A high-strength austenitic stainless steel with a yield strength of 420 MPa
By controlling the chromium-nickel equivalent ratio, Md30 temperature, and carbon-nitrogen solid solution strengthening intensity increment, and optimizing the Cu element content, a high-strength austenitic stainless steel was developed, solving the problems of insufficient corrosion resistance and strength in battery module frame materials, and achieving the effect of high strength and good plasticity.
Patent Information
- Application Number
- CN202510498771.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-21
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-04-21
AI Technical Summary
Existing battery module frame materials, such as galvanized carbon steel plates and aluminum alloys, have insufficient corrosion resistance and strength at the weld joints, and aluminum alloys have poor flame retardancy, making it difficult to meet the high strength and corrosion resistance requirements of new energy vehicle battery module frames.
A high-strength austenitic stainless steel with a yield strength of 420MPa was developed. By controlling the chromium-nickel equivalent ratio, Md30 temperature, and carbon-nitrogen solid solution strengthening strength increment, and optimizing the Cu element content, the material is ensured to have high strength and good plasticity, making it suitable for battery module frames in new energy vehicles.
It achieves a yield strength Rp0.2≥420MPa, tensile strength Rm≥700MPa, and elongation after fracture A≥40%, meeting the high requirements of new energy vehicle battery module frames and solving the technical defects of existing materials.
Smart Images

Figure BDA0005367832360000051
Abstract
Description
Technical Field
[0001] This invention belongs to the field of iron and steel metallurgy technology, and specifically relates to a high-strength austenitic stainless steel with a yield strength of 420MPa. Background Technology
[0002] New energy vehicles use rechargeable batteries as their power source, a relatively mature technology that offers advantages in terms of economy and environmental protection. However, these batteries are highly susceptible to overheating and runaway upon impact, potentially leading to fires or even explosions, endangering lives. The battery module frame, as the load-bearing structure of the battery module, must meet requirements for high strength and rigidity.
[0003] Currently, battery module frames are mainly made of galvanized carbon steel or aluminum alloy, but both materials have certain drawbacks. Specifically, battery module frames sometimes need to be connected by welding. Galvanized carbon steel has poor corrosion resistance at the weld seams and low strength; aluminum alloy has low density, is lightweight, and has good formability, but its flame retardancy is poor, and it can even act as a combustion agent, exacerbating the battery fire during collision deformation. Therefore, considering the current material situation and usage requirements, battery module frame materials need to have high yield strength and a certain yield strength ratio to ensure the energy absorption rate of the battery module frame during a collision and reduce the risk of battery compression. At the same time, battery module frame materials must also have certain corrosion resistance to meet the brand requirements of high-end vehicle models. Based on this, it is necessary to develop a high-strength stainless steel material for new energy battery module frames. Summary of the Invention
[0004] To address the aforementioned technical problems in the existing technology, this invention provides a high-strength austenitic stainless steel with a yield strength of 420 MPa. The chemical composition of this high-strength austenitic stainless steel, by weight percentage, is: C ≤ 0.10%, Si ≤ 1.00%, Mn: 6.00–7.50%, Cr: 17.50–19.50%, Ni: 2.50–4.00%, Cu: 1.00–2.00%, N ≤ 0.25%, with the remainder being Fe and unavoidable impurities. Furthermore, based on the above composition, the chromium-nickel equivalent ratio (CrE / NiE) of the high-strength austenitic stainless steel is controlled between 1.25 and 1.50. d30 The temperature is controlled between 30 and 60℃, and the carbon-nitrogen solid solution strengthening strength increment σ is controlled between 235 and 270 MPa, wherein:
[0005] The chromium equivalent CrE and nickel equivalent NiE are calculated using equations (1) and (2):
[0006] CrE=Gr%+1.5×Si%+Mo% (1)
[0007] NiE=Ni%+30×(C%+N%)+0.5×Mn% (2)
[0008] M d30 The temperature is calculated using equation (3):
[0009] M d30 =551-462×(C%+N%)-9.2×Si%-8.1×Mn%-29×Ni%-13.7×Cr% (3)
[0010] The carbon-nitrogen solid solution strengthening strength increment σ is calculated from equation (4):
[0011] σ = K C ×C%+K N ×N% (4)
[0012] Where K C K N K is the enhancement coefficient. C The value is 400MPa, K N The value is 1200MPa.
[0013] Furthermore, the aforementioned high-strength austenitic stainless steel with a yield strength of 420MPa has an austenitic structure in the solution-annealed state, with a yield strength Rp0.2≥420MPa, tensile strength Rm≥700MPa, and elongation after fracture A≥40%.
[0014] In addition, the present invention also provides a battery module frame for a new energy vehicle, the battery module frame being made of the aforementioned high-strength austenitic stainless steel with a yield strength of 420MPa.
[0015] The high-strength austenitic stainless steel with a yield strength of 420 MPa of the present invention has the following advantages and beneficial effects:
[0016] This invention introduces the chromium-nickel equivalent ratio CrE / NiE, M d30 By controlling the composition of stainless steel using three parameters—temperature, carbonitriding strength increment σ—high strength performance of the material is achieved. Simultaneously, the cold working performance of the material is improved by optimizing the Cu content in the stainless steel. This results in the development of a high-strength austenitic stainless steel with a yield strength of 420 MPa, possessing both high strength and good plasticity. This 420 MPa-grade high-strength austenitic stainless steel exhibits an austenitic structure in the solution-annealed state, with a yield strength Rp0.2 ≥ 420 MPa, tensile strength Rm ≥ 700 MPa, and elongation after fracture A ≥ 40%. This fully meets the high requirements of new energy vehicle battery module frames for stainless steel materials and solves the technical defects caused by existing battery module frames made of galvanized carbon steel plates or aluminum alloys. Detailed Implementation
[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of this invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0018] This invention aims to provide a high-strength austenitic stainless steel with a yield strength of 420 MPa, achieved by introducing a chromium-nickel equivalent ratio and M... d30 The composition of stainless steel is controlled by three parameters: temperature, carbon and nitrogen solid solution strengthening intensity increment, to achieve high strength performance of the material. At the same time, by optimizing the control of Cu element content in stainless steel, the cold working performance of the product is improved, thereby ensuring that the stainless steel material has both high strength and good plasticity.
[0019] Specifically, the chemical composition of the high-strength austenitic stainless steel with a yield strength of 420 MPa provided by this invention, by weight percentage, is as follows: C ≤ 0.10%, Si ≤ 1.00%, Mn: 6.00–7.50%, Cr: 17.50–19.50%, Ni: 2.50–4.00%, Cu: 1.00–2.00%, N ≤ 0.25%, with the remainder being Fe and unavoidable impurities. Furthermore, based on the above composition, the chromium-nickel equivalent ratio CrE / NiE of this austenitic stainless steel is controlled between 1.25 and 1.50, and Mn ≤ 0.25%. d30 The temperature is controlled between 30 and 60℃, and the carbon-nitrogen solid solution strengthening strength increment σ is controlled between 235 and 270 MPa, wherein:
[0020] The chromium equivalent CrE and nickel equivalent NiE are calculated using equations (1) and (2):
[0021] CrE=Gr%+1.5×Si%+Mo% (1)
[0022] NiE=Ni%+30×(C%+N%)+0.5×Mn% (2)
[0023] M d30 Temperature refers to the temperature at which 50% of the austenite in a material will transform into martensite after 30% cold deformation. In this invention, by using M... d30 Maintaining the temperature between 30 and 60°C makes it easier for the material to form deformable martensite during cold deformation, thereby improving the material's strength. d30 The temperature is calculated from equation (3) (unit: °C):
[0024] M d30=551-462×(C%+N%)-9.2×Si%-8.1×Mn%-29×Ni%-13.7×Cr% (3)
[0025] The carbonitriding strength increment σ refers to the strength increment of stainless steel produced by carbonitriding. Carbonitriding refers to the phenomenon where the strength of the base metal (solvent) increases due to the dissolution of C and N solute atoms. The strength increment is directly proportional to the difference in atomic radii between the solute and solvent; the greater the difference in atomic radii, the greater the strength increment. The carbonitriding strength increment σ is calculated using equation (4) (unit: MPa):
[0026] σ = K C ×C%+K N ×N% (4)
[0027] Where K C K N As a strengthening coefficient, K is used in this invention. C The value is 400MPa, K N The value is 1200MPa.
[0028] The design mechanism and rationale for determining the main components of the high-strength austenitic stainless steel with a yield strength of 420 MPa described in this invention are as follows:
[0029] C: C is an element that can strongly form, stabilize, and expand the austenite region. C can also act as a solid solution atom to hinder lattice deformation and improve strength. However, the C content cannot be too high, otherwise it will combine with Cr in the steel to form Cr-rich carbides, reducing the material's corrosion resistance. Therefore, in this invention, the C content is controlled to ≤0.10%.
[0030] Mn: Mn has a strong austenite-stabilizing effect, mainly by reacting with elements such as N to replace Ni. Simultaneously, the addition of Mn increases the solubility of N in steel. Therefore, in this invention, the Mn content is controlled at 6.00–7.50%.
[0031] Nitrogen (N): Nitrogen is a strong austenite-forming and stabilizing element. Adding it to steel can improve material strength by hindering lattice deformation. However, as the N content increases, the tendency to form nitrides and bubbles during solidification increases, affecting the surface quality of the cold-rolled steel sheet. Therefore, in this invention, the N content is controlled to ≤0.25%.
[0032] Ni: Ni is a strong element that expands and stabilizes austenite, reducing the cold work hardening tendency of austenitic stainless steel. However, adding too much will increase production costs. Therefore, in this invention, the Ni content is controlled at 2.50–4.00%.
[0033] Cr: Cr is an important element for steel to obtain corrosion resistance. In stainless steel, Cr ≥ 12.5% can form a stable surface passivation film and improve the corrosion resistance of steel. According to the corrosion resistance requirements of the material, the Cr content is controlled at 17.50 to 19.50% in this invention.
[0034] Cu: Cu can significantly reduce the cold work hardening tendency of austenitic stainless steel and improve the cold workability of the material. However, excessive Cu content will reduce the pitting and stress corrosion resistance of austenitic stainless steel. Therefore, in this invention, the Cu content is controlled at 1.00–2.00%.
[0035] In the high-strength austenitic stainless steel with a yield strength of 420 MPa of the present invention, because C and N atoms are dissolved in the matrix, the migration of large-radius atoms such as Cr, Mn, and Ni is blocked, thereby improving the strength of the material matrix. Moreover, when the material is subjected to external impact, for example, deformation occurs, and part of the austenite transforms into deformed martensite, further enhancing the material strength. Thus, under the combined effects of solid solution of small atomic radius elements and deformed martensite, the high-strength austenitic stainless steel with a yield strength of 420 MPa of the present invention exhibits high strength. Furthermore, by controlling the amount of Cu added in the high-strength austenitic stainless steel with a yield strength of 420 MPa of the present invention, the cold working performance of the product is improved, thereby ensuring that the material possesses both high strength and good plasticity.
[0036] The following detailed description of the high-strength austenitic stainless steel with a yield strength of 420 MPa is provided in conjunction with specific embodiments.
[0037] Example 1
[0038] In Example 1, austenitic stainless steel was smelted using an electric furnace + AOD + LF refining method. The chemical composition was controlled as shown in Table 1, and the chromium-nickel equivalent ratio (CrE / NiE) of this austenitic stainless steel was 1.40. d30 The temperature was 48.31℃, and the carbon and nitrogen solid solution strengthening strength increment σ was 238MPa.
[0039] The molten steel obtained from smelting is continuously cast into a billet with a thickness of 200mm. The billet is then hot-rolled into a plate. The plate is annealed and pickled in a continuous annealing and pickling production line to obtain high-strength austenitic stainless steel finished plate, which can be used, for example, in the manufacture of battery module frames for new energy vehicles.
[0040] Example 2
[0041] In Example 2, austenitic stainless steel was smelted using an electric furnace + VOD + LF refining method. The chemical composition was controlled as shown in Table 1, and the chromium-nickel equivalent ratio (CrE / NiE) of this austenitic stainless steel was 1.38. d30The temperature was 57.45℃, and the carbon-nitrogen solid solution strengthening strength increment σ was 252MPa.
[0042] The molten steel obtained from smelting is continuously cast into a billet with a thickness of 180mm. The billet is then hot-rolled into a plate. The plate is annealed and pickled in a continuous annealing and pickling production line to obtain high-strength austenitic stainless steel finished plate, which can be used, for example, in the manufacture of battery module frames for new energy vehicles.
[0043] Example 3
[0044] In Example 3, austenitic stainless steel was smelted using an electric furnace + AOD + LF refining method. The chemical composition was controlled as shown in Table 1, and the chromium-nickel equivalent ratio (CrE / NiE) of this austenitic stainless steel was 1.28. d30 The temperature was 31.28℃, and the carbon and nitrogen solid solution strengthening strength increment σ was 268MPa.
[0045] The molten steel obtained from smelting is continuously cast into a billet with a thickness of 180mm. The billet is then hot-rolled into a plate. The plate is annealed and pickled in a continuous annealing and pickling production line to obtain high-strength austenitic stainless steel finished plate, which can be used, for example, in the manufacture of battery module frames for new energy vehicles.
[0046] Table 1 Chemical composition of austenitic stainless steel according to embodiments of the present invention
[0047]
[0048] Mechanical property tests were conducted on the austenitic stainless steels of Examples 1 to 3, and the actual test results are shown in Table 2. It can be seen that the yield strength Rp0.2 of the austenitic stainless steels in each example of the present invention is higher than 420 MPa, the tensile strength Rm is higher than 700 MPa, and the elongation A is greater than 40%.
[0049] Table 2 Mechanical properties of austenitic stainless steel in embodiments of the present invention
[0050] Example Yield strength Rp0.2 / MPa Tensile strength Rm / MPa Elongation after fracture A / % Example 1 439 795 47 Example 2 431 785 49 Example 3 448 807 47
[0051] In summary, this invention improves upon existing technologies by introducing the chromium-nickel equivalent ratio and M. d30By controlling the composition of stainless steel using three parameters—temperature, carbonitriding strengthening strength increment, and other parameters—high strength performance of the material is achieved. Simultaneously, the cold working performance of the material is improved by optimizing the Cu content in the stainless steel. This results in the development of a high-strength austenitic stainless steel with a yield strength of 420 MPa, possessing both high strength and good plasticity. This 420 MPa-grade high-strength austenitic stainless steel exhibits an austenitic structure in the solution-annealed state, with a yield strength Rp0.2 ≥ 420 MPa, tensile strength Rm ≥ 700 MPa, and elongation after fracture A ≥ 40%. This fully meets the high requirements of new energy vehicle battery module frames for stainless steel materials and solves the technical defects caused by existing battery module frames made of galvanized carbon steel plates or aluminum alloys.
[0052] It should be noted that, unless otherwise specified, the terms used herein have the meanings commonly understood by those skilled in the art. Furthermore, when a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum. Further, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Moreover, when multiple ranges are provided to describe features, the ranges may be combined. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0053] It should also be noted that, in this document, the term "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device.
[0054] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit them. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the present invention.
Claims
1. A high-strength austenitic stainless steel with a yield strength of 420 MPa, characterized in that, The chemical composition of the high-strength austenitic stainless steel with a yield strength of 420 MPa, by weight percentage, is as follows: C ≤ 0.10%, Si ≤ 1.00%, Mn: 6.00~7.50%, Cr: 17.50~19.50%, Ni: 2.50~4.00%, Cu: 1.00~2.00%, N ≤ 0.25%, with the remainder being Fe and unavoidable impurities. Furthermore, based on the above composition, the chromium-nickel equivalent ratio (CrE / NiE) of the high-strength austenitic stainless steel with a yield strength of 420 MPa is controlled between 1.28 and 1.
40. d30 The temperature is controlled between 30 and 60℃, and the carbonitriding strength increment σ is controlled between 235 and 270 MPa, where: The chromium equivalent CrE and nickel equivalent NiE are calculated using equations (1) and (2): CrE=Gr%+1.5×Si%+Mo% (1) NiE=Ni%+30×(C%+N%)+0.5×Mn% (2) M d30 The temperature is calculated using equation (3): M d30 =551-462×(C%+N%)-9.2×Si%-8.1×Mn%-29×Ni%-13.7×Cr% (3) The carbon-nitrogen solid solution strengthening strength increment σ is calculated from equation (4): σ =K C ×C%+K N ×N% (4) Where K C K N K is the enhancement coefficient. C The value is 400MPa, K N The value is 1200 MPa; Austenitic stainless steel is smelted using an electric furnace + AOD + LF refining method. The molten steel is continuously cast into billets, which are then hot-rolled into plates. The plates are annealed and pickled in a continuous annealing and pickling production line to produce high-strength austenitic stainless steel finished plates. The high-strength austenitic stainless steel with a yield strength of 420MPa has an austenitic structure in the solution-annealed state, with a yield strength Rp0.2≥420MPa, tensile strength Rm≥700MPa, and elongation after fracture A≥40%.
2. A battery module frame for a new energy vehicle, characterized in that, The battery module frame is made of high-strength austenitic stainless steel with a yield strength of 420 MPa as described in claim 1.
Citation Information
Patent Citations
Nickel-saving high-nitrogen austenitic stainless steel with excellent pitting corrosion resistance and sulfuric acid corrosion resistance and manufacturing method
CN112501493A
High-strength medium-nitrogen austenitic stainless steel plate and preparation method
CN117026080A
Economical high-nitrogen easy-to-form austenitic stainless steel and manufacturing method thereof
CN119194252A