Machining method for carburizing and quenching multi-tooth part

The step-by-step carburizing and quenching treatment method solves the problem of inconsistent carburizing layer depth on multiple teeth, ensures the processing accuracy and strength of the gears, simplifies the process flow and reduces costs.

CN120683451APending Publication Date: 2025-09-23CHANGZHOU TIANSHAN HEAVY IND MACHINERY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510917438.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-03
Publication Date
2025-09-23

AI Technical Summary

Technical Problem

In the prior art, the carburized layer depth requirements for multiple teeth of the same part are inconsistent, which leads to processing difficulties. In particular, it is difficult for teeth with different modules to simultaneously meet the hardness and margin requirements during the carburizing and quenching process.

Method used

The step-by-step carburizing and quenching treatment method is adopted. First, the teeth that meet the depth requirements of the first heat treatment layer are rough-machined and carburized once. Then the hardened layer is removed and group-processed. Then all teeth are carburized and quenched twice. Finally, fine machining is performed to ensure that the carburized layer depth of each tooth meets the requirements.

Benefits of technology

The controllable deformation of the tooth surface of multiple teeth is achieved, the torque transmission capacity and overall strength of the gear are guaranteed, the process flow is simplified, the cost is reduced, and the split structure design is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120683451A_ABST
    Figure CN120683451A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of gear machining, and particularly relates to a machining method for carburizing and quenching of a multi-tooth part, which comprises the following steps: roughly machining a tooth part with a first heat treatment layer depth requirement, and not machining a tooth part with a second heat treatment layer depth requirement and carrying out anti-seepage protection; performing primary carburization on the tooth part required by the first heat treatment layer depth and the tooth part required by the second heat treatment layer depth at the same time; discharging after primary carburization is completed, turning off a hardened layer of the tooth part with the second heat treatment layer depth requirement, and performing group processing; carrying out secondary carburization on the tooth part with the first heat treatment layer depth requirement and the tooth part with the second heat treatment layer depth requirement at the same time, and carrying out quenching treatment after secondary carburization; and carrying out finish machining and deformation statistics on the tooth part required by the first heat treatment layer depth and the tooth part required by the second heat treatment layer depth. The technical problem of different carburizing and quenching layer depth requirements of the multi-tooth part of the same part is solved, it can be ensured that tooth surface deformation of the multi-tooth part is within a controllable range, and the torque transmission capacity of the gear is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gear processing, and in particular relates to a processing method for carburizing and quenching multiple teeth. Background Art

[0002] Carburizing and quenching is a common heat treatment process that can make the surface obtain very high hardness to improve its wear resistance. In the actual processing process, the same part has multiple teeth. The depth of the carburized layer of multiple teeth is closely related to the size of their modulus. The carburized layer depth of carburized and quenched teeth with different moduli is different. The tooth with a larger modulus has a deeper carburized layer depth, and the tooth with a smaller modulus has a shallower carburized layer depth.

[0003] It is a priority to heat treat a part together. If heat treated according to the high-depth requirements, the allowance of the tooth surface with a smaller module will increase greatly, which will cause great difficulty in the subsequent finishing of the tooth surface. If the tooth with a larger module is carburized first and the tooth with a smaller module is coated with an anti-seepage agent, it is impossible to completely guarantee that the tooth with a smaller module will not have any leakage, and some positions will still harden. Summary of the Invention

[0004] The purpose of the present invention is to solve the defects and deficiencies in the prior art and to provide a processing method for carburizing and quenching multiple teeth.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a processing method for carburizing and quenching multiple teeth, comprising the following steps:

[0006] (1) The teeth required by the first heat treatment layer depth are rough-machined, and the teeth required by the second heat treatment layer depth are not machined and are protected from seepage;

[0007] (2) Carburizing the teeth with the first heat treatment layer depth requirement and the teeth with the second heat treatment layer depth requirement at the same time;

[0008] (3) After the first carburizing is completed, the gear is taken out of the furnace, the hardened layer of the second heat treatment layer is turned to the required depth and the gear is assembled;

[0009] (4) performing secondary carburizing on the teeth of the first heat treatment layer depth requirement and the teeth of the second heat treatment layer depth requirement at the same time, and performing quenching treatment at the same time after the secondary carburizing;

[0010] (5) Perform fine machining and deformation statistics on the teeth required by the first heat treatment layer depth and the teeth required by the second heat treatment layer depth.

[0011] Preferably, the depth requirement of the first heat treatment layer is greater than the depth requirement of the second heat treatment layer.

[0012] Preferably, the tooth portion required by the first heat-treated layer depth includes a first tooth portion and a second tooth portion, and the tooth portion required by the second heat-treated layer depth includes a third tooth portion.

[0013] Preferably, the first tooth portion and the second tooth portion have opposite rotation directions to form a herringbone tooth structure, and the heat treatment layer depth of the third tooth portion is 1 mm less than that of the first tooth portion and the second tooth portion.

[0014] Preferably, the first heat-treated layer depth is required to be formed by superposition of primary carburizing and secondary carburizing, and the second heat-treated layer depth is required to be formed by secondary carburizing.

[0015] Preferably, the secondary carburizing comprises:

[0016] Preheating: 400℃ without nitrogen for 30min;

[0017] Carburizing temperature rise, using 800℃ uniform temperature for 60min;

[0018] Carburizing: Carburizing is carried out by heating to 900℃;

[0019] Carburizing cooling, use 830℃ uniform temperature for 180min.

[0020] Preferably, the carburizing process at 900° C. includes a 540-minute intensive carburizing stage, a 90-minute slow carbon reduction stage, and a 480-minute diffusion stage.

[0021] Preferably, after the carburizing is cooled, the carburizer enters the front chamber oil tank for quenching and cooling, the oil temperature in the oil tank is 50°C, the stirring motor speed is 900rpm / 1800s, the oil is poured for 10 minutes, and the temperature rise is no more than 20°C.

[0022] Preferably, the post-quenching cooling includes washing and foaming spraying with 30°C clean water for 25 minutes.

[0023] Preferably, low-temperature tempering is performed after the quenching and cooling, and the low-temperature tempering includes a first low-temperature tempering stage of tempering at 160-180° C. for 600 min and a second low-temperature tempering stage of tempering at 160-180° C. for 360 min.

[0024] After adopting the above technical solution, the present invention provides a method for carburizing and quenching multiple teeth, which has the following beneficial effects:

[0025] The present invention solves the technical problem of different carburizing and quenching layer depth requirements for multiple teeth of the same part, can ensure that the deformation of the tooth surface of the multiple teeth is within a controllable range, ensures the torque transmission capacity of the gear, overcomes the processing difficulties caused by inconsistent carburizing layer depth and hardness requirements for gears of different modules, and for integral parts with size and weight restrictions, there is no need to design the parts as a split structure for multiple gears of different modules, thereby ensuring the overall strength of the parts. It has the advantages of simple process, easy operation, low cost, good effect, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is the finished appearance of the workpiece prepared by the processing method of the present invention;

[0027] Figure 2 This is a heat treatment curve diagram of a processing method for carburizing and quenching multiple teeth according to the present invention.

[0028] Among them: a first tooth portion 1, a second tooth portion 2, and a third tooth portion 3. DETAILED DESCRIPTION

[0029] The present invention will be further described clearly and completely below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the embodiments described are only some, not all, of the embodiments of the present invention. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention, its application, or use. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort are intended to fall within the scope of protection of the present invention.

[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, they indicate the presence of features, steps, operations, devices, components and / or combinations thereof.

[0031] Unless otherwise specifically stated, the relative arrangement of the parts and steps, the numerical expressions and the numerical values ​​set forth in these embodiments do not limit the scope of the present invention. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the drawings are not drawn according to the actual proportional relationship. The techniques, methods and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but where appropriate, the techniques, methods and equipment should be considered as part of the authorization specification. In all examples shown and discussed here, any specific values ​​should be interpreted as being merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values. It should be noted that similar numbers and letters represent similar items in the following figures, and therefore, once an item is defined in one figure, it does not need to be further discussed in subsequent figures.

[0032] In the description of the present invention, it should be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "horizontal, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention; the directional words "inside and outside" refer to the inside and outside relative to the outline of each component itself.

[0033] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used herein to describe the spatial positional relationship of a device or feature to other devices or features as shown in the figures. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figures. For example, if the device in the drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0034] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0035] like Figure 1-2As shown, this embodiment provides a method for carburizing and quenching multiple teeth, comprising the following steps:

[0036] (1) The teeth required by the first heat treatment layer depth are rough-machined, and the teeth required by the second heat treatment layer depth are not machined and are protected from seepage;

[0037] (2) Carburizing the teeth with the first heat treatment layer depth requirement and the teeth with the second heat treatment layer depth requirement at the same time;

[0038] (3) After the first carburizing is completed, the gear is taken out of the furnace, the hardened layer of the second heat treatment layer is turned to the required depth and the gear is assembled;

[0039] (4) performing secondary carburizing on the teeth of the first heat treatment layer depth requirement and the teeth of the second heat treatment layer depth requirement at the same time, and performing quenching treatment at the same time after the secondary carburizing;

[0040] (5) Perform fine machining and deformation statistics on the teeth required by the first heat treatment layer depth and the teeth required by the second heat treatment layer depth.

[0041] In this embodiment, the first heat treatment layer depth requirement is greater than the second heat treatment layer depth requirement. Specifically, the tooth portion with the first heat treatment layer depth requirement includes the first tooth portion 1 and the second tooth portion 2, and the tooth portion with the second heat treatment layer depth requirement includes the third tooth portion 3, wherein the first tooth portion 1 and the second tooth portion 2 have opposite rotation directions to form a herringbone tooth structure, and the heat treatment layer depth of the third tooth portion 3 is 1 mm smaller than the heat treatment layer depth of the first tooth portion 1 and the second tooth portion 2.

[0042] It should be noted that the depth of the first heat treatment layer in this embodiment is required to be formed by superposition of primary carburizing and secondary carburizing, which requires that the layer depth during primary carburizing be controlled within the lower and middle limits, and the depth of the second heat treatment layer is required to be formed by secondary carburizing.

[0043] According to one embodiment of the present invention, the secondary carburizing comprises:

[0044] Preheating: 400℃ without nitrogen for 30min;

[0045] Carburizing temperature rise, using 800℃ uniform temperature for 60min;

[0046] Carburizing: Carburizing was carried out by heating the sample to 900 °C, which included a 540-min intensive carburizing stage, a 90-min slow carbon reduction stage, and a 480-min diffusion stage.

[0047] Carburizing cooling, use 830℃ uniform temperature for 180min.

[0048] According to one embodiment of the present invention, after carburizing and cooling, it enters the front chamber oil tank for quenching and cooling, the oil temperature in the oil tank is 50°C, the stirring motor speed is 900rpm / 1800s, the oil is poured for 10 minutes, and the temperature rise is not more than 20°C, wherein the cooling after quenching includes 30°C clean water washing and foaming spraying for 25 minutes.

[0049] According to one embodiment of the present invention, low-temperature tempering is performed after quenching and cooling, and the low-temperature tempering includes a first low-temperature tempering stage of tempering at 160-180°C for 600 minutes and a second low-temperature tempering stage of tempering at 160-180°C for 360 minutes. Furthermore, the tempering temperature of the first low-temperature tempering stage and the second low-temperature tempering stage are preferably 160°C. After the low-temperature tempering is completed, the steel can be taken out of the furnace and air-cooled.

[0050] In summary, the present invention solves the technical problem of different carburizing and quenching layer depth requirements for multiple teeth of the same part, can ensure that the deformation of the tooth surface of multiple teeth is within a controllable range, ensures the torque transmission capacity of the gear, overcomes the processing difficulties caused by inconsistent carburizing layer depth and hardness requirements for gears of different modules, and for integral parts with size and weight restrictions, there is no need to design the parts into a split structure of multiple gears of different modules, thereby ensuring the overall strength of the parts. It has the advantages of simple process, easy operation, low cost, and good effect.

[0051] The above description is only a preferred specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any technician familiar with the technical field, within the technical scope disclosed by the present invention, who makes equivalent replacements or changes based on the technical solution and inventive concept of the present invention, should be covered by the scope of protection of the present invention.

Claims

1. A method for carburizing and quenching multiple teeth, characterized in that: The following steps are involved: (1) The teeth required by the first heat treatment layer depth are rough-machined, and the teeth required by the second heat treatment layer depth are not machined and are protected from seepage; (2) Carburizing the teeth with the first heat treatment layer depth requirement and the teeth with the second heat treatment layer depth requirement at the same time; (3) After the first carburizing is completed, the gear is taken out of the furnace, the hardened layer of the second heat treatment layer is turned to the required depth and the gear is assembled; (4) performing secondary carburizing on the teeth of the first heat treatment layer depth requirement and the teeth of the second heat treatment layer depth requirement at the same time, and performing quenching treatment at the same time after the secondary carburizing; (5) Perform fine machining and deformation statistics on the teeth required by the first heat treatment layer depth and the teeth required by the second heat treatment layer depth.

2. A method for carburizing and quenching multiple teeth according to claim 1, characterized in that: The first heat treatment layer depth requirement is greater than the second heat treatment layer depth requirement.

3. A method for carburizing and quenching multiple teeth according to claim 1, characterized in that: The tooth portion required by the first heat-treated layer depth includes a first tooth portion and a second tooth portion, and the tooth portion required by the second heat-treated layer depth includes a third tooth portion.

4. A method for carburizing and quenching multiple teeth according to claim 3, characterized in that: The first tooth portion and the second tooth portion have opposite rotation directions, forming a herringbone tooth structure. The depth of the heat-treated layer of the third tooth portion is 1 mm less than that of the first tooth portion and the second tooth portion.

5. The method for carburizing and quenching multiple teeth according to claim 1, characterized in that: The first heat-treated layer depth is required to be formed by superposition of primary carburizing and secondary carburizing, and the second heat-treated layer depth is required to be formed by secondary carburizing.

6. The method for carburizing and quenching multiple teeth according to claim 1, characterized in that: The secondary carburizing comprises: Preheating: 400℃ without nitrogen for 30min; Carburizing temperature rise, using 800℃ uniform temperature for 60min; Carburizing: Carburizing is carried out by heating to 900℃; Carburizing cooling, use 830℃ uniform temperature for 180min.

7. A method for carburizing and quenching multiple teeth according to claim 6, characterized in that: The carburizing process at 900° C. includes a 540-minute intensive carburizing stage, a 90-minute slow carbon reduction stage, and a 480-minute diffusion stage.

8. The method for carburizing and quenching multiple teeth according to claim 6, characterized in that: After the carburizing is cooled, the carburizer enters the front chamber oil tank for quenching and cooling. The oil temperature in the oil tank is 50°C, the stirring motor speed is 900rpm / 1800s, the oil is poured for 10 minutes, and the temperature rise is no more than 20°C.

9. A method for carburizing and quenching multiple teeth according to claim 8, characterized in that: The post-quenching cooling includes washing and foaming with 30° C. clean water for 25 minutes.

10. The method for carburizing and quenching multiple teeth according to claim 8, characterized in that: After the quenching and cooling, low-temperature tempering is performed, and the low-temperature tempering includes a first low-temperature tempering stage of tempering at 160-180° C. for 600 minutes and a second low-temperature tempering stage of tempering at 160-180° C. for 360 minutes.