A method for laser cutting wafers

By coating the front side of the wafer with protective adhesive and liquid, combined with water rinsing and chemical solvent treatment, the problems of hot melt contamination and scratches after laser cutting are solved, achieving wafer protection and precise cutting, and ensuring the smooth progress of subsequent processes.

CN120727660BActive Publication Date: 2026-11-10GUANGDONG XINCHENG OPTOELECTRONICS SEMICONDUCTOR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510606426.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-05-12
Publication Date
2026-11-10
Estimated Expiration
2045-05-12

AI Technical Summary

Technical Problem

During current laser wafer cutting, the accumulation of molten material and residual contamination near the cutting path can cause the chip to crack, and the cleaning process may damage the wafer.

Method used

Protective adhesive and protective liquid are applied to the front side of the wafer. Combined with laser cutting, water rinsing and chemical solvent immersion, low-pressure water flow pretreatment and plasma treatment are used to remove hot melt and residues, thus protecting the wafer surface.

Benefits of technology

It effectively protects the front side of the wafer, preventing scratches and warping, ensuring cutting precision, removing residual hot melt and chemical solvents, preventing chip edges from being suspended, and improving the reliability of subsequent processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120727660B_ABST
    Figure CN120727660B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of wafer dicing technology and discloses a laser dicing method for wafers, comprising the following steps: sequentially coating the front side of a wafer with a protective adhesive and a protective liquid to obtain wafer A; attaching the back side of wafer A to a UV film and then performing laser dicing to obtain wafer B; subjecting wafer B to a first water stream rinse to obtain wafer C; expanding wafer C to obtain wafer D; sequentially immersing wafer D in a first chemical solvent and a second chemical solvent to obtain wafer E; exposing the front side of wafer E and then immersing it in a developer. This invention avoids the risk of scratches on the front side of the wafer when applying a protective adhesive to the wafer; it also improves the warping problem when applying a UV film to thin wafers; and it solves the problem of suspended chip edges on the front side of the wafer caused by chemical solvent immersion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wafer cutting technology, and specifically relates to a laser cutting method for wafers. Background Technology

[0002] Laser cutting, with its advantages of high precision, high speed, and narrow kerf width, is widely used in the mass production process of semiconductor chips. To protect semiconductor wafers from contamination and mechanical damage during laser cutting, a protective solution is typically applied to the chip surface before cutting. However, a large amount of molten material still accumulates and remains near the kerf. This molten material and damaged layer not only contaminate the chip surface but may also cause serious problems such as chip breakage during subsequent wafer picking and packaging. Currently, after laser cutting, wafers are generally cleaned using high-pressure water rinsing or chemical solvent immersion to remove the molten material. However, this cleaning process may also cause some damage to the wafer surface. Summary of the Invention

[0003] The present invention aims to improve at least one technical problem in the prior art.

[0004] This invention provides a laser cutting method for a wafer, the wafer having a front side on which a chip is formed and a back side corresponding to the front side. The laser cutting method includes the following steps:

[0005] Protective adhesive and protective liquid are coated sequentially on the front side of the wafer to obtain wafer A;

[0006] The back side of wafer A is attached to a UV film, and then laser-cut to obtain wafer B;

[0007] Wafer B is rinsed with a first stream of water to obtain wafer C;

[0008] Wafer C is expanded to obtain wafer D;

[0009] Wafer D is sequentially immersed in a first chemical solvent and a second chemical solvent to obtain wafer E;

[0010] The front side of wafer E is exposed and then immersed in developer.

[0011] The protective adhesive includes photoresist, and the thickness of the photoresist is 2μm-10μm;

[0012] The first chemical solvents include phosphoric acid and hydrogen peroxide;

[0013] The second chemical solvent includes ammonia;

[0014] The exposure was performed using ultraviolet light, with a wavelength ≤436nm and an energy density of 80mJ / cm². 2 -700mj / cm 2 ;

[0015] The soaking time in the developer solution is 5-15 minutes, and the soaking temperature in the developer solution is room temperature.

[0016] This invention uses photoresist as the protective adhesive for the front side of the wafer, which effectively improves the warpage of the thin wafer and provides ample protection for the front side when the back side of the wafer is subsequently attached to the UV film, preventing scratches. The protective solution in this invention avoids denaturation of the protective adhesive due to the high temperatures generated during laser cutting, preventing the hot melt from reacting with the protective adhesive and facilitating subsequent cleaning. The exposure process in this invention involves exposing the protective adhesive on the front side of the wafer to the developing solution, making it soluble and thus removing it by immersion in the developing solution. Furthermore, this invention combines water rinsing and chemical solvent cleaning methods. The first water rinsing removes the protective solution and some hot melt, while the subsequent chemical solvent cleaning removes the remaining hot melt, thereby protecting the wafer surface from hot melt contamination.

[0017] Furthermore, after soaking in the developer, a fourth water rinse is performed for 10-20 minutes.

[0018] In this invention, after soaking in the developer solution, further rinsing with water can further remove residues.

[0019] Further, after rinsing with the fourth water stream, a process to remove residual adhesive is performed.

[0020] The residual adhesive removal process involves plasma treatment, which includes oxygen plasma, and the treatment time is 1-5 minutes.

[0021] After immersion in the developer, a very thin layer of photoresist may still remain on the wafer surface. Descum removal uses plasma technology to thoroughly remove these residues and avoid affecting subsequent process steps.

[0022] Preferably, the water pressure of the first water flow is 0.3mPa-0.9mPa, and the rinsing time is 10min-20min.

[0023] In this invention, the first water flow rinse is equivalent to a pretreatment. Compared with the traditional high-pressure water flow rinse, the first water flow rinse uses lower water pressure and shorter time, which improves the convenience of operation.

[0024] Preferably, the volume concentration of phosphoric acid is ≥10%, the volume concentration of hydrogen peroxide is ≥10%, and the soaking time in the first chemical solvent is 10 min-30 min; the volume concentration of ammonia is 1%-10%, and the soaking time in the second chemical solvent is 1 min-2 min; the soaking temperature of the first chemical solvent and the second chemical solvent is room temperature.

[0025] Furthermore, after soaking in the first chemical solvent, a second water rinse is performed, and after soaking in the second chemical solvent, a third water rinse is performed.

[0026] The second water flow rinse lasts for 10-20 minutes, and the third water flow rinse lasts for 5-10 minutes.

[0027] In this invention, after soaking in the first chemical solvent and the second chemical solvent, the water is used for rinsing to further remove chemical solvent residues.

[0028] Preferably, the film expansion makes the distance between adjacent chips on the wafer 10μm-20μm.

[0029] Preferably, the wafer comprises one or more of Si, GaAs, GaAsAl, InP, and InGaAs.

[0030] The beneficial effects of this invention are as follows: the protective adhesive on the front side of the wafer can avoid the risk of scratches that may occur on the front side when applying UV film to the wafer; at the same time, it improves the warping problem when applying UV film to thin wafers; in addition, it also solves the problem of chip edge suspension on the front side of the wafer caused by chemical solvent immersion. Attached Figure Description

[0031] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0032] Figure 1 This is a diagram showing the case where the chip edge is floating.

[0033] Figure 2 This is a diagram showing the edge characteristics of a chip obtained by a laser cutting method according to an embodiment of the present invention. Detailed Implementation

[0034] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the description of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.

[0035] Currently, before laser cutting, semiconductor wafers have their back side attached to a UV film and placed on a cutting ring for subsequent cutting. Because the back side is the bonding surface, the wafer is face down when contacting the cutting platform, requiring precise handling and easily causing scratches on the wafer's front side. Furthermore, wafers with high warpage are more difficult to handle, and there may be issues such as incomplete vacuum adsorption by the machine's cutting platform.

[0036] This invention provides a laser cutting method for a wafer, the wafer having a front side on which a chip is formed and a back side corresponding to the front side. The laser cutting method includes the following steps:

[0037] Protective adhesive and protective liquid are coated sequentially on the front side of the wafer to obtain wafer A;

[0038] The back side of wafer A is attached to a UV film, and then laser-cut to obtain wafer B;

[0039] Wafer B is rinsed with a first stream of water to obtain wafer C;

[0040] Wafer C is expanded to obtain wafer D;

[0041] Wafer D is sequentially immersed in a first chemical solvent and a second chemical solvent to obtain wafer E;

[0042] The front side of wafer E is exposed and then immersed in developer.

[0043] In this embodiment, the wafer is Si. In other embodiments, the wafer may include one or more of Si, GaAs, GaAsAl, InP, and InGaAs.

[0044] In this embodiment, the protective adhesive is photoresist (in other embodiments, the protective adhesive may include, but is not limited to, resin materials such as photoresist), and the thickness of the photoresist is 5μm (in other embodiments, the thickness of the photoresist may be 2μm-10μm, such as 2μm, 4μm, 6μm, 10μm. If the thickness of the photoresist is too small, it is easy to fall off under the high temperature of laser cutting, which cannot fully protect the chip on the front side of the wafer, or it may be deformed and not conducive to subsequent removal. If the photoresist is too thick, it will affect the image recognition of the cutting equipment during laser cutting, thereby affecting the laser cutting accuracy).

[0045] In this embodiment, a protective adhesive is first applied to the front side of the wafer by spin coating or spraying. This provides sufficient protection for the front side of the wafer during the subsequent UV film application process on the back side, preventing scratches. For wafers with high warpage, the presence of the protective adhesive also offers some relief. Furthermore, this embodiment also spin-coates a protective liquid onto the front side of the wafer to prevent the high temperatures generated during laser cutting from denaturing the protective adhesive and to prevent the hot melt from reacting with the adhesive, facilitating subsequent cleaning.

[0046] In this embodiment, the water pressure of the first water flow is 0.5 mPa (in some other embodiments, the first water pressure of the first water flow can be 0.3-0.9 mPa, for example 0.3 mPa, 0.6 mPa, 0.9 mPa), and the rinsing time of the first water flow is 10 min (in some other embodiments, the rinsing time of the first water flow can be 10 min-20 min, for example 12 min, 15 min, 18 min, 20 min).

[0047] Compared to traditional high-pressure water rinsing, the first water rinsing in this embodiment serves as a pretreatment, using lower water pressure, shorter rinsing time, and simpler steps. Furthermore, under the protection of the protective layer, the first water rinsing removes the protective liquid and some of the hot melt material without damaging the chip formed on the front side of the wafer.

[0048] In this embodiment, the first chemical solvent includes phosphoric acid and hydrogen peroxide. The volume concentration of phosphoric acid is 10% (in some other embodiments, the volume concentration of phosphoric acid can be ≥10%, such as 15%, 20%, or 30%), and the volume concentration of hydrogen peroxide is 10% (in some other embodiments, the volume concentration of hydrogen peroxide can be ≥10%, such as 15%, 20%, or 30%). The soaking time in the first chemical solvent is 20 minutes (in some other embodiments, the soaking time in the first chemical solvent can be 10 minutes to 30 minutes, such as 10 minutes, 15 minutes, 25 minutes, or 30 minutes).

[0049] In this embodiment, chemical solvent cleaning is divided into a first chemical solvent immersion and a second chemical solvent immersion. The selection of the first chemical solvent is not complicated. A mixed solution of phosphoric acid and hydrogen peroxide with a specific volume concentration can be used to chemically etch away the remaining hot melt.

[0050] In this embodiment, the second chemical solvent includes ammonia water, the volume concentration of which is 2% (in other embodiments, the volume concentration of which can be 1%-10%, such as 1%, 3%, 5%, 10%), and the soaking time in the second chemical solvent is 2 minutes (in other embodiments, the soaking time in the second chemical solvent can be 1-2 minutes, such as 1 minute, 1.5 minutes, 1.8 minutes).

[0051] In this embodiment, the second chemical solvent soaking uses an ammonia solution of a specific volume concentration to remove the phosphoric acid and hydrogen peroxide remaining after the first chemical solvent soaking.

[0052] In this embodiment, the immersion temperature of the first chemical solvent and the second chemical solvent is room temperature.

[0053] In this embodiment, after the laser cutting protective liquid and some hot melt material are removed by the first water flow rinsing, the etching selectivity of the chemical solvent in the subsequent chemical solvent cleaning does not need to be as strict as that of traditional chemical solvent cleaning, and it can be carried out under normal temperature conditions.

[0054] Without the protective adhesive used in this embodiment to protect the front side of the wafer, the cutting protective solvent will be washed away by the first water stream after laser cutting. Therefore, during subsequent chemical solvent immersion, the chemical solvent will simultaneously act on the chip formed on the front side of the wafer and the sidewalls of the dicing track, causing the chip edge to be suspended (e.g., Figure 1 As shown in the diagram (circled to indicate the location), depending on the epitaxial / substrate material, the width of this gap is generally 0.5μm-4μm. This gap will pose a significant risk to the subsequent packaging of the chip and can easily cause the chip surface structure to peel off.

[0055] In this embodiment, ultraviolet light exposure is used, with a wavelength of 436 nm (in other embodiments, the wavelength of ultraviolet light can be ≤436 nm, such as 365 nm, 248 nm, or 193 nm), and the energy density of the ultraviolet light is 100 mJ / cm². 2 (In some other embodiments, the energy density of the ultraviolet light can be 80 mJ / cm²) 2 -700mj / cm 2 For example, 80mj / cm 2 100mj / cm 2 200mj / cm 2 500mj / cm 2 700mj / cm 2 If the energy density of ultraviolet light is too low, the exposure will be incomplete and the photoresist will not be completely removed by the developer. If the energy density of ultraviolet light is too high, it will affect the adhesion of the photoresist to the wafer and cause the chip to fall off abnormally when removing the photoresist. The soaking time of the developer solution is 10 minutes (in some other embodiments, the soaking time of the developer solution can be 5 minutes to 15 minutes, such as 5 minutes, 8 minutes, and 15 minutes), and the soaking temperature of the developer solution is room temperature.

[0056] In this embodiment, the exposure involves exposing the protective adhesive on the front side of the wafer to make it soluble in the developer, which can then be removed by soaking in the developer.

[0057] Furthermore, in this embodiment, a fourth water rinse is performed after soaking in the developer solution.

[0058] In this embodiment, the rinsing time of the fourth water flow is 15 minutes (in some other embodiments, the rinsing time of the fourth water flow can be 10 minutes to 20 minutes, for example, 10 minutes, 12 minutes, or 20 minutes).

[0059] In this invention, after soaking in the developer solution, further rinsing with water can further remove residues.

[0060] Furthermore, in this embodiment, residual adhesive removal is performed after rinsing with the fourth water stream.

[0061] In this embodiment, the residual adhesive removal process is plasma treatment, including oxygen plasma, and the residual adhesive removal process takes 5 minutes (in other embodiments, the residual adhesive removal process can take 1-5 minutes, for example, 1 minute, 2 minutes, or 3 minutes).

[0062] After immersion in the developer, a very thin layer of photoresist may still remain on the wafer surface. In this embodiment, the descum process uses plasma technology to thoroughly remove these residues, thus avoiding affecting subsequent process steps.

[0063] Furthermore, in this embodiment, after soaking in the first chemical solvent, a second water rinse is performed, and after soaking in the second chemical solvent, a third water rinse is performed.

[0064] In this embodiment, the second water rinse lasts for 15 minutes (in some other embodiments, the second water rinse lasts for 10-20 minutes, such as 10 minutes, 12 minutes, 17 minutes, or 20 minutes), and the third water rinse lasts for 5 minutes (in some other embodiments, the third water rinse lasts for 5-10 minutes, such as 6 minutes, 8 minutes, or 10 minutes).

[0065] In this embodiment, after soaking in the first and second chemical solvents, the water is used for rinsing to further remove chemical solvent residues.

[0066] Furthermore, in this embodiment, the film expansion makes the distance between adjacent chips on the wafer 10μm (in some other embodiments, the film expansion makes the distance between adjacent chips on the wafer 10μm-20μm, for example 12μm, 15μm, 20μm).

[0067] In this embodiment, the film expansion involves separating the chip, thereby increasing the contact area between the hot melt and the chemical solvent, which facilitates subsequent processing.

[0068] The edge condition of the chip obtained by the laser cutting method in this embodiment is shown in the figure below. Figure 2 As shown, there is no obvious gap at the edge of the chip, indicating that the chip is adequately protected by the protective film.

[0069] In the description of this specification, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Therefore, a feature defined with "first," "second," etc., may explicitly or implicitly include at least one of that feature.

[0070] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make several improvements and additions without departing from the method of the present invention, and these improvements and additions should also be considered within the scope of protection of the present invention.

Claims

1. A method for laser cutting a wafer, characterized in that, The wafer has a front side on which a chip is formed and a back side corresponding to the front side. The laser cutting method includes the following steps: A protective adhesive and a protective liquid are sequentially coated on the front side of the wafer to obtain wafer A; The back side of wafer A is attached to a UV film, and then laser-cut to obtain wafer B; The wafer B is rinsed with a first water stream to obtain wafer C; The wafer C is expanded to obtain wafer D; The wafer D is sequentially immersed in a first chemical solvent and a second chemical solvent to obtain wafer E; The front side of the wafer E is exposed and then immersed in a developing solution; The protective liquid is used to prevent the high temperature generated by laser cutting from denaturing the protective adhesive and to prevent the hot melt generated during cutting from reacting with the protective adhesive. The first water flow rinse is used to remove the protective liquid and some of the hot melt material; The film expansion is to separate adjacent chips, thereby increasing the contact area between the hot melt and the chemical solvent; The protective adhesive includes photoresist with a thickness of 2μm-10μm. The protective adhesive protects the chip formed on the front side of the wafer during immersion in the first chemical solvent and the second chemical solvent, so as to prevent the chemical solvent from acting on the edge of the chip and causing the edge of the chip to be suspended. The first chemical solvent includes phosphoric acid and hydrogen peroxide; The second chemical solvent includes ammonia; The exposure is performed using ultraviolet light, the wavelength of which is ≤436nm and the energy density of which is 80mj / cm2-700mj / cm2; The soaking time in the developer solution is 5-15 minutes, and the soaking temperature of the developer solution is room temperature.

2. The laser cutting method for wafers according to claim 1, characterized in that, After soaking in the developer, a fourth water rinse is performed for 10-20 minutes.

3. The wafer laser cutting method according to claim 2, characterized in that, After rinsing with the fourth water stream, a process to remove residual adhesive is performed.

4. The laser cutting method for wafers according to claim 3, characterized in that, The residual adhesive removal process is a plasma treatment, which includes oxygen plasma, and the duration of the residual adhesive removal process is 1-5 minutes.

5. The laser cutting method for wafers according to claim 1, characterized in that, After soaking in the first chemical solvent, a second water rinse is performed, and after soaking in the second chemical solvent, a third water rinse is performed.

6. The laser cutting method for wafers according to claim 5, characterized in that, The second water flow rinse lasts for 10-20 minutes; and / or the third water flow rinse lasts for 5-10 minutes.

7. The laser cutting method for wafers according to claim 1, characterized in that, The film expansion makes the distance between adjacent chips on the wafer 10μm-20μm.

8. The laser cutting method for wafers according to claim 1, characterized in that, The wafer comprises one or more of Si, GaAs, GaAsAl, InP, and InGaAs.

Citation Information

Patent Citations

  • Fabrication method for dicing of semiconductor wafers using laser cutting techniques

    CN102468233A

  • Material for forming resist protection film for liquid immersion lithography and method for forming resist pattern by using the protection film