Water storage container and preparation method and application thereof
A polypropylene water container with controlled water release channels addresses inefficiencies and environmental concerns of traditional water retention methods, ensuring stable water supply and high seedling survival rates.
Patent Information
- Application Number
- CN202510375450.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-03-27
- Publication Date
- 2025-07-15
AI Technical Summary
In the existing afforestation technology, water retention agents and water storage seepage membranes have a risk of environmental pollution. The cost of seepage technology and irrigation technology is high and the engineering volume is large, making it difficult to effectively ensure the water supply and survival rate of the seedlings.
The polypropylene foamed composition water storage container prepared by rotomolding process creates a fine water seepage channel in the container wall by adjusting the formula components to achieve slow water seepage and water retention, meeting the dynamic moisture needs of plants.
It improves the survival rate of saplings, reduces the frequency of artificial watering, is green and environmentally friendly, is suitable for natural water-deficient environments, and the container can be reused, reducing the risk of environmental pollution.
Smart Images

Figure CN120310129A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polyolefin compositions, and particularly relates to a water storage container made of a rotational molding processed polypropylene foaming composition, a preparation method thereof, and an application in afforestation. Background Art
[0003] The essence of afforestation is to use the growth and reproduction laws of forest trees, adopt measures and methods of artificial intervention and scientific management, and conduct artificial afforestation in areas suitable for afforestation. It has a great impact on the ecological environment temperature. In summer, the temperature in the forest is about 10 degrees lower than that on the urban open space, while in winter, the temperature in the forest area is 2 - 3 degrees higher than that on the urban open space. Leaves absorb carbon dioxide and release oxygen in the sun, so the forest area is also known as a natural oxygen bar and is a factory for manufacturing oxygen. The reduction of forests has led to a sharp increase in haze and harmful gases in the air. The greenhouse effect is caused by excessive carbon dioxide in the atmosphere, and one-third of the carbon dioxide pollution is caused by forest destruction.
[0004] Using semi-finished saplings for afforestation is a fast and effective method. It is required to select suitable tree species, wrap the roots of the seedlings completely with a wet cloth or film to prevent damage to the root systems of the seedlings, add water and soil, tie them firmly, and reduce the loss of internal moisture of the seedlings. Using plastic film to cover the soil in the afforestation area to prevent a large amount of water loss is a very effective technical measure for afforestation in arid and semi-arid regions. When the soil water content is 12% or more, the saplings are more likely to survive; when the soil water content is less than 12%, the saplings are not likely to survive. Ensure sufficient water supply, water manually twice a day in the morning and evening. When the soil nutrient components and water are satisfied, the survival rate of the saplings can be improved. The most crucial thing is whether the seedlings themselves can maintain water balance. Sufficient water supply in the early stage is the first key factor affecting the growth of saplings. Sufficient water supply can meet the needs of plant growth, improve the survival rate of seedlings. To increase the water content, water retaining agents, water storage and permeable film technology, and drip irrigation technology are usually used.
[0005] Water retainers are substances with strong water absorption properties. They can play a very good role in high - penetration association inside the resin, quickly absorb water through the mesh structure, store the water, and supply it for the normal growth of saplings. The soil on barren mountains is thin and the environmental conditions are harsh. Using water retainers can effectively ensure the water supply for saplings and prevent saplings from dying due to water shortage. The saplings are subjected to root - dipping treatment, and the water retainer is mixed into the soil at the roots of the saplings to ensure that the water retainer plays its full role. The disadvantages of water retainers are their impact on the environment. They are prone to causing soil pollution. The various chemical components that make up water retainers will, when used for a long time, make the soil contain toxic substances such as organic acids, which can easily lead to soil acidification, affect soil fertility, pollute the environment, and the water retainers cannot be degraded and will exist in the soil for a long time, posing a potential threat to the ecological environment, making the soil lose its natural vitality and possibly causing water pollution. Regarding the impact on plants, it will hinder the normal growth of plants. The water retainer will form a film covering the roots of plants, affecting the plants' absorption of water and nutrients, having an adverse impact on soil microorganisms, and affecting the soil ecological environment, resulting in the inability of plants to grow normally.
[0006] The main component of the water - storage and infiltration membrane used in the water - storage and infiltration membrane technology is a polymer composite material, which involves water - guiding coating materials and moisture controlled - release of coated fibers. It is to coat the water - guiding material on the surface of the supporting fibers and compound it with an environmentally friendly material to form a membrane. Using this membrane to package a certain amount of water and directly placing it at the roots of saplings can achieve water - free afforestation. The water consumption is only 1 / 40 - 1 / 20 of the traditional method, and it can effectively help saplings utilize the water in the soil. Through the application of the water - storage and infiltration membrane, the moisture in the soil can be gathered, increasing the water content of the soil in the growth area of saplings and ensuring sufficient water during the growth process of saplings. The use of the water - storage and infiltration membrane can not only effectively improve the utilization rate of soil water by saplings but also save a lot of watering time for foresters, which is of great help to the improvement of the economic benefits of the entire afforestation work. The water source provided by the water - storage and infiltration membrane technology is a slow - release water source. The disadvantage is that all infiltration membranes are prone to deformation and blockage due to soil compaction during use, and post - treatment is not easy, posing potential environmental pollution.
[0007] The infiltration irrigation technology can effectively lock the water in the soil and ensure the water supply necessary for the growth of seedlings. It has good use effects, but the construction volume is large during laying, the equipment cost is high, and the requirements for ground environmental conditions are high during use. Summary of the Invention
[0008] In view of the deficiencies of the prior art, the present invention provides a rotational molding processed hollow product with a stable water seepage effect and a preparation method thereof. By adjusting the formula components, while maintaining a certain strength of the product, controllable and fine water seepage channels are established in the wall to form a continuous osmotic effect on the soil. Slowly seep water and retain water for plants to achieve a dynamic balance between water seepage and plant absorption, with a continuous and slow water flow to make full use of water. Reduce excessive water seepage, avoid the formation of local supersaturation in a short time where plants cannot fully absorb and thus cause waste (the present invention is similar to a (micro) irrigation system), so as to improve the survival rate of plants.
[0009] One of the purposes of the present invention is to provide a water storage container.
[0010] Another purpose of the present invention is to provide a preparation method of the water storage container.
[0011] The third purpose of the present invention is to provide an application of the water storage container.
[0012] In order to achieve the above purposes of the present invention, the following technical solutions are specifically adopted:
[0013] In the first aspect, the present invention provides a water storage container, including the following raw materials by mass percentage:
[0014] 40 - 70% of polypropylene, and
[0015] 30 - 60% of foaming material;
[0016] Wherein the foaming material is prepared from the following raw materials by mass parts: 5 - 15 parts of polyethylene, 5 - 20 parts of potassium chloride, 5 - 15 parts of sodium chloride, 5 - 20 parts of wood powder, 3 - 5 parts of glycerol, 5 - 15 parts of epoxidized soybean oil, 10 - 20 parts of polyethylene wax, and 1 - 5 parts of sodium bicarbonate.
[0017] Preferably, the foaming material is prepared from the following raw materials by mass parts: 5 - 10 parts of polyethylene, 10 - 20 parts of potassium chloride, 5 - 15 parts of sodium chloride, 10 - 20 parts of wood powder, 3 - 5 parts of glycerol, 5 - 10 parts of epoxidized soybean oil, 10 - 20 parts of polyethylene wax, and 2 - 5 parts of sodium bicarbonate.
[0018] Preferably, the mesh number of the polypropylene is 20 - 40 mesh;
[0019] Preferably, the mesh number of the potassium chloride is 400 - 600 mesh;
[0020] Preferably, the mesh number of the sodium chloride is 50 - 100 mesh;
[0021] Preferably, the mesh number of the wood powder is 40 - 100 mesh, and the aspect ratio is 1 / 2 - 1 / 4.
[0022] The formulation amounts of polyethylene are, for example, 5, 6, 7, 8, 9, 10, 12, 14, 15 parts, but are not limited thereto. The formulation amounts of potassium chloride are, for example, 10, 12, 14, 15, 16, 18, 20 parts, but are not limited thereto. The formulation amounts of sodium chloride are, for example, 5, 6, 7, 8, 9, 10, 12, 14, 15 parts, but are not limited thereto. The formulation amounts of wood powder are, for example, 5, 6, 8, 10, 12, 14, 15, 16, 18, 20 parts, but are not limited thereto. The formulation amounts of glycerin are, for example, 3, 4, 5 parts, but are not limited thereto. The formulation amounts of epoxidized soybean oil are, for example, 5, 6, 7, 8, 9, 10 parts, but are not limited thereto. The formulation amounts of polyethylene wax are, for example, 10, 12, 14, 15, 16, 18, 20 parts, but are not limited thereto. The formulation amounts of sodium bicarbonate are, for example, 1, 2, 3, 4, 5 parts, but are not limited thereto.
[0023] In a second aspect, the present invention provides a method for preparing the above-mentioned water storage container, comprising the following steps:
[0024] Grind polypropylene into powder with a mesh size of 20 - 40 to obtain polypropylene powder;
[0025] Stir sodium chloride in a high-speed mixer, reduce the particle size through high-speed friction, control it to be 50 - 100 mesh, then add sodium bicarbonate, potassium chloride, glycerin, and epoxidized soybean oil and mix evenly, then add wood powder and mix evenly, and finally add polyethylene wax and polyethylene and mix. Discharge the material, granulate it with an extruder, and crush and screen the obtained particles to obtain a foaming material;
[0026] Mix the polypropylene powder and the foaming material in proportion and add them into a rotational molding machine for processing and molding to obtain a water storage container.
[0027] Preferably, the temperatures of the extruder are: feeding section 140°C, melting section 150°C, homogenizing section 160°C, head 175°C, die orifice 185°C.
[0028] Preferably, the maximum in-mold temperature of the rotational molding machine does not exceed 190°C, and the rotational molding processing and molding time is 30 - 40 minutes.
[0029] In a third aspect, the present invention provides an application of the above-mentioned water storage container in afforestation.
[0030] Beneficial effects:
[0031] The container prepared by the present invention has a large water storage capacity (10 - 25 liters) and has fine water seepage channels, forming a continuous infiltration effect on the soil. It slowly adds water to and retains water for plants to improve the survival rate of plants, achieving good practical effects. The present invention is green and environmentally friendly, and the products have good practicability. The hollow products prepared by the present invention are particularly suitable for the process of afforestation in natural water-scarce geographical environments and in cases where it is difficult to water manually (such as in mountainous areas with large slopes and soil environments with poor water retention). The water seepage rate of the container can be controlled by adjusting the formula. The container of the present invention is placed at the root of the sapling (close to the root of the sapling), and the water in the device is guided to the root water absorption area through special channels that generate capillary action, so that the water retention rate of the tree roots remains at a relatively high level for a long time. Once the tree is planted until it survives, watering is basically avoided, and the water utilization rate can reach 100%. It is suitable for poor natural environments, especially in areas where it is not easy to lay water pipes and it is difficult to operate manual watering. It reduces the intensity of manual care, can eliminate manual management, and can greatly improve the survival rate of afforestation. It is very friendly to the environment, has no any residues and potential damage, and the products can be reused multiple times, with convenient operation, green and environmentally friendly.
[0032] The production method of the water storage container of the present invention is simple and easy to operate in production.
[0033] The present invention has been described in detail above, but the above embodiments are essentially illustrative only and are not intended to limit the present invention. In addition, the present invention is not limited by any theory described in the foregoing prior art, invention content, or the following examples. Description of the Drawings
[0034] Figure 1 It is a schematic structural diagram of the water storage container of the present invention. Among them, No. 1 is the side view of the container, and the hollow part is the schematic diagram of the through and permeable water channel. No. 2 is the plan view of the container, and the solid part is the schematic diagram of the non-through surface holes. The openings above No. 1 and No. 2 are the rotational molding exhaust ports and also the water injection ports during use. Detailed Embodiments
[0035] The following further illustrates the present invention in conjunction with embodiments. It should be noted that the following embodiments are provided for illustrative purposes only and do not constitute a limitation to the scope of protection required by the present invention.
[0036] Unless otherwise specified, the raw materials, reagents, methods, etc. used in the embodiments are all conventional raw materials, reagents, and methods in the art.
[0037] Raw Materials:
[0038] Polypropylene, pp, density 0.892 g / cm 3 , melt index 18 g / 10 min, Qilu Petrochemical Company;
[0039] Low-density polyethylene, LDPE, density 0.922 g / cm3 , melt index 5.8 g / 10 min, Qilu Petrochemical Company;
[0040] Potassium chloride, industrial grade, density 1.98 g / cm 3 , 500 mesh, white crystal, commercially available from Jinan Shouyue Chemical Industry;
[0041] Sodium chloride, industrial grade, white crystal, purity 99%, Yangkou Salt Field, Shouguang, Shandong;
[0042] Wood powder, sifted through 80 mesh, miscellaneous wood (referring to wood powder particles obtained by crushing and grinding various woods without distinction, not a specific type), moisture content 3 - 5%, select a length-to-diameter ratio of 1 / 2 - 1 / 4, powder particle length 0.6 cm, produced by Wenshuo Company, Feixian, Shandong;
[0043] Glycerol, industrial grade, density 1.263 g / cm 3 , industrial grade, commercially available;
[0044] Epoxidized soybean oil, density 0.989 g / cm 3 , epoxy value 6.0, industrial grade, commercially available in Zibo, Shandong;
[0045] Polyethylene wax, density 0.9 g / cm 3 , white powder, industrial grade, produced by Shanghai Huayi Chemical Industry;
[0046] Sodium bicarbonate, density 2.2 g / cm 3 , white powder, industrial grade, Weifang Haiyuan Chemical Factory, commercially available.
[0047] Examples
[0048] The formulation components of the examples are shown in Table 1 and Table 2.
[0049] Table 1 Foaming Component Formulation (unit: parts by mass)
[0050] Foaming component Formulation 1 Formulation 2 Formulation 3 Formulation 4 Formulation 5 Formulation 6 Formulation 7 Formulation 8 Polyethylene 5 10 15 5 10 15 15 10 Polyethylene wax 10 15 20 15 20 15 20 10 Potassium chloride 5 10 15 20 10 15 20 15 Sodium chloride 5 10 15 5 10 15 5 15 Wood flour 5 10 15 20 10 15 20 15 Sodium bicarbonate 1 2 3 4 5 2 5 4 Glycerol 3 4 5 3 4 5 5 3 Epoxidized soybean oil 5 10 15 5 10 15 5 10
[0051] Table 2 Example Formulation (unit: parts by mass)
[0052]
[0053]
[0054] The process of the examples is as follows:
[0055] (1) Grind polypropylene to 30 - 40 mesh.
[0056] (2) Sodium chloride needs to be processed as follows. Quantified sodium chloride is stirred in a high-speed mixer to reduce the particle size through high-speed friction at 1000 rpm for 2 minutes. Usually, the particles are controlled to be around 50 - 100 mesh and then sieved.
[0057] (3) Sodium bicarbonate, potassium chloride, glycerol, and epoxidized soybean oil are added to (2) and mixed evenly, and then wood powder is added and mixed evenly at a low speed of 500 rpm for 3 minutes.
[0058] (4) Polyethylene wax and polyethylene are finally added to (3), and mixed at 500 rpm for 5 minutes. Then the material is discharged and pelletized by an extruder. The temperatures of the extruder are: feeding section 140°C, melting section 150°C, homogenizing section 160°C, die head 175°C, and die orifice 185°C. The pellets are crushed using a crusher and sieved through an 80-mesh sieve to obtain the foamed material.
[0059] (5) The polypropylene powder and the foamed material are mixed in proportion and added to a rotational molding machine for processing and molding. The maximum in-mold temperature does not exceed 190°C, and the time cycle is 35 minutes.
[0060] The test molded sample is a hollow container (with a wall thickness of 3 mm) of approximately 23 liters (40 cm × 40 cm × 15 cm).
[0061] Control example
[0062] The component formulation of the control example is shown in Table 3.
[0063] Table 3 Control example formulation (unit: parts by mass)
[0064] Comparative example 1 2 3 4 5 6 7 Polypropylene 45 50 55 60 65 70 75 Polyethylene 5 10 15 5 10 15 15 Polyethylene wax 10 0 20 0 30 0 40 Potassium chloride 5 10 0 20 15 0 0 Sodium chloride 5 10 15 0 0 5 15 Wood flour 5 0 15 0 10 15 20 Sodium bicarbonate 1 2 3 4 5 2 5 Glycerol 3 0 5 3 4 0 0 Epoxidized soybean oil 5 10 15 5 0 15 10
[0065] Control example process: Each component is added to a low-speed mixer and mixed for 5 minutes. Then the material is discharged, pelletized by extrusion, ground into powder, and processed by rotational molding according to the formulation. The same (rotational molding) process is used to produce products of the same shape and volume.
[0066] Test example
[0067] Water seepage rate: After the rotational molding hollow water storage container is filled with water and left to stand naturally, it is the amount of water seeping out per unit time through the seepage channel, measured in milliliters per hour.
[0068] Soil water retention rate: The water storage container is placed close to the tree root, and it is the average water content of the soil within the 10×10×10 cm 3 space around the tree root.
[0069] Water storage days (water retention time): The time it takes for the water storage container filled with water to seep out completely.
[0070] Seepage stable time: The time required for the seepage channel to gradually form and reach a stable and unobstructed seepage process after the water storage container is filled with water.
[0071] The results of the examples are shown in Table 4 below.
[0072] Table 4
[0073]
[0074] The results of the comparative examples are shown in Table 5 below.
[0075] Table 5
[0076]
[0077]
[0078] Analysis of the results of the examples and comparative examples: The examples of the present invention can stably seep water for a long time. During the 2-3 month adaptation period of the saplings to the environment and their subsequent growth period, appropriate water supply is available. Due to the continuous and moist supply of water, the saplings will not wither due to water shortage or drought. For the comparative examples of the present invention, from the start of adding water to the start of water seepage, a high water retention state can be quickly reached. A lot of water will be absorbed by the surrounding soil, resulting in loss and waste. Then it returns to a water-deficient state, which is likely to cause water saturation waste in the front stage and water shortage and drought in the back stage for the saplings, making it difficult to ensure normal survival needs and directly affecting their survival rate.
[0079] By selecting specific raw materials and matching them in specific proportions, the present invention constructs a stable and controllable water seepage channel. After the sodium bicarbonate foams, the formed channel is connected to the channels formed by water-soluble components therein or nearby, such as salts (dissolving to form void defects), glycerol (dissolving), and wood powder (shrinking in volume due to heating during processing, also forming physical channels). After that, there is an oily covering on the surface, achieving the purpose of not being easily blocked and stably seeping water.
[0080] Planting experiment:
[0081] Generally, trees are planted in spring and autumn.
[0082] Select saplings of poplar trees with a thickness circumference of 10 cm and a height of 1.6 m, and conduct planting experiments in mountainous hilly areas (Boshan Mountain Area of Zibo, in mid-March in early spring). The tree pits are uniformly 60 cm × 80 cm × 70 cm (length × width × depth). Place a rotational molding water storage container on any side of the tree pit and fill it with water. To facilitate removal, a thin layer of grass mat can be added to one side of the container. Appropriately place base fertilizer at the bottom of the seedling pit, and then place the sapling using the method of "burying three times, treading twice, and lifting the seedling once", that is, burying the soil three times, treading firmly twice, and lifting the sapling upward once. When specifically excavating the tree pit, put the topsoil (shallow soil) in a pile and the subsoil (deep soil) in another pile to prepare for filling soil during subsequent planting. After the tree pit is dug, first apply the base fertilizer to the bottom layer of the tree pit, then crush the topsoil, level and evenly place it on the fertilizer to ensure that the roots of the sapling do not directly contact the fertilizer, and at the same time, the crushed topsoil provides good conditions for the roots to grow downward and expand. Then place the sapling. After the sapling is placed, fill in the subsoil. When the soil filling reaches 1 / 2, pause the soil filling and slightly lift the sapling upward. The purpose is to prevent the sapling from having its roots curled, which will affect the survival and growth of the sapling. After lifting the sapling, do not immediately bury the soil. Instead, firmly step on the soil that has already been buried to make the root hairs of the sapling in close contact with the soil, quickly absorb water and nutrient elements, facilitate the downward growth of the roots, and be conducive to the survival and growth of the tree. Next, bury the remaining subsoil until it is flush with the ground and conduct the second treading. The purpose is to make the trunk of the sapling straight and also make the sapling closely combined with the soil to prevent it from being blown askew. After three months, the survival rate of the saplings is 100%.
[0083] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those of ordinary skill in the art should understand that: within the scope not departing from the spirit and essence defined by the claims of the present invention, the technical solutions recorded in the foregoing embodiments can be modified, or some or all of the technical features can be equivalently replaced; and these modifications or replacements are still within the scope defined by the claims of the present invention.
Claims
1. A water storage container, characterized in that, Comprising the following raw materials by mass percentage: 40 - 70% of polypropylene, and 30 - 60% of foaming material; Wherein the foaming material is prepared from the following raw materials by mass parts: 5 - 15 parts of polyethylene, 5 - 20 parts of potassium chloride, 5 - 15 parts of sodium chloride, 5 - 20 parts of wood powder, 3 - 5 parts of glycerol, 5 - 15 parts of epoxidized soybean oil, 10 - 20 parts of polyethylene wax, 1 - 5 parts of sodium bicarbonate.
2. The water storage container according to claim 1, wherein The foaming material is prepared from the following raw materials by mass parts: 5 - 10 parts of polyethylene, 10 - 20 parts of potassium chloride, 5 - 15 parts of sodium chloride, 10 - 20 parts of wood powder, 3 - 5 parts of glycerol, 5 - 10 parts of epoxidized soybean oil, 10 - 20 parts of polyethylene wax, 2 - 5 parts of sodium bicarbonate.
3. The water storage container according to claim 1, wherein, The mesh number of the polypropylene is 20 - 40 meshes.
4. The water storage container according to claim 1, characterized in that The mesh number of potassium chloride is 400 - 600 meshes.
5. The water storage container according to claim 1, characterized in that, The mesh number of sodium chloride is 50 - 100 meshes.
6. The water storage container according to claim 1, wherein The mesh number of wood powder is 40 - 100 meshes, and the length - to - diameter ratio is 1 / 2 - 1 / 4.
7. A method for preparing a water storage container according to any one of claims 1-6, characterized in that, Including the following steps: Grind the polypropylene into powder with a mesh number of 20 - 40 meshes to obtain polypropylene powder; Stir sodium chloride in a high - speed mixer, reduce the particle size through high - speed friction, control it at 50 - 100 meshes, then add sodium bicarbonate, potassium chloride, glycerol, and epoxidized soybean oil and mix evenly, then add wood powder and mix evenly, and finally add polyethylene wax and polyethylene, discharge the material, granulate with an extruder, and crush and screen the obtained particles to obtain the foaming material; Mix the polypropylene powder and the foaming material in proportion and add them into a rotational molding machine for processing and molding to obtain a water - storage container.
8. The preparation method according to claim 7, characterized in that, The temperatures of the extruder are: feeding section 140 ± 1°C, melting section 150 ± 1°C, homogenizing section 160 ± 1°C, head 175 ± 1°C, die orifice 185 ± 1°C.
9. The preparation method according to claim 7, characterized in that, The maximum in - mold temperature of the rotational molding machine does not exceed 190°C, and the rotational molding processing and molding time is 30 - 40 minutes.
10. The application of a water - storage container as described in any one of claims 1 - 6 or a water - storage container prepared by the preparation method as described in any one of claims 7 - 9 in afforestation.