Hollow polymer microsphere, pasty molding compound modified based on hollow polymer microsphere and preparation method of pasty molding compound

By preparing hollow polymer microspheres with modified concave and convex rod powder as template agents, the problem of high dielectric constant of traditional epoxy resin-based composite materials is solved, and a paste molding material with low dielectric constant and excellent wave transmissive performance is achieved, which is suitable for the field of high-performance composite materials.

CN120554702APending Publication Date: 2025-08-29JIANGXI GUANGYUAN CHEM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510936128.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-08
Publication Date
2025-08-29

AI Technical Summary

Technical Problem

In the prior art, traditional epoxy resin-based composite materials have a high dielectric constant and unstable performance in humid and heat environments, making it difficult to meet the needs of high-integration electronic equipment and radar systems, and the method of introducing hollow glass microspheres is costly and has complex surface modification.

Method used

The concave and concave rock stone is treated with pickling, calcining and surface modification to form modified concave and concave rod powder as template agent. Hollow polymer microspheres are prepared by suspension polymerization method, and mixed with components such as epoxy resin, acid anhydride curing agent, chopped quartz fiber, calcium carbonate and magnesium hydroxide to form a paste molding material modified by hollow polymer microspheres.

Benefits of technology

It effectively reduces the dielectric constant of the composite material, improves the wave transmittance performance, and maintains good mechanical properties. It is suitable for radar covers, wave transmittance structural materials and electronic packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120554702A_ABST
    Figure CN120554702A_ABST
Patent Text Reader

Abstract

The invention provides a hollow polymer microsphere, a pasty molding compound modified based on the hollow polymer microsphere and a preparation method of the pasty molding compound, and belongs to the technical field of pasty molding compounds. The pasty molding compound comprises the following components: hollow polymer microspheres, epoxy resin, an anhydride curing agent, chopped quartz fibers, calcium carbonate and magnesium hydroxide. The pasty molding compound disclosed by the invention has low dielectric constant, excellent wave-transparent property and good mechanical property, and is suitable for the field of high-performance composite materials such as radomes, wave-transparent structural materials and electronic packaging materials. By introducing the hollow polymer microspheres, the dielectric constant of the composite material is effectively reduced, the wave-transparent performance of the composite material is improved, meanwhile, good mechanical performance is kept, and the composite material has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of paste molding compounds, in particular to hollow polymer microspheres and a paste molding compound modified based on the hollow polymer microspheres and a preparation method thereof. Background Art

[0002] In modern electronics and aerospace, increasingly stringent requirements are placed on the dielectric and wave transmission properties of materials. While traditional epoxy resin-based composites offer excellent mechanical properties and processability, they suffer from high dielectric constants and unstable performance in hot and humid environments, making them difficult to meet the demands of highly integrated electronic devices and radar systems. Consequently, the development of composite materials with low dielectric constants, low dielectric losses, and excellent wave transmission properties has become a research hotspot.

[0003] However, existing technologies rarely incorporate hollow polymer microspheres into molding compound systems, and hollow glass microspheres are often used as fillers. Surface modification methods are complex and costly. Therefore, there is an urgent need for a new paste molding compound with excellent compatibility that can effectively reduce the dielectric constant of composite materials and improve wave transmission performance. Summary of the Invention

[0004] The object of the present invention is to provide a hollow polymer microsphere and a paste molding compound modified based on the hollow polymer microsphere and a preparation method thereof, so as to solve the above technical problems.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing hollow polymer microspheres, comprising the following steps:

[0007] 1) sequentially performing acid washing, calcining and surface modification treatments on attapulgite to obtain modified attapulgite powder;

[0008] 2) using the modified attapulgite powder as a template, adding it to the polymerization reaction solution, and performing a suspension polymerization method. After the polymerization reaction is completed, the attapulgite powder is separated to form hollow polymer microspheres;

[0009] The polymer reaction solution comprises an oil phase and a water phase, wherein the oil phase contains epoxy resin, a diluent and an initiator; and the addition amount of the modified attapulgite powder is 10-30% of the mass of the oil phase.

[0010] Furthermore, the pickling is to use hydrochloric acid or nitric acid to clean the attapulgite, and the concentration of the hydrochloric acid or nitric acid is independently 0.5 to 2 wt%;

[0011] The calcination temperature is 500-800° C., and the calcination time is 3-5 hours.

[0012] Furthermore, the surface modification treatment is to treat the surface of the attapulgite with a silane coupling agent, the addition amount of the silane coupling agent is 0.5-1 wt% of the mass of the attapulgite, and the silane coupling agent is KH550 and / or KH560.

[0013] Furthermore, in the oil phase, the mass ratio of epoxy resin, diluent and initiator is 100:10-20:0.5-3;

[0014] The aqueous phase comprises water, a dispersant and sodium chloride, wherein the concentration of the dispersant in the aqueous phase is 1 to 5 wt %, and the concentration of the sodium chloride in the aqueous phase is 0.1 to 1 wt %;

[0015] The mass ratio of the oil phase to the water phase is 1:1-2.

[0016] Furthermore, the epoxy resin comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and cyclopentadiene epoxy resin;

[0017] The diluent comprises one or more of butyl glycidyl ether, benzyl glycidyl ether and ethylene glycol diglycidyl ether;

[0018] The initiator comprises one or more of diaryliodonium salt, triarylsulfonium salt, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0019] Furthermore, the suspension polymerization method is as follows: ultrasonically dispersing the template in the oil phase, adding the oil phase dropwise to the stirred water phase, and emulsifying at 20-40°C to obtain a stable oil-in-water emulsion; continuing to heat to 70-90°C, keeping warm for 3-6 hours, cooling to room temperature after the end of the insulation, collecting the microsphere products, washing and drying.

[0020] The present invention also provides hollow polymer microspheres prepared by the above preparation method.

[0021] The present invention also provides a hollow polymer microsphere-modified paste molding compound, which is composed of the following components in parts by mass:

[0022]

[0023] Furthermore, the epoxy resin comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and cyclopentadiene epoxy resin;

[0024] The acid anhydride curing agent comprises one or more of phthalic anhydride, pyromellitic dianhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydroanhydride and nadic anhydride;

[0025] The brand of the magnesium hydroxide is one or more of GY-800, GY-3000 and GY-6000; the brand of the calcium carbonate is one or more of CC-800, CC-1250 and CC-3000 produced by Guangyuan Chemical;

[0026] The length of the chopped quartz fibers is 2 to 5 mm.

[0027] The present invention also provides a method for preparing a paste molding compound modified with hollow polymer microspheres, which comprises uniformly mixing the hollow polymer microspheres, epoxy resin, anhydride curing agent, chopped quartz fibers, calcium carbonate and magnesium hydroxide.

[0028] Beneficial effects of the present invention:

[0029] By introducing hollow polymer microspheres, the present invention effectively reduces the dielectric constant of the composite material, improving its wave transmission performance while maintaining good mechanical properties. This paste molding compound is suitable for high-performance composite materials such as radomes, wave-transmitting structural materials, and electronic packaging materials, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a microscopic morphology of the hollow polymer microspheres prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The present invention provides a method for preparing hollow polymer microspheres, comprising the following steps:

[0032] 1) sequentially performing acid washing, calcining and surface modification treatments on attapulgite to obtain modified attapulgite powder;

[0033] 2) using the modified attapulgite powder as a template, adding it to the polymerization reaction solution, and performing a suspension polymerization method. After the polymerization reaction is completed, the attapulgite powder is separated to form hollow polymer microspheres;

[0034] The polymer reaction solution comprises an oil phase and a water phase, wherein the oil phase contains epoxy resin, a diluent and an initiator; and the addition amount of the modified attapulgite powder is 10-30% of the mass of the oil phase.

[0035] In the present invention, the addition amount of the modified attapulgite powder is preferably 15 to 25% of the mass of the oil phase, and more preferably 20%.

[0036] In the present invention, the particle size of the attapulgite is 1 to 30 μm, preferably 5 to 25 μm.

[0037] In the present invention, the acid washing is to use hydrochloric acid or nitric acid to wash the attapulgite, and the concentration of the hydrochloric acid or nitric acid is independently 0.5-2wt%, preferably 1.0-1.5wt%, and more preferably 1.2-1.3wt%; the purpose of acid washing is to remove impurities on the surface of the attapulgite and improve its dispersibility.

[0038] The calcination temperature is 500-800°C, preferably 550-750°C, more preferably 600-700°C; the calcination time is 3-5 hours, preferably 4 hours. The purpose of calcination is to form a porous structure on the surface of the attapulgite, thereby improving its stability as a template.

[0039] In the present invention, the surface modification treatment involves treating the attapulgite surface with a silane coupling agent, the amount of which is 0.5-1 wt% (preferably 0.8 wt%) based on the mass of the attapulgite. The silane coupling agent is KH550 and / or KH560, preferably KH550. The purpose of the surface modification treatment is to enhance the bonding ability between the attapulgite powder and the polymer.

[0040] In the present invention, in the oil phase, the mass ratio of epoxy resin, diluent and initiator is 100:10-20:0.5-3, preferably 100:12-18:1-2, more preferably 100:14-16:1.5-2;

[0041] The aqueous phase comprises water, a dispersant and sodium chloride, wherein the concentration of the dispersant in the aqueous phase is 1 to 5 wt %, and the concentration of the sodium chloride in the aqueous phase is 0.1 to 1 wt %, preferably 0.5 to 0.8 wt %;

[0042] The mass ratio of the oil phase to the water phase is 1:1 to 2, preferably 1:1.

[0043] In the present invention, the epoxy resin is preferably one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and cyclopentadiene epoxy resin;

[0044] The diluent is preferably one or more of butyl glycidyl ether, benzyl glycidyl ether and ethylene glycol diglycidyl ether;

[0045] The initiator is preferably one or more of diaryliodonium salts, triarylsulfonium salts, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0046] In the present invention, the suspension polymerization method comprises: ultrasonically dispersing the template in the oil phase, adding the oil phase dropwise to the stirred aqueous phase, and emulsifying at 20-40°C to obtain a stable water-in-oil emulsion; then heating the mixture to 70-90°C, preferably 80°C; maintaining the temperature for 3-6 hours, preferably 4-5 hours; and cooling the mixture to room temperature after the end of the temperature maintenance period. The resulting microspheres are collected, washed, and dried. The temperature maintenance period allows the epoxy resin to undergo crosslinking and solidification, and nitrogen is continuously introduced during the reaction to prevent oxidation. After the reaction is completed, the microspheres are collected by filtration and repeatedly washed with deionized water and ethanol to remove residual dispersant and unreacted monomers on the surface. The resulting product is then acid-washed with hydrochloric acid or nitric acid at a concentration of 0.5-2 wt%, then centrifuged, washed with water to neutralize the solution, and dried at 100°C to obtain hollow polymer microspheres.

[0047] The present invention also provides hollow polymer microspheres prepared by the above preparation method.

[0048] The present invention also provides a hollow polymer microsphere-modified paste molding compound, which is composed of the following components in parts by mass:

[0049]

[0050] In the present invention, the content of the hollow polymer microspheres is preferably 20 to 40 parts by mass, and more preferably 25 to 35 parts by mass.

[0051] In the present invention, the content of the acid anhydride curing agent is preferably 110 to 120 parts by mass.

[0052] In the present invention, the content of the chopped quartz fibers is preferably 22 to 28 parts by mass, more preferably 25 parts by mass.

[0053] In the present invention, the content of calcium carbonate is preferably 25 to 35 parts by mass, more preferably 30 parts by mass.

[0054] In the present invention, the content of the magnesium hydroxide is preferably 22 to 28 parts by mass, more preferably 25 parts by mass.

[0055] In the present invention, the epoxy resin is preferably one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and cyclopentadiene epoxy resin;

[0056] The acid anhydride curing agent is preferably one or more of phthalic anhydride, pyromellitic dianhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydroanhydride and nadic anhydride;

[0057] The brand of the magnesium hydroxide is preferably one or more of GY-800, GY-3000 and GY-6000; the brand of the calcium carbonate is preferably one or more of CC-800, CC-1250 and CC-3000 produced by Guangyuan Chemical;

[0058] The length of the chopped quartz fibers is 2 to 5 mm, preferably 3 to 4 mm.

[0059] The present invention also provides a method for preparing a paste molding compound modified with hollow polymer microspheres, which comprises uniformly mixing the hollow polymer microspheres, epoxy resin, anhydride curing agent, chopped quartz fibers, calcium carbonate and magnesium hydroxide.

[0060] In the present invention, the obtained paste molding compound is pressed into a composite material plate, the pressing pressure is 2 to 10 MPa, preferably 5 to 8 MPa, and the pressing time is 2 to 4 hours, preferably 3 hours.

[0061] The technical solutions provided by the present invention are described in detail below with reference to the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0062] Example 1

[0063] Preparation of the template: Natural attapulgite with a particle size of 10 microns was selected and pickled with 1% dilute hydrochloric acid to remove surface impurities; it was then calcined at 600°C for 3 hours to form a porous structure on its surface; finally, 0.9wt% of a coupling agent was added to graft the silane coupling agent KH550 on the surface of the attapulgite to obtain modified attapulgite powder.

[0064] Preparation of hollow polymer microspheres: In an oil phase system, 100 parts of bisphenol A epoxy resin, 15 parts of butyl glycidyl ether diluent, and 1 part of diaryliodonium salt initiator were mixed uniformly. A modified attapulgite powder template (20% by weight of the oil phase) was added, and ultrasonic dispersion was performed for 30 minutes. In an aqueous phase system, 3 wt% of polyvinyl alcohol dispersant was dissolved in deionized water, and 0.5 wt% of sodium chloride was added to adjust the ionic strength. The oil phase was slowly added dropwise to the vigorously stirred aqueous phase at a 1:1 oil phase to aqueous phase ratio. Emulsification was performed at 25°C to form a stable water-in-oil emulsion. The temperature was raised to 80°C and the reaction was maintained for 4 hours, with nitrogen continuously flowing throughout the reaction. After the reaction, the mixture was cooled to room temperature and acid-washed with 1 wt% hydrochloric acid. The mixture was centrifuged, washed with water to neutralize the solution, and dried at 100°C to obtain hollow polymer microspheres.

[0065] Preparation of paste molding compound: 10 parts of the prepared hollow polymer microspheres were mixed evenly with 100 parts of bisphenol A epoxy resin, 110 parts of pyromellitic dianhydride curing agent, 3 mm long chopped quartz fiber, 30 parts of CC-1250 calcium carbonate produced by Guangyuan Chemical, and 30 parts of GY-3000 magnesium hydroxide. The mixture was pressed into a composite material plate under the conditions of a pressing temperature of 180°C, a pressing pressure of 6 MPa, and a pressing time of 3 h.

[0066] Performance test: dielectric constant 2.8; dielectric loss 0.008; impact strength 25kJ / m2.

[0067] Example 2

[0068] Preparation of the template: Natural attapulgite with a particle size of 15 microns was used and pickled with 1.5% nitric acid; calcined at 700°C for 4 hours to form a porous structure on its surface; finally, 1wt% of a coupling agent was added to graft the silane coupling agent KH560 on the surface of the attapulgite to obtain modified attapulgite powder.

[0069] Preparation of hollow polymer microspheres: The oil phase system contains 100 parts of bisphenol F epoxy resin, 12 parts of benzyl glycidyl ether diluent, and 1.5 parts of triarylsulfonium salt initiator. A modified attapulgite powder template accounting for 15% of the oil phase mass is added and ultrasonically dispersed for 30 minutes. The aqueous phase system is prepared in the same way as in Example 1. During suspension polymerization, the oil phase is slowly added dropwise to the vigorously stirred aqueous phase at a mass ratio of 1:1. Emulsification is carried out at a certain temperature to form a stable oil-in-water emulsion. The temperature is raised to 75°C and the reaction is kept warm for 5 hours under nitrogen protection. After the reaction is completed, the hollow polymer microspheres are obtained by acid washing with 0.8wt% nitric acid, centrifugation, washing, and drying.

[0070] Preparation of paste molding compound: Mix 30 parts of hollow polymer microspheres with 100 parts of bisphenol F epoxy resin, 115 parts of tetrahydrophthalic anhydride curing agent, 20 parts of chopped quartz fiber with a length of 2.5 mm, 30 parts of Guangyuan Chemical CC-800 calcium carbonate, and 20 parts of GY-800 magnesium hydroxide, and press them into a composite material plate at 180°C, a pressing pressure of 5 MPa, and a pressing time of 3.5 hours.

[0071] Performance test: dielectric constant 2.9; dielectric loss 0.009; impact strength 22kJ / m2.

[0072] Example 3

[0073] Preparation of the template: Natural attapulgite with a particle size of 20 microns was pickled with 0.8% dilute hydrochloric acid; calcined at 550°C for 5 hours to form a porous structure on its surface; and finally, 0.8wt% of a coupling agent was added to graft a mixture of silane coupling agents KH550 and KH560 onto the surface of the attapulgite to obtain modified attapulgite powder.

[0074] Preparation of hollow polymer microspheres: The oil phase system consists of 100 parts cyclopentadiene epoxy resin, 18 parts ethylene glycol diglycidyl ether as diluent, and 0.8 parts 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO) as initiator. A modified attapulgite powder template (25% by weight of the oil phase) is added and ultrasonically dispersed for 30 minutes. The aqueous phase system is prepared as in Example 1. During suspension polymerization, the oil phase is slowly added dropwise to the vigorously stirred aqueous phase at a mass ratio of 1:1.5. Emulsification is performed at a constant temperature to form a stable water-in-oil emulsion. The reaction is then heated to 85°C and maintained for 3.5 hours under nitrogen protection. After the reaction, the hollow polymer microspheres are treated with 1.2 wt% hydrochloric acid pickling to obtain the hollow polymer microspheres.

[0075] Preparation of paste molding compound: 40 parts of hollow polymer microspheres are mixed with 100 parts of cyclopentadiene epoxy resin, 120 parts of methyl tetrahydroanhydride curing agent, 30 parts of 2 mm long chopped quartz fiber, 30 parts of Guangyuan Chemical CC-3000 calcium carbonate, and 20 parts of GY-6000 magnesium hydroxide, and pressed into a composite material plate under the conditions of pressing temperature of 180°C, pressing pressure of 7 MPa, and pressing time of 2.5 h.

[0076] Performance test: dielectric constant 2.7; dielectric loss 0.007; impact strength 26kJ / m 2 .

[0077] Comparative Example 1

[0078] 100 parts of bisphenol A epoxy resin, 100 parts of pyromellitic dianhydride curing agent, 3 mm long chopped quartz fiber, 30 parts of CC-1250 calcium carbonate produced by Guangyuan Chemical, and 30 parts of GY-3000 magnesium hydroxide were directly mixed and evenly pressed into a composite material plate under the conditions of a pressing temperature of 180°C, a pressing pressure of 6 MPa, and a pressing time of 3 h. No hollow polymer microspheres were added.

[0079] Performance test: dielectric constant 3.8; dielectric loss 0.018; impact strength 18kJ / m2.

[0080] As can be seen from the above examples, the present invention provides hollow polymer microspheres, a paste molding compound modified with these hollow polymer microspheres, and methods for preparing the same. The paste molding compound of the present invention exhibits a low dielectric constant, excellent wave transmission, and good mechanical properties, making it suitable for use in high-performance composite materials such as radomes, wave-transmitting structural materials, and electronic packaging materials. By introducing hollow polymer microspheres, the present invention effectively reduces the dielectric constant of the composite material and improves its wave transmission while maintaining good mechanical properties, thus possessing broad application prospects.

[0081] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing hollow polymer microspheres, characterized in that: The following steps are involved: 1) sequentially performing acid washing, calcining and surface modification treatments on attapulgite to obtain modified attapulgite powder; 2) using the modified attapulgite powder as a template, adding it to the polymerization reaction solution, and performing a suspension polymerization method. After the polymerization reaction is completed, the attapulgite powder is separated to form hollow polymer microspheres; The polymer reaction solution comprises an oil phase and a water phase, wherein the oil phase contains epoxy resin, a diluent and an initiator; and the addition amount of the modified attapulgite powder is 10-30% of the mass of the oil phase.

2. The method for preparing hollow polymer microspheres according to claim 1, wherein: The pickling is to use hydrochloric acid or nitric acid to clean the attapulgite, and the concentration of the hydrochloric acid or nitric acid is independently 0.5 to 2 wt%; The calcination temperature is 500-800° C., and the calcination time is 3-5 hours.

3. The method for preparing hollow polymer microspheres according to claim 2, wherein: The surface modification treatment is to treat the surface of the attapulgite with a silane coupling agent, the addition amount of the silane coupling agent is 0.5-1wt% of the mass of the attapulgite, and the silane coupling agent is KH550 and / or KH560.

4. The method for preparing hollow polymer microspheres according to claim 1 or 3, characterized in that: In the oil phase, the mass ratio of epoxy resin, diluent and initiator is 100:10-20:0.5-3; The aqueous phase comprises water, a dispersant and sodium chloride, wherein the concentration of the dispersant in the aqueous phase is 1 to 5 wt %, and the concentration of the sodium chloride in the aqueous phase is 0.1 to 1 wt %; The mass ratio of the oil phase to the water phase is 1:1-2.

5. The method for preparing hollow polymer microspheres according to claim 4, wherein: The epoxy resin comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and cyclopentadiene epoxy resin; The diluent comprises one or more of butyl glycidyl ether, benzyl glycidyl ether and ethylene glycol diglycidyl ether; The initiator comprises one or more of diaryliodonium salt, triarylsulfonium salt, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

6. The method for preparing hollow polymer microspheres according to claim 1 or 5, characterized in that: The suspension polymerization method comprises the following steps: ultrasonically dispersing the template in the oil phase, dropping the oil phase into the stirred water phase, and emulsifying at 20-40° C. to obtain a stable water-in-oil emulsion; continuously heating the mixture to 70-90° C. and keeping the temperature for 3-6 hours. After the temperature is kept, the mixture is cooled to room temperature, the microsphere products are collected, washed, and dried.

7. Hollow polymer microspheres prepared by the method for preparing hollow polymer microspheres according to any one of claims 1 to 6.

8. A paste molding compound modified with hollow polymer microspheres, characterized in that: It is composed of the following components in parts by mass: The method according to claim 7 9. The hollow polymer microsphere-modified paste molding compound according to claim 8, characterized in that: The epoxy resin comprises one or more of bisphenol A epoxy resin, bisphenol F epoxy resin and cyclopentadiene epoxy resin; The acid anhydride curing agent comprises one or more of phthalic anhydride, pyromellitic dianhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydroanhydride and nadic anhydride; The brand of the magnesium hydroxide is one or more of GY-800, GY-3000 and GY-6000; the brand of the calcium carbonate is one or more of CC-800, CC-1250 and CC-3000 produced by Guangyuan Chemical; The length of the chopped quartz fibers is 2 to 5 mm.

10. The method for preparing the paste molding compound modified with hollow polymer microspheres according to claim 8 or 9, characterized in that: The hollow polymer microspheres, epoxy resin, anhydride curing agent, short-cut quartz fibers, calcium carbonate and magnesium hydroxide are uniformly mixed.