A type of cable filled with flame-retardant composite fiber paper rope
By combining inorganic and organic materials and using the synergistic effect of modified flame retardants, the problems of insufficient flame retardant and mechanical properties of cable filling materials have been solved, achieving high-efficiency flame retardancy, durability and safety of cables, and promoting the environmentally friendly and safe development of the cable industry.
Patent Information
- Application Number
- CN202510670303.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-23
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2045-05-23
AI Technical Summary
Existing cable filling materials are inadequate in terms of flame retardancy, mechanical properties, and durability. In particular, their mechanical properties gradually decrease after prolonged use, which limits the stability and safety of the cable.
By employing a rational combination of inorganic and organic materials, and through the synergistic effect of modified inorganic flame retardants, organic flame retardants, antioxidants, and ultraviolet absorbers, combined with crosslinking agents and toughening agents, a flame-retardant composite fiber paper rope for cable filling is formed, thereby improving the flame retardant performance, mechanical strength, and aging resistance of the material.
It significantly improves the flame retardant properties, mechanical strength, and oxidation resistance of cable filling materials, ensuring stability and safety under high temperature and long-term use conditions, and extending the service life of cables.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable filling paper rope technology, and more specifically, to a cable filling flame-retardant composite fiber paper rope. Background Technology
[0002] With the rapid development of industries such as power and communications, cables, as a critical infrastructure, play a vital role. Especially in the selection of internal filling materials for cables, properties such as fire resistance, flame retardancy, and aging resistance are crucial. Traditional cable filling materials mostly use natural or synthetic fibers, but these materials are prone to combustion in fire or high-temperature environments, potentially posing significant safety hazards. Therefore, developing filling materials with good flame-retardant properties has become an urgent need in the current cable manufacturing industry.
[0003] In the past, research on flame-retardant composite materials focused on the addition of flame retardants, with inorganic flame retardants (such as magnesium hydroxide) and small-molecule organic flame retardants (such as DOPO) being widely used. However, a single flame retardant often cannot fully meet the requirements of cable filling materials in terms of flame retardancy, mechanical properties, and durability. Therefore, more and more research is beginning to focus on designing composite materials that combine the advantages of inorganic and organic materials to develop highly efficient flame-retardant composite materials.
[0004] Currently, some composite fiber paper rope materials are available on the market. Although they possess certain flame-retardant properties, they still have shortcomings in terms of tensile strength, aging resistance, and processing performance. For example, while flame-retardant properties have been improved to some extent, the mechanical properties of the material gradually decrease after prolonged use, leading to limitations in the stability and safety of the cable.
[0005] Therefore, developing a new type of flame-retardant composite fiber paper rope for cable filling, employing a rational combination of inorganic and organic materials, particularly through the synergistic effects of flame retardant modification, antioxidants, and UV absorbers, can effectively improve the material's flame-retardant properties and mechanical strength while ensuring its stability under high-temperature and long-term use conditions. This technological advancement will not only enhance cable safety but also bring new technological breakthroughs to the cable industry, propelling it towards a more environmentally friendly, safe, and durable direction.
[0006] With the increasing demand for green, environmentally friendly, and high-performance materials, future research on flame-retardant composite fiber paper ropes for cable filling will focus more on multifunctionality, high efficiency, and environmental friendliness. Summary of the Invention
[0007] The purpose of this invention is to provide a cable-filled flame-retardant composite fiber paper rope, which has excellent flame-retardant properties, good mechanical strength and anti-aging properties.
[0008] A flame-retardant composite fiber paper rope for cable filling, characterized in that: the flame-retardant composite fiber paper rope for cable filling has the following component ratio: 35-50 parts of inorganic material composition, 100 parts of organic material composition, 30-42 parts of modified inorganic flame retardant, 2-6 parts of organic flame retardant, 1-3 parts of antioxidant composition, 0.4-2 parts of ultraviolet absorber composition, 0.4-2 parts of crosslinking agent, 2-6 parts of toughening agent, 4-10 parts of reinforcing agent, and 0.6-1 parts of flow agent.
[0009] Preferably, the inorganic material composition is aluminum silicate fiber and expanded perlite in a mass ratio of 1:1.
[0010] Preferably, the organic material composition is polypropylene fiber and polyester fiber in a mass ratio of 1:1.5.
[0011] Preferably, the modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. The preparation method is as follows: γ-aminopropyltriethoxysilane and aluminum hydroxide are placed in a reaction vessel with a mass ratio of 0.4-0.6:1. The mixture is stirred and reacted at 50-70°C for 2-4 hours, cooled to room temperature, washed with deionized water and dried to obtain the modified inorganic flame retardant.
[0012] Preferably, the organic flame retardant is melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber are placed in a reaction vessel, mixed evenly, and then placed in a nitrogen atmosphere. The mixture is reacted at 80-100°C for 100-140 minutes, cooled to room temperature, washed with deionized water and dried to obtain flame-retardant modified polyester fiber.
[0013] Preferably, the antioxidant composition is antioxidant DLTP and antioxidant 1010 in a mass ratio of 1:3.
[0014] Preferably, the ultraviolet absorber composition is UV-326 and UV-1577 in a mass ratio of 1:1.
[0015] Preferably, the crosslinking agent is benzoyl peroxide, the toughening agent is polyvinyl alcohol, the reinforcing agent is glass fiber, and the flow agent is polyethylene wax.
[0016] Preferably, the preparation method of the cable-filled flame-retardant composite fiber paper rope is as follows: weigh each substance in the formula according to the formula and complete the corresponding reaction. Then, put all the materials into a reaction vessel and mix them evenly. Based on the organic material composition, add 20-40 parts of deionized water and stir evenly to form a slurry. Place it in a mesh mold for stretching and extrusion, and cure it at 80-100℃ for 40-60 minutes. Then, place it at 120-140℃ for cross-linking and curing for 20-40 minutes. Cool it to room temperature to obtain the cable-filled flame-retardant composite fiber paper rope.
[0017] Compared with the prior art, the advantages of this invention are: (1) The present invention has excellent flame retardant properties. Modified inorganic flame retardant: Aluminum hydroxide is modified by using γ-aminopropyltriethoxysilane. γ-aminopropyltriethoxysilane reacts with the hydroxyl groups on the surface of aluminum hydroxide to generate silane groups Al-O-Si bonds. These silane groups can react with the hydroxyl groups in polyester fibers, improving the compatibility of the inorganic flame retardant with organic materials. This allows the modified inorganic flame retardant to be uniformly dispersed in the composite fiber paper rope used to fill cables, effectively preventing the spread of flames and improving the fire resistance of the material.
[0018] Organic flame retardant: As an organic flame retardant, melamine phosphate reacts chemically with the phosphate groups on polyester fibers to form stable phosphate-fiber bonds, allowing melamine phosphate to be uniformly dispersed in the matrix material, further enhancing the flame retardant ability of the composite material and ensuring that it can maintain a good flame retardant effect even at high temperatures.
[0019] (2) The present invention improves mechanical strength and tensile properties. Inorganic material composition: The combination of aluminum silicate fiber and expanded perlite not only enhances the mechanical strength of the composite fiber paper rope, but also improves the material's impact resistance, ensuring that it is not easily broken or damaged during cable use.
[0020] Organic material composition: The appropriate ratio of polypropylene fiber and polyester fiber provides the flexibility and tensile strength of the composite fiber paper rope, ensuring that it can meet the bending and stretching requirements in cable filling.
[0021] (3) The present invention has excellent antioxidant properties and durability. Antioxidant composition: Hindered phenolic oxidant 1010 has excellent thermal stability and migration resistance. When combined with sulfate ester antioxidant DLTP, it can effectively slow down the oxidation reaction of composite fiber paper rope in high temperature and high oxygen environment, reduce the risk of discoloration, extend its service life, and ensure that the cable filling material still has good stability during long-term use.
[0022] (4) The present invention has good ultraviolet protection performance. UV absorber composition: Benzotriazole UV absorber UV-326 has low volatility, high temperature resistance and antioxidant synergistic effect. When combined with UV-1577, it effectively improves the UV absorption capacity of composite fiber paper rope, thereby reducing the damage and discoloration of cables caused by UV radiation and extending the service life of cables in outdoor environments.
[0023] (5) The present invention has superior processing performance. Synergistic effect of crosslinking agent and toughening agent: The combination of benzoyl peroxide as a crosslinking agent and polyvinyl alcohol as a toughening agent enables the composite fiber paper rope to form a three-dimensional network crosslinking structure during processing, maintaining good stability, while improving the durability and toughness of the finished product.
[0024] Use of flow agents: Polyethylene wax is used as a flow agent to improve the processing flowability of composite fiber paper ropes and ensure uniformity and precision during the molding process. Detailed Implementation
[0025] Example 1: According to the formula, weigh out 35 parts of an inorganic material composition of aluminum silicate fiber and expanded perlite in a 1:1 mass ratio, 100 parts of an organic material composition of polypropylene fiber and polyester fiber in a 1:1.5 mass ratio, 30 parts of a modified inorganic flame retardant, 2 parts of an organic flame retardant, 1 part of an antioxidant composition of DLTP and antioxidant 1010 in a 1:3 mass ratio, 0.4 parts of a UV-326 and UV-1577 ultraviolet absorber composition in a 1:1 mass ratio, 0.4 parts of a crosslinking agent benzoyl peroxide, 2 parts of a toughening agent polyvinyl alcohol, 4 parts of a reinforcing agent glass fiber, and 0.6 parts of a flow agent polyethylene wax. The modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. Its preparation method is as follows: γ-aminopropyltriethoxysilane and aluminum hydroxide... The two materials were placed in a reaction vessel at a mass ratio of 0.4:1 and stirred at 50°C for 2 hours. After cooling to room temperature, they were washed with deionized water and dried. The organic flame retardant was melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber were placed in the reaction vessel, mixed evenly, and then placed in a nitrogen atmosphere. The mixture was reacted at 80°C for 100 minutes. After cooling to room temperature, the mixture was washed with deionized water and dried. Then, all the materials were placed in the reaction vessel and mixed evenly. Based on the organic material composition, 20 parts of deionized water were added and stirred evenly to form a slurry. The slurry was placed in a mesh mold, stretched and extruded, and cured at 80°C for 40 minutes. Then, it was cross-linked and cured at 120°C for 20 minutes and cooled to room temperature to obtain the cable-filled flame-retardant composite fiber paper rope.
[0026] Example 2: According to the formula, weigh out 38 parts of an inorganic material composition of aluminum silicate fiber and expanded perlite in a 1:1 mass ratio, 100 parts of an organic material composition of polypropylene fiber and polyester fiber in a 1:1.5 mass ratio, 33 parts of a modified inorganic flame retardant, 3 parts of an organic flame retardant, 1.5 parts of an antioxidant composition of DLTP and antioxidant 1010 in a 1:3 mass ratio, 0.8 parts of a UV-326 and UV-1577 ultraviolet absorber composition in a 1:1 mass ratio, 0.8 parts of a crosslinking agent benzoyl peroxide, 3 parts of a toughening agent polyvinyl alcohol, 5.5 parts of a reinforcing agent glass fiber, and 0.7 parts of a flow agent polyethylene wax. The modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. Its preparation method is as follows: γ-aminopropyltriethoxysilane and aluminum hydroxide... The two materials were placed in a reaction vessel at a mass ratio of 0.45:1 and stirred at 55°C for 2.5 hours. After cooling to room temperature, they were washed with deionized water and dried. The organic flame retardant was melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber were placed in the reaction vessel, mixed evenly, and then placed in a nitrogen atmosphere. The mixture was reacted at 85°C for 110 minutes. After cooling to room temperature, the mixture was washed with deionized water and dried. Then, all the materials were placed in the reaction vessel and mixed evenly. Based on the organic material composition, 25 parts of deionized water were added and stirred evenly to form a slurry. The slurry was placed in a mesh mold, stretched and extruded, and cured at 85°C for 45 minutes. Then, it was cross-linked and cured at 125°C for 25 minutes and cooled to room temperature to obtain the cable-filled flame-retardant composite fiber paper rope.
[0027] Example 3: According to the formula, weigh out 42 parts of an inorganic material composition of aluminum silicate fiber and expanded perlite in a 1:1 mass ratio, 100 parts of an organic material composition of polypropylene fiber and polyester fiber in a 1:1.5 mass ratio, 36 parts of a modified inorganic flame retardant, 4 parts of an organic flame retardant, 2 parts of an antioxidant composition of DLTP and antioxidant 1010 in a 1:3 mass ratio, 1.2 parts of an ultraviolet absorber composition of UV-326 and UV-1577 in a 1:1 mass ratio, 1.2 parts of a crosslinking agent benzoyl peroxide, 4 parts of a toughening agent polyvinyl alcohol, 7 parts of a reinforcing agent glass fiber, and 0.8 parts of a flow agent polyethylene wax. The modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. Its preparation method is as follows: γ-aminopropyltriethoxysilane and aluminum hydroxide... The two materials were placed in a reaction vessel at a mass ratio of 0.5:1 and stirred at 60°C for 3 hours. After cooling to room temperature, the mixture was washed with deionized water and dried. The organic flame retardant was melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber were placed in the reaction vessel, mixed evenly, and then placed in a nitrogen atmosphere. The mixture was reacted at 90°C for 120 minutes, cooled to room temperature, washed with deionized water and dried. Then, all the materials were placed in the reaction vessel and mixed evenly. Based on the organic material composition, 30 parts of deionized water were added and stirred evenly to form a slurry. The slurry was placed in a mesh mold, stretched and extruded, and cured at 90°C for 50 minutes. Then, it was cross-linked and cured at 130°C for 30 minutes and cooled to room temperature to obtain the cable-filled flame-retardant composite fiber paper rope.
[0028] Example 4: According to the formula, weigh out 46 parts of an inorganic material composition of aluminum silicate fiber and expanded perlite in a 1:1 mass ratio, 100 parts of an organic material composition of polypropylene fiber and polyester fiber in a 1:1.5 mass ratio, 39 parts of a modified inorganic flame retardant, 5 parts of an organic flame retardant, 2.5 parts of an antioxidant composition of DLTP and antioxidant 1010 in a 1:3 mass ratio, 1.6 parts of an ultraviolet absorber composition of UV-326 and UV-1577 in a 1:1 mass ratio, 1.6 parts of a crosslinking agent benzoyl peroxide, 5 parts of a toughening agent polyvinyl alcohol, 8.5 parts of a reinforcing agent glass fiber, and 0.9 parts of a flow agent polyethylene wax. The modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. Its preparation method is as follows: γ-aminopropyltriethoxysilane and aluminum hydroxide... The two materials were placed in a reaction vessel at a mass ratio of 0.55:1 and stirred at 65°C for 3.5 hours. After cooling to room temperature, they were washed with deionized water and dried. The organic flame retardant was melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber were placed in the reaction vessel, mixed evenly, and then placed in a nitrogen atmosphere. The mixture was reacted at 95°C for 130 minutes. After cooling to room temperature, the mixture was washed with deionized water and dried. Then, all the materials were placed in the reaction vessel and mixed evenly. Based on the organic material composition, 35 parts of deionized water were added and stirred evenly to form a slurry. The slurry was placed in a mesh mold, stretched and extruded, and cured at 95°C for 55 minutes. Then, it was cross-linked and cured at 135°C for 35 minutes and cooled to room temperature to obtain the cable-filled flame-retardant composite fiber paper rope.
[0029] Example 5: According to the formula, weigh out 50 parts of an inorganic material composition of aluminum silicate fiber and expanded perlite in a 1:1 mass ratio, 100 parts of an organic material composition of polypropylene fiber and polyester fiber in a 1:1.5 mass ratio, 42 parts of a modified inorganic flame retardant, 6 parts of an organic flame retardant, 3 parts of an antioxidant composition of DLTP and antioxidant 1010 in a 1:3 mass ratio, 2 parts of an ultraviolet absorber composition of UV-326 and UV-1577 in a 1:1 mass ratio, 2 parts of a crosslinking agent benzoyl peroxide, 6 parts of a toughening agent polyvinyl alcohol, 10 parts of a reinforcing agent glass fiber, and 1 part of a flow agent polyethylene wax. The modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. Its preparation method is as follows: place γ-aminopropyltriethoxysilane and aluminum hydroxide in a reaction mixture... In a container, the mass ratio of the two is 0.6:1. The mixture is stirred and reacted at 70°C for 4 hours, cooled to room temperature, washed with deionized water and dried. The organic flame retardant is melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber are placed in a reaction container, mixed evenly, and then placed in a nitrogen atmosphere. The mixture is reacted at 100°C for 140 minutes, cooled to room temperature, washed with deionized water and dried. Then all the materials are placed in a reaction container and mixed evenly. Based on the organic material composition, 40 parts of deionized water are added and stirred evenly to form a slurry. The slurry is placed in a mesh mold, stretched and extruded, and cured at 100°C for 60 minutes. Then it is cross-linked and cured at 140°C for 40 minutes and cooled to room temperature to obtain a cable-filled flame-retardant composite fiber paper rope.
[0030] Performance testing Flame retardant performance test The flame-retardant composite fiber paper ropes for cable filling obtained in Examples 1-5 were made into strips of 25mm × 25mm, dried at 60°C for 24 hours, and their flame-retardant performance was tested using an FPA-2000 electric heating test furnace, referring to the national standard GB / T2408-2008. The test results are shown in the table below: Limiting Oxygen Index Test The flame-retardant composite fiber paper ropes for cable filling obtained in Examples 1-5 were made into strips of 25mm × 25mm, dried at 60°C for 24 hours, and subjected to limiting oxygen index testing using an ATS-LOI limiting oxygen index tester, referring to the national standard GB / T 2406.2-2009. The test results are shown in the table below: Tensile strength and elongation test The cable-filled flame-retardant composite fiber paper ropes obtained in Examples 1-5 were made into 50mm × 10mm strip samples, dried at 60°C for 24 hours, and their tensile strength and elongation were tested using an Instron 5569 electronic universal testing machine. The tensile rate of the testing machine was set to 50mm / min. Referring to the national standard GB / T 528-2009, the test results are shown in the table below: Temperature resistance test The flame-retardant composite fiber paper ropes for cable filling obtained in Examples 1-5 were made into 50mm×50mm strip samples, dried at 60°C for 24 hours, and their temperature resistance was tested using a TA Instruments TGA Q500 thermogravimetric analyzer. The heating rate of the thermogravimetric analyzer was set to 10°C / min, and the temperature was heated from room temperature to 600°C. The test results are shown in the table below, referring to the national standard GB / T 2925-2008. UV aging resistance test The cable-filled flame-retardant composite fiber paper ropes obtained in Examples 1-5 were made into strips of 100mm × 20mm, dried at 60°C for 24 hours, and subjected to ultraviolet aging resistance tests using a Q-LAB UV-C114 electronic universal testing machine. The ultraviolet radiation intensity was set to 0.89W / m² / nm, a UV-A lamp was used, and the irradiation time was 1000 hours. Referring to the national standard GB / T 16422.2-2009, the test results are shown in the table below:
Claims
1. A type of cable-filled flame-retardant composite fiber paper rope, characterized in that: The composition ratio of the flame-retardant composite fiber paper rope filled in the cable is as follows: 35-50 parts of inorganic material composition, 100 parts of organic material composition, 30-42 parts of modified inorganic flame retardant, 2-6 parts of organic flame retardant, 1-3 parts of antioxidant composition, 0.4-2 parts of ultraviolet absorber composition, 0.4-2 parts of crosslinking agent, 2-6 parts of toughening agent, 4-10 parts of reinforcing agent, and 0.6-1 parts of flow agent; The inorganic material composition is aluminum silicate fiber and expanded perlite in a mass ratio of 1:1; The organic material composition is polypropylene fiber and polyester fiber in a mass ratio of 1:1.5; The modified inorganic flame retardant is a product obtained by modifying aluminum hydroxide with γ-aminopropyltriethoxysilane. The preparation method is as follows: γ-aminopropyltriethoxysilane and aluminum hydroxide are placed in a reaction vessel with a mass ratio of 0.4-0.6:
1. The mixture is stirred and reacted at 50-70℃ for 2-4 hours, cooled to room temperature, washed with deionized water and dried to obtain the modified inorganic flame retardant. The organic flame retardant is melamine phosphate. According to the mass ratio in the formula, melamine phosphate and polyester fiber are placed in a reaction vessel, mixed evenly, and then placed in a nitrogen atmosphere. The mixture is reacted at 80-100℃ for 100-140 minutes, cooled to room temperature, washed with deionized water and dried to obtain flame-retardant modified polyester fiber. The antioxidant composition is antioxidant DLTP and antioxidant 1010 in a mass ratio of 1:3; The ultraviolet absorber composition is UV-326 and UV-1577 in a mass ratio of 1:
1. The crosslinking agent is benzoyl peroxide, the toughening agent is polyvinyl alcohol, the reinforcing agent is glass fiber, and the flow agent is polyethylene wax; The preparation method of the cable-filled flame-retardant composite fiber paper rope is as follows: weigh each substance in the formula according to the formula and complete the corresponding reaction. Then, put all the materials into a reaction vessel and mix them evenly. Based on the organic material composition, add 20-40 parts of deionized water and stir evenly to form a slurry. Place it in a mesh mold for stretching and extrusion, and cure it at 80-100℃ for 40-60 minutes. Then, place it at 120-140℃ for cross-linking and curing for 20-40 minutes. Cool to room temperature to obtain the cable-filled flame-retardant composite fiber paper rope.
Citation Information
Patent Citations
Low-smoke environmentally friendly anti-extrusion cable filling rope
CN108299801A
Cable filling strip with anti-electromagnetic interference function and excellent heat conduction property and preparation method thereof
CN109504019A
Low-odor light-weight polypropylene composite material for automobile
CN111073144A
Phosphorus-nitrogen synergistic structure type flame-retardant PET (polyethylene terephthalate) and preparation method thereof
CN118878801A
Insulated electrical wire and cable having resistance to heat deterioration, properties for water resistance and insulation, and fire retardance
JP2001312925A