A selective etching method for P-type polysilicon layers and its application
By preparing a reverse osmosis layer on the back of a silicon wafer and using laser sintering to reduce the boron doping concentration, combined with acid-base etching methods, the etching problem of high boron-doped P-type polycrystalline silicon layers was solved, thereby increasing the production capacity of TBC cells and reducing production costs.
Patent Information
- Application Number
- CN202510557212.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-04-29
AI Technical Summary
Existing technologies struggle to effectively remove high boron-doped P-type polycrystalline silicon layers, making wet etching difficult in TBC cell production, impacting cell efficiency and production capacity, and increasing equipment investment costs.
A reverse osmosis layer is prepared on the back side of the silicon wafer, and boron is diffused into the reverse osmosis layer by laser sintering to reduce the boron doping concentration in the laser sintering area. The P-type polycrystalline silicon layer is then selectively removed by acid-base etching.
It reduces the difficulty of wet etching of P-type polycrystalline silicon layers, improves the production capacity and photoelectric performance of TBC cells, reduces equipment costs, and has good compatibility with existing TOPCon cell production lines.
Smart Images

Figure CN120475797B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of wet etching technology for solar cells, specifically to a selective etching method for P-type polycrystalline silicon layers and its application. Background Technology
[0002] TBC (Top-Condition Tunneling Oxide Passivated Contact) batteries are a novel type of crystalline silicon battery developed based on Top-Con crystalline silicon technology. They feature the emitter, surface field, and metal electrodes all located on the back of the battery and arranged in an interdigitated pattern. Because TBC batteries have no electrode grid lines obstructing the front, they maximize the utilization of incident light, reduce optical losses, and provide a larger effective power generation area, resulting in higher photoelectric conversion efficiency. Furthermore, the solid-color front appearance of TBC batteries is more aesthetically pleasing and conforms to popular tastes, giving them a competitive edge in the market.
[0003] In TBC (Top-Con) cells, both the n+ and p+ emitters are located on the back side of the crystalline silicon cell and are arranged in an interdigitated pattern. Currently, one strategy for fabricating the n+ and p+ emitters is as follows (see publications CN119342910B and CN116845140A):
[0004] First, either side of a double-polished n-type silicon wafer can be used as the back side. A first tunneling oxide layer and an intrinsic amorphous silicon layer (ia-Si layer) are sequentially deposited on the back side of the silicon wafer. Then, the ia-Si layer is transformed into a P-type Poly Si layer (i.e., a P-type polycrystalline silicon layer, such as a boron-doped polycrystalline silicon layer) by boron doping, while a borosilicate glass layer (BSG layer) is formed on the back surface of the P-type polycrystalline silicon layer. Next, according to a specific pattern, the BSG layer is patterned by laser ablation (also known as selective laser ablation) to remove the BSG layer in the laser ablation area. Then, alkaline etching is used to etch away the P-type polycrystalline silicon layer and the first tunneling oxide layer in the laser ablation area along the longitudinal direction of the BSG layer removal area to expose the back surface of the silicon wafer in the laser ablation area, while retaining the P-type polycrystalline silicon layer and the first tunneling oxide layer in the non-laser ablation area. Finally, a second tunneling oxide layer and an n-type Poly Si layer (i.e., an n-type polycrystalline silicon layer) are sequentially deposited on the exposed back side of the silicon wafer through a second deposition. In this way, an interdigitated structure can be formed on the back of the silicon wafer, in which the n+ emitter (comprising a first tunneling oxide layer and a p-type polycrystalline silicon layer located in a localized area on the back of the silicon wafer) and the p+ emitter (comprising a second tunneling oxide layer and an n-type polycrystalline silicon layer located in a localized area on the back of the silicon wafer) are interdigitated. This interdigitated structure is key to the fabrication of TBC cells. Subsequent processes such as laser grooving, wet etching, passivation, and metallization can ultimately form a TBC cell with a complete interdigitated distribution of n+ and p+ emitters, and an isolation region between the n+ and p+ emitters.
[0005] To achieve optimal photoelectric performance in TBC cells, the boron doping concentration in the P-type polycrystalline silicon layer needs to meet a high specific doping concentration range. However, the etching difficulty of the P-type polycrystalline silicon layer by the alkaline solution used in alkaline etching increases exponentially with the increase of boron doping concentration. The P-type polycrystalline silicon layer with high boron doping concentration cannot be effectively etched away, which will seriously affect the improvement of TBC cell efficiency. The current solutions are mainly: (1) increasing the alkaline etching time of the P-type polycrystalline silicon layer. (2) controlling the junction depth and doping concentration of boron doping in the intrinsic amorphous silicon layer, that is, preparing a P-type polycrystalline silicon layer with a shallower junction depth and a lower doping concentration to reduce the etching difficulty of the P-type polycrystalline silicon layer. (3) replacing the laser with a laser with higher power and emission frequency during laser ablation to destroy part of the P-type polycrystalline silicon layer with high boron doping concentration while selectively ablation (removing the BSG layer), thereby reducing the burden of alkaline etching. (4) In addition, as shown in CN119342910B, by adjusting the deposition temperature and deposition pressure of the polysilicon layer, a low-concentration doped region is formed on the back side of the high-concentration doped region of the first doped polysilicon layer, so as to offset the effect of laser treatment on increasing the doping concentration of the doped polysilicon layer, so as to avoid putting a greater burden on the alkaline etching doped polysilicon layer.
[0006] However, while increasing the alkaline etching time can more thoroughly remove the P-type polysilicon layer in the laser-etched region, the extended etching time also leads to a decrease in TBC cell production capacity. Controlling the junction depth and doping concentration of boron doping in the intrinsic amorphous silicon layer requires a long process exploration time. Furthermore, a decrease in the boron doping concentration of the P-type polysilicon layer can prevent it from matching the optimal TBC cell structure, further affecting the photoelectric performance (such as contact performance) of the finished cell. Replacing the laser with a higher power and emission frequency can achieve the same effect of removing the P-type polysilicon layer in the laser-etched region, but this requires investment in new equipment, which is costly. In addition, the solution shown in CN119342910B only offsets the effect of laser treatment on increasing the doping concentration of the polysilicon layer; its effect on reducing the difficulty of alkaline etching of the doped polysilicon layer is limited. Moreover, it increases the difficulty and cost of the polysilicon layer deposition process and subsequent metallization process (the first metal electrode needs to penetrate the low-concentration doped region to contact the high-concentration doped region). Summary of the Invention
[0007] The purpose of this invention is to overcome the shortcomings of the prior art and provide a selective etching method for P-type polycrystalline silicon layers and its application, so as to solve the problem of the difficulty of wet etching in local areas of P-type polycrystalline silicon layers with high boron doping concentration in the current TBC battery production process.
[0008] Based on this, the present invention discloses a selective etching method for a P-type polysilicon layer, comprising the following steps:
[0009] Step 1: Sequentially prepare a tunneling oxide layer, a first p-type polycrystalline silicon layer, and a borosilicate glass layer on the back side of the silicon wafer;
[0010] Step 2: Prepare a reverse osmosis layer on the back side of the first p-type polycrystalline silicon layer;
[0011] Step 3: Perform patterned laser sintering on the back side of the reverse osmosis layer, so that the reverse osmosis layer, borosilicate glass layer, first p-type polycrystalline silicon layer, tunneling oxide layer and back surface layer of silicon wafer in the laser sintering area melt sequentially, causing boron in the borosilicate glass layer and the first p-type polycrystalline silicon layer to diffuse into the reverse osmosis layer and the back surface layer of silicon wafer, so as to form a second p-type polycrystalline silicon layer with a boron doping concentration lower than that of the first p-type polycrystalline silicon layer on the back surface of silicon wafer in the laser sintering area, and form a surface oxide layer on the back side of the second p-type polycrystalline silicon layer;
[0012] Step 4: Wet etching to remove the surface oxide layer and the second p-type polysilicon layer of the laser-sintered area to expose the silicon surface of the laser-sintered area, and to remove the reverse osmosis layer of the non-laser-sintered area.
[0013] Preferably, in step 1, the silicon wafer is an n-type silicon wafer that has been polished on both sides;
[0014] Step 1 specifically includes:
[0015] Step 11: Sequentially deposit a tunneling oxide layer and an intrinsic amorphous silicon layer on the back side of the silicon wafer;
[0016] Step 12: Perform boron diffusion treatment on the intrinsic amorphous silicon layer to transform the intrinsic amorphous silicon layer into a first p-type polycrystalline silicon layer and a borosilicate glass layer located on the outer surface of the first p-type polycrystalline silicon layer.
[0017] Specifically, in step 12, the boron doping concentration of the first p-type polysilicon layer is 2E19~1E20cm⁻¹. -3 (e.g. 6E19cm) -3 Correspondingly, after the patterned laser sintering in step 3, the boron doping concentration of the first p-type polycrystalline silicon layer in the non-laser sintering region remains at 2E19~1E20cm⁻¹. -3 The boron doping concentration of the surface oxide layer and the second p-type polysilicon layer in the laser sintering region is lower than that of the first p-type polysilicon layer in the non-laser sintering region.
[0018] Preferably, in step 2, the reverse osmosis layer is an intrinsic amorphous silicon layer with a thickness of 100-500 nm;
[0019] The reverse osmosis layer is prepared by chemical vapor deposition or physical vapor deposition.
[0020] More preferably, in step 2, when preparing the reverse osmosis layer using chemical vapor deposition, the silicon source injection rate is 500-2000 sccm, and the deposition temperature is 550-650℃.
[0021] Alternatively, when preparing the reverse osmosis layer using physical vapor deposition, a silicon deposition target is used, with a deposition power of 10-50KV, a deposition temperature of 200-400℃, and a pressure of less than 10Pa within the deposition chamber.
[0022] Preferably, in step 3, the process conditions for patterned laser sintering include: laser power of 5-30W, laser wavelength of 400-700nm, and laser spot area of 200-3000μm. 2 The number of times the light spot is repeatedly sintered is 1-20 times.
[0023] More preferably, in step 3, the patterned laser sintering is performed using SE equipment or laser-enhanced contact optimization equipment in a tunnel oxide passivation contact battery production line.
[0024] Preferably, step 4 specifically includes:
[0025] Step 41: First, perform acid etching to remove the surface oxide layer in the laser sintering area;
[0026] Step 42: Perform alkaline etching to remove the second p-type polysilicon layer in the laser-sintered region and the reverse osmosis layer in the non-laser-sintered region.
[0027] More preferably, in step 41, the acid etching process conditions include: acid etching using hydrofluoric acid solution, with an HF concentration of 0.5-10 w.t.%, an etching temperature of 40-80℃, and an etching time of 50-500s.
[0028] More preferably, in step 42, the alkaline etching process conditions include: alkaline etching using an aqueous solution of NaOH and surface modifiers, wherein the concentration of NaOH is 0.3-5 wt.%, the concentration of the surface modifiers is 0.01-0.5 wt%, the etching temperature is 50-90℃, and the etching time is 50-500 s.
[0029] This invention also discloses an application of a selective etching method for P-type polycrystalline silicon layers, which applies the selective etching method for P-type polycrystalline silicon layers described above to the fabrication of tunnel oxide passivated contact back contact batteries (especially TBC batteries).
[0030] The present invention provides a selective etching method for a P-type polysilicon layer, the technical principle of which and its advantages are as follows:
[0031] 1. In practice, the lower the boron doping concentration in boron-doped polycrystalline silicon, the easier the wet etching process. This invention prepares an ia-Si layer (intrinsic amorphous silicon layer) as a reverse diffusion layer on the back surface of a borosilicate glass layer (BSG layer) after boron diffusion. During laser sintering, the laser heating temperature decreases from the reverse diffusion layer (such as the intrinsic amorphous silicon reverse diffusion layer) towards the back surface of the silicon wafer, causing the solid solubility of silicon for boron to decrease from the outside to the inside (i.e., the solid solubility of silicon for boron decreases from the intrinsic amorphous silicon reverse diffusion layer towards the back surface of the silicon wafer). Furthermore, there is a boron concentration difference between the intrinsic amorphous silicon reverse diffusion layer and the internal borosilicate glass layer and the first p-type polycrystalline silicon layer. This facilitates the reverse diffusion of boron from the borosilicate glass layer and the first p-type polycrystalline silicon layer into the intrinsic amorphous silicon reverse diffusion layer, thus reducing the original borosilicate glass layer concentration. The boron doping concentration in the glass layer and the first p-type polysilicon layer (that is, the boron doping concentration of the second p-type polysilicon layer formed after laser sintering is less than the boron doping concentration of the first p-type polysilicon layer in the non-laser sintering region) reduces the difficulty of wet etching (including alkaline etching) of local areas of the original p-type polysilicon layer (the original p-type polysilicon layer refers to the first p-type polysilicon layer before the laser sintering step, corresponding to the first p-type polysilicon layer in the non-laser sintering region after the laser sintering step) (this local area is the laser sintering region of the present invention).
[0032] 2. It should be noted that laser sintering can melt the intrinsic amorphous silicon reverse osmosis layer, borosilicate glass layer, first p-type polycrystalline silicon layer, tunneling oxide layer, and silicon wafer back contact surface layer in the laser sintering region from the outside to the inside in a short time. This is conducive to the rapid diffusion (reverse diffusion) of boron in the original borosilicate glass layer and the first p-type polycrystalline silicon layer into the intrinsic amorphous silicon reverse osmosis layer. This forms a second p-type polycrystalline silicon layer in the laser sintering region with a boron doping concentration lower than that of the first p-type polycrystalline silicon layer in the non-laser sintering region, thereby reducing the difficulty of wet etching in local areas of the original p-type polycrystalline silicon layer.
[0033] 3. Moreover, laser sintering can destroy passivation layers such as tunneling oxide layers, allowing boron in the first p-type polysilicon layer to diffuse to the surface of the back contact surface of the silicon wafer, further reducing the boron doping concentration in the original first p-type polysilicon layer (that is, further reducing the boron doping concentration in the second p-type polysilicon layer in the laser sintering region of the present invention), and further reducing the difficulty of wet etching in local areas of the original p-type polysilicon layer.
[0034] 4. Furthermore, this laser sintering process can be performed using existing equipment such as the SE (Selective Emitter) in TOPCon battery production lines, eliminating the need to purchase new equipment and significantly reducing equipment investment costs; the selective etching method of this invention has good compatibility with existing TOPCon and TBC battery production lines.
[0035] In summary, the selective etching method of the present invention not only effectively reduces the difficulty of wet etching in local areas of the original p-type polysilicon layer and effectively removes the second p-type polysilicon layer in the laser sintering region, but also has the following advantages: the method is simple, the etching efficiency is high, which is conducive to improving the production capacity of TBC cells, no new equipment is required, the equipment cost can be reduced, and the production cost of TBC cells can be reduced. It also has good compatibility with existing TOPCon cells and TBC cell production lines and will not affect subsequent TBC cell processes, thus having good universality.
[0036] Compared with the prior art, the present invention has at least the following beneficial effects:
[0037] A reverse osmosis layer is prepared on the back side of the borosilicate glass layer. Then, using existing SE equipment in the TOPCon cell production line, secondary boron diffusion (i.e., reverse diffusion) is achieved in the local high boron doping concentration area through laser sintering. This reduces the boron doping concentration of the second p-type polysilicon layer in the laser-sintered area, making the boron doping concentration of the second p-type polysilicon layer in the laser-sintered area lower than that of the first p-type polysilicon layer in the non-laser-sintered area. This reduces the difficulty of wet etching the local area of the original p-type polysilicon layer (the first p-type polysilicon layer before the laser sintering step, corresponding to the first p-type polysilicon layer in the non-laser-sintered area after the laser sintering step). Thus, the second p-type polysilicon layer in the laser-sintered area can be completely removed by wet etching, which is beneficial for the subsequent preparation of the n-type polysilicon layer.
[0038] Moreover, compared with existing solutions such as CN119342910B, the selective etching method of the present invention can not only effectively reduce the difficulty of wet etching in local areas of the original p-type polysilicon layer and effectively remove the second p-type polysilicon layer in the laser sintering area, but also has the following advantages: the method is simple, the etching efficiency is high, which is conducive to improving the production capacity of TBC cells, no need to add new equipment, which can reduce equipment costs and help reduce the production cost of TBC cells, and has good compatibility with existing TOPCon cells and TBC cells production lines, and will not affect subsequent TBC cell processes, thus having good universality. Attached Figure Description
[0039] Figure 1 This is a schematic diagram of a partial cross-sectional structure after step S1 processing in the selective etching method for a P-type polysilicon layer according to the present invention.
[0040] Figure 2 This is a schematic diagram of a partial cross-sectional structure after step S2 of the selective etching method for a P-type polysilicon layer according to the present invention.
[0041] Figure 3This is a schematic diagram of a partial cross-sectional structure after step S3 of the selective etching method for a P-type polysilicon layer according to the present invention.
[0042] Figure 4 This is a schematic diagram of a partial cross-sectional structure after step S4 of the selective etching method for a P-type polysilicon layer according to the present invention.
[0043] Figure 5 This is a schematic diagram of a partial cross-sectional structure after step S5 of the selective etching method for a P-type polysilicon layer according to the present invention.
[0044] Figure 6 These are surface micrographs of the laser-sintered and non-laser-sintered areas on the back surface of the sample after wet etching, according to Embodiment 1 of the present invention.
[0045] Figure 7 This is a 3D photograph showing the etching depth analysis of the laser-sintered and non-laser-sintered regions on the back surface of the sample after wet etching in Embodiment 1 of the present invention.
[0046] Figure 8 This is a surface micrograph of the laser-sintered and non-laser-sintered areas on the back surface of the sample after wet etching, as shown in Comparative Example 1.
[0047] Figure 9 This is a 3D photograph of the etching depth analysis of the laser-sintered and non-laser-sintered areas on the back surface of the sample after wet etching, which is Comparative Example 1.
[0048] Figure 10 This is a surface micrograph of the back surface of the sample after wet etching, which is Comparative Example 2.
[0049] Reference numerals: 1. Silicon wafer; 2. Tunneling oxide layer; 3. Intrinsic amorphous silicon layer; 31. First p-type polycrystalline silicon layer; 32. Borosilicate glass layer; 4. Intrinsic amorphous silicon reverse osmosis layer; 5. Second p-type polycrystalline silicon layer; 51. Surface oxide layer; 6. Clean n-type silicon surface. Detailed Implementation
[0050] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0051] A selective etching method for a P-type polysilicon layer according to the present invention, see [link to relevant documentation]. Figure 1-5 It includes the following steps:
[0052] Step S1: A tunneling oxide layer 2 and an intrinsic amorphous silicon layer 3 (ia-Si layer) are sequentially deposited on the back side of silicon wafer 1. Therefore, after step S1, silicon wafer 1 with a tunneling oxide layer 2 and an intrinsic amorphous silicon layer 3 deposited on its back side is obtained (e.g., ...). Figure 1 (As shown).
[0053] In step S1, silicon wafer 1 is a double-sided polished silicon wafer, that is, both the front and back sides of silicon wafer 1 have been polished; moreover, silicon wafer 1 is an n-type silicon wafer.
[0054] Step S2: The back side of the silicon wafer 1 after step S1 is subjected to boron diffusion treatment to diffuse boron doping into the intrinsic amorphous silicon layer 3, thereby transforming the amorphous silicon into polycrystalline silicon. Therefore, after boron diffusion treatment, the intrinsic amorphous silicon layer 3 is transformed into a first p-type polycrystalline silicon layer 31 (i.e., a first p-type Si layer, also known as a first boron-doped polycrystalline silicon layer) and a borosilicate glass layer 32 (BSG layer) formed on the outer surface of the first p-type polycrystalline silicon layer 31 (including the back side). That is, after boron diffusion in step S2, the intrinsic amorphous silicon layer 3 is transformed into a first p-type polycrystalline silicon layer 31 and a borosilicate glass layer 32 (i.e., a first p-type Si layer, also known as a first boron-doped polycrystalline silicon layer). Figure 2 (As shown).
[0055] The specific processes of steps S1 and S2 are based on existing technologies and will not be described in detail here.
[0056] Step S3: See Figure 3 An intrinsic amorphous silicon reverse osmosis layer 4 (i.e., ia-Si reverse osmosis layer) is deposited on the back side of the borosilicate glass layer 32.
[0057] In step S3, the deposition process of the intrinsic amorphous silicon reverse osmosis layer 4 includes, but is not limited to, chemical vapor deposition (CVD) and physical vapor deposition (PVD). CVD includes atmospheric pressure CVD, low pressure CVD, plasma-enhanced CVD, high-density plasma-enhanced CVD, and atomic layer deposition (ALD). PVD includes vacuum evaporation deposition, vacuum sputtering deposition, and vacuum ion deposition.
[0058] In one example of the present invention, when the deposition process of the intrinsic amorphous silicon reverse osmosis layer 4 is CVD, the silicon source flow rate is 500-2000 sccm (e.g., 1000 sccm), the deposition temperature is 550-650℃ (e.g., 600℃), and the thickness of the intrinsic amorphous silicon reverse osmosis layer 4 is 100-500 nm (e.g., 200 nm).
[0059] In another example of the present invention, when the deposition process of the intrinsic amorphous silicon reverse osmosis layer 4 is PVD, the main component of the deposition target is silicon (Si), the deposition power is 10-50KV, the deposition temperature is 200-400℃, the pressure in the deposition chamber is less than 10Pa, and the thickness of the intrinsic amorphous silicon reverse osmosis layer 4 is 100-500nm.
[0060] Step S4: Laser sintering (i.e., patterned laser sintering, selective laser sintering, or localized laser sintering) is performed on the back side of the intrinsic amorphous silicon reverse osmosis layer 4 according to a preset pattern on the laser sintering area. This causes the intrinsic amorphous silicon reverse osmosis layer 4, borosilicate glass layer 32, first p-type polycrystalline silicon layer 31, tunneling oxide layer 2, and the back surface layer of silicon wafer 1 to melt sequentially from the outside to the inside in the laser sintering area. This also causes boron in the borosilicate glass layer 32 and the first p-type polycrystalline silicon layer 31 to reverse osmosis into the intrinsic amorphous silicon. Layer 4 and the back surface layer of silicon wafer 1 undergo reverse diffusion, thereby forming a second p-type polysilicon layer 5 (i.e., a second boron-doped polysilicon layer) and a surface oxide layer 51 (surface SiOx layer) oxidized on the back surface of the second p-type polysilicon layer 5 in the laser sintering region. The front side of the second p-type polysilicon layer 5 reaches into the back surface layer of silicon wafer 1, and the boron doping concentration of the second p-type polysilicon layer 5 and the surface oxide layer 51 is less than the boron doping concentration of the first p-type polysilicon layer 31. That is, after the patterned laser sintering in step S4, a second p-type polysilicon layer 5 and a surface oxide layer 51 (i.e., a second boron-doped polysilicon layer) are formed in the laser sintering region. Figure 4 (As shown); moreover, the boron doping concentration of the first p-type polysilicon layer 31 in the non-laser sintering region is still 2E19~1E20cm⁻¹. -3 (e.g. 6E19cm) -3 The boron doping concentration of the surface oxide layer 51 and the second p-type polysilicon layer 5 in the laser sintering region is lower than that of the first p-type polysilicon layer 31 in the non-laser sintering region.
[0061] In step S4, the equipment used in the patterned laser sintering process includes, but is not limited to, all equipment capable of emitting lasers that have a sintering effect, such as the SE (Selective emitter) equipment and LECO equipment (Laser Enhanced Contact Optimization equipment) of the TOPCon cell (tunnel oxide passivated contact cell) production line.
[0062] In step S4, when patterned laser sintering is performed on the back side of the intrinsic amorphous silicon reverse osmosis layer 4 using an SE device, the laser power is 5-30W, the laser wavelength is 400-700nm, and the laser spot area is 200-3000μm. 2 The number of times the light spot is repeatedly sintered is 1-20 times.
[0063] Step S5: Perform wet etching on the silicon wafer 1 processed in step S4 to remove the surface oxide layer 51 in the laser-sintered region, the second p-type polycrystalline silicon layer 5 in the laser-sintered region, and the intrinsic amorphous silicon reverse diffusion layer 4 in the non-laser-sintered region, thereby exposing a clean n-type silicon surface 6 in the laser-sintered region (e.g., ...). Figure 5 (As shown).
[0064] In step S5, the wet etching process includes:
[0065] Step S51: First, use an acidic solution to etch (referred to as acid etching) to remove the surface oxide layer 51; during the acidic solution etching process, the intrinsic amorphous silicon reverse osmosis layer 4 in the non-laser sintering area will not be removed; moreover, during the acidic solution etching process, the borosilicate glass layer 32 in the non-laser sintering area is covered and protected by the intrinsic amorphous silicon reverse osmosis layer 4 and will not be removed.
[0066] In step S51, the acidic solution includes, but is not limited to, a deionized aqueous solution of HF (hydrofluoric acid solution), wherein the concentration of HF is 0.5-10 w.t.%, the etching temperature is 40-80℃, and the etching time is 50-500s.
[0067] Step S52: Then, use an alkaline solution to perform etching (referred to as alkaline etching) to remove the second p-type polycrystalline silicon layer 5 in the laser sintered region and the intrinsic amorphous silicon reverse osmosis layer 4 in the non-laser sintered region.
[0068] In step S52, the alkaline solution comprises a deionized aqueous solution of NaOH (sodium hydroxide) and surface modifier (ADD), wherein the concentration of NaOH is 0.3-5 wt.%, the concentration of surface modifier is 0.01-0.5 wt%, the etching temperature is 50-90℃, and the etching time is 50-500 s.
[0069] At this point, it is important to note that before and after etching in steps S51 and S52, the residual liquid on the surface must be completely washed away with deionized water.
[0070] The selective etching method for a P-type polycrystalline silicon layer shown in steps S1-S5 of the present invention can be applied to the fabrication of solar cells, especially TBC cells.
[0071] The following is a specific embodiment of the selective etching method for a P-type polysilicon layer according to the present invention:
[0072] Example 1
[0073] This embodiment describes a selective etching method for a P-type polysilicon layer. See [link to relevant documentation]. Figure 1-5 It includes the following steps:
[0074] Step S1: A tunneling oxide layer 2 and an intrinsic amorphous silicon layer 3 are sequentially deposited on the back side of silicon wafer 1 (which is a double-sided polished n-type silicon wafer). Therefore, after step S1, a silicon wafer 1 with a tunneling oxide layer 2 and an intrinsic amorphous silicon layer 3 deposited on the back side is obtained (e.g., ...). Figure 1 (As shown).
[0075] Step S2: See Figure 2The back side of the silicon wafer 1 after step S1 is subjected to boron diffusion treatment, so that the intrinsic amorphous silicon layer 3 is transformed into a first p-type polycrystalline silicon layer 31 (i.e., a first boron-doped polycrystalline silicon layer) and a borosilicate glass layer 32 formed on the outer surface of the first p-type polycrystalline silicon layer 31.
[0076] Step S3: See Figure 3 An intrinsic amorphous silicon reverse osmosis layer 4 is deposited on the back side of the borosilicate glass layer 32.
[0077] In step S3 of this embodiment, an intrinsic amorphous silicon reverse osmosis layer 4 is prepared using a PVD deposition process. The deposition process includes: a silicon target material, a deposition power of 25KV, a deposition temperature of 300℃, a pressure in the deposition chamber of less than 10Pa, and a thickness of 200nm for the intrinsic amorphous silicon reverse osmosis layer 4.
[0078] Step S4: See Figure 4 Laser sintering is performed on the back side of the intrinsic amorphous silicon reverse osmosis layer 4 according to a preset pattern, so that the intrinsic amorphous silicon reverse osmosis layer 4, borosilicate glass layer 32, first p-type polycrystalline silicon layer 31, tunneling oxide layer 2 and back surface layer of silicon wafer 1 in the laser sintering area melt sequentially from the outside to the inside, and the boron in borosilicate glass layer 32 and first p-type polycrystalline silicon layer 31 diffuses in the reverse direction to the intrinsic amorphous silicon reverse osmosis layer 4 and back surface layer of silicon wafer 1, thereby forming a second p-type polycrystalline silicon layer 5 (i.e., a second boron-doped polycrystalline silicon layer) and a surface oxide layer 51 oxidized on the back surface of the second p-type polycrystalline silicon layer 5 in the laser sintering area. The front side of the second p-type polycrystalline silicon layer 5 reaches the back surface layer of silicon wafer 1, and the boron doping concentration of the second p-type polycrystalline silicon layer 5 and the surface oxide layer 51 is less than the boron doping concentration of the first p-type polycrystalline silicon layer 31.
[0079] In step S4 of this embodiment, patterned laser sintering is performed on the back side of the intrinsic amorphous silicon reverse osmosis layer 4 using an SE device. The laser power is 15W, the laser wavelength is 550nm, and the laser spot area is 1500μm. 2 The number of times the light spot is repeatedly sintered is 10.
[0080] Step S5: See Figure 5 Wet etching is performed on the silicon wafer 1 after step S4 to remove the surface oxide layer 51 in the laser sintering area, the second p-type polycrystalline silicon layer 5 in the laser sintering area, and the intrinsic amorphous silicon reverse osmosis layer 4 in the non-laser sintering area, thereby exposing a clean n-type silicon surface 6 in the laser sintering area.
[0081] In step S5, the wet etching process includes:
[0082] Step S51: First, use an acidic solution to etch (referred to as acid etching) to remove the surface oxide layer 51.
[0083] In step S51, the acidic solution is a deionized aqueous solution of HF (hydrofluoric acid solution), wherein the concentration of HF is 5 w.t.%, the etching temperature is 60℃, and the etching time is 250s.
[0084] Step S52: Then, use an alkaline solution to perform etching (referred to as alkaline etching) to remove the second p-type polycrystalline silicon layer 5 in the laser sintered region and the intrinsic amorphous silicon reverse osmosis layer 4 in the non-laser sintered region.
[0085] In step S52, the alkaline solution is a deionized aqueous solution of NaOH and surface modifier (ADD), wherein the concentration of NaOH is 2.5 wt%, the concentration of surface modifier is 0.3 wt%, the etching temperature is 80 °C, and the etching time is 250 s.
[0086] Before and after etching in steps S51 and S52, the residual liquid on the surface must be completely cleaned with deionized water.
[0087] The selective etching method for a P-type polycrystalline silicon layer shown in steps S1-S5 of this embodiment can be applied to the fabrication of solar cells, especially TBC cells.
[0088] Comparative Example 1
[0089] This comparative example provides a selective etching method for a P-type polysilicon layer. Steps 1 and 2 are the same as steps S1 and S2 in Example 1, respectively, and steps 3 and 4 are the same as steps S4 and S5 in Example 1. The main difference between this method and Example 1 is:
[0090] Step S3 of Example 1 is omitted in this comparative example.
[0091] Comparative Example 2
[0092] This comparative example provides an etching method for a P-type polysilicon layer. Steps 1 and 2 are the same as steps S1 and S2 in Example 1, respectively. The main difference between this method and Example 1 is that:
[0093] Steps S3 and S4 of Example 1 have been omitted.
[0094] Furthermore, the wet etching process conditions for step 3 of this comparative example are as follows:
[0095] In step 3 of this comparative example, the acidic solution is a deionized aqueous solution of HF (hydrofluoric acid solution), wherein the concentration of HF is 10 w.t.%, the etching temperature is 80℃, and the etching time is 500s.
[0096] In step 3 of this comparative example, the alkaline etching solution is a deionized aqueous solution of NaOH and surface modifier (ADD), wherein the concentration of NaOH is 5 wt.% and the concentration of surface modifier is 0.5 wt%. The etching temperature is 90°C and the etching time is 500 s to accelerate the etching process. The remaining wet etching processes in step 3 of this comparative example are all in accordance with step S5 of Example 1.
[0097] Performance testing
[0098] 1. Surface micrographs of the back surfaces of the samples after wet etching in Example 1, Comparative Example 1, and Comparative Example 2 were collected respectively, as shown in the figures below. Figure 6 , Figure 8 and Figure 10 As shown.
[0099] 2. 3D images of the etching depth analysis of the back surface of the samples after wet etching in Example 1 and Comparative Example 1 were collected respectively, as shown below. Figure 7 and Figure 9 As shown.
[0100] Combination Figure 6-10 Therefore, we can conclude that:
[0101] (1) In Comparative Example 1, no significant difference in etching depth was observed between the laser-sintered area and the non-laser-sintered area on the back surface of the sample after wet etching (e.g., Figure 8-9 As shown in the figure, if step S3 (depositing an intrinsic amorphous silicon reverse diffusion layer 4 on the back side of the borosilicate glass layer 32) is omitted, and patterned laser sintering and wet etching are performed directly (as shown in Comparative Example 1), it is difficult to guide the boron in the borosilicate glass layer 32 and the first p-type polycrystalline silicon layer 31 in the laser sintering region to diffuse in the reverse direction to other layers. As a result, it is difficult to obtain a p-type polycrystalline silicon layer in the laser sintering region with a lower boron doping concentration than that in the non-laser sintering region. Consequently, it is difficult to reduce the wet etching difficulty in the local area of the p-type polycrystalline silicon layer (which is the laser sintering region of the present invention), which will lead to an insignificant difference in etching depth between the laser sintering region and the non-laser sintering region.
[0102] (2) No obvious etching depth was observed on the back surface of the sample after wet etching in Comparative Example 2 (e.g., Figure 10As shown in the figure, if steps S3 (depositing the intrinsic amorphous silicon reverse osmosis layer 4) and S4 (patterning laser sintering) are omitted, and the local area of the first p-type polysilicon layer 31 is directly wet-etched (as shown in Comparative Example 2), even if the etching time is extended to 1000s (500s acid etching time + 500s alkaline etching time) for 500s, it is still difficult to completely remove the local area of the first p-type polysilicon layer 31. This will result in an insignificant etching depth on the back surface of the sample in Comparative Example 2, which further verifies that the p-type polysilicon layer with high boron doping concentration is difficult to be directly removed by wet etching.
[0103] (3) Compared with Comparative Examples 1 and 2, the back surface of the sample after wet etching in Example 1 shows a significant difference in etching depth between the laser-sintered region and the non-laser-sintered region. It can be seen that the selective etching method for the p-type polysilicon layer of the present invention, based on steps S1-S2, combined with steps S3 (depositing intrinsic amorphous silicon reverse osmosis layer 4), S4 (patterned laser sintering), and S5 (wet etching), can shorten the wet etching time, improve etching efficiency and production capacity, and ensure the removal effect of the p-type polysilicon layer (i.e., the second p-type polysilicon layer 5) in the laser-sintered region, thereby reducing its wet etching.
[0104] Although preferred embodiments of the present invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present invention.
[0105] The technical solution provided by the present invention has been described in detail above. Specific examples have been used to illustrate the principle and implementation of the present invention. The description of the above embodiments is only for the purpose of helping to understand the method and core idea of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation and application scope based on the idea of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for selective etching of a P-type polysilicon layer, characterized in that, The selective etching method for the P-type polycrystalline silicon layer is applied to the fabrication of tunnel oxide passivated contact back contact cells, and includes the following steps: Step 1: Sequentially prepare a tunneling oxide layer, a first p-type polycrystalline silicon layer, and a borosilicate glass layer on the back side of the silicon wafer; Step 2: Prepare a reverse osmosis layer on the back side of the first p-type polycrystalline silicon layer; Step 3: Perform patterned laser sintering on the back side of the reverse osmosis layer, so that the reverse osmosis layer, borosilicate glass layer, first p-type polycrystalline silicon layer, tunneling oxide layer and back surface layer of silicon wafer in the laser sintering area melt sequentially, so that the boron in the borosilicate glass layer and the first p-type polycrystalline silicon layer diffuses into the reverse osmosis layer and the back surface layer of silicon wafer, so as to form a second p-type polycrystalline silicon layer with a boron doping concentration lower than that of the first p-type polycrystalline silicon layer on the back surface of silicon wafer in the laser sintering area, and form a surface oxide layer on the back side of the second p-type polycrystalline silicon layer. Step 4: Wet etching to remove the surface oxide layer and the second p-type polysilicon layer of the laser-sintered area to expose the silicon surface of the laser-sintered area, and to remove the reverse osmosis layer of the non-laser-sintered area.
2. The selective etching method for a P-type polysilicon layer according to claim 1, characterized in that, In step 1, the silicon wafer is an n-type silicon wafer that has been polished on both sides; Step 1 specifically includes: Step 11: Sequentially deposit a tunneling oxide layer and an intrinsic amorphous silicon layer on the back side of the silicon wafer; Step 12: Perform boron diffusion treatment on the intrinsic amorphous silicon layer to transform the intrinsic amorphous silicon layer into a first p-type polycrystalline silicon layer and a borosilicate glass layer located on the outer surface of the first p-type polycrystalline silicon layer.
3. The selective etching method for a P-type polysilicon layer according to claim 1, characterized in that, In step 2, the reverse osmosis layer is an intrinsic amorphous silicon layer with a thickness of 100-500 nm. The reverse osmosis layer is prepared by chemical vapor deposition or physical vapor deposition.
4. The selective etching method for a P-type polysilicon layer according to claim 3, characterized in that, In step 2, when preparing the reverse osmosis layer using chemical vapor deposition, the silicon source injection rate is 500-2000 sccm, and the deposition temperature is 550-650℃. Alternatively, when preparing the reverse osmosis layer using physical vapor deposition, a silicon deposition target is used, with a deposition power of 10-50KV, a deposition temperature of 200-400℃, and a pressure of less than 10Pa within the deposition chamber.
5. The selective etching method for a P-type polysilicon layer according to claim 1, characterized in that, In step 3, the process conditions for patterned laser sintering include: laser power of 5-30W, laser wavelength of 400-700nm, and laser spot area of 200-3000μm. 2 The number of times the light spot is repeatedly sintered is 1-20 times.
6. A selective etching method for a P-type polysilicon layer according to claim 1 or 5, characterized in that, In step 3, the patterned laser sintering is performed using SE equipment or laser-enhanced contact optimization equipment in a tunnel oxide passivation contact battery production line.
7. The selective etching method for a P-type polysilicon layer according to claim 1, characterized in that, Step 4 specifically includes: Step 41: First, perform acid etching to remove the surface oxide layer in the laser sintering area; Step 42: Perform alkaline etching to remove the second p-type polysilicon layer in the laser-sintered region and the reverse osmosis layer in the non-laser-sintered region.
8. The selective etching method for a P-type polysilicon layer according to claim 7, characterized in that, In step 41, the acid etching process conditions include: acid etching using hydrofluoric acid solution, with an HF concentration of 0.5-10wt%, an etching temperature of 40-80℃, and an etching time of 50-500s.
9. The selective etching method for a P-type polysilicon layer according to claim 7, characterized in that, In step 42, the alkaline etching process conditions include: alkaline etching using an aqueous solution of NaOH and surface modifiers, wherein the concentration of NaOH is 0.3-5wt%, the concentration of surface modifiers is 0.01-0.5wt%, the etching temperature is 50-90℃, and the etching time is 50-500s.
Citation Information
Patent Citations
Preparation method of TBC battery
CN116845140A
Back structure of TBC battery and preparation method thereof, TBC battery and preparation method thereof
CN119342910B
Inverse diffusion based solar cell selective doping method
CN105140334A
Manufacturing method of TBC structure back contact battery and back contact battery
CN118380513A