Rolling process for improving core quality of high-carbon-chromium bearing steel
Patent Information
- Application Number
- CN202510716487.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-30
- Publication Date
- 2025-09-26
AI Technical Summary
In the existing technology, high carbon chromium bearing steel is prone to produce microscopic porosity defects during the rolling process, resulting in failure in flaw detection, increasing costs and the risk of product scrapping.
A multi-stage heating and soaking process is adopted, combined with high-pressure water descaling, precise control of rolling parameters and final rolling deformation, and a KOCKS final rolling unit and ultrasonic flaw detection are used to ensure that there are no microscopic pore defects.
It significantly improves the quality of the core of the rolled material, increases the inspection pass rate, avoids rejection due to defects, and reduces production costs.
Smart Images

Figure CN120696209A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of steel rolling, in particular to a rolling process for improving the core quality of high-carbon chromium bearing steel. Background Art
[0002] High-carbon chromium bearing steel, with a carbon content of approximately 1.0%, is a hypereutectoid steel. Dendritic segregation occurs during casting and solidification. In areas of severe segregation, a eutectic reaction occurs, producing eutectic carbides with a melting point of 1216°C. During the heating process for rolling, if the carbides cannot dissolve and diffuse, they will form liquid precipitation within the steel. However, if the heating temperature is too high and the diffusion time is too long, the carbides will dissolve or disappear, leaving behind pores. If these pores cannot be welded together during subsequent rolling, microporosity will form. Microporosity is a structural defect within bearing steel, and national standards clearly stipulate that microporosity is not permitted for bearing steel with a diameter of 60 mm or less. Microporosity, as seen in metallographic examination images, appears as intermittent, irregular cracks or pores along grain boundaries. These microporosity defects are primarily located in the center of the steel, with a banded distribution along the rolling direction. Analysis reveals carbide segregation in these defective areas, with large carbide accumulations in localized areas. The existence of this defect will result in failure in the flaw detection, and the core may crack during processing and use by the user, and the bearing ring product may be scrapped. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to overcome the shortcomings of the existing technology and provide a rolling process for improving the quality of the core of high carbon chromium bearing steel, which can solve the micropore defects in the core of the rolled material, improve the pass rate of flaw detection, and avoid scrapping or re-judgment due to unqualified flaw detection, which increases costs.
[0004] In order to solve the above technical problems, the technical solutions of the present invention are as follows: A rolling process for improving the core quality of high carbon chromium bearing steel, characterized by comprising the following steps: S1: The slab is kept in a heating furnace at 1200-1240°C for at least 150 minutes; S2: After descaling with high-pressure water, rough rolling and intermediate rolling are carried out in sequence. The rough rolling reduction is 40-50%, and the intermediate rolling reduction is 30-40%. S3: The incoming material size of φ40 finished rolled products before final rolling is φ59mm rolled products; S4: Rolled using the KOCKS finishing mill with a specification range of φ40.11-φ43.03mm, with a final rolling deformation of 54% and a final rolling temperature of 780℃-850℃; S5: The core quality of round steel is tested by ultrasonic testing to ensure that there are no microscopic pore defects.
[0005] A further preferred embodiment of the present invention is that: the heating in S1 adopts multi-stage heating and equalizing, wherein the temperature of the first heating stage is 900-1000°C, the temperature of the second heating stage is 1100-1200°C, the temperature of the first equalizing stage is 1200-1240°C, the temperature of the second equalizing stage is 1200-1230°C, and the high temperature stage is kept warm for at least 150 minutes.
[0006] A further preferred embodiment of the present invention is that: the rough rolling stage in S2 adopts reduced speed rolling, with a rolling speed of ≤0.6 m / s and a reduction of ≥15% per pass.
[0007] A further preferred embodiment of the present invention is that the size of the KOCKS finishing mill in S4 is a positive tolerance, and other steel grades of the same specification with a relatively wide range of dimensional accuracy need to be produced for dimensional debugging before rolling. The roll gap control accuracy is ±0.05mm, and the rolling force fluctuation range is ≤5%, ensuring that the final rolling dimensional tolerance is ±0.1mm.
[0008] The beneficial effects of the present invention are: The present invention increases the original final rolling deformation of 26% to ≥54%. The increase in final rolling deformation can significantly improve the core penetration ability of the rolled piece and improve the core quality. At the same time, combined with the pre-finishing rolling size adjustment (φ59mm) and the optimization of the roller system specifications, the welding ability of the core defects of the rolled piece is enhanced to achieve qualified core quality, effectively solving the problems of insufficient center penetration and serious micropore defects in the existing technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] Figure 1 This is a microscopic gold image of the cross section of Example 1; Figure 2 This is a microscopic gold image of the longitudinal cross section of Example 1; Figure 3 This is a graph of unqualified internal detection using the process of the present invention; Figure 4 This is a qualified map for internal exploration using the process of the present invention. DETAILED DESCRIPTION
[0010] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below based on specific implementation methods. Example 1
[0011] This embodiment provides a rolling process for improving the core quality of high carbon chromium bearing steel, which specifically includes the following steps: S1: The steel billet is heated in multiple stages in a heating furnace, wherein the temperature of the first heating stage is 1000°C, the temperature of the second heating stage is 1100°C, the temperature of the first and second soaking stages are both 1200°C, and the temperatures are kept at this temperature for 160 minutes; S2: After descaling with high-pressure water, the steel is rolled in sequence through rough rolling, intermediate rolling, pre-finishing rolling and final rolling. The steel is rolled in different specifications ranging from φ16 to 50 mm. The rough rolling speed is 0.4 m / s and the reduction per pass is ≥15%; S3: The incoming material size of φ40 finished rolled products before final rolling is φ59mm rolled products; S4: Rolling is carried out using the KOCKS finishing mill with a specification range of φ40.11-φ43.03mm, a final rolling deformation of 54%, and a final rolling temperature of 800℃. Before rolling, other steel grades of the same specification with a relatively wide range of dimensional accuracy must be produced for dimensional debugging to ensure the final rolling dimensional tolerance; S5: The core quality of round steel is tested by ultrasonic testing to ensure that there are no microscopic pore defects. After inspection, the qualified rate of internal inspection of rolled materials is 100%. Example 2
[0012] S1: The billet is heated in multiple stages in a heating furnace, wherein the temperature of the first stage is 1000°C, the temperature of the second stage is 1200°C, the temperature of the first soaking stage is 1240°C, the temperature of the second soaking stage is 1230°C, and the temperature is kept at this temperature for 170 minutes; S2: After descaling with high-pressure water, the steel is rolled in sequence through rough rolling, intermediate rolling, pre-finishing rolling and final rolling. The steel is rolled in different specifications ranging from φ16 to 50 mm. The rough rolling speed is 0.4 m / s and the reduction per pass is ≥15%; S3: The incoming material size of φ40 finished rolled products before final rolling is φ59mm rolled products; S4: Rolling is carried out using the KOCKS finishing mill with a specification range of φ40.11-φ43.03mm, a final rolling deformation of 54%, and a final rolling temperature of 820°C. Before rolling, other steel grades of the same specification with a relatively wide range of dimensional accuracy must be produced for dimensional debugging to ensure the final rolling dimensional tolerance; S5: The core quality of round steel is tested by ultrasonic testing to ensure that there are no microscopic pore defects. After inspection, the qualified rate of internal inspection of rolled materials is 100%. Example 3
[0013] S1: The steel billet is heated in a heating furnace in multiple stages, wherein the first stage is heated at 1000°C, the second stage is heated at 1180°C, the first stage is soaked at 1220°C, the second stage is soaked at 1210°C, and the temperatures are kept at this temperature for 180 minutes. S2: After descaling with high-pressure water, the steel is rolled in sequence through rough rolling, intermediate rolling, pre-finishing rolling and final rolling. The steel is rolled in different specifications ranging from φ16 to 50 mm. The rough rolling speed is 0.4 m / s and the reduction per pass is ≥15%; S3: The incoming material size of φ40 finished rolled products before final rolling is φ59mm rolled products; S4: Rolling is carried out using the KOCKS finishing mill with a specification range of φ40.11-φ43.03mm, a final rolling deformation of 54%, and a final rolling temperature of 830°C. Before rolling, other steel grades of the same specification with a relatively wide range of dimensional accuracy must be produced for dimensional debugging to ensure the final rolling dimensional tolerance; S5: The core quality of round steel is tested by ultrasonic testing to ensure that there are no microscopic pore defects. After inspection, the qualified rate of internal inspection of rolled materials is 100%.
[0014] In addition to the above embodiments, the present invention may also have other implementation methods; any technical solutions formed by equivalent replacement or equivalent transformation fall within the protection scope required by the present invention.
Claims
1. A rolling process for improving the core quality of high carbon chromium bearing steel, characterized by: The specific steps include: S1: The slab is kept in a heating furnace at 1200-1240°C for at least 150 minutes; S2: After descaling with high-pressure water, rough rolling and intermediate rolling are carried out in sequence. The rough rolling reduction is 40-50%, and the intermediate rolling reduction is 30-40%. S3: The incoming material size of φ40 finished rolled products before final rolling is φ59mm rolled products; S4: Rolled using the KOCKS finishing mill with a specification range of φ40.11-φ43.03mm, with a final rolling deformation of 54% and a final rolling temperature of 780℃-850℃; S5: The core quality of round steel is tested by ultrasonic testing to ensure that there are no microscopic pore defects.
2. A rolling process for improving the core quality of high carbon chromium bearing steel according to claim 1, characterized in that: The heating in S1 adopts multi-stage heating and soaking, wherein the temperature of the first heating stage is 900-1000℃, the temperature of the second heating stage is 1100-1200℃, the temperature of the first soaking stage is 1200-1240℃, the temperature of the second soaking stage is 1200-1230℃, and the high temperature stage is kept warm for at least 150 minutes.
3. The rolling process for improving the core quality of high carbon chromium bearing steel according to claim 1, characterized in that: The rough rolling stage in S2 adopts reduced speed rolling, with a rolling speed of ≤0.6 m / s and a reduction of ≥15% per pass.
4. The rolling process for improving the core quality of high carbon chromium bearing steel according to claim 1, characterized in that: The dimensions of the KOCKS finishing mill in S4 are positive tolerances, and other steel grades of the same specification with a relatively wide range of dimensional accuracy need to be dimensionally debugged before rolling. The roll gap control accuracy is ±0.05mm, and the rolling force fluctuation range is ≤5%, ensuring that the final rolling dimensional tolerance is ±0.1mm.