Modified negative electrode materials and their preparation methods, negative electrode sheets, secondary batteries and electrical devices

By coating the graphite anode material of a lithium-ion battery with a three-dimensional network structure of silicate material, the problem of poor fast-charging performance of graphite-based lithium-ion batteries is solved, and efficient transmission and stability of lithium-ion batteries under high-rate charge and discharge conditions are achieved.

CN120709365BActive Publication Date: 2026-11-10CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410347485.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2026-11-10
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

When existing lithium-ion batteries use carbon-based materials such as graphite, their fast-charging performance is poor. Existing modification methods have failed to effectively improve the lithium-ion transport rate on the graphite surface, leading to increased battery polarization.

Method used

Using silicate materials as a coating layer, a three-dimensional network structure is formed by the co-oxygen connection of silicon-oxygen tetrahedra and metal-oxygen octahedra at their vertices, which improves the transport rate of lithium ions on the surface of the core material. The coating layer is uniformly coated on the surface of the core material by gelation, forming a coating layer with high porosity and specific surface area.

Benefits of technology

It significantly improves the fast-charging performance of lithium-ion batteries, reduces battery polarization caused by ion migration, and enhances the charging and discharging efficiency and stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120709365B_ABST
    Figure CN120709365B_ABST
Patent Text Reader

Abstract

This application relates to a modified negative electrode material and its preparation method, a negative electrode sheet, a secondary battery, and an electrical device. The modified negative electrode material includes a core and a coating layer covering at least a portion of the surface of the core. The core comprises a carbon-based material, and the coating layer comprises a silicate material. The framework structure of the silicate material is composed of a three-dimensional network formed by the interconnection of silicon-oxygen tetrahedra and metal-oxygen octahedrons at their vertices. At 25°C, the ionic conductivity of the silicate material is 1×10⁻⁶. ‑5 S·cm ‑1 -9×10 ‑4 S·cm ‑1 The coating layer of the modified negative electrode material not only has stable chemical properties, which can protect the surface of the core material during cycling and alleviate the volume expansion and particle breakage of the core material, but also improves the rate of lithium ion transport on the surface of the core material. Under high-rate charge and discharge conditions, it reduces battery polarization caused by ion migration and can significantly improve the fast-charging performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of lithium-ion battery technology, and in particular to a modified negative electrode material and its preparation method, a negative electrode sheet, a secondary battery, and an electrical device. Background Technology

[0002] The statements herein are provided only as background information in connection with this application and do not necessarily constitute prior art.

[0003] In recent years, with the increasingly widespread application of lithium-ion batteries, they have been widely used in energy storage systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric cars, military equipment, aerospace, and many other fields. With current societal development, the demand for fast-charging performance of lithium-ion batteries is also increasing. However, when the negative electrode material contains carbon-based materials such as graphite, the fast-charging performance of lithium-ion batteries is poor. Therefore, improving the fast-charging performance of lithium-ion batteries using carbon-based materials such as graphite as the negative electrode material is a pressing issue that needs to be addressed. Summary of the Invention

[0004] This application provides a modified negative electrode material that can effectively improve the fast charging performance of lithium-ion batteries containing carbon-based materials, as well as its preparation method, negative electrode sheet, secondary battery, and power device.

[0005] To achieve the above objectives, a first aspect of this application provides a modified negative electrode material, the modified negative electrode material comprising:

[0006] Core, the core comprising carbon-based material; and

[0007] A coating layer covers at least a portion of the surface of the core; the coating layer comprises a silicate material comprising a framework structure consisting of a three-dimensional network of interconnected silicon-oxygen tetrahedra and metal-oxygen octahedra at their vertices; the silicate material has an ionic conductivity of 1 × 10⁻⁶ at 25°C. -6 S·cm -1 -1×10 -4 S·cm -1 .

[0008] Therefore, the modified anode material in this application uses silicate material as the coating layer, and the silicate material includes a framework structure composed of a three-dimensional network formed by the interconnection of silicon-oxygen tetrahedra and metal-oxygen octahedra at their vertices, with an ionic conductivity of 1×10⁻⁶. -6 S·cm -1 -1×10 -4 S·cm -1The coating layer of the modified negative electrode material not only has stable chemical properties, but can also protect the surface of the core material during cycling, and alleviate the volume expansion and particle breakage of the core material; at the same time, it can improve the rate of lithium ion transport on the surface of the core material. Under high-rate charge and discharge conditions, it can reduce battery polarization caused by ion migration, thereby significantly improving the fast charging performance of the battery.

[0009] In some embodiments, the ionic conductivity of the silicate material at 25°C is 5 × 10⁻⁶. -6 S·cm -1 -8×10 -5 S·cm -1 .

[0010] In some embodiments, the silicate material has the chemical formula A. x B y SiO4, element A includes one or more of Li, Na and K, element B includes one or more of Ca, Fe, Mg, Al, Mn and Ni, 0.4≤x≤2.5, 0.2≤y≤2;

[0011] Alternatively, 0.4 ≤ x ≤ 1.6; 0.8 ≤ y ≤ 1.5.

[0012] In some embodiments, the mass ratio of the covering layer to the core is (0.1-5):100, and optionally (0.2-1):100.

[0013] In some embodiments, the carbon-based material includes one or more of artificial graphite, natural graphite, hard carbon, soft carbon, and mesophase microspheres.

[0014] The second aspect of this application provides a method for preparing the modified negative electrode material of the first aspect of this application, comprising the following steps:

[0015] A gel-like mixture is prepared by heating a mixture containing the silicate material, the core, and the gelling agent.

[0016] The modified negative electrode material is prepared by subjecting the gel-like mixture to a first sintering treatment.

[0017] In some embodiments, the method for preparing the silicate material includes:

[0018] A mixture containing silicon dioxide, a salt or oxide containing element A, and a salt or oxide containing element B is subjected to a second sintering treatment to prepare a material with the chemical formula A. x B y SiO4 silicate materials;

[0019] Wherein, element A includes one or more of Li, Na and K, and element B includes one or more of Ca, Fe, Mg, Al, Mn and Ni, with 0.4≤x≤2.5 and 0.2≤y≤2;

[0020] Alternatively, 0.4 ≤ x ≤ 1.6; 0.8 ≤ y ≤ 1.5.

[0021] In some embodiments, the salt containing element A includes one or more of sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts containing element A; and / or

[0022] The salts containing element B include one or more of the following: sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts.

[0023] In some embodiments, the second sintering process includes at least one of the following conditions:

[0024] (1) The temperature of the second sintering treatment is 700℃-1000℃, and can be selected as 800℃-950℃;

[0025] (2) The second sintering treatment time is 3h-12h, and can be selected as 5h-10h;

[0026] (3) The atmosphere for the second sintering treatment is an inert gas, which may be argon;

[0027] (4) The heating rate of the second sintering treatment is 5℃ / min-15℃ / min.

[0028] In some embodiments, the mass ratio of the silicate material to the core is (0.1-5):100, optionally (0.2-1):100; and / or

[0029] The mass of the gelling agent accounts for 10%-25% of the mass of the core, and can be optionally 15%-20%.

[0030] In some embodiments, the gelling agent comprises one or more of hydrochloric acid, p-toluenesulfonic acid, acetic acid, succinic acid, maleic acid, boric acid, sulfuric acid, nitric acid, ammonia, sodium hydroxide, EDTA, and citric acid.

[0031] In some embodiments, the temperature of the first sintering treatment is 200℃-500℃, optionally 300℃-400℃; and / or

[0032] The first sintering treatment takes 1-2 hours, or 1-1.5 hours.

[0033] In some embodiments, the temperature of the heat treatment is 80℃-120℃, optionally 80℃-90℃; and / or

[0034] The heating treatment time is 1-2 hours, or 1-1.5 hours.

[0035] The third aspect of this application provides a negative electrode sheet comprising the modified negative electrode material of the first aspect of this application or the modified negative electrode material prepared by the preparation method of the second aspect of this application.

[0036] A fourth aspect of this application provides a secondary battery, including the negative electrode sheet of the third aspect of this application. The secondary battery of this application includes the modified negative electrode material of this application and has excellent fast-charging performance.

[0037] A fifth aspect of this application provides an electrical device that includes a secondary battery as described in the fourth aspect of this application. The electrical device of this application includes the secondary battery provided in this application and therefore has at least the same advantages as said secondary battery.

[0038] Details of one or more embodiments of this application are set forth in the following drawings and description. Other features, objects, and advantages of this application will become apparent from the specification, drawings, and claims. Attached Figure Description

[0039] To better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described embodiments or examples, or the best mode of conduct of these applications as currently understood. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0040] Figure 1 This is a schematic diagram of a battery cell according to one embodiment of this application.

[0041] Figure 2 for Figure 1 An exploded view of a battery cell according to one embodiment of this application is shown.

[0042] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.

[0043] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0044] Figure 5 for Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.

[0045] Figure 6This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to an embodiment of this application.

[0046] Figure 7 This is a cross-sectional SEM image of the modified negative electrode material in Example 1.

[0047] Explanation of reference numerals in the attached figures:

[0048] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Battery cell; 51 Housing; 52 Electrode assembly; 53 Cover plate; 6 Electrical device. Detailed Implementation

[0049] The modified negative electrode material, its preparation method, negative electrode sheet, secondary battery, and power device of this application are described in detail below with appropriate reference to the accompanying drawings. However, some unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of actually identical structures may be omitted. This is to avoid making the following description unnecessarily lengthy and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0050] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints; any endpoint can be independently included or excluded, and they can be combined arbitrarily, meaning any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0051] In this application, the terms "multiple" or "various" are used unless otherwise specified, referring to a quantity greater than or equal to 2. For example, "one or more" means one or more types.

[0052] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0053] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0054] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, preferably sequentially. For example, if the method includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, if the method may also include step (c), it means that step (c) can be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0055] In this application, open-ended technical features or solutions described using terms such as "containing," "including," or "comprising" do not exclude additional members beyond those listed unless otherwise specified. They can be considered as providing both closed-ended features or solutions comprised of the listed members and open-ended features or solutions that include additional members beyond the listed members. For example, if A includes a1, a2, and a3, it may also include other members or exclude additional members unless otherwise specified. This can be considered as providing both the feature or solution that "A consists of a1, a2, and a3" and the feature or solution that "A includes not only a1, a2, and a3, but also other members." In this application, unless otherwise specified, A (e.g., B) indicates that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0056] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0057] When the negative electrode material contains carbon-based materials such as graphite, lithium-ion insertion can only occur from the end face. However, due to the difficulty in preparing graphite products with high isotropy, the fast-charging performance of lithium-ion batteries with graphite negative electrodes is poor. In related technologies, the methods to improve the fast-charging performance of lithium-ion battery negative electrodes mainly include: (1) Modification of the graphite material itself, such as increasing the interlayer spacing of graphite particles, increasing the specific surface area, and reducing the particle size; (2) Coating the graphite surface, mainly with amorphous carbon or hard carbon coating layers, to enhance the fast-charging capability by improving the isotropy of the particle surface; (3) Improving the slurry of the negative electrode material to make the graphite slurry and the substrate have higher adhesion, avoiding the situation where the adhesion deteriorates due to the rapid insertion and extraction of lithium ions, resulting in powder shedding, lithium plating, gas generation, and other deterioration of cycle performance.

[0058] However, while modifying the graphite particles themselves—increasing the specific surface area and decreasing the particle size—can improve fast-charging performance, it also increases the number of active sites on the graphite surface, reducing the coulombic efficiency of the anode material and increasing lithium consumption. Coating the graphite surface with amorphous carbon only increases the channels for lithium-ion insertion on the graphite particle surface; it does not improve the rate of lithium-ion diffusion on the particle surface. Improving the anode material slurry only alleviates the capacity decay caused by particle breakage during fast charging, and does not effectively improve fast-charging capability.

[0059] Based on this, this application uses silicate material to coat the negative electrode material. The framework structure of the silicate material is composed of a three-dimensional network formed by the interconnection of silicon-oxygen tetrahedra and metal-oxygen octagons at their vertices. This framework structure contains channels and interconnected cavities. The cavities can accommodate cations and water molecules, and the cations can move easily in the channels. Therefore, the rate of lithium ion transport on the graphite surface can be effectively improved. Under high-rate charging and discharging conditions, the battery changes caused by ion migration are reduced, which can significantly improve the fast charging performance of the battery.

[0060] An embodiment of this application provides a modified anode material, which includes a core and a coating layer covering at least a portion of the surface of the core; the core comprises a carbon-based material, and the coating layer comprises a silicate material, wherein the silicate material comprises a framework structure consisting of a three-dimensional network formed by the interconnection of silicon-oxygen tetrahedra and metal-oxygen octahedrons at their vertices; at 25°C, the ionic conductivity of the silicate material is 1×10⁻⁶. -6 S·cm -1-1×10 -4 S·cm -1 .

[0061] At 25℃, the ionic conductivity of silicates is 1×10⁻⁶. -6 S·cm -1 -1×10 -4 S·cm -1 This can effectively improve the transport rate of lithium ions on the surface of the core material.

[0062] Silicate materials comprise a framework structure consisting of a three-dimensional network formed by interconnected silicon-oxygen tetrahedra and metal-oxygen octagons at their vertices. This framework structure contains channels and interconnected voids. The voids can accommodate cations and water molecules, and the cations can move easily within the channels. Therefore, silicate materials can provide a pathway for the rapid transport of lithium ions. Simultaneously, the polyanionic structure of silicate materials possesses a robust crystal structure and stable chemical properties.

[0063] Understandably, the coating layer of the modified negative electrode material in this application not only has stable chemical properties, but can also protect the surface of the core material during cycling, and alleviate the volume expansion and particle breakage of the core material; at the same time, it can improve the rate of lithium ion transport on the surface of the core material, and reduce battery polarization caused by ion migration under high-rate charge and discharge conditions, thereby significantly improving the fast charging performance of the battery.

[0064] As an example, the framework structure of the silicate materials mentioned above can be determined using X-ray diffraction (XRD).

[0065] As an example, the ionic conductivity of the aforementioned silicate materials can be determined using electrochemical impedance spectroscopy (EIS); specifically as follows:

[0066] The test used a blocked electrode symmetric cell, and the ionic conductivity σ was calculated using the following formula: σ = d / Re × S; where d is the thickness of the sample (cm); Re is the bulk impedance of the sample (ohms), which can be obtained from the intersection of the semicircle and the oblique line in the Nyquist plot of the electrochemical impedance spectroscopy; and S is the effective area of ​​the electrode (cm²). 2 Test instrument: Princeton VersaSTAT electrochemical workstation. Test conditions: frequency range 0.1 MHz - 1 MHz, perturbation amplitude 10 mV, test temperature 25°C, held at the set temperature for 30 min before measurement. In some embodiments, the ionic conductivity of the silicate material at 25°C is 5 × 10⁻⁶. -6 S·cm -1 -8×10 -5 S·cm -1 .

[0067] In some embodiments, the silicate material has the chemical formula A. x B y SiO4, where element A includes one or more of Li, Na, and K, and element B includes one or more of Ca, Fe, Mg, Al, Mn, and Ni, with 0.4 ≤ x ≤ 2.5 and 0.2 ≤ y ≤ 2. This composition is beneficial for forming a framework structure of silicon-oxygen tetrahedra and metal-oxygen octahedra, maintaining structural stability, and also for further improving ionic conductivity.

[0068] In some alternative implementations, 0.4 ≤ x ≤ 1.6; 0.8 ≤ y ≤ 1.5.

[0069] As one possible implementation, the mass ratio of the coating layer to the core is (0.1-5):100; for example, it can be, but is not limited to, 0.1:100, 0.3:100, 0.5:100, 0.8:100, 1:100, 1.2:100, 1.5:100, 1.8:100, 2:100, 2.3:100, 2.5:100, 2.7:100, 3:100, 3.3:100, 3.5:100, 3.8:100, 4:100, 4.2:100, 4.5:100, 4.8:100, 5:100, or any range between two of the above ratios. When the mass ratio of the coating layer to the core is within the above range, it is beneficial for the core to carry out electrochemical reactions and for improving the lithium-ion transport rate, thereby enhancing fast charging capability.

[0070] In some alternative implementations, the mass ratio of the overlay to the core is (0.2-1):100.

[0071] As an example, the mass ratio of the coating layer to the core mentioned above can be determined by measuring the mass of silicon and metal elements using ICP, and then the chemical formula of the silicate material can be deduced based on the measurement results, thereby deducing the mass ratio of the coating layer to the core.

[0072] In some embodiments, the carbon-based material includes one or more of artificial graphite, natural graphite, hard carbon, soft carbon, and mesophase microspheres.

[0073] The embodiments of this application provide a method for preparing a modified negative electrode material, which can be used to prepare the modified negative electrode material provided in the embodiments of this application. The method for preparing the modified negative electrode material includes the following steps:

[0074] A gel-like mixture is prepared by heating a mixture containing silicate material, core and gelling agent; the gel-like mixture is then subjected to a first sintering treatment to prepare a modified anode material.

[0075] Understandably, by uniformly coating silicates onto the surface of core material particles using a gel method to form a coating layer with high porosity and specific surface area, the transport rate of lithium ions on the surface of the core material can be further improved, thereby further improving the fast charging performance of the battery.

[0076] In addition, this preparation method is simple to operate, does not require expensive equipment, and can prepare single and multi-component mixtures with uniform distribution, high purity, uniform particle size distribution and high chemical activity at relatively low temperatures.

[0077] It should be noted that the "gel-like mixture" mentioned above refers to a mixture with similar gel properties.

[0078] As one possible implementation, the mixture also includes a solvent, which includes one or more of methanol, ethanol, propanol, butanol, ethylene glycol, ethylene oxide, triethanolamine, and xylene.

[0079] In some embodiments, the method for preparing silicate materials includes: subjecting a mixture containing silicon dioxide, a salt or oxide containing element A, and a salt or oxide containing element B to a second sintering treatment to prepare a material with the chemical formula A. x B y SiO4 is a silicate material; wherein element A includes one or more of Li, Na and K, element B includes one or more of Ca, Fe, Mg, Al, Mn and Ni, 0.4≤x≤2.5, and 0.2≤y≤2.

[0080] In some alternative implementations, 0.4 ≤ x ≤ 1.6; 0.8 ≤ y ≤ 1.5.

[0081] As one possible implementation, the salt containing element A includes one or more of the following: sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts containing element A.

[0082] In some exemplary embodiments, the salt containing element B includes one or more of the following: sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts containing element B.

[0083] In some embodiments, the temperature of the second sintering treatment during the preparation of the cobaltate material is 700℃-1000℃; for example, it can be, but is not limited to, 700℃, 730℃, 750℃, 77℃, 800℃, 820℃, 850℃, 870℃, 900℃, 930℃, 950℃, 970℃, 1000℃, or any range between two of the above temperatures. Optionally, the temperature of the second sintering treatment is 800℃-950℃.

[0084] In some optional embodiments, the second sintering treatment time during the preparation of silicate materials is 3h-12h; for example, it can be, but is not limited to, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, or any range between two of the above times. Optionally, the second sintering treatment time is 5h-10h.

[0085] As one possible implementation, when preparing silicate materials, the atmosphere for the second sintering treatment is an inert gas, which may be argon.

[0086] In some possible implementations, the heating rate of the second sintering process is 5°C / min to 15°C / min; for example, it can be, but is not limited to, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min, 12°C / min, 13°C / min, 14°C / min, 15°C / min, or any range between any two of the above heating rates.

[0087] It should be noted that the temperature, time, atmosphere, and heating rate of the second sintering treatment can be combined in any suitable way, and the four can be selected from any of the temperature, time, atmosphere, and heating rate of the second sintering treatment described in this article.

[0088] In one possible implementation, when preparing silicate materials, a mixture containing silicon dioxide, a salt or oxide containing element A, and a salt or oxide containing element B is ball-milled in a ball mill at a speed of 200 rpm to 500 rpm for 10 h to 20 h. After the mixture is removed, a second sintering treatment is carried out in an inert atmosphere in a sealed crucible.

[0089] The rotational speed of the mixture in the ball mill can be, but is not limited to, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, or any range between two of the above speeds. The ball milling time can be, but is not limited to, 10 h, 11 h, 12 h, 13 h, 14 h, 15 h, 16 h, 17 h, 18 h, 19 h, 20 h, or any range between two of the above time periods.

[0090] In some embodiments, the mass ratio of silicate material to the core is (0.1-5):100; for example, it can be, but is not limited to, 0.1:100, 0.3:100, 0.5:100, 0.8:100, 1:100, 1.2:100, 1.5:100, 1.8:100, 2:100, 2.3:100, 2.5:100, 2.7:100, 3:100, 3.3:100, 3.5:100, 3.8:100, 4:100, 4.2:100, 4.5:100, 4.8:100, 5:100, or any range between two of the above ratios. When the mass ratio of silicate material to the core is within the above range, it is beneficial for the core to carry out electrochemical reactions and for improving the lithium-ion transport rate, thereby enhancing fast charging capability.

[0091] Optionally, the mass ratio of silicate material to core is (0.2-1):100.

[0092] As one possible implementation, the mass of the gelling agent accounts for 10%-25% of the mass of the core; for example, it can be, but is not limited to, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, or any range between two of the above values. When the percentage of the gelling agent's mass to the core mass is within the above range, it is beneficial to uniformly coat the silicate material onto the core surface.

[0093] In some embodiments, the gelling agent includes one or more of hydrochloric acid, p-toluenesulfonic acid, acetic acid, succinic acid, maleic acid, boric acid, sulfuric acid, nitric acid, ammonia, sodium hydroxide, EDTA, and citric acid.

[0094] In some optional embodiments, the temperature of the first sintering treatment is 200℃-500℃; for example, it can be, but is not limited to, 200℃, 220℃, 250℃, 280℃, 300℃, 320℃, 350℃, 380℃, 400℃, 430℃, 450℃, 470℃, 500℃, or any range between two of the above temperatures. Optionally, the temperature of the first sintering treatment is 300℃-400℃.

[0095] As one possible implementation, the first sintering treatment time is 1h-2h; for example, it can be, but is not limited to, 1h, 1.1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.6h, 1.7h, 1.8h, 1.9h, 2h, or any range between two of the above times. Optionally, the first sintering treatment time is 1h-1.5h.

[0096] It should be noted that the temperature and time of the first sintering treatment can be combined in any suitable way, and both can be selected from any of the first sintering treatment temperatures and times described in this article.

[0097] In some embodiments, the heat treatment temperature is 80℃-120℃; for example, it can be, but is not limited to, 80℃, 90℃, 100℃, 110℃, 120℃, or any range between two of the above temperatures. Optionally, the heat treatment temperature is 80℃-90℃.

[0098] As one possible implementation, the heat treatment time is 1-2 hours; for example, it can be, but is not limited to, 1 hour, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2 hours, or any range between two of the above times. Optionally, the heat treatment time is 1-1.5 hours.

[0099] It should be noted that the temperature and time of the heat treatment can be combined in any suitable way, and both can be selected from any of the heat treatment temperatures and times described in this article.

[0100] In some embodiments, the preparation method of the modified negative electrode material includes the following steps:

[0101] A mixture containing silica, a salt or oxide containing element A, and a salt or oxide containing element B is ball-milled at 200-500 rpm for 10-20 hours. The mixture is then removed and subjected to a second sintering treatment in a sealed crucible under an inert atmosphere, with the temperature increased at a rate of 5-15°C / min to 700-1000°C for 3-12 hours. This process yields silicate material A. x B y SiO4; Element A includes one or more of Li, Na, and K; Element B includes one or more of Ca, Fe, Mg, Al, Mn, and Ni, with a value of 0.4 ≤ x ≤ 2.5 and 0.2 ≤ y ≤ 2. Salts containing Element A include one or more of sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts. Salts containing Element B include one or more of sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts containing Element B.

[0102] A silicate hydrochloric acid material and a core are dispersed in a solvent, and a gelling agent is added to prepare a mixture. The mixture containing the silicate material, core, and gelling agent is stirred and heated to prepare a gel-like mixture. The mass ratio of silicate material to core is (0.1-5):100. The mass of the gelling agent accounts for 10%-25% of the mass of the core. The gelling agent includes one or more of hydrochloric acid, p-toluenesulfonic acid, acetic acid, succinic acid, maleic acid, boric acid, sulfuric acid, nitric acid, ammonia, sodium hydroxide, EDTA, and citric acid. The heating temperature is 80℃-120℃, and the time is 1h-2h. The solvent includes one or more of methanol, ethanol, propanol, butanol, ethylene glycol, ethylene oxide, triethanolamine, and xylene.

[0103] A modified anode material was prepared by subjecting a gel-like mixture to a first sintering treatment. The temperature of the first sintering treatment was 200℃-500℃, and the time was 1h-2h.

[0104] In addition, the secondary battery and power-consuming device of this application will be described below with appropriate reference to the accompanying drawings.

[0105] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0106] The secondary battery of this application includes the modified negative electrode material of this application, which has excellent fast charging performance.

[0107] Negative electrode sheet

[0108] The negative electrode sheet includes a negative current collector and a negative active material layer located on at least one side of the negative current collector. The negative active material layer includes the modified negative electrode material of the first aspect of this application or the modified negative electrode material prepared by the preparation method of the second aspect of this application.

[0109] As a non-limiting example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0110] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on the polymeric material substrate. Non-limiting examples of the metal material in the negative electrode current collector may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the negative electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0111] In some embodiments, the negative electrode active material layer may also include other negative electrode active materials known in the art for use in batteries. As a non-limiting example, the negative electrode active material may also include one or more of the following materials: tin-based materials and lithium titanate, etc. Tin-based materials may include one or more of elemental tin, tin oxides, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0112] In some embodiments, the negative electrode active material layer may optionally include a binder. Optionally, the binder may include one or more of polytetrafluoroethylene, polyvinylidene fluoride, polyacrylic acid, polyimide, and polyacrylonitrile. The binder may also optionally include one or more of sodium polyacrylate (PAAS), polyacrylamide (PAM), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0113] In some embodiments, the negative electrode active material layer may optionally include a conductive agent. Optionally, the conductive agent may include one or more of conductive carbon black, superconducting carbon black, conductive graphite, acetylene black, Ketjen black, graphene, and carbon nanotubes.

[0114] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0115] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as modified negative electrode material, conductive agent, binder, and any other components, in a solvent (a non-limiting example of a solvent is deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto at least one surface of a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing, and other processes. The surface of the negative electrode current collector coated with the negative electrode slurry can be a single surface of the negative electrode current collector or both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt%-60wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000mPa·s-10000mPa·s. When coating the negative electrode slurry, the coating unit areal density (excluding solvent) on a dry weight basis can be 0.05-0.18g / 1540.25mm. 2 The compaction density of the negative electrode sheet can be 1.0 g / cm³. 3 -1.8g / cm 3 .

[0116] In some embodiments, after dispersing the negative electrode active material, conductive agent, binder and any other components in a solvent, the mixture can be stirred using a turbine, paddle, propeller, screw or planetary agitator to form a negative electrode slurry.

[0117] Positive electrode sheet

[0118] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer including a positive active material.

[0119] As a non-limiting example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0120] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be obtained by forming a metal material on a polymeric material substrate. Non-limiting examples of the metal material in the positive electrode current collector may include one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of the polymeric material substrate in the positive electrode current collector may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).

[0121] In some embodiments, the positive electrode active material may further include one or more of ternary materials and lithium manganese iron phosphate materials; wherein, the ternary material includes Li x (Ni a Co b Mn c )1-dM d O2-yA y (x is 0.2-1.2) and / or Li x A a (Ni a Co b Mn c )1-dM d O2-yA y (x+a is 0.2-1.2); Lithium manganese iron phosphate materials include Li a Mn 1-y B y P 1-z C z O 4-n D n (a is 0-1.1) and / or Li a A x Mn 1-y B y P 1-z C z O 4-n D n (a+x is 0-1.1).

[0122] It should be noted that the above limitation on x includes the molar content of Li under different charge and discharge states of the battery (typically the battery voltage is between 2-5V).

[0123] Understandably, lithium (Li) is intercalated and deintercalated during the charging and discharging process of a battery, and the Li content in the positive electrode varies depending on the state of discharge. Unless otherwise specified, the Li content in the examples of positive electrode materials listed in this application refers to the initial state of the material. When a positive electrode material is applied to a positive electrode in a battery system, the Li content in the positive electrode material typically changes after charge-discharge cycles. The Li content can be measured using molar content, but is not limited to this. Regarding "Li content refers to the initial state of the material," the initial state of the material refers to its state before being added to the positive electrode slurry. It is understood that new materials obtained by appropriately modifying the listed positive electrode materials are also within the scope of positive electrode materials. The aforementioned appropriate modification refers to acceptable modification methods for positive electrode materials, and non-limiting examples include coating modification.

[0124] In the examples of cathode materials in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause changes in the molar content of oxygen, and the actual O content will fluctuate. The O content can be measured in molar content, but is not limited to this.

[0125] In some embodiments, the positive electrode active material may also employ other positive electrode active materials known in the art for use in batteries. As a non-limiting example, the positive electrode active material may include one or more of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, one or more of lithium cobalt oxides (such as LiCoO2), lithium nickel oxides, lithium manganese oxides, lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, lithium nickel cobalt manganese oxides, lithium nickel cobalt aluminum oxides, and their modified compounds. Non-limiting examples of lithium-containing phosphates with an olivine structure include, but are not limited to, one or more of lithium iron phosphate, lithium iron phosphate and carbon composites, lithium manganese phosphate, lithium manganese phosphate and carbon composites, lithium iron manganese phosphate, and lithium manganese iron phosphate and carbon composites. Non-limiting examples of lithium cobalt oxides may include LiCoO2; non-limiting examples of lithium nickel oxides may include LiNiO2; non-limiting examples of lithium manganese oxides may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 Examples of lithium nickel cobalt aluminum oxides include LiNi, etc. 0.80 Co 0.15 Al 0.05O2.

[0126] In some embodiments, the positive electrode active material layer may optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.

[0127] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0128] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as the positive active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry; coating the positive electrode slurry onto at least one surface of the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing, and other processes. The solvent can be selected from, but is not limited to, any of the solvents described in the foregoing embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode current collector coated with the positive electrode slurry can be a single surface or both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt%-80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000 mPa·s-25000 mPa·s. When coating the positive electrode slurry, the coating areal density per unit area (dry weight, minus solvent) can be 0.2-0.45 g / 1540.25 mm. 2 The compaction density of the positive electrode sheet can be 2.4 g / cm³. 3 -2.8g / cm 3 2.4g / cm³ is an optional value. 3 -2.7g / cm 3 .

[0129] electrolytes

[0130] Electrolytes function to conduct ions between the positive and negative electrode plates. This application does not impose any particular restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or completely solid.

[0131] In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent.

[0132] In some embodiments, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorophosphate (LiPO2F2), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).

[0133] In some embodiments, the solvent may include ethylene carbonate (EC, ), propylene carbonate (PC, ), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butene carbonate ( One or more of the following: fluoroethylene carbonate (FEC), methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0134] In some embodiments, the electrolyte may optionally include additives. For example, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0135] In some embodiments, the additives in the electrolyte may include, but are not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethyl ethylene carbonate (TFPC), etc.

[0136] Separating membrane

[0137] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0138] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0139] In some embodiments, the thickness of the separator is 6-40 μm, optionally 10-16 μm.

[0140] In some embodiments, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding process or a stacking process.

[0141] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.

[0142] In some embodiments, the outer packaging of the secondary battery can be a rigid shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft pack, such as a pouch-type soft pack. The material of the soft pack can be plastic; further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0143] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.

[0144] In this application, unless otherwise specified, "cell battery" refers to the basic unit capable of converting chemical energy into electrical energy, and generally includes at least a positive electrode, a negative electrode, and an electrolyte. During the charging and discharging process of the battery, active ions move back and forth between the positive and negative electrode plates, inserting and extracting. The electrolyte acts as a conductor for the active ions between the positive and negative electrode plates.

[0145] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 The example shown is a square-structured battery cell 5.

[0146] In some of these embodiments, reference is made to Figure 2 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator may be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, which can be selected by those skilled in the art according to actual needs.

[0147] The secondary battery can be either battery module 4 or battery pack 1.

[0148] A battery module includes at least one battery cell. The number of battery cells in a battery module can be one or more, and those skilled in the art can select an appropriate number based on the application and capacity of the battery module.

[0149] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.

[0150] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0151] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more. Those skilled in the art can select an appropriate number according to the application and capacity of the battery pack.

[0152] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0153] In addition, this application also provides an electrical device, which includes the secondary battery provided in this application. The secondary battery can be used as the power source of the electrical device or as the energy storage unit of the electrical device. The electrical device may include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc. Among them, mobile devices may be, for example, mobile phones, laptops, etc.; electric vehicles may be, for example, pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc., but are not limited to.

[0154] As an electrical device, a rechargeable battery can be selected based on its usage requirements.

[0155] Figure 6 Here is an example of an electrical device 6. This electrical device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this electrical device, a battery pack or battery module can be used.

[0156] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a rechargeable battery as their power source.

[0157] Example

[0158] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the technology or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0159] I. Preparation of Modified Anode Materials

[0160] Example 1

[0161] (1) 1 mol SiO2, 0.5 mol Al2O3 and 0.5 mol Li2O were ball-milled at 500 rpm for 10 h, and then sintered at 900 °C for 8 h in a muffle furnace to obtain LiAlSiO4 material (as a silicate material).

[0162] (2) Add 15g citric acid (as a gelling agent), 0.5g LiAlSiO4, and 100g artificial graphite (as a core) to 1L of deionized water, and heat at 80°C until a gel-like mixture is formed.

[0163] (3) The gel-like mixture was placed in a muffle furnace and sintered at 350°C for 1 hour to obtain the modified negative electrode material.

[0164] The cross-sectional SEM image of the modified negative electrode material prepared in Example 1 is shown below. Figure 7 As shown, by Figure 7 It can be seen that the modified negative electrode material prepared in Example 1 has a core-shell structure, with LiAlSiO4 material (coating layer) coated on the surface of artificial graphite (core).

[0165] Example 2-22

[0166] The preparation methods for Examples 2-22 and Example 1 are similar, with differences detailed in Table 1. The preparation methods for the silicate materials in Examples 5-13 are as follows:

[0167] In Example 5, the silicate material Li 1.6 Al 0.8The preparation method of SiO4 is as follows: 1 mol SiO2, 0.4 mol Al2O3 and 0.8 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain Li. 1.6 Al 0.8 SiO4 material (as a silicate material).

[0168] In Example 6, the silicate material Li 0.4 Al 1.2 The preparation method of SiO4 is as follows: 1 mol SiO2, 0.6 mol Al2O3 and 0.2 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain Li. 0.4 Al 1.2 SiO4 material (as a silicate material).

[0169] In Example 7, the silicate material LiMg 1.5 The preparation method of SiO4 is as follows: 2 mol SiO2, 3 mol MgO and 1 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain LiMg. 1.5 SiO4 material (as a silicate material).

[0170] In Example 8, the silicate material LiMn 1.5 The preparation method of SiO4 is as follows: 2 mol SiO2, 3 mol MnO and 1 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain LiMnO4. 1.5 SiO4 material (as a silicate material).

[0171] In Example 9, the silicate material LiCa 1.5 The preparation method of SiO4 is as follows: 2 mol SiO2, 3 mol CaO and 1 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain LiCa. 1.5 SiO4 material (as a silicate material).

[0172] In Example 10, the silicate material LiNi 1.5 The preparation method of SiO4 is as follows: 2 mol SiO2, 3 mol NiO and 1 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain LiNi. 1.5SiO4 material (as a silicate material).

[0173] The preparation method of the silicate material LiFeSiO4 in Example 11 is as follows: 1 mol SiO2, 0.5 mol Fe2O3 and 0.5 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900 °C for 8 h in a muffle furnace to obtain LiFeSiO4 material (as silicate material).

[0174] The preparation method of the silicate material NaAlSiO4 in Example 12 is as follows: 1 mol SiO2, 0.5 mol Al2O3 and 0.5 mol Na2O are ball-milled at 500 rpm for 10 h, and then sintered at 900 °C for 8 h in a muffle furnace to obtain NaAlSiO4 material (as silicate material).

[0175] The preparation method of the silicate material KAlSiO4 in Example 13 is as follows: 1 mol SiO2, 0.5 mol Al2O3 and 0.5 mol K2O are ball-milled at 500 rpm for 10 h, and then sintered at 900 °C for 8 h in a muffle furnace to obtain KAlSiO4 material (as silicate material).

[0176] Comparative Example 1

[0177] The preparation methods of Comparative Example 1 and Example 1 are similar, except that artificial graphite is used as the negative electrode material in Comparative Example 1 and is not modified; see Table 1 for details.

[0178] Comparative Example 2

[0179] The preparation methods of Comparative Example 2 and Example 2 are similar, except that: natural graphite was used as the negative electrode material in Comparative Example 2 and was not modified; see Table 1 for details.

[0180] Comparative Example 3

[0181] The preparation methods of Comparative Example 3 and Example 3 are similar, except that soft carbon is used as the negative electrode material in Comparative Example 3 and it is not modified; see Table 1 for details.

[0182] Comparative Example 4

[0183] The preparation methods of Comparative Example 4 and Example 4 are similar, except that: in Comparative Example 4, hard carbon is used as the negative electrode material and it is not modified; see Table 1 for details.

[0184] Comparative Example 5

[0185] The preparation methods of Comparative Example 5 and Example 1 are similar, except that the type of silicate material used in Comparative Example 5 is different; the silicate material used in Comparative Example 5 is Li. 2.8 Al 0.4 SiO4 has an ionic conductivity of 1.1 × 10⁻⁶. -4 .

[0186] Comparative Example 5: Silicate Material Li2Al 0.66 The preparation method of SiO4 is as follows: 1.4 mol SiO2, 0.2 mol Al2O3 and 1 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain Li. 2.8 Al 0.4 SiO4 material (as a silicate material).

[0187] Comparative Example 6

[0188] The preparation methods of Comparative Example 6 and Example 1 are similar, except that the type of silicate material used in Comparative Example 6 is different; the silicate material used in Comparative Example 6 is Li. 0.1 Al 1.3 SiO4 has an ionic conductivity of 8.2 × 10⁻⁶. -7 .

[0189] Comparative Example 6: Li silicate material 0.1 Al 1.3 The preparation method of SiO4 is as follows: 1 mol SiO2, 0.65 mol Al2O3 and 0.05 mol Li2O are ball-milled at 500 rpm for 10 h, and then sintered at 900℃ in a muffle furnace for 8 h to obtain Li. 0.1 Al 1.3 SiO4 material (as a silicate material).

[0190] The preparation parameters for the above embodiments and comparative examples are shown in Table 1.

[0191] Table 1

[0192]

[0193] In Table 1, n represents the mass percentage of silicate material in the core.

[0194] The ionic conductivity of the aforementioned silicate materials was determined using electrochemical impedance spectroscopy (EIS), as detailed below:

[0195] The test used a blocked electrode symmetric cell, and the ionic conductivity σ was calculated using the following formula: σ = d / Re × S; where d is the thickness of the sample (cm); Re is the bulk impedance of the sample (ohms), which can be obtained from the intersection of the semicircle and the oblique line in the Nyquist plot of the electrochemical impedance spectroscopy; and S is the effective area of ​​the electrode (cm²). 2 Test instrument: Princeton VersaSTAT electrochemical workstation. Test conditions: frequency range 0.1 MHz - 1 MHz, disturbance amplitude 10 mV, test temperature 25℃, and measurement after holding at the set temperature for 30 min.

[0196] II. Preparation of Secondary Batteries

[0197] 1. Preparation of positive electrode sheet

[0198] Lithium iron phosphate, conductive carbon black (SP), and binder (PVDF) were dispersed in N-methylpyrrolidone solvent at a weight ratio of 96:2:2 and mixed evenly to obtain a positive electrode slurry. The positive electrode slurry was then uniformly coated onto both sides of a positive electrode current collector aluminum foil. After drying and cold pressing, a positive electrode sheet was obtained, with a coating weight per unit area of ​​0.25 g / 1540.25 mm² on both sides. 2 .

[0199] 2. Preparation of negative electrode sheet

[0200] Modified negative electrode material, polyvinylidene fluoride binder, and acetylene black conductive agent were mixed at a mass ratio of 98:1:1, and deionized water was added. The mixture was stirred under vacuum to obtain a negative electrode slurry. The negative electrode slurry was then uniformly coated onto both sides of a copper foil. After the copper foil was dried at room temperature, it was transferred to a 120℃ oven for 1 hour. The foil was then cold-pressed and slit to obtain negative electrode sheets, with a coating weight of 0.15 g / 1540.25 mm² on both sides. 2 .

[0201] 3. Separating membrane

[0202] A 12μm thick polyethylene separator film was selected.

[0203] 4. Preparation of electrolyte

[0204] The organic solvent was a mixture containing ethylene carbonate (EC) and diethyl carbonate (DEC), with a volume ratio of EC to DEC of 3:7. In an argon-atmosphere glove box with a water content of <10 ppm, thoroughly dried lithium salt LiPF6 was dissolved in the organic solvent, and 2 wt% of fluoroethylene carbonate (FEC) was added and mixed thoroughly to obtain the electrolyte. The concentration of the lithium salt was 1 mol / L.

[0205] 5. Battery manufacturing

[0206] The battery cell is formed by stacking the positive electrode, separator, and negative electrode in sequence. The bare battery cell is placed in an outer package, injected with the electrolyte, and sealed. After processes such as settling, hot and cold pressing, formation, clamping, and capacity testing, a secondary battery is obtained. The formation process involves charging at 0.04C to 30% of the remaining capacity (SOC).

[0207] III. Performance Testing

[0208] 1. Lithium plating window test

[0209] The lithium plating window is used to characterize the rate limit of the negative electrode. A copper wire with a diameter of 200 micrometers is placed on the anode surface. The copper wire is led out to an electrode and a nickel sheet is welded to it to serve as a third electrode (reference electrode), thus obtaining a three-electrode cell. The lithium plating window at different rates is verified at room temperature using the following method:

[0210] (1) Lithium plating on copper wire: Connect the positive terminal of the charge-discharge tester to the battery cathode and the negative terminal of the charge-discharge tester to the copper wire. Charge at a current of 20 microamps for two hours to deposit lithium ions from the cathode onto the copper wire. Then connect the positive terminal of the charge-discharge tester to the battery anode and the negative terminal to the copper wire. Charge at a current of 20 microamps for two hours to deposit lithium ions from the anode onto the copper wire.

[0211] (2) Charge and discharge at different rates: At room temperature, different rates are selected for charging, while the potential of the third electrode (copper wire) and the anode potential are monitored to make the potential difference (potential) between the two 0 volts to cut off. The SOC (state of charge, which is equal to the charging capacity / the total capacity of the cell) at different rates is monitored to characterize the lithium plating window on the surface of the anode in the battery.

[0212] 2. Ratio Performance Test

[0213] At 25°C, discharge to 2.0V at 3C. Then perform charge-discharge cycles as follows: let stand for 5 minutes, charge to 3.65V at 3C, charge at 3.65V constant voltage to 0.05C, and record the number of cycles required to decay to 80% SOH.

[0214] The test results of the above embodiments and comparative examples are shown in Table 2.

[0215] Table 2

[0216]

[0217] As can be seen from the comparison of the results in Table 2, compared with Comparative Examples 1-6, the charging window of Examples 1-22 is increased, and the number of cycles required to decay to 80% SOH is significantly increased; indicating that the modified negative electrode material provided in this application has excellent fast charging performance and cycle performance.

[0218] The description of the various embodiments above tends to emphasize the differences between the various embodiments. The similarities or similarities between them can be referred to, and for the sake of brevity, they will not be repeated here.

[0219] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A modified negative electrode material, characterized in that, The modified negative electrode material includes: Core, the core comprising carbon-based material; and A coating layer covers at least a portion of the surface of the core; the coating layer comprises a silicate material comprising a framework structure consisting of a three-dimensional network of interconnected silicon-oxygen tetrahedra and metal-oxygen octahedra at their vertices; the silicate material has an ionic conductivity of 1 × 10⁻⁶ at 25°C. -6 S·cm -1 -1×10 -4 S·cm -1 .

2. The modified negative electrode material as described in claim 1, characterized in that, At 25°C, the ionic conductivity of the silicate material is 5 × 10⁻⁶. -6 S·cm -1 -8×10 -5 S·cm -1 .

3. The modified negative electrode material according to any one of claims 1 to 2, characterized in that, The chemical formula of the silicate material is A. x B y SiO4, element A includes one or more of Li, Na and K, element B includes one or more of Ca, Fe, Mg, Al, Mn and Ni, 0.4≤x≤2.5, 0.2≤y≤2.

4. The modified negative electrode material as described in claim 3, characterized in that, 0.4≤x≤1.6; 0.8≤y≤1.

5.

5. The modified negative electrode material according to any one of claims 1 to 2 and 4, characterized in that, The mass ratio of the coating layer to the core is (0.1-5):

100.

6. The modified negative electrode material according to any one of claims 1 to 2, 4, characterized in that, The mass ratio of the coating layer to the core is (0.2-1):

100.

7. The modified negative electrode material according to any one of claims 1 to 2, 4, characterized in that, The carbon-based material includes one or more of artificial graphite, natural graphite, hard carbon, soft carbon, and mesophase microspheres.

8. A method for preparing the modified negative electrode material according to any one of claims 1 to 7, characterized in that, The process includes the following steps: heating a mixture containing the silicate material, the core, and the gelling agent to prepare a gel-like mixture; The modified negative electrode material is prepared by subjecting the gel-like mixture to a first sintering treatment.

9. The method for preparing the modified negative electrode material as described in claim 8, characterized in that, The method for preparing the silicate material includes: A mixture containing silicon dioxide, a salt or oxide containing element A, and a salt or oxide containing element B is subjected to a second sintering treatment to prepare a material with the chemical formula A. x B y SiO4 silicate materials; Wherein, element A includes one or more of Li, Na and K, and element B includes one or more of Ca, Fe, Mg, Al, Mn and Ni, with 0.4≤x≤2.5 and 0.2≤y≤2.

10. The method for preparing the modified negative electrode material as described in claim 9, characterized in that, 0.4≤x≤1.6; 0.8≤y≤1.

5.

11. The method for preparing the modified negative electrode material according to any one of claims 9 to 10, characterized in that, The salts containing element A include one or more of the following: sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts containing element A; and / or The salts containing element B include one or more of the following: sulfates, sulfites, carbonates, bicarbonates, nitrates, hydrochlorides, and ammonium salts.

12. The method for preparing the modified negative electrode material according to any one of claims 9 to 10, characterized in that, The second sintering process includes at least one of the following conditions: (1) The temperature of the second sintering treatment is 700℃-1000℃; (2) The second sintering treatment time is 3h-12h; (3) The atmosphere for the second sintering treatment is an inert gas; (4) The heating rate of the second sintering treatment is 5℃ / min-15℃ / min.

13. The method for preparing the modified negative electrode material according to any one of claims 9 to 10, characterized in that, The temperature of the second sintering treatment is 800℃-950℃.

14. The method for preparing the modified negative electrode material according to any one of claims 9 to 10, characterized in that, The second sintering treatment takes 5-10 hours.

15. The method for preparing the modified negative electrode material according to any one of claims 9 to 10, characterized in that, The atmosphere for the second sintering treatment is argon.

16. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The mass ratio of the silicate material to the core is (0.1-5):100; and / or The mass of the gelling agent accounts for 10%-25% of the mass of the core.

17. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The mass ratio of the silicate material to the core is (0.2-1):

100.

18. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The mass of the gelling agent accounts for 15%-20% of the mass of the core.

19. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The gelling agent includes one or more of the following: hydrochloric acid, p-toluenesulfonic acid, acetic acid, succinic acid, maleic acid, boric acid, sulfuric acid, nitric acid, ammonia, sodium hydroxide, EDTA, and citric acid.

20. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The temperature of the first sintering treatment is 200℃-500℃; and / or The first sintering treatment takes 1-2 hours.

21. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The temperature of the first sintering treatment is 300℃-400℃.

22. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The first sintering treatment takes 1-1.5 hours.

23. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The heat treatment temperature is 80℃-120℃; and / or The heating treatment time is 1-2 hours.

24. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The temperature for the heat treatment is 80℃-90℃.

25. The method for preparing the modified negative electrode material according to any one of claims 8 to 10, characterized in that, The heating treatment time is 1 hour to 1.5 hours.

26. A negative electrode sheet, characterized in that, The modified negative electrode material comprises the modified negative electrode material according to any one of claims 1 to 7 or the modified negative electrode material prepared by the preparation method of the modified negative electrode material according to any one of claims 8 to 25.

27. A secondary battery, characterized in that, Includes the negative electrode sheet as described in claim 26.

28. An electrical appliance, characterized in that, Includes the secondary battery as described in claim 27.

Citation Information

Patent Citations

  • Silicon-based negative electrode material and preparation method and application thereof

    CN112186188A

  • Negative electrode active material for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, method for producing negative electrode material for non-aqueous secondary battery, and method for producing non-aqueous electrolyte secondary battery

    US20180261833A1