Method for extracting vanadium from high-calcium steel slag and titanium white waste acid
The method effectively recycles high calcium steel slag and titanium white waste acid to produce high-purity vanadium products, addressing environmental pollution and resource waste.
Patent Information
- Application Number
- CN202510492102.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-18
- Publication Date
- 2025-07-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
High-calcium steel slag and titanium dioxide waste acid are not effectively utilized, resulting in environmental pollution and waste of resources, especially vanadium elements that are not efficiently extracted.
By crushing high-calcium steel slag and mixing it with titanium dioxide waste acid, heating and stirring, solid-liquid separation, purification and purification, obtaining high-purity vanadium product.
It has realized the resource utilization of high-calcium steel slag and titanium dioxide waste acid, reduced environmental pollution, and obtained high-purity vanadium products, suitable for steel, aerospace and chemical fields.
Smart Images

Figure CN120311027A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of resource utilization of metallurgical and chemical wastes, and particularly to a method for extracting vanadium using high-calcium steel slag and titanium white waste acid. Background Art
[0002] High-calcium steel slag is a solid waste generated during the steelmaking process, containing a large amount of calcium, silicon, aluminum, magnesium, vanadium and trace amounts of heavy metal elements. A large amount of waste acid is generated during the production process of titanium dioxide. For example, the sulfuric acid process for titanium dioxide production is one of the main production processes for titanium dioxide, and waste sulfuric acid and the like are generated during the production process, which is called titanium white waste acid. The direct discharge of these waste acids not only pollutes the environment but also wastes the useful components therein. Vanadium is an important strategic metal and is widely used in fields such as steel, aerospace, and chemistry. Therefore, how to effectively utilize high-calcium steel slag and titanium white waste acid to achieve efficient extraction of vanadium has important environmental protection and economic value. Summary of the Invention
[0003] To solve the above problems, the present invention provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid.
[0004] The present invention provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid, and the method includes the following steps:
[0005] Crush the high-calcium steel slag to obtain high-calcium steel slag powder;
[0006] Mix the high-calcium steel slag powder and the titanium white waste acid to obtain a mixture;
[0007] Heat and stir the mixture for reaction, and then perform solid-liquid separation to obtain a filtrate containing vanadate;
[0008] Purify the filtrate containing vanadate to obtain a purified filtrate;
[0009] Purify and refine the purified filtrate to obtain a vanadium product.
[0010] Further, the particle size of the high-calcium steel slag powder is <200 mesh.
[0011] Further, the weight ratio of the high-calcium steel slag powder to the titanium white waste acid is 1:(1.5 - 2.5).
[0012] Further, the weight ratio of the high-calcium steel slag powder to the titanium white waste acid is 1:2.
[0013] Further, the working parameters of the heat and stir reaction include: temperature is 75 - 85 °C, time is 1.5 - 2.5 hours, and pH is 1.5 - 1.8.
[0014] Further, the hydrogen ion concentration in the titanium white waste acid is 2.5 - 3.0 mol / L; the weight content of vanadium element in the high-calcium steel slag powder is 2.5 - 3.2 wt%.
[0015] Further, the purification treatment method includes precipitation and filtration; the purification and refinement method includes extraction, crystallization, and resin adsorption.
[0016] Further, the vanadium product is ammonium metavanadate, and its purity is more than 99.5% in terms of vanadium pentoxide.
[0017] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0018] The embodiment of the present invention provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid. This method comprehensively treats high-calcium steel slag and titanium white waste acid, realizes the resource utilization of waste, reduces environmental pollution, has a simple and easy process, strong operability, does not require additional specific equipment, and has good industrial application prospects. At the same time, the obtained vanadium product has high purity and can be widely used in fields such as steel, aerospace, and chemical industry. Description of the Drawings
[0019] The drawings here are incorporated into the specification and constitute a part of this specification, showing embodiments consistent with the present invention and used together with the specification to explain the principles of the present invention.
[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following will briefly introduce the drawings required for use in the description of the embodiments or the prior art. Obviously, for those of ordinary skill in the art, without creative efforts, other drawings can also be obtained based on these drawings.
[0021] Figure 1 It is a flowchart of the method for extracting vanadium using high-calcium steel slag and titanium white waste acid provided in the embodiment of the present invention. Detailed Embodiments
[0022] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the following will clearly and completely describe the technical solutions of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are some, but not all, of the embodiments of the present invention. All other embodiments obtained by those of ordinary skill in the art without creative efforts based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0023] Unless otherwise specifically stated, all kinds of raw materials, reagents, instruments, and equipment used in the present invention can be obtained through market purchase or can be prepared by existing methods.
[0024] The present invention provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid. As Figure 1 shown, the method includes the following steps:
[0025] Crush the high-calcium steel slag to obtain high-calcium steel slag powder;
[0026] Mix the high-calcium steel slag powder and titanium white waste acid to obtain a mixture;
[0027] Heat and stir the mixture for reaction, and then perform solid-liquid separation to obtain a filtrate containing vanadate;
[0028] Purify the filtrate containing vanadate to obtain a purified filtrate;
[0029] Purify and refine the purified filtrate to obtain a vanadium product.
[0030] The present invention provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid. This method comprehensively processes high-calcium steel slag and titanium white waste acid, realizes the resource utilization of waste, reduces environmental pollution, has a simple and easy process, strong operability, does not require additional specific equipment, and has good industrial application prospects. At the same time, the obtained vanadium product has high purity and can be widely used in fields such as steel, aerospace, and chemical industry.
[0031] In some specific embodiments, the particle size of the high-calcium steel slag powder is <200 mesh.
[0032] In some specific embodiments, the weight ratio of the high-calcium steel slag powder to the titanium white waste acid is 1:(1.5 - 2.5).
[0033] In some specific embodiments, the weight ratio of the high-calcium steel slag powder to the titanium white waste acid is 1:2.
[0034] In some specific embodiments, the working parameters of the heating and stirring reaction include: temperature is 75 - 85 °C, time is 1.5 - 2.5 hours, and pH is 1.5 - 1.8.
[0035] In some specific embodiments, the hydrogen ion concentration in the titanium white waste acid is 2.5 - 3.0 mol / L; the weight content of vanadium element in the high-calcium steel slag powder is 2.5 - 3.2 wt%.
[0036] In some specific embodiments, the purification treatment method includes precipitation and filtration; the purification and refinement method includes extraction, crystallization, and resin adsorption.
[0037] In some specific embodiments, the vanadium product is ammonium metavanadate, and its purity is greater than 99.5% in terms of vanadium pentoxide.
[0038] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and not to limit the scope of the present invention. For the experimental methods without specific conditions indicated in the following embodiments, they are generally determined according to national standards. If there is no corresponding national standard, they are carried out according to general international standards, conventional conditions, or conditions recommended by the manufacturer.
[0039] Example 1
[0040] This example provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid, which specifically includes the following processes:
[0041] Step (1): Collect the waste acid generated by the titanium dioxide factory to obtain titanium white waste acid with a hydrogen ion concentration of 2.8 mol / L, and store it in a waste acid storage tank for standby;
[0042] Step (2): Crush, grind, and screen the high-calcium steel slag to obtain high-calcium steel slag powder with a particle size <200 mesh, and detect its vanadium element weight content to be 3.0 Wt%;
[0043] Step (3): Mix and heat-stir the high-calcium steel slag powder with a vanadium element weight content of 3.0 wt% obtained in step (2) and the titanium white waste acid obtained in step (1) according to a weight ratio of 1:2, and carry out a stirring reaction at 80 °C for 2 hours. After the reaction, carry out solid-liquid separation to obtain a filtrate containing vanadate;
[0044] Step (4): Purify the filtrate containing vanadate obtained in step (3) to obtain a purified filtrate; among them, the purification process includes: oxidation, neutralization, iron removal, etc.;
[0045] Step (5): Purify and refine the purified filtrate obtained in step (4) to obtain a vanadium product; among them, the purification and refinement include the following processes: removing impurities such as phosphorus, arsenic, and silicon, followed by precipitation and centrifugation to dry.
[0046] The vanadium product obtained in this example is ammonium metavanadate, and its purity is 99.5%.
[0047] Example 2
[0048] This example provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid, which specifically includes the following processes:
[0049] Step (1): Collect the waste acid generated by the titanium dioxide factory to obtain titanium white waste acid with a hydrogen ion concentration of 2.5 mol / L, and store it in a waste acid storage tank for standby;
[0050] Step (2): Crush, grind, and screen the high-calcium steel slag to obtain high-calcium steel slag powder with a particle size <200 mesh, and detect its vanadium element weight content to be 2.5 wt%;
[0051] Step (3): Mix and heat with stirring the high-calcium steel slag powder with a vanadium element weight content of 2.5 wt% obtained in step (2) and the titanium white waste acid obtained in step (1) at a weight ratio of 1:1.5, carry out the stirring reaction at 75 °C for 2.5 hours, and after the reaction is completed, carry out solid-liquid separation to obtain a filtrate containing vanadate.
[0052] Step (4): Purify the filtrate containing vanadate obtained in step (3) to obtain a purified filtrate; wherein, the purification process includes: oxidation, neutralization, and impurity removal.
[0053] Step (5): Purify and refine the purified filtrate obtained in step (4) to obtain a vanadium product; wherein, the purification and refinement includes the following process:.
[0054] The vanadium product obtained in this example is ammonium metavanadate, and its purity is more than 99.5% in terms of vanadium pentoxide.
[0055] Example 3
[0056] This example provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid, which specifically includes the following process:
[0057] Step (1): Collect the waste acid generated by the titanium dioxide factory to obtain titanium white waste acid with a hydrogen ion concentration of 3.0 mol / L, and store it in a waste acid storage tank for standby.
[0058] Step (2): Crush, grind, and screen the high-calcium steel slag to obtain high-calcium steel slag powder with a particle size < 200 mesh, and detect its vanadium element weight content to be 3.2 wt%.
[0059] Step (3): Mix and heat with stirring the high-calcium steel slag powder with a vanadium element weight content of 3.2 wt% obtained in step (2) and the titanium white waste acid obtained in step (1) at a weight ratio of 1:2.5, carry out the stirring reaction at 85 °C for 1.5 hours, and after the reaction is completed, carry out solid-liquid separation to obtain a filtrate containing vanadate.
[0060] Step (4): Purify the filtrate containing vanadate obtained in step (3) to obtain a purified filtrate; wherein, the purification process includes: oxidation, neutralization, and impurity removal.
[0061] Step (5): Purify and refine the purified filtrate obtained in step (4) to obtain a vanadium product; wherein, the purification and refinement includes the following process: removing impurities such as phosphorus, arsenic, and silicon, precipitating, and centrifuging to dry.
[0062] The vanadium product obtained in this example is ammonium metavanadate, and its purity is 99.5% in terms of vanadium pentoxide.
[0063] In summary, the present invention provides a method for extracting vanadium using high-calcium steel slag and titanium white waste acid. This method comprehensively processes high-calcium steel slag and titanium white waste acid, realizing the resource utilization of waste, reducing environmental pollution, being simple and easy to implement, highly operable, and not requiring additional specific equipment, thus having good industrial application prospects. At the same time, the obtained vanadium product has high purity and can be widely applied in fields such as steel, aerospace, and chemical engineering.
[0064] The various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be construed as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and individual values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and individual numbers within the range, such as 1, 2, 3, 4, 5, and 6, and this applies regardless of the range. Additionally, whenever a numerical range is indicated herein, it means including any cited number (fraction or integer) within the indicated range.
[0065] The above are only specific embodiments of the present invention, enabling those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be obvious to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to these embodiments shown herein, but rather will conform to the broadest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for extracting vanadium using high-calcium steel slag and titanium white waste acid, characterized in that, The method comprises the following steps: Crush high-calcium steel slag to obtain high-calcium steel slag powder; Mix the high-calcium steel slag powder with waste titanium white acid to obtain a mixture; Heat and stir the mixture for reaction, and then perform solid-liquid separation to obtain a filtrate containing vanadate; Purify the filtrate containing vanadate to obtain a purified filtrate; Purify and refine the purified filtrate to obtain a vanadium product.
2. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claim 1, wherein The particle size of the high-calcium steel slag powder is <200 mesh.
3. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claim 1, characterized in that, The weight ratio of the high-calcium steel slag powder to the waste titanium white acid is 1:(1.5 - 2.5).
4. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claim 1, wherein The weight ratio of the high-calcium steel slag powder to the waste titanium white acid is 1:
2.
5. The method for extracting vanadium using high-calcium steel slag and titanium white waste acid according to claim 1, characterized in that, The operating parameters of the heat and stir reaction include: temperature is 75 - 85°C, time is 1.5 - 2.5 hours, and pH is 1.5 - 1.
8.
6. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claim 1, characterized in that, The operating parameters of the heat and stir reaction include: temperature is 80°C, time is 2 hours.
7. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claim 1, characterized in that, The hydrogen ion concentration in the waste titanium white acid is 2.5 - 3.0 mol / L; the weight content of vanadium element in the high-calcium steel slag powder is 2.5 - 3.2 wt%.
8. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claim 1, characterized in that The purification treatment method includes precipitation and filtration; the purification and refinement method includes extraction, crystallization, and resin adsorption.
9. The method for extracting vanadium by using high-calcium steel slag and titanium white waste acid according to claims 1 to 8, characterized in that, The vanadium product is ammonium metavanadate, and its purity is the purity of vanadium pentoxide is greater than 99.5%.
Citation Information
Patent Citations
Method for extracting vanadium pentoxide from vanadium-containing rotary furnace steel slag
CN101397150A
Method for treating titanium white waste acid by steel slag
CN108264168A
Comprehensive treatment method for steel slag, vanadium slag and titania waste acid
CN108359806A
Method for co-extracting vanadium and scandium by using titanium dioxide waste acid and vanadium-containing high-calcium high-phosphorus slag
CN112176208A
Horizontal rotary reactor and method for treating titanium dioxide waste acid by using vanadium-containing steel slag
CN112301235A
Cited By
Method for neutralizing waste acid and enriching iron and vanadium from vanadium-containing steel slag
CN121294839A