cut.

[0077] Example 2

[0078] 1. Preparation of PE gasket film

[0079] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 25%, middle layer 45%, and inner layer 30%.

[0080] The raw materials for each layer are as follows, by mass: outer layer: low-density polyethylene 2420H: 68 parts, metallocene low-density polyethylene SP1520: 20 parts, processing aid PA0895LD: 0.8 parts;

[0081] Middle layer: Low-density polyethylene 2420H: 70 parts, high-density polyethylene H377C: 15 parts, processing aid PA0895LD: 0.5 parts;

[0082] Inner layer: Low-density polyethylene 2420H: 68 parts, metallocene low-density polyethylene 1520: 20 parts, processing aid PA0895LD: 0.8 parts.

[0083] The preparation method is the same as in Example 1.

[0084] 2. A composite film was prepared using the PE gasket film prepared in Example 2, and the preparation method was the same as in Example 1.

[0085] Example 3

[0086] 1. Preparation of PE gasket film

[0087] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 30%, middle layer 40%, and inner layer 30%.

[0088] The raw materials for each layer are as follows, by weight: outer layer: low-density polyethylene 2420H: 30 parts, metallocene low-density polyethylene SP1520: 28 parts, processing aid PA0895LD: 0.8 parts;

[0089] Middle layer: Low-density polyethylene 2420H: 35 parts, high-density polyethylene H377C: 22 parts, processing aid PA0895LD: 0.5 parts;

[0090] Inner layer: Low-density polyethylene 2420H: 30 parts, metallocene low-density polyethylene 1520: 28 parts, processing aid PA0895LD: 0.8 parts.

[0091] The preparation method is the same as in Example 1.

[0092] 2. A composite film was prepared using the PE gasket film prepared in Example 3, and the preparation method was the same as in Example 1.

[0093] Example 4

[0094] 1. Preparation of PE gasket film

[0095] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 25%, middle layer 50%, and inner layer 25%.

[0096] The raw materials for each layer are as follows, by mass: outer layer: low-density polyethylene 2420H: 45 parts, metallocene low-density polyethylene SP1520: 25 parts, processing aid PA0895LD: 0.8 parts;

[0097] Middle layer: Low-density polyethylene 2420H: 58 parts, high-density polyethylene H377C: 42 parts, processing aid PA0895LD: 0.5 parts;

[0098] Inner layer: Low-density polyethylene 2420H: 45 parts, metallocene low-density polyethylene 1520: 25 parts, processing aid PA0895LD: 0.8 parts.

[0099] The preparation method is the same as in Example 1.

[0100] 2. A composite film was prepared using the PE gasket film prepared in Example 4, and the preparation method was the same as in Example 1.

[0101] Example 5

[0102] 1. Preparation of PE gasket film

[0103] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 20%, middle layer 60%, and inner layer 20%.

[0104] The raw materials for each layer are as follows, by mass: outer layer: low-density polyethylene 2420H: 55 parts, metallocene low-density polyethylene SP1520: 18 parts, processing aid PA0895LD: 0.8 parts;

[0105] Middle layer: Low-density polyethylene 2420H: 43 parts, high-density polyethylene H377C: 35 parts, processing aid PA0895LD: 0.5 parts;

[0106] Inner layer: Low-density polyethylene 2420H: 55 parts, metallocene low-density polyethylene 1520: 18 parts, processing aid PA0895LD: 0.8 parts.

[0107] The preparation method is the same as in Example 1.

[0108] 2. A composite film was prepared using the PE gasket film prepared in Example 5, and the preparation method was the same as in Example 1.

[0109] Example 6

[0110] 1. Preparation of PE gasket film

[0111] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 25%, middle layer 45%, and inner layer 30%.

[0112] The raw materials for each layer are as follows, by mass: outer layer: low-density polyethylene 2420H: 60 parts, metallocene low-density polyethylene SP1520: 30 parts, processing aid PA0895LD: 0.8 parts;

[0113] Middle layer: Low-density polyethylene 2420H: 20 parts, high-density polyethylene H377C: 48 parts, processing aid PA0895LD: 0.5 parts;

[0114] Inner layer: Low-density polyethylene 2420H: 72 parts, metallocene low-density polyethylene 1520: 15 parts, processing aid PA0895LD: 0.8 parts.

[0115] The preparation method is the same as in Example 1.

[0116] 2. A composite film was prepared using the PE gasket film prepared in Example 6, and the preparation method was the same as in Example 1.

[0117] Comparative Example 1

[0118] 1. Preparation of PE gasket film

[0119] The PE gasket film in this comparative example has a three-layer structure, consisting of an outer layer, a middle layer, and an inner layer. The weight percentage of the raw materials for each layer is as follows: outer layer 30%, middle layer 40%, and inner layer 30%. The sources and amounts of the raw materials used in the outer, middle, and inner layers are shown in Table 3.

[0120] Table 3 Comparative Example 1: Raw Material Sources and Usage

[0121]

[0122] The preparation method is the same as in Example 1. The temperatures and pressures of the outer, middle, and inner layer extruders, as well as the temperature of the die head, are shown in Table 4.

[0123] Table 4 Extruder temperature and pressure, die temperature

[0124] temperature Zone 1 / ℃ Zone 2 / ℃ Zone 3 / ℃ Zone 4 / ℃ 5 zones / ℃ Pressure / bar outer layer 168 175 170 164 160 235 Middle layer 170 175 172 165 160 295 Inner layer 167 172 165 160 160 330 mold head 183 188 182 180 / /

[0125] 2. Preparation of composite membranes

[0126] A composite membrane was prepared using the PE membrane prepared in Comparative Example 1, and the preparation method was the same as in Example 1.

[0127] Comparative Example 2

[0128] 1. Preparation of PE gasket film

[0129] The PE gasket film in this embodiment has a three-layer structure, namely an outer layer, a middle layer and an inner layer. The weight percentage of the raw materials in each layer is as follows: outer layer 30%, middle layer 40%, and inner layer 30%.

[0130] The raw materials for each layer are as follows, by mass: outer layer: low-density polyethylene 2420H: 25 parts, metallocene low-density polyethylene SP1520: 52 parts, processing aid PA0895LD: 0.8 parts;

[0131] Middle layer: Low-density polyethylene 2420H: 42 parts, high-density polyethylene H377C: 8 parts, processing aid PA0895LD: 0.5 parts;

[0132] Inner layer: Low-density polyethylene 2420H: 28 parts, metallocene low-density polyethylene SP1520: 65 parts, processing aid PA0895LD: 0.8 parts.

[0133] The preparation method is the same as in Example 1.

[0134] 2. A composite film was prepared using the PE gasket film prepared in Comparative Example 2, and the preparation method was the same as in Example 1.

[0135] Performance testing

[0136] The mechanical properties, wetting tension, and number of crystal points of the PE gasket films prepared in Examples 1-6 and Comparative Examples 1-2 were tested. The test methods and results are shown in Table 5.

[0137] Table 5. Performance Test Results of PE Gasket Film

[0138]

[0139] As can be seen from the data in Table 1, the PE gasket film prepared by this invention has good mechanical properties and wetting tension, and has few crystal points. In Comparative Example 1, the raw materials were changed, and although the PE film obtained had better mechanical properties, the number of crystal points increased significantly, and there were more impurities. In Comparative Example 2, the amount of SP1520 in the outer layer was increased and the amount of H377C in the middle layer was decreased, and the number of crystal points in the PE gasket film obtained also increased significantly, indicating that the ratio of raw materials has a significant impact on the performance of PE gasket film.

[0140] The mechanical and die-cutting properties of the composite films prepared in Examples 1-6 and Comparative Examples 1-2 were tested. The test methods and results are shown in Table 6.

[0141] Table 6. Performance Test Results of Composite Membrane

[0142]

[0143] As can be seen from the data in Table 6, the composite film provided by the present invention has good mechanical properties and does not fray during die cutting. The composite film in Comparative Example 1 has severe fraying, and the composite film in Comparative Example 2 also shows fraying, which cannot meet the requirements of bottle cap gaskets.

[0144] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A PE gasket film, characterized by, It includes an outer layer, a middle layer, and an inner layer that are stacked in sequence; The outer layer is prepared by the following raw materials in parts by weight: 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.3-0.8 parts of processing aids. The raw materials for preparing the middle layer, by mass parts, are: 20-70 parts of low-density polyethylene, 10-50 parts of high-density polyethylene, and 0.5-1 parts of processing aids; The raw materials for preparing the inner layer, by mass parts, are: 30-80 parts of low-density polyethylene, 10-30 parts of metallocene low-density polyethylene, and 0.5-1 part of processing aids; The low-density polyethylene used in the outer layer, the middle layer and the inner layer has a melt index of 1.5-2.5 g / 10 min and a density of 0.92-0.93 g / cm 3 ; the high-density polyethylene used in the middle layer has a melt index of 6-8.5 g / 10 min and a density of 0.955-0.965 g / cm 3 ; and the metallocene low-density polyethylene used in the outer layer and the inner layer has a melt index of 1.9-2.5 g / 10 min and a density of 0.908-0.92 g / cm 3 . The outer, middle, and inner layers are made of low-density polyethylene grade 2420H; the outer and inner layers are made of metallocene low-density polyethylene grade SP1520 or SP2320; the middle layer is made of high-density polyethylene grade H377C; the outer, middle, and inner layers are made of processing aid grade PA0895LD; the PE gasket film has a longitudinal tensile strength of 22~23.5MPa, a transverse tensile strength of 20~21.5MPa, a longitudinal elongation of 410%~435%, a transverse elongation of 535%~555%, a longitudinal modulus of elasticity of 330~350MPa, and a transverse modulus of elasticity of 335~365MPa.

2. The PE spacer film according to claim 1, characterized in that, The outer layer, the middle layer and the inner layer adopt a processing aid with a melt index of 1.5-3 g / 10 min and a density of 0.91-0.925 g / cm 3 .

3. The method of producing a PE spacer film according to any one of claims 1 to 2, characterized by, Includes the following steps: The raw materials for the outer, middle, and inner layers are co-extruded in three layers to obtain the PE gasket film.

4. A composite film, characterized by, It includes a printed layer, a barrier layer and a heat-sealing layer stacked in sequence; the heat-sealing layer is the PE gasket film according to any one of claims 1 to 2 or the PE gasket film prepared by the preparation method according to claim 3.

5. The composite film of claim 4, wherein, The printed layer is a polyester film; the barrier layer is an aluminum foil.

6. The method of producing a composite film according to claim 4 or 5, characterized by, Includes the following steps: After laminating the printed layer and the barrier layer with an adhesive, a first curing process is performed to obtain a printed layer / barrier layer composite film. The printed layer / barrier layer composite film and the PE gasket film are bonded together with an adhesive and then subjected to a second curing process to obtain the composite film.

7. The application of the PE gasket film according to any one of claims 1 to 2 or the composite film according to claim 4 or 5 in bottle cap gaskets.

Citation Information

Patent Citations

  • Modified PE film, modified PE aluminum laminated film and preparation methods of modified PE film and modified PE aluminum laminated film

    CN113263814A