Preparation method and application of sulfonated polysulfone

By introducing side chains on the main chain of the polysulfone molecule, the problem of weak anti-swelling ability of sulfonated polysulfone in the proton exchange membrane fuel cell is solved, and the mechanical strength and proton conduction performance of the membrane are improved.

CN120424339APending Publication Date: 2025-08-05DONGFENG MOTOR GRP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202510408071.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-04-02
Publication Date
2025-08-05

AI Technical Summary

Technical Problem

The existing sulfonated polysulfone has weak anti-swelling ability in proton exchange membrane fuel cells, resulting in membrane deformation and degradation of performance.

Method used

By connecting chloromethyl to the main chain of the polysulfone molecule, and then performing a nucleophilic substitution reaction through 4-hydroxybenzene sulfonate, 1,2-dihydroxybenzene-3,5-disulfonate, and dodecylbenzene sulfonate, the side chain is introduced to increase steric hindrance, improve molecular flexibility and reduce crystallinity, and increase intermolecular voids to accommodate water molecules.

Benefits of technology

The anti-swelling ability of sulfonated polysulfone is improved, the volume changes during water absorption are reduced, and the mechanical strength and proton conduction properties of the membrane are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120424339A_ABST
    Figure CN120424339A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of sulfonated polysulfone. The preparation method of sulfonated polysulfone comprises the following steps: providing polysulfone, and providing a predetermined reagent; carrying out chloromethylation reaction on the polysulfone and bis (chloromethoxy) butane to obtain chloromethylated polysulfone; the predetermined reagent and chloromethyl in the chloromethylated polysulfone are subjected to a nucleophilic substitution reaction, sulfonated polysulfone is obtained, and the predetermined reagent is at least one of 4-hydroxybenzene sulfonate, 1, 2-dihydroxybenzene-3, 5-disulfonic acid disalt and dodecylbenzene sulfonate. According to the sulfonated polysulfone provided by the embodiment of the invention, the volume change is relatively small when the sulfonated polysulfone absorbs water and swells, so that the sulfonated polysulfone has relatively strong anti-swelling capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to fuel cells, and more particularly to proton exchange materials. Background Art

[0002] Sulfonated polysulfones are polysulfone molecules with sulfonic acid groups attached to the main chain or as side chains. Sulfonated polysulfones typically maintain their structural stability even at high temperatures, with thermal decomposition temperatures exceeding 400°C, demonstrating excellent heat resistance. Sulfonated polysulfones also possess high chemical stability, exhibiting excellent corrosion resistance to many organic solvents, acids, and bases. Furthermore, because sulfonic acid groups can ionize protons, sulfonated polysulfones exhibit high proton conductivity. Therefore, sulfonated polysulfones are used as electrolyte materials in applications such as proton exchange membrane fuel cells. However, PEMFCs generate significant amounts of water during operation, and while the sulfonated polysulfones currently used in PEMFCs exhibit good hydrophilicity, they lack strong swelling resistance. Summary of the Invention

[0003] The embodiments of the present application provide a preparation method of sulfonated polysulfone and its application to solve the technical problem of weak anti-swelling ability of sulfonated polysulfone used in proton exchange membrane fuel cells.

[0004] In a first aspect, the present invention provides a method for preparing sulfonated polysulfone, the method comprising the following steps:

[0005] Provide polysulfone and predetermined reagents;

[0006] Carrying out a chloromethylation reaction between the polysulfone and bis(chloromethoxy)butane to obtain chloromethylated polysulfone;

[0007] The predetermined reagent is subjected to a nucleophilic substitution reaction with the chloromethyl group in the chloromethylated polysulfone to obtain the sulfonated polysulfone,

[0008] The predetermined reagent is at least one of 4-hydroxybenzenesulfonate, 1,2-dihydroxybenzene-3,5-disulfonic acid disalt, and dodecylbenzenesulfonate.

[0009] In some embodiments of the present application, the temperature of the chloromethylation reaction is 20-40°C.

[0010] In some embodiments of the present application, the temperature of the nucleophilic substitution reaction is 80-120° C.; and / or,

[0011] The time of the nucleophilic substitution reaction is 20 to 30 hours.

[0012] In a second aspect, an embodiment of the present application provides a proton exchange membrane, wherein the proton exchange membrane comprises sulfonated polysulfone prepared by the preparation method of sulfonated polysulfone described in any embodiment of the first aspect.

[0013] In some embodiments of the present application, the proton exchange membrane comprises:

[0014] Expanded polytetrafluoroethylene film;

[0015] a first ionomer layer disposed on one side of the expanded polytetrafluoroethylene film;

[0016] a second ionomer layer disposed on the other side of the expanded polytetrafluoroethylene film,

[0017] The material of the first ionomer layer includes perfluorosulfonic acid resin, and the material of the second ionomer layer includes perfluorosulfonic acid resin and the sulfonated polysulfone.

[0018] In some embodiments of the present application, the thickness of the expanded polytetrafluoroethylene film is 5 to 10 μm; and / or,

[0019] The porosity of the expanded polytetrafluoroethylene film is greater than 60%.

[0020] In some embodiments of the present application, in the second ionomer layer, the mass ratio of the sulfonated polysulfone to the perfluorosulfonic acid resin is 1 to 2:1.

[0021] In a third aspect, an embodiment of the present application provides a membrane electrode, which includes the proton exchange membrane described in any embodiment of the second aspect.

[0022] In a fourth aspect, an embodiment of the present application provides a method for preparing a membrane electrode, the method comprising the following steps:

[0023] Providing an anode catalyst slurry and a first gas diffusion layer, applying the anode catalyst slurry to the surface of the first gas diffusion layer, and forming the anode catalyst layer after the anode catalyst slurry is dried;

[0024] Providing a first ionomer solution, and applying the first ionomer solution to the surface of the anode catalyst layer to form a first ionomer layer;

[0025] Providing an expanded polytetrafluoroethylene film, and coating the expanded polytetrafluoroethylene film on the surface of the first ionomer layer;

[0026] providing a second ionomer solution, and applying the second ionomer solution to the surface of the expanded polytetrafluoroethylene film to form a second ionomer layer;

[0027] Providing a cathode catalyst slurry, and applying the cathode catalyst slurry to the surface of the second ionomer layer to form a cathode catalyst slurry layer;

[0028] Providing a second gas diffusion layer, attaching the second gas diffusion layer to the surface of the cathode catalytic slurry layer, and then performing hot pressing on the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode,

[0029] The solute of the first ionomer solution includes perfluorosulfonic acid resin, and the solute of the second ionomer solution includes perfluorosulfonic acid resin and the sulfonated polysulfone.

[0030] In some embodiments of the present application, the temperature of the hot pressing is 100-140° C.; and / or,

[0031] The hot pressing pressure is 0.1-1 MPa.

[0032] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0033] The sulfonated polysulfone provided in the embodiment of the present application is connected to the polysulfone molecule main chain by making the polysulfone undergo chloromethylation reaction, and then the chloromethyl is subjected to nucleophilic substitution reaction by 4-hydroxybenzenesulfonate, 1,2-dihydroxybenzene-3,5-disulfonic acid disalt, and dodecylbenzenesulfonate, and the side chain is connected to the polysulfone molecule main chain. The side chain has a large steric hindrance. After the side chain is connected to the polysulfone molecule main chain, the molecular flexibility is improved and the molecular crystallinity is reduced. The large steric hindrance of the side chain makes it possible for the sulfonated polysulfone molecule to have more spaces between itself and other sulfonated polysulfone molecules, and the spaces can accommodate water molecules. This makes the volume change of the sulfonated polysulfone during water absorption and swelling smaller, thereby having a stronger anti-swelling ability. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0036] Figure 1 A schematic flow chart of a method for preparing sulfonated polysulfone provided in an embodiment of the present application;

[0037] Figure 2 Statistical graph of the electrochemically active area of the membrane electrode provided in Example 1, Comparative Example 1, and Comparative Example 2 of the present application;

[0038] Figure 3This is a statistical diagram of the internal resistance of the membrane electrode provided in Example 1, Comparative Example 1, and Comparative Example 2 of the present application. DETAILED DESCRIPTION

[0039] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0040] Unless otherwise specified, the terms used herein should be understood as commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs. In the event of any conflict, the present specification shall take precedence.

[0041] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0042] Sulfonated polysulfone currently used in proton exchange membrane fuel cells has a technical problem of weak anti-swelling ability.

[0043] The technical solutions provided in the embodiments of this application are intended to solve the above technical problems, and the overall idea is as follows:

[0044] In a first aspect, the present invention provides a method for preparing sulfonated polysulfone, the method comprising the following steps:

[0045] S11: providing polysulfone and predetermined reagents;

[0046] S12: subjecting the polysulfone to a chloromethylation reaction with bis(chloromethoxy)butane to obtain a chloromethylated polysulfone;

[0047] S13: allowing the predetermined reagent to undergo a nucleophilic substitution reaction with the chloromethyl group in the chloromethylated polysulfone to obtain the sulfonated polysulfone,

[0048] The predetermined reagent is at least one of 4-hydroxybenzenesulfonate, 1,2-dihydroxybenzene-3,5-disulfonic acid disalt, and dodecylbenzenesulfonate.

[0049] It is easy to understand that the chemical reaction formula of the chloromethylation reaction in step S2 is:

[0050]

[0051] It is easy to understand that, taking the case where the predetermined reagents are all sodium salts as an example,

[0052] The chemical reaction formula of the nucleophilic substitution reaction of 4-hydroxybenzenesulfonate and chloromethylated polysulfone is:

[0053]

[0054] The chemical reaction formula of the nucleophilic substitution reaction of 1,2-dihydroxybenzene-3,5-disulfonic acid disalt and chloromethylated polysulfone is:

[0055]

[0056] The chemical reaction formula of the nucleophilic substitution reaction of dodecylbenzenesulfonate and chloromethylated polysulfone is:

[0057]

[0058] The sulfonated polysulfone described in the present application is connected to the polysulfone molecule main chain by chloromethylation of the polysulfone, and then the chloromethyl is subjected to a nucleophilic substitution reaction by 4-hydroxybenzenesulfonate, 1,2-dihydroxybenzene-3,5-disulfonic acid disalt, and dodecylbenzenesulfonate, and a side chain is connected to the polysulfone molecule main chain. The side chain has a large steric hindrance. After the side chain is connected to the polysulfone molecule main chain, the molecular flexibility is improved and the molecular crystallinity is reduced. The large steric hindrance of the side chain causes more gaps between the sulfonated polysulfone molecule itself and other sulfonated polysulfone molecules, and the gaps can accommodate water molecules. This makes the volume change of the sulfonated polysulfone smaller when it absorbs water and swells, thereby having a stronger anti-swelling ability.

[0059] In some embodiments of the present application, the temperature of the chloromethylation reaction is 20-40°C.

[0060] It is easy to understand that the beneficial effect of the chloromethylation reaction temperature being 20-40° C. is that it can ensure that the chloromethylation reaction can proceed more thoroughly and at the same time make the chloromethylation reaction proceed more smoothly.

[0061] As an example, the temperature of the chloromethylation reaction can be 20°C, 25°C, 30°C, 35°C, or 40°C.

[0062] In some embodiments of the present application, the temperature of the nucleophilic substitution reaction is 80-120° C.; and / or,

[0063] The time of the nucleophilic substitution reaction is 20 to 30 hours.

[0064] It is easy to understand that the beneficial effect of the nucleophilic substitution reaction temperature being 80-120° C. is that it ensures that the nucleophilic substitution reaction can proceed more thoroughly and at the same time allows the nucleophilic substitution reaction to proceed more smoothly.

[0065] It is easy to understand that the nucleophilic substitution reaction is generally quite complete after 20 hours. Further extending the nucleophilic substitution reaction time will continue, but the efficiency will decrease. Extending the nucleophilic substitution reaction time to more than 30 hours will hardly further improve the anti-swelling ability of the sulfonated polysulfone molecule.

[0066] As an example, the temperature of the nucleophilic substitution reaction can be 80°C, 90°C, 100°C, 110°C, or 120°C.

[0067] As an example, the time of the nucleophilic substitution reaction can be 20 h, 23 h, 25 h, 27 h, or 30 h.

[0068] In a second aspect, an embodiment of the present application provides a proton exchange membrane, wherein the proton exchange membrane comprises sulfonated polysulfone prepared by the preparation method of sulfonated polysulfone described in any embodiment of the first aspect.

[0069] The proton exchange membrane is realized based on the preparation method of sulfonated polysulfone described in any embodiment of the first aspect. The specific implementation of the proton exchange membrane can refer to the above embodiments and common knowledge in the field. Since the proton exchange membrane adopts part or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here.

[0070] In some embodiments of the present application, the proton exchange membrane comprises:

[0071] Expanded polytetrafluoroethylene film;

[0072] a first ionomer layer disposed on one side of the expanded polytetrafluoroethylene film;

[0073] a second ionomer layer disposed on the other side of the expanded polytetrafluoroethylene film,

[0074] The material of the first ionomer layer includes perfluorosulfonic acid resin, and the material of the second ionomer layer includes perfluorosulfonic acid resin and the sulfonated polysulfone.

[0075] It is easy to understand that the expanded polytetrafluoroethylene film can provide the proton exchange membrane with higher mechanical strength, and the expanded polytetrafluoroethylene film has more pores, which is beneficial to the transmission of protons.

[0076] It is easy to understand that when the proton exchange membrane is applied to a membrane electrode, the second ionomer layer is located on the cathode side of the proton exchange membrane close to the membrane electrode, which is beneficial to reducing the swelling pressure of water generated by the cathode reaction on the proton exchange membrane.

[0077] In some embodiments of the present application, the thickness of the expanded polytetrafluoroethylene film is 5 to 10 μm; and / or,

[0078] The porosity of the expanded polytetrafluoroethylene film is greater than 60%.

[0079] It is easy to understand that the beneficial effect of the expanded polytetrafluoroethylene film having a thickness of 5 to 10 μm is that it can provide sufficient mechanical strength for the proton exchange membrane without affecting the transmission of protons.

[0080] It is easy to understand that the beneficial effect of the porosity of the expanded polytetrafluoroethylene film being above 60% is to ensure the proton transmission capability of the expanded polytetrafluoroethylene film.

[0081] As an example, the thickness of the expanded polytetrafluoroethylene film can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm.

[0082] In some embodiments of the present application, in the second ionomer layer, the mass ratio of the sulfonated polysulfone to the perfluorosulfonic acid resin is 1 to 2:1.

[0083] It is easy to understand that the beneficial effect of the mass ratio of the sulfonated polysulfone to the perfluorosulfonic acid resin being 1 to 2:1 is that it provides sufficient anti-swelling ability for the second ionomer layer while ensuring that the second ionomer layer has sufficiently high proton transfer efficiency.

[0084] As an example, the mass ratio of the sulfonated polysulfone to the perfluorosulfonic acid resin can be 1:1, 1.2:1, 1.5:1, 1.8:1, 2:1.

[0085] In a third aspect, an embodiment of the present application provides a membrane electrode, which includes the proton exchange membrane described in any embodiment of the second aspect.

[0086] The membrane electrode is realized based on the proton exchange membrane described in any embodiment of the second aspect. The specific implementation of the membrane electrode can refer to the above embodiments and common knowledge in the field. Since the membrane electrode adopts part or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here.

[0087] In a fourth aspect, an embodiment of the present application provides a method for preparing a membrane electrode, the method comprising the following steps:

[0088] S21: providing an anode catalyst slurry and a first gas diffusion layer, applying the anode catalyst slurry to the surface of the first gas diffusion layer, and forming the anode catalyst layer after the anode catalyst slurry is dried;

[0089] S22: providing a first ionomer solution, and applying the first ionomer solution to the surface of the anode catalyst layer to form a first ionomer layer;

[0090] S23: providing an expanded polytetrafluoroethylene film, and coating the expanded polytetrafluoroethylene film on the surface of the first ionomer layer;

[0091] S24: providing a second ionomer solution, and applying the second ionomer solution to the surface of the expanded polytetrafluoroethylene film to form a second ionomer layer;

[0092] S25: providing a cathode catalyst slurry, and applying the cathode catalyst slurry to the surface of the second ionomer layer to form a cathode catalyst slurry layer;

[0093] S26: providing a second gas diffusion layer, attaching the second gas diffusion layer to the surface of the cathode catalytic slurry layer, and then performing hot pressing on the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode.

[0094] The solute of the first ionomer solution includes perfluorosulfonic acid resin, and the solute of the second ionomer solution includes perfluorosulfonic acid resin and the sulfonated polysulfone.

[0095] Those skilled in the art will understand that there are generally two methods for preparing membrane electrodes:

[0096] The first method is to first take a proton exchange membrane, coat an anode catalyst layer and a cathode catalyst layer on both sides of the proton exchange membrane, and then laminate a gas diffusion layer on the anode catalyst layer and the cathode catalyst layer. The gas diffusion layer is pressed together to make the anode catalyst layer and the cathode catalyst layer tightly adhere to the proton exchange membrane to form a membrane electrode.

[0097] The second method is to first take two gas diffusion layers and coat the anode catalyst layer and the cathode catalyst layer on them respectively, then take a proton exchange membrane, attach the anode catalyst layer and the cathode catalyst layer to the two sides of the proton exchange membrane respectively, and then press the two gas diffusion layers so that the anode catalyst layer and the cathode catalyst layer are tightly attached to the proton exchange membrane to form a membrane electrode.

[0098] There are some inherent problems with membrane electrodes prepared by these two methods. In the first method, the anode catalyst layer and the cathode catalyst layer are generally coated on the proton exchange membrane in the form of an aqueous slurry. The proton exchange membrane easily absorbs water, swells and deforms, and the surface of the proton exchange membrane is relatively flat. Directly coating the anode catalyst layer or the cathode catalyst layer on the surface of the proton exchange membrane will make the contact area between the catalyst layer and the proton exchange membrane smaller, thereby making the utilization efficiency of the catalyst low. The problem with the second method is that the anode catalyst layer and the cathode catalyst layer are generally coated on the gas diffusion layer in the form of an aqueous slurry. The slurry can easily penetrate the pores and embed into the interior of the gas diffusion layer, resulting in a decrease in the utilization rate of the catalyst and an increase in the internal resistance of the membrane electrode.

[0099] In step S22 of the present application, the first ionomer solution is directly applied to the surface of the anode catalyst layer to form the first ionomer layer. Since the first ionomer layer is directly formed on the surface of the anode catalyst layer, the degree of deformation after swelling is very low. In addition, since the first ionomer layer is formed by directly applying the first ionomer solution to the surface of the anode catalyst layer, the contact area between the first ionomer layer and the anode catalyst layer is large, and the catalyst utilization efficiency is high. In steps S24 to S25 of the present application, the second ionomer layer and the cathode catalyst layer are prepared layer by layer by coating. Since the second ionomer layer contains the sulfonated polysulfone, it has a strong anti-swelling ability. After the cathode catalyst layer is formed, the second ionomer layer is not easily deformed due to swelling due to water absorption. In this application, an expanded polytetrafluoroethylene (EPTFE) film is disposed between the first and second ionomer layers. The expanded polytetrafluoroethylene (EPTFE) film separates the first and second ionomer layers, preventing water from the cathode catalyst layer from penetrating the first ionomer layer. Furthermore, the film increases the mechanical strength of the membrane electrode while ensuring proton transport capacity. Furthermore, in the membrane electrode fabrication method described herein, each functional layer of the membrane electrode is fabricated layer by layer. With the exception of the expanded polytetrafluoroethylene (EPTFE) film and the second gas diffusion layer, the remaining functional layers are formed by coating onto the other functional layers rather than being bonded together by press-fitting after fabrication. This results in a larger contact area and closer contact between the functional layers of the fabricated membrane electrode, which is beneficial for improving catalyst utilization efficiency and reducing the internal resistance of the membrane electrode.

[0100] In some embodiments of the present application, the temperature of the hot pressing is 100-140° C.; and / or,

[0101] The hot pressing pressure is 0.1-1 MPa.

[0102] As an example, the temperature of the hot pressing may be 100°C, 120°C, 130°C, or 140°C.

[0103] As an example, the hot pressing pressure may be 0.1 MPa, 0.2 MPa, 0.5 MPa, 0.8 MPa, or 1 MPa.

[0104] The present application will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present application only and are not intended to limit the scope of the present application. The experimental methods in the following examples where specific conditions are not specified are generally measured according to industry standards. If there are no corresponding industry standards, then the methods are carried out according to general international standards, conventional conditions, or the conditions recommended by the manufacturer.

[0105] Example 1

[0106] First, this embodiment provides a method for preparing sulfonated polysulfone, which comprises the following steps:

[0107] Sa11: Weigh 2g of polysulfone into a beaker;

[0108] Sa12: Add 25 mL of chloroform to a beaker to dissolve the polysulfone in the chloroform. Then, slowly add an excess of bis(chloromethoxy)butane to the solution while stirring. Allow the polysulfone and bis(chloromethoxy)butane to react at room temperature. After the reaction is complete, separate the chloromethylated polysulfone by filtration and wash the obtained chloromethylated polysulfone.

[0109] Sa13: Add chloromethylated polysulfone to a flask, add dimethyl sulfoxide to dissolve the polysulfone, then add excess sodium 4-hydroxybenzenesulfonate to the flask, react at 100°C for 24 hours, then filter and wash to obtain sulfonated polysulfone.

[0110] The thickness of the expanded polytetrafluoroethylene film is 5 to 10 μm, and the porosity of the expanded polytetrafluoroethylene film is greater than 60%.

[0111] Then, this embodiment also provides a membrane electrode, which is prepared by the following steps:

[0112] Sa21: A platinum-carbon catalyst having a platinum content of 40%, deionized water, and isopropyl alcohol are mixed in a mass ratio of 1:4:4 and ball-milled to obtain a catalyst slurry, which is used to provide a first gas diffusion layer. The catalyst slurry is applied to the surface of the first gas diffusion layer, and the catalyst slurry on the surface of the first gas diffusion layer is dried to form an anode catalyst layer;

[0113] Sa22: providing a first ionomer solution, and applying the first ionomer solution to the surface of the anode catalyst layer using a 20 μm wire rod to form a first ionomer layer, wherein the first ionomer solution is a 5% perfluorosulfonic acid resin solution;

[0114] Sa23: Providing an expanded polytetrafluoroethylene film, and coating the expanded polytetrafluoroethylene film on the surface of the first ionomer layer;

[0115] Sa24: 0.1 g of sulfonated polysulfone was added to 1 g of a 5% perfluorosulfonic acid resin solution to obtain a second ionomer solution. The second ionomer solution was applied to the surface of the expanded polytetrafluoroethylene film using a 20 μm wire rod to form a second ionomer layer.

[0116] Sa25: applying a catalyst slurry onto the surface of the second ionomer layer to form a cathode catalyst slurry layer;

[0117] Sa26: Providing a second gas diffusion layer, attaching the second gas diffusion layer to the surface of the cathode catalytic slurry layer, and then performing hot pressing on the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode.

[0118] The hot pressing temperature is 120° C., and the hot pressing pressure is 0.5 MPa.

[0119] Example 2

[0120] The difference between this embodiment and embodiment 1 is that:

[0121] In step Sa13, the reagent reacting with the chloromethylated polysulfone is disodium 1,2-dihydroxybenzene-3,5-disulfonate, and the reaction temperature is 120° C.;

[0122] In step Sa24, the second ionomer solution is formed by mixing 0.1 g of sulfonated polysulfone and 2 g of a 5% perfluorosulfonic acid resin solution;

[0123] The diameter of the wire rod used in step Sa22 and step Sa24 is 30 μm.

[0124] The details are as follows:

[0125] First, this embodiment provides a method for preparing sulfonated polysulfone, which comprises the following steps:

[0126] Sa11: Weigh 2g of polysulfone into a beaker;

[0127] Sa12: Add 25 mL of chloroform to a beaker to dissolve the polysulfone in the chloroform. Then, slowly add an excess of bis(chloromethoxy)butane to the solution while stirring. Allow the polysulfone and bis(chloromethoxy)butane to react at room temperature. After the reaction is complete, separate the chloromethylated polysulfone by filtration and wash the obtained chloromethylated polysulfone.

[0128] Sa13: Add chloromethylated polysulfone into a flask, add dimethyl sulfoxide to dissolve the polysulfone, then add an excess of 1,2-dihydroxybenzene-3,5-disulfonic acid disodium into the flask, react at 120°C for 24 hours, then filter and wash to obtain sulfonated polysulfone.

[0129] The thickness of the expanded polytetrafluoroethylene film is 5 to 10 μm, and the porosity of the expanded polytetrafluoroethylene film is greater than 60%.

[0130] Then, this embodiment also provides a membrane electrode, which is prepared by the following steps:

[0131] Sa21: A platinum-carbon catalyst having a platinum content of 40%, deionized water, and isopropyl alcohol are mixed in a mass ratio of 1:4:4 and ball-milled to obtain a catalyst slurry, which is used to provide a first gas diffusion layer. The catalyst slurry is applied to the surface of the first gas diffusion layer, and the catalyst slurry on the surface of the first gas diffusion layer is dried to form an anode catalyst layer;

[0132] Sa22: providing a first ionomer solution, and applying the first ionomer solution to the surface of the anode catalyst layer using a 30 μm wire rod to form a first ionomer layer, wherein the first ionomer solution is a 5% perfluorosulfonic acid resin solution;

[0133] Sa23: Providing an expanded polytetrafluoroethylene film, and coating the expanded polytetrafluoroethylene film on the surface of the first ionomer layer;

[0134] Sa24: 0.1 g of sulfonated polysulfone was added to 2 g of a 5% perfluorosulfonic acid resin solution to obtain a second ionomer solution. The second ionomer solution was then applied to the surface of the expanded polytetrafluoroethylene film using a 30 μm wire rod to form a second ionomer layer.

[0135] Sa25: applying a catalyst slurry onto the surface of the second ionomer layer to form a cathode catalyst slurry layer;

[0136] Sa26: Providing a second gas diffusion layer, attaching the second gas diffusion layer to the surface of the cathode catalytic slurry layer, and then performing hot pressing on the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode.

[0137] The hot pressing temperature is 120° C., and the hot pressing pressure is 0.5 MPa.

[0138] Example 3

[0139] The difference between this embodiment and embodiment 1 is that:

[0140] In step Sa13, the reagent reacting with the chloromethylated polysulfone is sodium dodecylbenzenesulfonate, and the reaction temperature is 80° C.;

[0141] The diameter of the wire rod used in step Sa22 and step Sa24 is 30 μm.

[0142] First, this embodiment provides a method for preparing sulfonated polysulfone, which comprises the following steps:

[0143] Sa11: Weigh 2g of polysulfone into a beaker;

[0144] Sa12: Add 25 mL of chloroform to a beaker to dissolve the polysulfone in the chloroform. Then, slowly add an excess of bis(chloromethoxy)butane to the solution while stirring. Allow the polysulfone and bis(chloromethoxy)butane to react at room temperature. After the reaction is complete, separate the chloromethylated polysulfone by filtration and wash the obtained chloromethylated polysulfone.

[0145] Sa13: Add chloromethylated polysulfone into a flask, add dimethyl sulfoxide to dissolve the polysulfone, then add excess sodium dodecylbenzenesulfonate into the flask, react at 80°C for 24 hours, then filter and wash to obtain sulfonated polysulfone.

[0146] The thickness of the expanded polytetrafluoroethylene film is 5 to 10 μm, and the porosity of the expanded polytetrafluoroethylene film is greater than 60%.

[0147] Then, this embodiment also provides a membrane electrode, which is prepared by the following steps:

[0148] Sa21: A platinum-carbon catalyst having a platinum content of 40%, deionized water, and isopropyl alcohol are mixed in a mass ratio of 1:4:4 and ball-milled to obtain a catalyst slurry, which is used to provide a first gas diffusion layer. The catalyst slurry is applied to the surface of the first gas diffusion layer, and the catalyst slurry on the surface of the first gas diffusion layer is dried to form an anode catalyst layer;

[0149] Sa22: providing a first ionomer solution, and applying the first ionomer solution to the surface of the anode catalyst layer using a 30 μm wire rod to form a first ionomer layer, wherein the first ionomer solution is a 5% perfluorosulfonic acid resin solution;

[0150] Sa23: Providing an expanded polytetrafluoroethylene film, and coating the expanded polytetrafluoroethylene film on the surface of the first ionomer layer;

[0151] Sa24: 0.1 g of sulfonated polysulfone was added to 1 g of a 5% perfluorosulfonic acid resin solution to obtain a second ionomer solution. The second ionomer solution was then applied to the surface of the expanded polytetrafluoroethylene film using a 30 μm wire rod to form a second ionomer layer.

[0152] Sa25: applying a catalyst slurry onto the surface of the second ionomer layer to form a cathode catalyst slurry layer;

[0153] Sa26: Providing a second gas diffusion layer, attaching the second gas diffusion layer to the surface of the cathode catalytic slurry layer, and then performing hot pressing on the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode.

[0154] The hot pressing temperature is 120° C., and the hot pressing pressure is 0.5 MPa.

[0155] Comparative Example 1

[0156] This comparative example provides a membrane electrode, which is prepared by the following method:

[0157] A platinum-carbon catalyst having a platinum content of 40%, deionized water, and isopropyl alcohol were mixed in a mass ratio of 1:4:4 and ball-milled to obtain a catalyst slurry;

[0158] Providing a perfluorosulfonic acid resin proton exchange membrane, and applying the catalyst slurry to both sides of the perfluorosulfonic acid resin proton exchange membrane to form a cathode catalyst layer and an anode catalyst layer, respectively;

[0159] A first gas diffusion layer and a second gas diffusion layer are provided. After the first gas diffusion layer and the second gas diffusion layer are respectively adhered to the surfaces of the anode catalyst layer and the cathode catalyst layer, the first gas diffusion layer and the second gas diffusion layer are hot pressed to obtain the membrane electrode, wherein the hot pressing temperature is 120°C and the hot pressing pressure is 0.5 MPa.

[0160] Comparative Example 2

[0161] This comparative example provides a membrane electrode, which is prepared by the following method:

[0162] A platinum-carbon catalyst having a platinum content of 40%, deionized water, and isopropyl alcohol were mixed in a mass ratio of 1:4:4 and ball-milled to obtain a catalyst slurry;

[0163] Providing a first gas diffusion layer and a second gas diffusion layer, applying the catalyst slurry to the first gas diffusion layer to form an anode catalyst layer, and applying the catalyst slurry to the second gas diffusion layer to form a cathode catalyst layer;

[0164] Providing a perfluorosulfonic acid resin proton exchange membrane, laminating the anode catalyst layer and the cathode catalyst layer to respective surfaces of the perfluorosulfonic acid resin proton exchange membrane, and then hot-pressing the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode, wherein the hot-pressing temperature is 120° C. and the hot-pressing pressure is 0.5 MPa;

[0165] Related experiments and effect data:

[0166] The electrochemical active areas of the membrane electrodes provided by Example 1, Comparative Example 1, and Comparative Example 2 were tested by cyclic voltammetry. The measured electrochemical active areas were statistically summarized and prepared Figure 1 .Depend on Figure 1 It can be seen that the electrochemically active area of the membrane electrode of Example 1 is significantly higher than that of Comparative Example 1 and Comparative Example 2. This may be because the functional layers in Example 1 are prepared layer by layer, and except for the expanded polytetrafluoroethylene film and the second gas diffusion layer, the remaining functional layers are coated on other functional layers to form, rather than being combined together by pressing after forming. This makes the contact area between the functional layers of the prepared membrane electrode larger and the contact more intimate, which is beneficial to improving the utilization efficiency of the catalyst. In particular, the first ionomer layer is prepared by directly scraping the first ionomer solution onto the anode catalyst layer, so that the contact area between the anode catalyst layer and the first ionomer layer is larger, which is beneficial to improving the catalyst utilization rate of the anode catalyst layer, and thus the electrochemically active area of Example 1 is larger.

[0167] The internal resistance of the membrane electrodes provided in Example 1, Comparative Example 1 and Comparative Example 2 at different current densities was tested by the AC impedance method, and the measured internal resistances were statistically summarized and prepared. Figure 2 .Depend on Figure 2 It can be seen that the internal resistance of the membrane electrode in Example 1 is significantly lower than that of the membrane electrodes in Comparative Examples 1 and 2 at all current densities. This may be because the functional layers of the membrane electrode in Example 1 are prepared layer by layer, and except for the expanded polytetrafluoroethylene film and the second gas diffusion layer, the remaining functional layers are coated onto the other functional layers rather than being bonded together by pressing after formation. This results in a larger contact area and closer contact between the functional layers of the prepared membrane electrode, which is beneficial for reducing the internal resistance of the membrane electrode.

[0168] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a hard limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numbers within the range. For example, the description of a range from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0169] In this application, unless otherwise stated, directional terms such as "upper" and "lower" refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of this application specification, the terms "include", "comprise", etc. mean "including but not limited to". Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device comprising a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the phrase "include..." do not exclude the presence of other identical elements in the process, method, article or device comprising the elements. In this article, relational terms such as "first" and "second" are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. For the association relationship of more than three associated objects described with "and / or", it means that these three associated objects can exist alone, or any at least two of them exist simultaneously. For example, for A, and / or B, and / or C, it can be represented that any one of A, B, and C exists alone, or any two of them exist simultaneously, or three of them exist simultaneously. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "at least one of the following (individuals)" or similar expressions refer to any combination of these items, including any combination of single item (individuals) or plural items (individuals). For example, "at least one of a, b, or c (individuals)," or "at least one of a, b, and c (individuals)", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple respectively. "Number representation" involved in this application, such as parts by weight, parts by mass, etc., represents the proportional relationship between each component. In the proportional relationship involved in this application, the parameters that need to be described by proportion should be understood as the first term of the proportional formula in the order of description, and the proportional numbers should be understood as the second term of the proportional formula. For example, if the mass ratio of substance A, substance B and substance C is 1:2:3, then substance A, substance B and substance C should correspond one-to-one to the proportional numbers in the proportional formula in the order of description, that is, the mass of substance A: the mass of substance B: the mass of substance C = 1:2:3.

[0170] The foregoing is merely a list of specific embodiments of the present application, intended to enable those skilled in the art to understand or implement the present application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application is not limited to the embodiments shown herein, but is intended to conform to the broadest scope consistent with the principles and novel features of the present application.

Claims

1. A method for preparing sulfonated polysulfone, characterized in that: The preparation method of the sulfonated polysulfone comprises the following steps: Provide polysulfone and predetermined reagents; Carrying out a chloromethylation reaction between the polysulfone and bis(chloromethoxy)butane to obtain chloromethylated polysulfone; The predetermined reagent is subjected to a nucleophilic substitution reaction with the chloromethyl group in the chloromethylated polysulfone to obtain the sulfonated polysulfone, The predetermined reagent is at least one of 4-hydroxybenzenesulfonate, 1,2-dihydroxybenzene-3,5-disulfonic acid disalt, and dodecylbenzenesulfonate.

2. The sulfonated polysulfone according to claim 1, wherein The temperature of the chloromethylation reaction is 20-40°C.

3. The sulfonated polysulfone according to claim 1, wherein The temperature of the nucleophilic substitution reaction is 80-120° C.; and / or, The time of the nucleophilic substitution reaction is 20 to 30 hours.

4. A proton exchange membrane, characterized in that The proton exchange membrane comprises the sulfonated polysulfone prepared by the preparation method of the sulfonated polysulfone according to any one of claims 1 to 3.

5. The proton exchange membrane according to claim 4, characterized in that The proton exchange membrane comprises: Expanded polytetrafluoroethylene film; a first ionomer layer disposed on one side of the expanded polytetrafluoroethylene film; a second ionomer layer disposed on the other side of the expanded polytetrafluoroethylene film, The material of the first ionomer layer includes perfluorosulfonic acid resin, and the material of the second ionomer layer includes perfluorosulfonic acid resin and the sulfonated polysulfone.

6. The proton exchange membrane according to claim 5, characterized in that The expanded polytetrafluoroethylene film has a thickness of 5 to 10 μm; and / or, The porosity of the expanded polytetrafluoroethylene film is greater than 60%.

7. The proton exchange membrane according to claim 5, characterized in that In the second ionomer layer, the mass ratio of the sulfonated polysulfone to the perfluorosulfonic acid resin is 1 to 2:

1.

8. A membrane electrode, characterized in that The membrane electrode comprises the proton exchange membrane described in any embodiment of the second aspect.

9. A method for preparing a membrane electrode, characterized in that: The method for preparing the membrane electrode comprises the following steps: Providing an anode catalyst slurry and a first gas diffusion layer, applying the anode catalyst slurry to the surface of the first gas diffusion layer, and forming the anode catalyst layer after the anode catalyst slurry is dried; Providing a first ionomer solution, and applying the first ionomer solution to the surface of the anode catalyst layer to form a first ionomer layer; Providing an expanded polytetrafluoroethylene film, and coating the expanded polytetrafluoroethylene film on the surface of the first ionomer layer; Providing a second ionomer solution, and applying the second ionomer solution to the surface of the expanded polytetrafluoroethylene film to form a second ionomer layer; Providing a cathode catalyst slurry, and applying the cathode catalyst slurry to the surface of the second ionomer layer to form a cathode catalyst slurry layer; Providing a second gas diffusion layer, attaching the second gas diffusion layer to the surface of the cathode catalytic slurry layer, and then performing hot pressing on the first gas diffusion layer and the second gas diffusion layer to obtain the membrane electrode, The solute of the first ionomer solution includes perfluorosulfonic acid resin, and the solute of the second ionomer solution includes perfluorosulfonic acid resin and the sulfonated polysulfone.

10. The method for preparing a fuel cell according to claim 9, wherein: The temperature of the hot pressing is 100-140° C.; and / or, The hot pressing pressure is 0.1-1 MPa.

Citation Information

Cited By

  • Hydrophilic polysulfone resin and preparation method thereof

    CN121270924A