Tungsten copper block and chromium zirconium copper brazing method for thermonuclear fusion
By spraying copper-based brazing filler metal powder on the surface of tungsten-copper blocks and chromium-zirconium-copper, the problems of high equipment cost and poor thermal conductivity in the existing welding process are solved, efficient and precise welding connections are achieved, and the stable operation capability of the fusion device is improved.
Patent Information
- Application Number
- CN202511000893.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-21
- Publication Date
- 2025-09-05
AI Technical Summary
The existing welding process of tungsten copper blocks and chromium zirconium copper has the disadvantages of high equipment cost, low single-batch production capacity, insufficient welding, and difficult to control foil thickness, resulting in poor thermal conductivity. In addition, the process is complex, which increases cost and difficulty, affecting the long-term stable operation of the fusion device.
The copper-based brazing filler metal powder is evenly sprayed on the tungsten copper block and the chromium zirconium copper to be welded using spraying technology to form a 0.05mm to 0.4mm brazing filler metal layer, and then heated to 930℃ to 1050℃ under a protective atmosphere and kept warm for 5min to 40min to complete the brazing connection.
It improves the welding rate and welding accuracy, reduces thermal resistance, improves thermal conductivity, simplifies the process, reduces costs, and extends the service life of components.
Smart Images

Figure CN120587575A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heterogeneous material welding, and particularly relates to a method for brazing a tungsten-copper block and chromium-zirconium-copper for thermonuclear fusion. Background Art
[0002] The divertor is a key component in a fusion reactor that withstands extreme heat loads and particle flow impacts. The core of its manufacturing lies in achieving a high-performance connection between tungsten copper (plasma-facing material) and chromium zirconium copper (heat sink material). Existing technology has significant drawbacks:
[0003] The existing welding processes for tungsten copper blocks and chromium zirconium copper are mainly divided into hot isostatic pressing welding and brazing. The hot isostatic pressing process has problems such as high equipment cost, low single-batch production capacity, and difficulty in meeting engineering needs. The main problem with the brazing process is that the brazing paste is unevenly applied, resulting in insufficient welding. The preparation process of the foil brazing material is complicated, and the thickness uniformity is difficult to control, which makes the foil assembly difficult. In addition, the thickness of the foil directly affects the thermal conductivity efficiency. At present, the thickness of the foil is difficult to achieve below 0.1mm, which will have a great impact on the thermal conductivity of the product. The foil has high hardness and poor ductility. When it is bonded to complex curved surfaces, it requires the assistance of laser precision etching, which significantly increases the complexity and cost of the process.
[0004] The above-mentioned problems cause existing divertor components to be prone to local overheating and increased interface thermal resistance during service, becoming a key bottleneck restricting the long-term stable operation of fusion devices. Summary of the Invention
[0005] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion, thereby solving the welding problem of tungsten copper blocks and chromium zirconium copper.
[0006] In order to solve the technical problem, the technical method of the present invention is: a method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion, comprising the following steps:
[0007] Step 1: Surface treatment is performed on the oxygen-free copper surface to be welded and the chromium-zirconium copper surface to be welded of the tungsten copper block, the roughness is controlled to 0.8um≤Ra≤3.2um, and ultrasonic cleaning is performed on them, and drying is performed after cleaning;
[0008] Step 2: Use spraying technology to evenly spray copper-based solder powder on the oxygen-free copper surface to be welded and the chromium-zirconium-copper surface to be welded of the cleaned tungsten copper block to form a solder layer with a thickness of 0.05mm to 0.4mm;
[0009] Step 3: Tightly assemble the tungsten copper sprayed with copper-based brazing filler metal powder and the chromium zirconium copper, heat to 930℃~1050℃ under protective atmosphere, and keep warm for 5min~40min to complete the brazing connection.
[0010] Preferably, the grade of the oxygen-free copper of the tungsten copper block in step 1 is TU1, TU0 or TU00.
[0011] Preferably, in step 1, the surface treatment of the oxygen-free copper surface to be welded and the chromium-zirconium-copper surface to be welded of the tungsten-copper block is grinding.
[0012] Preferably, the copper-based solder powder in step 2 has a particle size of 20 μm to 80 μm.
[0013] Preferably, the spraying technology of the copper-based solder powder in step 2 is atmospheric plasma spraying, vacuum plasma spraying, cold spraying or supersonic flame spraying.
[0014] Preferably, in step 2, the copper-based solder powder is sprayed only on the surface to be welded of the oxygen-free copper of the tungsten copper block.
[0015] Preferably, in step 2, the copper-based solder powder is sprayed only on the surface to be welded of the chromium-zirconium-copper;
[0016] Preferably, in step 2, the copper-based solder powder is sprayed onto the oxygen-free copper surface to be welded and the chromium-zirconium-copper surface to be welded of the tungsten-copper block respectively.
[0017] Preferably, in step 3, the protective atmosphere includes nitrogen, argon, helium or vacuum; the purity of nitrogen is ≥99.99%, the purity of argon is ≥99.99%, the purity of helium is ≥99.99%, and the vacuum degree is ≤1×10-3Pa.
[0018] The heating method in step 3 is induction heating, resistance heating or radiation heating.
[0019] Compared with the prior art, the advantages of the present invention are:
[0020] (1) The present invention discloses a method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion. The method uses a spraying technique to evenly disperse and spread solder powder on the surface to be welded, thereby improving the welding rate and welding accuracy, and avoiding problems such as poor welding quality caused by manual application of solder paste or surface defects of foil.
[0021] (2) The overspray technology of the present invention can control the solder powder to a required thickness, reduce thermal resistance, and improve thermal conductivity;
[0022] (3) The present invention adopts the method of spraying powder, which reduces multiple processes such as foil preparation, foil assembly and solder paste coating, reduces costs and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 , the present invention provides a method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion. DETAILED DESCRIPTION
[0024] The specific implementation of the present invention is described below in conjunction with examples:
[0025] It should be noted that the contents shown in the drawings of this specification are only used to match the principles, features and content descriptions disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the conditions under which the present invention can be implemented. Without affecting the effects and purposes that can be achieved by the present invention, they should still fall within the scope of the technical content disclosed in the present invention.
[0026] like Figure 1 As shown, the present invention discloses a method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion, comprising the following steps:
[0027] Step 1: Surface treatment is performed on the oxygen-free copper surface to be welded and the chromium-zirconium copper surface to be welded of the tungsten copper block, the roughness is controlled to 0.8um≤Ra≤3.2um, and ultrasonic cleaning is performed on them, and drying is performed after cleaning;
[0028] Step 2: Use spraying technology to evenly spray copper-based solder powder on the oxygen-free copper surface to be welded and the chromium-zirconium-copper surface to be welded of the cleaned tungsten copper block to form a solder layer with a thickness of 0.05mm to 0.4mm;
[0029] Step 3: Tightly assemble the tungsten copper sprayed with copper-based brazing filler metal powder and the chromium zirconium copper, heat to 930℃~1050℃ under protective atmosphere, and keep warm for 5min~40min to complete the brazing connection.
[0030] Example 1
[0031] This embodiment includes the following steps:
[0032] (1) The oxygen-free copper (TU1) surface to be welded of the tungsten copper sheet was ground to Ra0.8um, and the surface to be welded of the chromium zirconium copper plate was ground to Ra3.2um, and then ultrasonically cleaned and dried with anhydrous ethanol to ensure that there were no defects such as oxidation on the surface;
[0033] (2) Using plasma spraying method, CuMn38Ni9 powder is sprayed on the oxygen-free copper surface to be welded of the tungsten copper sheet, and the spraying thickness is 0.05mm-0.1mm;
[0034] (3) The sprayed tungsten copper sheet and the chromium zirconium copper plate are tightly fitted together and heated in a nitrogen atmosphere at a heating temperature of 1050°C and a holding time of 5 minutes to achieve a brazing connection between the flat tungsten copper sheet and the chromium zirconium copper plate.
[0035] Results: welding rate>98%, shear strength 170MPa, tungsten surface temperature 793℃ after 1000 times of 20MW thermal irradiation.
[0036] Example 2
[0037] This embodiment includes the following steps:
[0038] (1) The oxygen-free copper (TU00) surface to be welded of the tungsten copper block is milled to Ra2.4um, and the surface to be welded of the chromium zirconium copper tube is turned to Ra1.6um, and then ultrasonically cleaned and dried with anhydrous ethanol to ensure that there are no defects such as oxidation on the surface;
[0039] (2) using supersonic flame spraying to spray Cu12MnNi4 powder on the oxygen-free copper surface to be welded of the tungsten copper block, with a spraying thickness of 0.2mm-0.25mm, and using plasma spraying to spray Cu12MnNi4 powder on the surface to be welded of the chromium zirconium copper tube, with a spraying thickness of 0.1mm-0.15mm;
[0040] (3) The sprayed tungsten copper block and the chromium zirconium copper tube are tightly fitted together and heated in a vacuum atmosphere at a heating temperature of 1000°C and a holding time of 20 minutes to achieve the brazing connection between the through-tube type tungsten copper block and the chromium zirconium copper tube.
[0041] Results: welding rate>99%, shear strength 200MPa, tungsten surface temperature 1068℃ after 15WM thermal irradiation 2000 times.
[0042] Example 3
[0043] This embodiment includes the following steps:
[0044] (1) Grind the oxygen-free copper (TU00) surface of the tungsten copper sheet to be welded to Ra3.2um, and grind the surface of the chromium zirconium copper plate to be welded to Ra0.8um, and then ultrasonically clean and dry them with anhydrous ethanol to ensure that there are no defects such as oxidation on the surface;
[0045] (2) Using a cold spraying method, CuSn19Ti10 powder is sprayed on the oxygen-free copper surface to be welded of the tungsten copper sheet with a spraying thickness of 0.1 mm to 0.15 mm. Using a supersonic flame spraying method, CuSn19Ti10i powder is sprayed on the surface to be welded of the chromium zirconium copper plate with a spraying thickness of 0.35 mm to 0.4 mm.
[0046] (3) The sprayed tungsten copper sheet and the chromium zirconium copper plate are tightly fitted together and heated in an argon atmosphere at a temperature of 930°C and a holding time of 40 minutes to achieve a brazing connection between the flat tungsten copper sheet and the chromium zirconium copper plate.
[0047] Results: welding rate>97%, shear strength 160MPa, tungsten surface temperature 805℃ after 1000 times of 20MW thermal irradiation.
[0048] Comparative Example 1
[0049] The spray coating method in step 2 of Example 3 was replaced with a 0.45-0.55 mm thick CuMn38Ni9 solder paste. The flat tungsten-copper sheet / chromium-zirconium-copper plate structure of Comparative Example 1 was then obtained according to step 3. Weldability, shear strength, and 1000 cycles of 20 MW thermal irradiation tests were conducted. The weldability, shear strength, and tungsten surface temperature are shown in Table 1.
[0050] Table 1 Comparison of Example 3 and Comparative Example 1
[0051]
[0052] From the comparison in Table 1, it can be seen that the flat-type tungsten copper sheet / chromium zirconium copper plate prepared by spraying has a high welding rate and high shear strength. The tungsten surface temperature after 1000 times of 20MW thermal irradiation can be judged that the thermal diffusion coefficient of the spraying method is higher, so the tungsten surface temperature is lower.
[0053] Comparative Example 2
[0054] The brazing filler metal in step 2 of Example 2 was replaced with a 0.3-0.4 mm thick Cu12MnNi4 foil. The tube-penetrating tungsten copper block / chromium zirconium copper tube structure of Comparative Example 2 was then obtained according to step 3. Weldability, shear strength, and 2000 cycles of 15 MW thermal irradiation tests were conducted. The weldability, shear strength, and tungsten surface temperature are shown in Table 2.
[0055] Table 2 Comparison of Example 2 and Comparative Example 1
[0056] Welding rate Shear strength Tungsten surface temperature Example 2 >99% 200MPa 1068℃ Comparative Example 2 >88% 146MPa 1150℃
[0057] From the comparison in Table 2, it can be seen that the through-tube type tungsten copper block / chromium zirconium copper prepared by spraying has a high welding rate and high shear strength. The tungsten surface temperature after 2000 times of 15MW thermal irradiation can be judged that the thermal diffusion coefficient of the spraying method is higher, so the tungsten surface temperature is lower.
[0058] The present invention achieves precise control of the brazing material layer through powder spraying technology, significantly improving the thermal conductivity and service life of the divertor components, and providing a technological breakthrough for the manufacturing of key components of fusion reactors.
[0059] The present invention discloses a method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion. The method can evenly disperse the brazing material powder on the surface to be welded by spraying technology, thereby improving the welding rate and welding accuracy, and avoiding problems such as poor welding quality caused by manual application of brazing paste or surface defects of foil.
[0060] Various changes can be made within the scope of knowledge possessed by ordinary geologists in this field without departing from the scope of the present invention.
[0061] Many other changes and modifications can be made without departing from the spirit and scope of the present invention. It should be understood that the present invention is not limited to the specific embodiments, and the scope of the present invention is defined by the appended claims.
Claims
1. A method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion, characterized in that: The following steps are involved: Step 1: Surface treatment is performed on the oxygen-free copper surface to be welded and the chromium-zirconium copper surface to be welded of the tungsten copper block, the roughness is controlled to 0.8um≤Ra≤3.2um, and ultrasonic cleaning is performed on them, and drying is performed after cleaning; Step 2: Use spraying technology to evenly spray copper-based solder powder on the oxygen-free copper surface to be welded and the chromium-zirconium-copper surface to be welded of the cleaned tungsten copper block to form a solder layer with a thickness of 0.05mm to 0.4mm; Step 3: Tightly assemble the tungsten copper sprayed with copper-based brazing filler metal powder and the chromium zirconium copper, heat to 930℃~1050℃ under protective atmosphere, and keep warm for 5min~40min to complete the brazing connection.
2. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: The grade of oxygen-free copper of the tungsten copper block in step 1 is TU1, TU0 or TU00.
3. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: In step 1, the surface treatment of the oxygen-free copper to be welded surface and the chromium-zirconium copper to be welded surface of the tungsten copper block is grinding.
4. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: The copper-based solder powder in step 2 has a particle size of 20 μm to 80 μm.
5. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: The spraying technology of the copper-based solder powder in step 2 is atmospheric plasma spraying, vacuum plasma spraying, cold spraying or supersonic flame spraying.
6. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: In step 2, the copper-based solder powder is sprayed only on the surface of the oxygen-free copper of the tungsten copper block to be welded.
7. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: In step 2, the copper-based solder powder is sprayed only on the surface to be welded of the chromium-zirconium-copper.
8. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: In step 2, the copper-based solder powder is sprayed on the oxygen-free copper surface to be welded and the chromium-zirconium-copper surface to be welded of the tungsten-copper block respectively.
9. The method for brazing tungsten copper blocks and chromium zirconium copper for thermonuclear fusion according to claim 1, characterized in that: In step 3, the protective atmosphere includes nitrogen, argon, helium or vacuum; the purity of nitrogen is ≥99.99%, the purity of argon is ≥99.99%, the purity of helium is ≥99.99%, and the vacuum degree is ≤1×10 -3 Pa.