Anode materials, their preparation methods, and batteries
By coating a hard carbon material with P and N co-doped carbon materials, an oxygen-free environment is constructed, which solves the problem of POx functional group generation in hard carbon materials during the doping process. This results in a negative electrode material with high reversible capacity and low potential plateau capacity, thus improving the electrochemical performance of sodium-ion batteries.
Patent Information
- Application Number
- CN202510550007.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2025-04-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2045-04-28
AI Technical Summary
Existing sodium-ion battery anode materials suffer from low sodium storage capacity and insufficient potential plateau capacity. In particular, hard carbon materials are prone to forming POx functional groups during phosphorus doping, which hinders further phosphorus doping and limits the improvement of material performance.
Using hard carbon material as the core and coated with P and N co-doped carbon material on the outside, a core-shell structured anode material is formed by calcining phosphorus and nitrogen sources in an oxygen-free environment. This avoids the formation of POx and NOx functional groups, increases the doping amount, and enhances the interlayer spacing and conductivity of the material.
It significantly improves the reversible capacity and low potential plateau capacity of the anode material, enhances the material's reactivity and electronic conductivity, and strengthens its cycle and rate performance.
Smart Images

Figure CN120674453B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of batteries, specifically to a negative electrode material, its preparation method, and a battery. Background Technology
[0002] Due to the increasingly serious environmental and energy crises, there is an urgent need to develop renewable and sustainable energy sources such as wind and solar power. Developing large-scale energy storage systems is crucial to addressing these intermittent energy conversion problems. Sodium-ion batteries are considered the most promising alternative to lithium-ion batteries for large-scale energy storage applications because of their low cost, abundant natural sodium resources, and similar rocking-chair operation. Significant progress has been made in the practical application of sodium-ion battery cathodes over the past decade, including polyanionic compounds, layered oxides, and Prussian analogs. For anodes, various materials, such as carbonaceous materials, alloy metals, and metal chalcogenides, have been extensively explored. However, due to their complex preparation processes and inherent electrochemical defects, most candidate materials exhibit serious limitations in large-scale applications. Carbonaceous materials are considered the most promising anode materials because they are low-cost, easy to prepare, and reproducible. Unlike the successful application of graphite in traditional lithium-ion batteries, the narrow carbon interlayer spacing (0.335 nm) and thermodynamic instability of graphite intercalation compounds hinder sodium ion intercalation. It is generally accepted that graphite cannot be directly used as the anode material for sodium-ion batteries. Hard carbon consists of interlaced graphite microcrystalline layers, abundant micropores, and defects. It has a relatively large interlayer spacing, can store a large number of sodium ions, and has a large reversible capacity. Furthermore, due to the increasing demands on batteries, and to meet the requirements of full cells in practical applications, there is an urgent need for hard carbon anodes with high reversible capacity and appropriate low potential plateau capacity. Summary of the Invention
[0003] In view of this, the present invention aims to provide a negative electrode material, a method for preparing the same, and a battery thereof, wherein the negative electrode material has high reversible capacity and low potential plateau capacity.
[0004] To solve the above-mentioned technical problems, this application is implemented as follows:
[0005] This invention provides a negative electrode material, the negative electrode material comprising a hard carbon material and a coating layer covering at least a portion of the surface of the hard carbon material;
[0006] The coating layer includes a carbon material, which includes a carbon material matrix and doping elements doped in the carbon material matrix, wherein the doping elements include P and N;
[0007] The oxygen content in the negative electrode material is 0.
[0008] In any embodiment, the hard carbon material further includes doping elements, including P and N.
[0009] In any embodiment, based on the mass of the negative electrode material, the doping amount of P element in the negative electrode material is 0.5wt% to 1wt%.
[0010] In any embodiment, the amount of nitrogen doping in the negative electrode material is 0.5 wt% to 1 wt%, based on the mass of the negative electrode material.
[0011] In any embodiment, the thickness of the coating layer is 2 nm to 10 nm.
[0012] In any embodiment, the particle size of the hard carbon material is 4 μm to 8 μm.
[0013] In any embodiment, the hard carbon material includes spherical hard carbon material.
[0014] In any embodiment, based on the atomic content of the coating layer, the doping amount of P element in the carbon material is 10 at% to 15 at%.
[0015] In any embodiment, based on the atomic content of the coating layer, the nitrogen doping amount in the carbon material is 5 at% to 10 at%.
[0016] A second aspect of this application provides a method for preparing a negative electrode material, comprising the following steps:
[0017] The hard carbon precursor was calcined in a reducing atmosphere to obtain the hard carbon material.
[0018] Under a first inert atmosphere, a mixed solution of hard carbon material, phosphorus source and nitrogen source is mixed with metal hydride and subjected to a second calcination to obtain the negative electrode material;
[0019] The negative electrode material includes a hard carbon material and a coating layer covering at least a portion of the surface of the hard carbon material;
[0020] The coating layer includes a carbon material, which includes a carbon material matrix and doping elements doped in the carbon material matrix, wherein the doping elements include P and N;
[0021] The oxygen content in the negative electrode material is 0.
[0022] In any embodiment, the hard carbon precursor comprises resin and / or biomass material.
[0023] In any embodiment, the resin includes at least one of phenolic resin, epoxy resin, polyacrylonitrile, and polyimide.
[0024] In any embodiment, the particle size of the phenolic resin is 5 μm to 10 μm.
[0025] In any embodiment, the reducing atmosphere comprises a mixture of hydrogen and a second inert atmosphere.
[0026] In any embodiment, the volume percentage of hydrogen in the mixed atmosphere is 3% to 5%.
[0027] In any embodiment, the second inert atmosphere includes at least one of nitrogen, argon, helium, and neon.
[0028] In any embodiment, the flow rate of the reducing atmosphere is 50 mL / min to 100 mL / min.
[0029] In any embodiment, the temperature of the first calcination is 1000℃~1400℃, the time of the first calcination is 2h~5h, and the heating rate of the first calcination is 2℃ / min~5℃ / min.
[0030] In any embodiment, the first inert atmosphere includes at least one of nitrogen, argon, helium, and neon.
[0031] In any embodiment, the flow rate of the first inert atmosphere is 50 mL / min to 150 mL / min.
[0032] In any embodiment, the molar ratio of phosphorus source to nitrogen source in the mixed solution of phosphorus source and nitrogen source is 1:1 to 4:1.
[0033] In any embodiment, the ratio of the mixed solution of the phosphorus source and nitrogen source to the hard carbon material is (2-20) mL: 1 g.
[0034] In any embodiment, the mass ratio of the metal hydride to the hard carbon material is 0.5 to 2:1.
[0035] In any embodiment, the phosphorus source includes at least one of phosphorus trichloride, phenyl phosphorus dichloride, and phosphorus tribromide.
[0036] In any embodiment, the nitrogen source includes at least one of pyrrole, pyridine, and quinoline.
[0037] In any embodiment, the metal hydride includes at least one of calcium hydride, magnesium hydride, potassium hydride, and beryllium hydride.
[0038] In any embodiment, the temperature of the second calcination is 600℃~900℃, the time of the second calcination is 2h~5h, and the heating rate of the second calcination is 2℃ / min~5℃ / min.
[0039] In any embodiment, after the second calcination is completed, the process further includes: cooling and acid washing the product obtained after the second calcination to obtain the negative electrode material.
[0040] In any embodiment, the pickling reagent includes at least one of hydrochloric acid solution, sulfuric acid solution and oxalic acid solution.
[0041] In any embodiment, the concentration of the reagent is 1 mol / L to 3 mol / L.
[0042] In any embodiment, the pickling time is 1 hour to 4 hours.
[0043] A third aspect of this application provides a battery including a negative electrode sheet, the negative electrode sheet comprising the negative electrode material described above, or a negative electrode material prepared by the method described above.
[0044] The beneficial technical effects of the present invention through the above technical solution are as follows:
[0045] The negative electrode material of this application has a core-shell structure, in which the core is made of hard carbon material with zero oxygen content, and the outer shell or shell layer includes carbon material co-doped with phosphorus (P) and nitrogen (N). That is, the negative electrode material mainly consists of hard carbon material and P and N co-doped carbon material coated on the surface of the hard carbon material, and the oxygen content in the negative electrode material is zero. By constructing an oxygen-free environment, the sodium storage capacity of the hard carbon material is improved, thereby enhancing the high reversible capacity and low potential capacity of the material. Simultaneously, the P and N diatomic doping also improves the reactivity and electronic conductivity of the negative electrode material, significantly improving its cycle and rate performance.
[0046] Other features and advantages of the present invention will be described in detail in the following detailed description section. Attached Figure Description
[0047] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof.
[0048] Figure 1 The diagram shows the apparatus for synthesizing the negative electrode material of this invention.
[0049] Figure 2 The image shown is an EDS surface scan of the hard carbon material prepared in Example 1;
[0050] Figure 3 The image shown is an EDS line scan of the hard carbon material prepared in Example 1;
[0051] Figure 4The image shown is an EDS surface scan of the negative electrode material prepared in Example 1; wherein, Figure 4 (a) is the EDS surface scan of N element in the negative electrode material, and (b) is the EDS surface scan of P element in the negative electrode material.
[0052] Figure 5 The image shown is a TEM image of the negative electrode material prepared in Example 1.
[0053] Legend:
[0054] 10 - Air intake;
[0055] 20 - Mixer;
[0056] 30 - Air outlet;
[0057] 40-Tube furnace. Detailed Implementation
[0058] This invention discloses a negative electrode material, its preparation method, and a battery. Those skilled in the art can refer to the content of this document and appropriately modify the process parameters to achieve the desired result. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in this invention. The methods and applications of this invention have been described through preferred embodiments. Those skilled in the art can clearly modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit, and scope of this invention to realize and apply the technology of this invention.
[0059] In the description of this invention, the list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0060] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges or individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.
[0061] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0062] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0063] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0064] In sodium-ion batteries, cathode materials such as layered oxides, polyanionic compounds, and Prussian blue have been well-developed, but high-performance anode materials with high sodium storage capacity and low cost are lacking. Among anode materials for sodium-ion batteries, "hard carbon," as a non-graphitizable carbon, has become the most suitable microstructure for SIB anodes due to its randomly distributed turbine structure, possessing large interlayer spacing (over 0.37 nm) and closed nanopores. Generally, hard carbon is synthesized from thermosetting precursors (such as cellulose, peanut shells, sucrose, glucose, phenolic resins, starch, anthracite, etc.) through high-temperature carbonization. During pyrolysis, the carbon layers in the precursor readily form vortex layers and disordered microstructures composed of surface defects, nanopores or voids, and graphite domains. During curing, Na ions are first adsorbed in the tilted region (0.1-1V vs Na / Na). + At the hard carbon defect sites, then in the plateau region (0-0.1V vs Na / Na) + This leads to the formation of near-metallic Na clusters. However, hard carbon electrodes exhibit a considerably low plateau capacity, which plays a crucial role in determining the operating voltage and energy density of a fully charged battery. In existing technologies, phosphorus (P) is typically used to dope and modify hard carbon materials. However, because phosphorus inevitably forms POx functional groups on the material surface during doping, it hinders further doping of the bulk phase by P, resulting in a low doping amount and failing to effectively improve the low sodium storage capacity of hard carbon materials. Therefore, there is an urgent need to develop a hard carbon anode material for sodium-ion batteries with high capacity and a low potential plateau capacity ratio.
[0065] In view of this, this application proposes a negative electrode material, a method for preparing the same, and a battery thereof, wherein the negative electrode material has high reversible capacity and low potential plateau capacity. The following provides a more detailed description of this application and its optional embodiments.
[0066] [Anode Material]
[0067] In some embodiments, this application provides a negative electrode material, which includes a hard carbon material and a coating layer covering at least a portion of the surface of the hard carbon material;
[0068] The coating layer includes carbon material, which includes a carbon material matrix and doping elements doped in the carbon material matrix, including P and N.
[0069] The oxygen content in the negative electrode material is 0.
[0070] It should be noted that, in this application, the term "coating" is not limited to direct coating, but also includes indirect coating. For example, when a coating layer coats a hard carbon material, it may mean that there are no other structures between the coating layer and the outer surface of the hard carbon material, or it may mean that there are one or more other structures between the coating layer and the outer surface of the hard carbon material. Preferably, there are no other structures between the coating layer and the outer surface of the hard carbon material.
[0071] The aforementioned coating layer, formed or coated on at least a portion of the surface of the hard carbon material, can protect or improve the hard carbon material, and can be used to improve the structural stability, reversible capacity, and low-potential capacity of the hard carbon material, and optimize the conductivity of the negative electrode material. "Formed or coated on at least a portion of the surface of the hard carbon material" means that the coating layer can completely encapsulate the hard carbon material within the coating layer, or the coating layer can only coat a portion of the outer surface of the hard carbon material; that is, the coating layer can completely coat the hard carbon material, or it can coat a portion of the surface of the hard carbon material, preferably completely coat it.
[0072] The negative electrode material of this application has a core-shell structure, in which the core is made of hard carbon material with zero oxygen content, and the outer shell or shell layer includes carbon material co-doped with P and N. That is, the negative electrode material mainly consists of hard carbon material and P and N co-doped carbon material coated on the surface of the hard carbon material, and the oxygen content in the negative electrode material is zero. By constructing an oxygen-free environment, the sodium storage capacity of the hard carbon material is improved, thereby increasing the high reversible capacity and low potential capacity of the material. Simultaneously, the P and N dual-atom doping also improves the reactivity and electronic conductivity of the negative electrode material, significantly improving its cycle and rate performance. In detail:
[0073] This application constructs an oxygen-free environment by doping P and N elements into the coating layer of a hard carbon material. This effectively prevents the formation of POx and NOx functional groups on the material surface by the dopant elements P and N, increasing the doping amount of P and N in the material, providing more defect structures, and thus providing more active sites for sodium ion storage, thereby significantly improving the sodium storage capacity of the material. Simultaneously, achieving dual doping of P and N elements in the coating layer can also change the local bonding environment and electron distribution on the surface of the anode material, significantly expanding the interlayer spacing, thereby improving the reactivity and electronic conductivity of the anode material. Furthermore, the presence of the carbon material coating layer can further reduce the specific surface area of the material and increase the number of closed pores, thus significantly improving the cycle and rate performance of the material. Therefore, this anode material can improve the cycle and rate performance of sodium-ion batteries.
[0074] This application, by simultaneously introducing doping elements P and N into the coating carbon material based on hard carbon material, alters the local bonding environment and electron distribution on the surface of the hard carbon anode material. This provides high-density active sites, promotes rapid sodium ion migration, and improves the structural stability of the material. Therefore, it can improve the overall electrochemical performance of the material.
[0075] Therefore, the negative electrode material provided in this application can be a structurally stable negative electrode material with high sodium storage capacity and good conductivity. This negative electrode material consists of a hard carbon material and a P- and N-doped carbon material coated on the surface of the hard carbon material. Simultaneously, the oxygen content in the negative electrode material is 0. This not only achieves a uniform carbon material coating layer on the surface of the hard carbon material but also enables high P and N doping levels within the coating layer, providing more sodium storage space, improving the material's reactivity and conductivity, and significantly enhancing the cycle and rate performance of the negative electrode material.
[0076] In this application, the term "hard carbon material" generally refers to an amorphous carbon material formed by high-temperature carbonization (usually 800-1500°C) of carbon-containing precursors (such as resins, polymers, biomass, etc.); wherein, the oxygen content of the above-mentioned "hard carbon material" is 0, and it can be the carbonization product of carbon-containing precursors under a reducing atmosphere. By constructing an oxygen-free environment, the generation of POx and NOx functional groups on the material surface by doping elements P and N can be effectively avoided, providing conditions for subsequently increasing the doping amount of P and N in the material.
[0077] In this application, the term "carbon material" refers to a material primarily composed of carbon elements without a constant structure or properties. The oxygen content in this "carbon material" is zero. It can be produced by the pyrolysis of phosphorus-containing compounds and nitrogen-containing organic matter under an inert atmosphere, resulting in carbonaceous material that is uniformly deposited on the surface of the hard carbon material to form a coating layer. By constructing an oxygen-free environment and simultaneously limiting phosphorus-containing compounds and nitrogen-containing organic matter, the generation of POx and NOx functional groups on the material surface by doping elements P and N can be effectively avoided. Simultaneously, a carbon material coating layer is formed on the surface of the hard carbon material, improving both the conductivity and cycle performance of the anode material.
[0078] In some embodiments, the hard carbon material further includes doping elements, including P and N.
[0079] In this application, by introducing doping elements P and N into hard carbon materials, the synergistic effect of the two can enhance the conductivity of hard carbon materials, reduce charge transfer impedance, and improve the overall rate performance and cycle life of the anode material.
[0080] In some embodiments, the doping amount of phosphorus (P) in the negative electrode material is 0.5 wt% to 1 wt%, based on the mass of the negative electrode material. As an example, the doping amount of P in the hard carbon material can be any one of 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, and 1 wt%, or a range between any two, based on the mass of the negative electrode material.
[0081] In this application, the doping amount of P element in the negative electrode material is calculated as follows: ((total mass of negative electrode material - mass of carbon material matrix) × mass content of P element in negative electrode material) / total mass of negative electrode material.
[0082] In some embodiments, the nitrogen doping amount in the negative electrode material is 0.5 wt% to 1 wt%, based on the mass of the negative electrode material. As an example, the nitrogen doping amount in the hard carbon material can be any one of 0.5 wt%, 0.6 wt%, 0.7 wt%, 0.8 wt%, 0.9 wt%, and 1 wt%, or a range between any two, based on the mass of the negative electrode material.
[0083] In this application, the method for calculating the amount of N doping in the negative electrode material is: ((total mass of negative electrode material - mass of carbon material matrix) × mass content of N element in negative electrode material) / total mass of negative electrode material.
[0084] In this application, by controlling the doping amounts of P and N elements in the negative electrode material within the aforementioned mass range, the sodium storage capacity, cycle stability, and rate performance of the material can be improved while maintaining structural stability. Excessive P and N doping will obstruct electron transport paths in the material, hindering sodium ion diffusion and triggering side reactions, thereby reducing the material's conductivity and cycle stability. Insufficient P and N doping will not improve the material's conductivity.
[0085] In some embodiments, the thickness of the coating layer is 2 nm to 10 nm. As an example, the thickness of the coating layer can be any one of 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, and 10 nm, or a range between any two.
[0086] In this application, by controlling the thickness of the coating layer within the aforementioned range, the coating layer can form a continuous and dense protective layer, which can both enable rapid diffusion of sodium ions and prevent electrolyte penetration, thereby improving the rate performance and cycle stability of the negative electrode material. If the coating layer is too thick, the diffusion path of sodium ions will be prolonged, increasing the diffusion resistance and affecting the rate performance and cycle stability of the negative electrode material. If the coating layer is too thin, the effect of improving the rate performance and cycle stability of the material will not be achieved.
[0087] In some embodiments, the particle size of the hard carbon material is 4 μm to 8 μm. As an example, the particle size of the hard carbon material can be any one of 4 μm, 5 μm, 6 μm, 7 μm, and 8 μm, or a range between any two.
[0088] In some embodiments, the hard carbon material includes spherical hard carbon material.
[0089] In this application, spherical hard carbon materials are beneficial to improving the compaction density of the negative electrode material, which can further improve the overall energy density of the battery.
[0090] In some embodiments, the doping amount of P element in the carbon material is 10 at% to 15 at%, based on the atomic content of the coating layer. As an example, based on the atomic content of the coating layer, the doping amount of P element in the carbon material can be any one of 10 at%, 11 at%, 12 at%, 13 at%, 14 at%, and 15 at%, or a range between any two.
[0091] In some embodiments, the nitrogen doping amount in the carbon material is 5 at% to 10 at%, based on the atomic content of the coating layer. As an example, based on the atomic content of the coating layer, the nitrogen doping amount in the carbon material can be any one of 5 at%, 6 at%, 7 at%, 8 at%, 9 at%, and 10 at%, or a range between any two.
[0092] In this application, the method for testing the doping amount of P and N elements in carbon materials is as follows: the results are obtained by scanning electron microscopy and EDS energy dispersive spectroscopy; specifically, an area is selected for EDS surface scanning at a scanning electron microscope voltage of 15KV and a magnification of 10K to obtain the elemental percentage.
[0093] In this application, by constructing an oxygen-free environment, the formation of POx and NOx functional groups by dopants P and N on the material surface is avoided, significantly increasing the doping amount of P and N. This achieves a P doping amount of 5 at%–10 at% and a N doping amount of 3 at%–6 at% in the carbon material, which is beneficial for improving the sodium storage capacity and enhancing the reactivity and electronic conductivity of the anode material. If the doping amount of P and N is too high, it will disrupt the continuity of the carbon framework of the coating layer, hinder electron transport, and affect the conductivity of the anode material.
[0094] Therefore, the provided anode materials, such as P and N co-doped carbon materials coating hard carbon materials with zero oxygen content, achieve high doping levels of P and N elements by constructing an oxygen-free environment and introducing doping elements P and N on the basis of carbon coating. This not only improves the sodium storage capacity of the material, but also improves the high reversible capacity and low potential capacity of the material. At the same time, the dual doping of P and N also changes the local bonding environment and electron distribution on the surface of the hard carbon anode material, improving the material's reactivity and conductivity, while forming a uniform carbon material coating layer, thus improving the structural stability of the material.
[0095] [Preparation methods for negative electrode materials]
[0096] A second aspect of this application provides a method for preparing a negative electrode material, the method comprising the following steps:
[0097] The hard carbon precursor was calcined in a reducing atmosphere to obtain the hard carbon material.
[0098] Under a first inert atmosphere, a mixed solution of hard carbon material, phosphorus source and nitrogen source is mixed with metal hydride and subjected to a second calcination to obtain the negative electrode material;
[0099] The negative electrode material includes hard carbon material and a coating layer covering at least part of the surface of the hard carbon material;
[0100] The coating layer includes carbon material, which includes a carbon material matrix and doping elements doped in the carbon material matrix, including P and N.
[0101] The oxygen content in the negative electrode material is 0.
[0102] The method for preparing the anode material provided in this application involves calcining a hard carbon material precursor in a reducing atmosphere, followed by calcination with a phosphorus source, a nitrogen source, and a metal hydride in an inert atmosphere to obtain the anode material. In this method, a P / N dual-doped carbon material is used to coat the hard carbon material by creating an oxygen-free environment. Specifically:
[0103] Oxygen is removed from the derived hard carbon material from the hard carbon precursor material under a reducing atmosphere to obtain a hard carbon material with zero oxygen content. Then, under the protection of an inert atmosphere, a mixed solution of the hard carbon material, phosphorus source, and nitrogen source, along with a metal hydride, is calcined. While avoiding the introduction of oxygen, the metal oxide decomposes during calcination to produce reducing hydrogen gas, thereby improving the oxygen-free purity of the material surface and preventing the introduction of oxygen during the material preparation process.
[0104] In the synthesis process of the anode material in this application embodiment, an oxygen-free carbon microsphere substrate is obtained through a reducing atmosphere, thus constructing an oxygen-free synthesis environment. Simultaneously, phosphorus and nitrogen sources are introduced to achieve high-level N / P dual doping in the coating layer. Dual-atom doping alters the local bonding environment and electron distribution on the surface of the hard carbon anode material, resulting in a significantly expanded interlayer spacing, thereby improving the reactivity and electronic conductivity of the hard carbon anode material. The presence of the coating layer further reduces the specific surface area of the material, increases the number of closed pores, and enhances the cycle and rate performance of the material.
[0105] It should be understood that all the characteristics and advantages described above for "anode materials" also apply to the "preparation method of anode materials", and will not be repeated here.
[0106] In some specific embodiments, the preparation method of the phosphorus-containing composite anode material includes the following steps (a) to (b):
[0107] Step (a): Preparation of hard carbon materials.
[0108] In some embodiments, in step (a), the hard carbon precursor is first calcined under a reducing atmosphere to obtain a hard carbon material.
[0109] Optionally, in step (a), the hard carbon precursor includes resin and / or biomass material. The hard carbon precursor may include resin, biomass material, or both.
[0110] Optionally, the resin includes at least one of phenolic resin, epoxy resin, polyacrylonitrile, and polyimide.
[0111] Preferably, the resin includes phenolic resin.
[0112] Optionally, the particle size of the phenolic resin is 5 μm to 10 μm. As an example, the particle size of the phenolic resin can be any one of 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, and 10 μm, or a range between any two.
[0113] Optionally, in step (a), the reducing atmosphere includes a mixture of hydrogen and a second inert atmosphere.
[0114] Optionally, the volume percentage of hydrogen in the mixed atmosphere is 3% to 5%. As an example, the volume percentage of hydrogen in the mixed atmosphere is any one of 3%, 3.5%, 4%, 4.5%, 5%, or a range between any two.
[0115] In this application, by controlling the hydrogen content in the reducing atmosphere within the aforementioned volume percentage range, oxygen in the hard carbon material can be effectively removed, ensuring that the oxygen content in the hard carbon material is 0, thus promoting the densification of the carbon skeleton. Normally, oxygen in hard carbon after high-temperature calcination exists in the form of functional groups (such as carboxyl, carbonyl, and ester groups). In this application, a reducing atmosphere is introduced during high-temperature calcination. The hydrogen in the reducing atmosphere can react with the functional groups in the hard carbon, achieving the purpose of removing oxygen from the hard carbon material (specifically, in a high-temperature environment, the CO bonds in the functional groups break, oxygen atoms escape, and hydrogen reacts with the oxygen-containing functional groups in a redox reaction, generating effusible substances such as water, which are then removed).
[0116] Optionally, the second inert atmosphere includes at least one of nitrogen, argon, helium, and neon.
[0117] Optionally, in step (a), the flow rate of the reducing atmosphere is 50 mL / min to 100 mL / min. As an example, the flow rate of the reducing atmosphere can be any one of 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min, or 100 mL / min, or a range between any two.
[0118] Optionally, in step (a), the temperature of the first calcination is 1000℃~1400℃, the time of the first calcination is 2h~5h, and the heating rate of the first calcination is 2℃ / min~5℃ / min. As an example, the temperature of the first calcination can be any one of 1000℃, 1050℃, 1100℃, 1150℃, 1200℃, 1250℃, 1300℃, 1350℃, 1400℃ or any range between two; the time of the first calcination can be any one of 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h or any range between two; and the heating rate of the first calcination can be any one of 2℃ / min, 2.5℃ / min, 3℃ / min, 3.5℃ / min, 4℃ / min, 4.5℃ / min, 5℃ / min or any range between two.
[0119] In this application, during the first calcination process, the hard carbon precursor (such as resin, biomass, etc.) is pyrolyzed under high temperature conditions, eliminating oxygen and forming a hard carbon material. By controlling the conditions of the first calcination within the aforementioned range, a hard carbon material with excellent sodium storage performance and excellent cycle stability can be prepared.
[0120] As an example, step (a) includes:
[0121] Hard carbon precursors (such as phenolic resin with a particle size of 5μm to 10μm) are calcined at 1000℃ to 1400℃ for 2h to 5h in a reducing atmosphere (such as a mixture of hydrogen and nitrogen with a hydrogen volume percentage of 3% to 5%) at a heating rate of 2℃ / min to 5℃ / min to obtain hard carbon materials.
[0122] Step (b): Coating and doping
[0123] In some embodiments, in step (b), a phosphorus source and a nitrogen source are mixed to obtain a mixed solution; a hard carbon material and a metal hydride are mixed to obtain a mixture; the mixed solution is mixed with the mixture using a first inert gas, and a second calcination is performed. After the second calcination, the mixture is naturally cooled to room temperature, and then the resulting product is acid-washed to obtain the negative electrode material. Exemplarily, the apparatus in step (b) is as follows: Figure 1 As shown, a certain amount of phosphorus source and nitrogen source are weighed and placed in a three-necked flask, and dispersed at room temperature under the stirring of stirrer 20 to obtain a mixed solution; a first inert atmosphere is introduced into the mixed solution through inlet 10, and then the mixed solution is sent into tube furnace 40 through outlet 30; hard carbon material and metal hydride are mixed and placed in tube furnace 40 for a second calcination. After the second calcination is completed, the mixture is naturally cooled to room temperature, and then the obtained product is acid washed to obtain the negative electrode material.
[0124] Optionally, the first inert atmosphere includes at least one of nitrogen, argon, helium, and neon.
[0125] Optionally, the flow rate of the first inert atmosphere is 50 mL / min to 150 mL / min. As an example, the flow rate of the first inert atmosphere can be any one of 50 mL / min, 60 mL / min, 80 mL / min, 100 mL / min, 120 mL / min, 140 mL / min, or 150 mL / min, or a range between any two.
[0126] Optionally, the molar ratio of phosphorus source to nitrogen source in the mixed solution is 1:1 to 4:1. As an example, the molar ratio of phosphorus source to nitrogen source in the mixed solution can be any one of 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1 or any range between the two.
[0127] In this application, by controlling the amounts of phosphorus source and nitrogen source within the above-mentioned molar ratio range, the sodium storage capacity of the material can be improved through synergistic doping effect and surface chemical regulation, thereby enhancing the conductivity of the material's reactivity and producing a high-performance anode material.
[0128] Optionally, the ratio of the mixed solution of phosphorus and nitrogen sources to the hard carbon material is (2–20) mL:1 g. As an example, the ratio of the mixed solution of phosphorus and nitrogen sources to the hard carbon material can be any one of the following values or a range between any two: 2:1 g, 5:1 g, 10 mL:1 g, 11 mL:1 g, 12 mL:1 g, 13 mL:1 g, 14 mL:1 g, 15 mL:1 g, 16 mL:1 g, 17 mL:1 g, 18 mL:1 g, 19 mL:1 g, 20 mL:1 g.
[0129] In this application, by controlling the ratio of the mixed solution of phosphorus source and nitrogen source to hard carbon material within the above-mentioned range, it can be ensured that the subsequent mixed solution forms a P and N co-doped carbon material coating layer of appropriate thickness on the surface of hard carbon material, and at the same time, it can also be ensured that the doping amount of P and N in the carbon material coating layer is within a reasonable range.
[0130] Optionally, the mass ratio of metal hydride to hard carbon material is 0.5 to 2:1. As an example, the mass ratio of metal hydride to hard carbon material can be any one of the following values or a range between the two: 0.5:1, 0.8:1, 1:1, 1.2:1, 1.4:1, 1.5:1, 1.6:1, 1.8:1, and 2:1.
[0131] Optionally, the phosphorus source includes at least one of phosphorus trichloride, phenyl phosphorus dichloride, and phosphorus tribromide.
[0132] Optionally, the nitrogen source includes at least one of pyrrole, pyridine, and quinoline.
[0133] In this application, the selection of the above-mentioned phosphorus and nitrogen sources can control the entry of oxygen elements during the preparation process, which is beneficial to increasing the doping amount of P and N and improving the electrochemical performance of the material.
[0134] Optionally, the metal hydride includes at least one of calcium hydride, magnesium hydride, potassium hydride, and beryllium hydride.
[0135] Optionally, the temperature of the second calcination is 600℃~900℃, the time of the second calcination is 2h~5h, and the heating rate of the second calcination is 2℃ / min~5℃ / min. As an example, the temperature of the second calcination can be any one of 600℃, 650℃, 700℃, 750℃, 800℃, 850℃, or 900℃, or a range between any two; the time of the second calcination can be any one of 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, or 5h, or a range between any two; and the heating rate of the second calcination can be any one of 2℃ / min, 2.5℃ / min, 3℃ / min, 3.5℃ / min, 4℃ / min, 4.5℃ / min, or 5℃ / min, or a range between any two.
[0136] In this second calcination, the phosphorus and nitrogen sources decompose at high temperature to form a P- and N co-doped carbon material coating layer. Simultaneously, the hydrogen released from the decomposition of the metal hydride reacts with oxygen-containing functional groups, further improving the oxygen-free purity of the material and preventing the introduction of oxygen during the preparation process. By precisely controlling the calcination conditions (temperature, atmosphere, time) and elemental ratios, the doping efficiency and material integrity are balanced, ultimately optimizing the electrochemical performance of the hard carbon material.
[0137] Optionally, after the second calcination, the product obtained after the second calcination is naturally cooled to room temperature and acid-washed to obtain the negative electrode material.
[0138] In this application, unless otherwise specified, room temperature refers to 10–30°C.
[0139] The above-mentioned pickling can be performed using conventional procedures well known to those skilled in the art. For example, the pickling reagent includes at least one of hydrochloric acid solution, sulfuric acid solution, and oxalic acid solution; the concentration of the reagent is 1 mol / L to 3 mol / L; and the pickling time is 1 h to 4 h. For example, the reagent concentration can be any one of 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, or 3 mol / L, or a range between any two; and the pickling time can be any one of 1 h, 1.5 h, 2 h, 2.5 h, 3 h, 3.5 h, or 4 h, or a range between any two.
[0140] As an example, step (b) includes:
[0141] In such Figure 1 In the synthesis apparatus diagram shown, a phosphorus source (such as phenyl phosphorus dichloride) and a nitrogen source (such as pyrrole) are placed in a three-necked flask at a molar ratio of 1:1 to 4:1 and mixed at room temperature with a stirrer at 20°C to obtain a mixed solution.
[0142] A first inert atmosphere (such as nitrogen) is introduced into the mixed solution through the inlet 10, and then the mixed solution is sent into the tube furnace 40 through the outlet 30.
[0143] Hard carbon material and metal hydride (such as calcium hydride) are mixed at a mass ratio of 0.5 to 2:1 and fed into a tube furnace 40 using an alumina boat. The ratio of the mixed solution of phosphorus source and nitrogen source to hard carbon material is (10 to 20) mL: 1 g. The mixture is then calcined at 600 to 900°C for 2 to 5 hours at a heating rate of 2°C / min to 5°C / min. After calcination, the product is naturally cooled to room temperature and then acid-washed for 1 to 4 hours with a reagent (such as a hydrochloric acid solution with a concentration of 1 mol / L to 3 mol / L) to obtain the negative electrode material.
[0144] A third aspect of this application provides a battery including a negative electrode sheet, the negative electrode sheet comprising the aforementioned negative electrode material, or a negative electrode material prepared by the aforementioned method for preparing the negative electrode material.
[0145] Because the negative electrode includes the negative electrode material provided in the embodiments of this application, it can exhibit good electrochemical performance, such as high initial charge-discharge capacity and excellent initial coulombic efficiency.
[0146] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on the two opposite surfaces of the negative electrode current collector. It is understood that the negative electrode active material layer may also be stacked on either of the two surfaces of the negative electrode current collector.
[0147] This application does not impose any particular restrictions on the material of the negative electrode current collector, as long as it can achieve the purpose of this application, and can be selected according to actual needs. As an example, the negative electrode current collector can be made of metal materials such as aluminum, copper, nickel, stainless steel, nickel-plated steel, or foil with a surface coating.
[0148] In some embodiments, the negative electrode active material layer includes the hard carbon negative electrode material described above as provided in this application. Further, the negative electrode active material layer may optionally include a conductive agent. Further, the negative electrode active material layer may optionally include a binder. This application does not particularly limit the types of conductive agents and binders in the negative electrode active material layer, as long as they achieve the purpose of this application.
[0149] In some embodiments, the battery further includes a positive electrode, an electrolyte, and a separator. That is, the battery includes a positive electrode, a negative electrode, an electrolyte, and a separator.
[0150] In this embodiment of the application, the specific materials and structures of the positive electrode, separator, and electrolyte are not limited. Any components and structures known in the art that can be used in secondary batteries can be selected, as long as they can achieve the purpose of this application.
[0151] The battery mentioned in the embodiments of this application can be a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in this application can be a battery cell, or the battery can include a battery module (or battery pack), etc.
[0152] In some embodiments, the battery includes an electrode assembly and an electrolyte. The electrode assembly includes a positive electrode, a negative electrode, and a separator between the positive and negative electrode. The electrode assembly can be a wound structure or a stacked structure, and the embodiments of this application are not limited in this regard.
[0153] In some embodiments, the battery can be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module.
[0154] In some embodiments, the battery can be a battery pack, which may include a housing and individual battery cells, with the individual battery cells or battery modules housed within the housing.
[0155] It should be understood that multiple battery cells can be assembled into a battery module or battery pack. The number of battery cells contained in a battery module or battery pack can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module or battery pack.
[0156] In some embodiments, the battery can be an energy storage device. Energy storage devices include energy storage containers, energy storage cabinets, etc.
[0157] In the embodiments of this application, the methods for preparing battery cells or batteries are well known. In some embodiments, a positive electrode, a separator, a negative electrode, and an electrolyte can be assembled to form a battery cell. As an example, the positive electrode, separator, and negative electrode can be formed into an electrode assembly through a winding process and / or a stacking process. The electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping processes, a battery cell is obtained. Optionally, multiple battery cells can be further connected in series, parallel, or a hybrid configuration to form a battery module. Optionally, multiple battery modules can be connected in series, parallel, or a hybrid configuration to form a battery pack. Optionally, in some embodiments, multiple battery cells can also be directly assembled into a battery pack.
[0158] The present invention will be further described in detail below through examples. All raw materials used in the examples are commercially available.
[0159] Example 1
[0160] The preparation method of the negative electrode material includes the following steps:
[0161] (1) Place 100g of phenolic resin microspheres with a particle size of 5μm in a ceramic boat and place it in a tube furnace. Under a hydrogen-argon mixed atmosphere with a flow rate of 50mL / min and a hydrogen content of 5%, the temperature is raised to calcination temperature of 1300℃ at a heating rate of 2℃ / min and held for 2h to obtain hard carbon material.
[0162] (2) 179g of phenyl phosphorus dichloride and 67g of pyrrole were placed in a three-necked flask and stirred continuously at room temperature for 1h to obtain 205mL of mixed liquid; nitrogen gas was introduced into the bottom of the mixed solution through the gas inlet, and the mixed solution was sent into the tube furnace by the nitrogen gas flow rate of 100mL / min; 26g of magnesium hydride and 50g of hard carbon material were mixed evenly and placed into a corundum boat, and then the corundum boat was placed in the middle of the tube furnace. Under the nitrogen atmosphere, the temperature was raised to the calcination temperature of 800℃ at a heating rate of 2℃ / min and held for 2h. After the end, the material was naturally cooled. Then the material was acid washed in 500mL of 1mol / L hydrochloric acid solution for 2h to obtain the negative electrode material.
[0163] In the negative electrode material prepared in Example 1, based on the total mass of the negative electrode material, the doping amount of N element is 0.61 wt% and the doping amount of P element is 0.92 wt%. In the coating layer of the negative electrode material, based on the atomic content of the coating layer, the doping amount of N element is 6.7 at and the doping amount of P element is 14.2 at.
[0164] Example 2
[0165] The preparation method of the negative electrode material includes the following steps:
[0166] (1) Place 100g of phenolic resin microspheres with a particle size of 5μm in a ceramic boat and place it in a tube furnace. Under a hydrogen-argon mixed atmosphere with a flow rate of 50mL / min and a hydrogen content of 5%, the temperature is raised to calcination temperature of 1300℃ at a heating rate of 2℃ / min and held for 2h to obtain hard carbon material.
[0167] (2) 205g of phosphorus trichloride and 67g of pyrrole were placed in a three-necked flask and stirred continuously at room temperature for 1h to obtain 203mL of mixed liquid. Nitrogen gas was introduced into the bottom of the mixed solution through the gas inlet, and the mixed solution was sent into the tube furnace through the nitrogen gas flow rate of 100mL / min. 42g of calcium hydride and 50g of hard carbon material were mixed evenly and placed into a corundum boat. The corundum boat was then placed in the middle of the tube furnace. Under the nitrogen atmosphere, the temperature was increased to the calcination temperature of 800℃ at a heating rate of 2℃ / min and held for 2h. After the heating was completed, the material was naturally cooled. Then the material was acid washed in 500mL of 1mol / L hydrochloric acid solution for 2h to obtain the negative electrode material.
[0168] Example 3
[0169] The preparation method of the negative electrode material includes the following steps:
[0170] (1) Place 100g of phenolic resin microspheres with a particle size of 5μm in a ceramic boat and place it in a tube furnace. Under a hydrogen-argon mixed atmosphere with a flow rate of 50mL / min and a hydrogen content of 5%, the temperature is raised to calcination temperature of 1400℃ at a heating rate of 2℃ / min and held for 2h to obtain hard carbon material.
[0171] (2) 205g of phosphorus trichloride and 67g of pyrrole were placed in a three-necked flask and stirred continuously at room temperature for 1h to obtain 203mL of mixed liquid; Argon gas was introduced into the bottom of the mixed solution through the gas inlet, and the mixed solution was sent into the tube furnace through a nitrogen gas flow rate of 100mL / min; 42g of calcium hydride and 50g of hard carbon material were mixed evenly and placed into a corundum boat, which was then placed in the middle of the tube furnace. Under a nitrogen atmosphere, the temperature was increased to 700℃ at a heating rate of 2℃ / min and held for 2h. After the heating was completed, the material was naturally cooled. Then the material was acid washed in 500mL of 1mol / L hydrochloric acid solution for 2h to obtain the negative electrode material.
[0172] Example 4
[0173] The preparation method of the negative electrode material includes the following steps:
[0174] (1) Place 100g of phenolic resin microspheres with a particle size of 5μm in a ceramic boat and place it in a tube furnace. Under a hydrogen-argon mixed atmosphere with a flow rate of 50mL / min and a hydrogen content of 5%, the temperature is raised to calcination temperature of 1400℃ at a heating rate of 2℃ / min and held for 2h to obtain hard carbon material.
[0175] (2) 205g of phosphorus trichloride and 129g of quinoline were placed in a three-necked flask and stirred continuously at room temperature for 1h to obtain 251mL of mixed liquid. Nitrogen gas was introduced into the bottom of the mixed solution through the gas inlet, and the mixed solution was sent into the tube furnace through a nitrogen gas flow rate of 100mL / min. 11g of beryllium hydride and 50g of hard carbon material were mixed evenly and placed in a corundum boat. The corundum boat was then placed in the middle of the tube furnace. Under a nitrogen atmosphere, the temperature was increased to 800℃ at a heating rate of 2℃ / min and held for 2h. After the heating was completed, the material was naturally cooled. Then the material was acid washed in 500mL of 1mol / L hydrochloric acid solution for 2h to obtain the negative electrode material.
[0176] Example 5
[0177] The preparation method of the negative electrode material is similar to that in Example 1, except that:
[0178] In step (1), the heating rate is 5℃ / min, the calcination temperature is 1400℃, and the holding time is 5h.
[0179] Example 6
[0180] The preparation method of the negative electrode material is similar to that in Example 1, except that:
[0181] In step (2), the heating rate is 5℃ / min, the calcination temperature is 1200℃, and the holding time is 2h.
[0182] Example 7
[0183] The preparation method of the negative electrode material is similar to that in Example 1, except that:
[0184] In step (2), the mass of phenylphosphine dichloride is 208.5g, the mass of pyrrole is 100.5g, and the solution volume is 308ml.
[0185] Comparative Example 1
[0186] The preparation method of the negative electrode material includes the following steps:
[0187] 100g of phenolic resin microspheres with a particle size of 5μm were placed in a ceramic boat and placed in a tube furnace. Under a nitrogen atmosphere with a flow rate of 50mL / min, the temperature was increased to calcination temperature of 1400℃ at a heating rate of 2℃ / min and held for 2h to obtain phenolic resin-based carbon spheres, which are the negative electrode materials.
[0188] Comparative Example 2
[0189] The preparation method of the negative electrode material includes the following steps:
[0190] (1) Place 100g of phenolic resin microspheres with a particle size of 5μm in a ceramic boat and place it in a tube furnace. Under a hydrogen-argon mixed atmosphere with a flow rate of 50mL / min and a hydrogen content of 5%, the temperature is raised to calcination temperature of 1300℃ at a heating rate of 2℃ / min and held for 2h to obtain hard carbon material.
[0191] (2) Place 50g of hard carbon material, 20g of sodium dihydrogen phosphate and 10g of urea in a ceramic boat and place it in the middle of a tube furnace. Under a nitrogen atmosphere, heat the material to a calcination temperature of 700℃ at a heating rate of 2℃ / min and hold for 2 hours. After the calcination is completed, allow it to cool naturally to obtain phenolic resin-based carbon spheres-OPN, which is the negative electrode material.
[0192] In the negative electrode material prepared in Comparative Example 2, based on the atomic content in the negative electrode material, the doping amount of N element is 0.51 at, the doping amount of P element is 0.42 at, and the doping amount of O element is 4.6 at.
[0193] Comparative Example 3
[0194] The preparation method of the negative electrode material includes the following steps:
[0195] (1) Place 100g of phenolic resin microspheres with a particle size of 5μm in a ceramic boat and place it in a tube furnace. Under a nitrogen atmosphere with a flow rate of 50mL / min, heat the furnace to a calcination temperature of 1400℃ at a heating rate of 2℃ / min and hold for 2h to obtain hard carbon material.
[0196] (2) Place 50g of hard carbon material, 20g of sodium dihydrogen phosphate and 10g of urea in a ceramic boat and place it in the middle of a tube furnace. Under a nitrogen atmosphere, heat the material to a calcination temperature of 700℃ at a heating rate of 2℃ / min and hold for 2 hours. After the calcination is completed, allow it to cool naturally to obtain the intermediate material.
[0197] (3) Mix 30g of intermediate material and 5g of asphalt and stir for 1 hour. Then place it in a ceramic boat in the middle of a tube furnace. Under a nitrogen atmosphere, heat the material to 700℃ at a heating rate of 2℃ / min and hold for 2 hours. After the heating is completed, allow it to cool naturally to obtain phenolic resin carbon balls @ONP-coated, which is the negative electrode material.
[0198] Battery fabrication and performance testing
[0199] 1. Preparation of sodium-ion batteries
[0200] (1) The negative electrode material, conductive agent carbon black and binder carboxymethyl cellulose prepared in the above embodiments and comparative examples are mixed and added to N-methylpyrrolidone (NMP) solvent to obtain a slurry. The mass ratio of negative electrode material, conductive agent and binder is 8:1:1. The obtained slurry is evenly coated on aluminum foil and dried in a vacuum drying oven at 100°C for 12 hours to obtain a negative electrode sheet.
[0201] (2) Provide a sodium metal sheet as the positive electrode of the counter electrode;
[0202] (3) Provide a glass fiber diaphragm as a separation membrane;
[0203] (4) Provide an electrolyte solution, which is a 1 mol / L diethylene glycol dimethyl ether solution of NaPF6;
[0204] (5) Assemble the negative electrode, separator and positive electrode in the order of negative electrode, separator and positive electrode, and wet them with electrolyte respectively. Assemble them into CR2032 button cell in argon glove box.
[0205] 2. Battery performance test
[0206] (1) Initial discharge capacity test: Using the Land battery test system, under the condition of 25℃, constant current discharge to 0V at a current density of 0.1C was performed, and the discharge capacity at this time was recorded as the initial discharge capacity; the test results are shown in Table 1.
[0207] (2) Initial charge capacity test: Using the Land battery test system, the battery was charged to 2V at a constant current density of 0.1C under the condition of 25℃. The charging capacity at this time was recorded as the initial charge capacity. The test results are shown in Table 1.
[0208] (3) Initial Coulombic Efficiency (First-Effect) Test: Under the condition of 25℃, constant current discharge to 0V at a current density of 0.1C, and record the discharge capacity at this time as the initial discharge capacity; constant current charging to 2V at a current density of 0.1C, and record the charging capacity at this time as the initial charging capacity; initial coulombic efficiency = initial charging capacity / initial discharge capacity * 100%; the test results are shown in Table 1;
[0209] (4) Capacity retention rate (cycle performance) test: Under the condition of 25℃, discharge to 0V at a constant current rate of 1C, and then charge to 2V at a constant current rate of 1C. This constitutes a complete charge-discharge cycle. Record one cycle. Repeat this process until the number of cycles equals 500. End the test and record the charging capacity on the 500th cycle. Then, the capacity retention rate on the 500th cycle = charging capacity on the 500th cycle / charging capacity on the 1st cycle * 100%; the test results are shown in Table 1.
[0210] Table 1
[0211]
[0212]
[0213] As shown in Table 1, the coin cells of the high-performance sodium-ion battery anode composite materials prepared from the anode materials in the examples all exhibit high initial charge / discharge capacities (over 420 mAh / g) and initial charge efficiency exceeding 90%, while the initial discharge capacity of Comparative Example 1 is only 332.5 mAh / g, the initial charge capacity is only 281.3 mAh / g, and the initial coulombic efficiency is 84.6%. This indicates that the carbon coating layer effectively reduces the specific surface area of the material and decreases the defect concentration, which is beneficial to improving the initial coulombic efficiency of the material. At the same time, the diatomic doping expands the carbon layer spacing of the carbon material, providing more active sites and enhancing the specific capacity. Therefore, the anode material prepared in this invention has high reversible capacity and low potential capacity.
[0214] The coin cells of the novel sodium-ion battery anode composite materials prepared from the anode materials in the examples all exhibited high cycle retention rates (greater than 90%) and excellent cycle stability, while the capacity retention rate of Comparative Example 1 was only 80.1%. This indicates that achieving high-doping N and P dual-doping in the coating layer, with two-atom doping, can alter the local bonding environment and electron distribution on the surface of the hard carbon anode material, resulting in a significantly expanded interlayer spacing and thus improving the reactivity and electronic conductivity of the hard carbon anode material. The presence of the coating layer further reduces the specific surface area of the material, increases the number of closed pores, and enhances the cycle and rate performance. In Comparative Example 2, elemental doping was performed in an aerobic environment, increasing the number of active adsorption sites and achieving the goal of increasing the material capacity, but the performance of the anode material was lower than that of the examples. Comparative Example 3, based on Comparative Example 2, underwent a coating process, which effectively improved the initial efficiency of the material, but the effect was lower than that of the examples. This indicates that a large amount of doping of elements cannot be achieved in an aerobic environment, thus failing to significantly improve the material performance.
[0215] 3. Performance testing of negative electrode materials: The specific surface area of the negative electrode materials in the examples and comparative examples was tested using the nitrogen adsorption-desorption method. The test results are shown in Table 2.
[0216] Table 2
[0217]
[0218]
[0219] As shown in Table 2, the negative electrode materials prepared in the examples all have small specific surface areas (all less than 2m²). 2 / g), while the specific surface area of the negative electrode materials prepared in the comparative example is greater than 6m². 2 / g, even exceeding 10m 2 / g. This indicates that Comparative Example 2, which was not coated, has the largest specific surface area, which is caused by the open pores generated during the calcination process. Comparative Example 3, after being coated with asphalt, can effectively reduce the specific surface area, but the coating effect is not uniform enough, and some pores are still not coated. The example achieves uniform coating of the material by uniformly transporting the carbon source through airflow, thus resulting in a greater reduction in specific surface area.
[0220] The EDS surface scan of the hard carbon material prepared in Example 1 is shown below. Figure 2 As shown.
[0221] The EDS line scan image of the hard carbon material prepared in Example 1 is shown below. Figure 3 As shown. By Figure 2 , Figure 3 It can be seen that hard carbon materials contain only carbon elements, indicating that hard carbon materials do not contain oxygen elements.
[0222] The EDS surface scan of the negative electrode material prepared in Example 1 is shown below. Figure 4 As shown. By Figure 4 It can be seen that the P and N elements in the anode material have been successfully doped and are uniformly distributed.
[0223] TEM image of the negative electrode material prepared in Example 1 is shown below. Figure 5 As shown. By Figure 5 It can be seen that carbon material was successfully coated in the anode material, and the coating thickness was 4.6 nm.
[0224] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a negative electrode material, characterized in that, Includes the following steps: The hard carbon precursor was subjected to a first calcination under a reducing atmosphere to obtain the hard carbon material. Phosphorus source and nitrogen source are mixed to obtain a mixed solution; hard carbon material and metal hydride are mixed to obtain a mixture; the mixed solution is mixed with the mixture under a first inert atmosphere and subjected to a second calcination. After the second calcination, the mixture is naturally cooled to room temperature, and then the obtained product is acid washed to obtain the negative electrode material. The negative electrode material includes a hard carbon material and a coating layer covering at least a portion of the surface of the hard carbon material; The coating layer includes a carbon material, which includes a carbon material matrix and doping elements doped in the carbon material matrix, wherein the doping elements include P and N; The oxygen content in the negative electrode material is 0; The reducing atmosphere includes a mixture of hydrogen and a second inert atmosphere; The volume percentage of hydrogen in the mixed atmosphere is 3% to 5%; The second inert atmosphere includes at least one of nitrogen, argon, helium, and neon; The flow rate of the reducing atmosphere is 50 mL / min to 100 mL / min; The first inert atmosphere includes at least one of nitrogen, argon, helium, and neon; The flow rate of the first inert atmosphere is 50 mL / min to 150 mL / min; The molar ratio of phosphorus source to nitrogen source in the mixed solution of phosphorus source and nitrogen source is 1:1 to 4:1; The ratio of the mixed solution of the phosphorus source and nitrogen source to the hard carbon material is (2~20) mL: 1 g; The mass ratio of the metal hydride to the hard carbon material is 0.5~2:1; The phosphorus source includes at least one of phosphorus trichloride, phenyl phosphorus dichloride, and phosphorus tribromide; The nitrogen source includes at least one of pyrrole, pyridine, and quinoline; The metal hydride includes at least one of calcium hydride, magnesium hydride, potassium hydride, and beryllium hydride.
2. The method for preparing the negative electrode material according to claim 1, characterized in that, Hard carbon precursors include resins and / or biomass materials; The resin includes at least one of phenolic resin, epoxy resin, polyacrylonitrile, and polyimide.
3. The method for preparing the negative electrode material according to claim 2, characterized in that, The particle size of the phenolic resin is 5µm to 10µm.
4. The method for preparing the negative electrode material according to claim 1, characterized in that, The first calcination temperature is 1000℃~1400℃, the first calcination time is 2h~5h, and the first calcination heating rate is 2℃ / min~5℃ / min.
5. The method for preparing the negative electrode material according to any one of claims 1 to 4, characterized in that, The second calcination temperature is 600℃~900℃, the second calcination time is 2h~5h, and the second calcination heating rate is 2℃ / min~5℃ / min.
6. The method for preparing the negative electrode material according to any one of claims 1 to 4, characterized in that, The pickling reagent includes at least one of hydrochloric acid solution, sulfuric acid solution and oxalic acid solution; The concentration of the reagent is 1 mol / L to 3 mol / L; The pickling time is 1 hour to 4 hours.
7. A negative electrode material prepared by the preparation method according to any one of claims 1 to 6, characterized in that, The negative electrode material includes hard carbon material and a coating layer covering at least a portion of the surface of the hard carbon material; The coating layer includes a carbon material, which includes a carbon material matrix and doping elements doped in the carbon material matrix, wherein the doping elements include P and N; The oxygen content in the negative electrode material is 0; The hard carbon material also includes doping elements, including P and N. Based on the mass of the negative electrode material, the doping amount of P element in the negative electrode material is 0.5wt%~1wt%; Based on the mass of the negative electrode material, the nitrogen doping amount in the negative electrode material is 0.5wt%~1wt%; The thickness of the coating layer is 2nm~10nm; The particle size of the hard carbon material is 4µm~8µm; The hard carbon material includes spherical hard carbon material; Based on the atomic content of the coating layer, the doping amount of P element in the carbon material is 10 at%~15 at%; Based on the atomic content of the coating layer, the doping amount of N element in the carbon material is 5 at% to 10 at%.
8. A battery, comprising a negative electrode, characterized in that, The negative electrode sheet includes the negative electrode material prepared by the method of any one of claims 1 to 6, or includes the negative electrode material as described in claim 7.
Citation Information
Patent Citations
Preparation method of biomass composite hard carbon negative electrode material, negative electrode material and application
CN115881919A
Hard carbon negative electrode material, preparation method thereof, negative electrode plate and application of negative electrode plate
CN116632210A