Gallium nitride electronic devices and methods of making the same

By introducing metallic impurities into gallium nitride electronic devices to form a compensation layer, the problem of high impurity concentration on the surface of gallium nitride substrates is solved, leakage current is reduced and output power is increased, the fabrication process is simplified, and device performance is improved.

CN120730768BActive Publication Date: 2026-11-10SUZHOU NANOWIN SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202510896845.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-06-30
Publication Date
2026-11-10
Estimated Expiration
2045-06-30

AI Technical Summary

Technical Problem

In the prior art, when reducing the concentration of impurity atoms adsorbed on the surface of gallium nitride substrates, especially the concentration of silicon atoms, gallium nitride electronic devices suffer from severe leakage current and low output power. Traditional carbon doping methods have problems such as excessive carbon concentration and carbon atoms occupying nitrogen sites to form deep energy level traps, which affect device performance.

Method used

By using metallic impurities such as Fe, Ni, or Mn as deep-level acceptor impurities, a compensation layer is formed on the surface of gallium nitride substrates through a combination of heat treatment and growth source. This compensates for shallow-level donor impurities, reduces the Si atom concentration, simplifies the fabrication process, and avoids the challenges brought by carbon doping.

Benefits of technology

It effectively reduces leakage current and increases output power in gallium nitride electronic devices, simplifies the fabrication process, and improves device quality and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120730768B_ABST
    Figure CN120730768B_ABST
Patent Text Reader

Abstract

The application discloses a gallium nitride electronic device and a preparation method thereof, and belongs to the technical field of semiconductors. The gallium nitride electronic device comprises a gallium nitride substrate and a semiconductor structure layer arranged on the gallium nitride substrate. The gallium nitride substrate has shallow energy level donor impurities and deep energy level acceptor impurities. The deep energy level acceptor impurities are used for compensating the shallow energy level donor impurities, and the deep energy level acceptor impurities are metal impurities. A compensation layer is arranged at the interface between the gallium nitride substrate and the semiconductor structure layer. The concentration of the deep energy level acceptor impurities in the compensation layer is greater than the concentration of the deep energy level acceptor impurities in the gallium nitride substrate. The metal impurities are doped in the gallium nitride substrate as the deep energy level acceptor impurities to compensate the shallow energy level donor impurities, so that the concentration of the impurity atoms adsorbed on the surface of the gallium nitride substrate is reduced, and the performance of the gallium nitride electronic device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor technology, and more specifically, relates to a gallium nitride electronic device and its fabrication method. Background Technology

[0002] Gallium nitride (GaN)-based semiconductor materials possess excellent properties such as a large bandgap, high breakdown voltage, high strong-field drift velocity, high temperature resistance, and radiation resistance. GaN-based high-electron-mobility transistors (HEMTs) can generate high-density, high-mobility two-dimensional electron gases, making them particularly suitable for fabricating high-voltage, high-efficiency, high-density, and high-power microwave and millimeter-wave devices. GaN-based HEMT transistors are widely used in cutting-edge equipment in microwave and millimeter-wave frequency bands, and have extremely important applications in phased-array radar, aerospace, smart weapons, satellite communications, and electronic warfare.

[0003] GaN homogeneous substrates obtained through hydride vapor phase epitaxy (HVPE), or GaN substrate materials obtained through metal-organic chemical vapor deposition (MOCVD) and molecular beam epitaxy (MBE), will have a high concentration of silicon (Si) impurities during growth and storage. The sources of Si impurities are mainly twofold: adsorption during substrate storage and the background Si concentration of the substrate itself. If GaN single-crystal substrates are exposed to air during storage, Si impurities (such as silicon dioxide or silicon particles) will adsorb from the air onto the surface. This adsorption has a cumulative effect over time; the longer the storage time, the greater the adsorption, leading to a significant increase in Si concentration at the interface. During GaN single-crystal growth, trace amounts of Si elements may be introduced from the raw materials or growth environment, forming a "background Si concentration" on the substrate. During subsequent epitaxy or heat treatment, high temperatures accelerate Si diffusion, causing it to accumulate at the interface. As a shallow donor, Si leads to the formation of an n-type conductive layer on the GaN substrate surface, increasing parasitic capacitance and reducing the switching speed of HEMT devices. Furthermore, Si impurities can induce parasitic conductive channels at the homoepitaxial regeneration interface, causing leakage in the GaN buffer layer of the aluminum gallium nitride / gallium nitride heterojunction material. This results in poor pinch-off characteristics and poor electrical isolation between devices on the same chip in HEMT devices.

[0004] In existing technologies, carbon doping is commonly used to compensate for the leakage current problem in gallium nitride (GaN) HEMT devices caused by Si impurities. Carbon doping compensates for the donor characteristics of Si, and as an acceptor impurity, its charge compensation mechanism with Si can reduce the background carrier concentration and improve the device breakdown voltage. However, carbon doping of GaN layers in HEMT devices presents several challenges in terms of device performance, besides the need for epitaxial growth and the relatively long process. Specifically, the carbon doping concentration is closely related to MOCVD growth conditions. Low temperatures (below 1000℃) and low V / III ratios (below 2000) lead to a significant increase in carbon concentration, but this is accompanied by a three-dimensional island growth mode, resulting in increased surface roughness (RMS roughness greater than 2nm) and deep pit defects (depth greater than 50nm), directly affecting the device breakdown voltage. On the other hand, carbon atoms occupying nitrogen sites form deep energy level traps (energy level approximately 0.9eV), which couple with the piezoelectric field generated by the spontaneous polarization of the aluminum gallium nitride barrier layer, leading to a decrease in the two-dimensional electron gas mobility.

[0005] Traditional surface treatment methods (such as cleaning) cannot effectively reduce the concentration of Si impurity atoms, nor can they ensure that the GaN regrowth interface is not damaged. While carbon doping can address Si impurity leakage in existing technologies, it still has many adverse effects on device performance. Therefore, effectively reducing the concentration of impurity atoms (especially Si atoms) adsorbed on the surface of GaN homogeneous substrates and improving the performance of GaN HEMT devices is a pressing technical problem that needs to be solved. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this invention provides a gallium nitride electronic device and its fabrication method. The purpose is to solve the problems of severe leakage and low output power in existing gallium nitride electronic devices when the concentration of impurity atoms adsorbed on the surface of the gallium nitride substrate is reduced.

[0007] According to one aspect of the present invention, a gallium nitride electronic device is provided, comprising a gallium nitride substrate and a semiconductor structure layer disposed on the gallium nitride substrate;

[0008] The gallium nitride substrate has shallow-level donor impurities and deep-level acceptor impurities. The deep-level acceptor impurities are used to compensate for the shallow-level donor impurities, and the deep-level acceptor impurities are metallic impurities.

[0009] A compensation layer is provided at the interface between the gallium nitride substrate and the semiconductor structure layer, wherein the concentration of deep-level acceptor impurities in the compensation layer is greater than the concentration of deep-level acceptor impurities in the gallium nitride substrate.

[0010] Preferably, the melting point of the deep-level acceptor impurity is greater than the decomposition temperature of gallium nitride;

[0011] And / or, the material of the compensation layer includes GaN;

[0012] And / or, the deep-level acceptor impurity is a Fe impurity, a Ni impurity, or a Mn impurity;

[0013] And / or, the concentration of Fe impurities in the gallium nitride substrate is 5 × 10⁻⁶. 17 cm- 3 1×10 19 cm- 3 ;

[0014] And / or, the concentration of Fe impurities in the compensation layer is 5 × 10⁻⁶. 18 cm- 3 ~5×10 19 cm- 3 ;

[0015] And / or, the thickness of the compensation layer is 20nm to 60nm;

[0016] And / or, the formation temperature of the compensation layer is 850℃~1100℃.

[0017] Preferably, the gallium nitride electronic device is a HEMT.

[0018] Preferably, the semiconductor structure layer includes a buffer layer, a channel layer, and a barrier layer sequentially disposed along a direction away from the gallium nitride substrate, wherein the barrier layer has a groove;

[0019] The semiconductor structure layer further includes a dielectric layer and a passivation layer. The dielectric layer is disposed on the inner wall and bottom of the groove, and the passivation layer is disposed on the barrier layer.

[0020] The gallium nitride electronic device further includes a source electrode, a drain electrode, and a gate electrode, wherein the gate electrode covers the dielectric layer; the source electrode and the drain electrode are disposed on the side of the barrier layer away from the gallium nitride substrate and are spaced apart.

[0021] The buffer layer and the channel layer are made of GaN; and / or the barrier layer is made of AlGaN; and / or the sum of the thicknesses of the buffer layer and the compensation layer is 80nm to 120nm.

[0022] According to another aspect of the present invention, a method for fabricating a gallium nitride electronic device is provided, comprising:

[0023] A first gallium nitride substrate is provided; wherein the first gallium nitride substrate has shallow-level donor impurities and deep-level acceptor impurities, and the deep-level acceptor impurities are metallic impurities, and the deep-level acceptor impurities are used to compensate for the shallow-level donor impurities;

[0024] The first gallium nitride substrate is heat-treated and a growth source is introduced to form a gallium nitride substrate and a compensation layer.

[0025] A semiconductor structure layer is formed on the compensation layer;

[0026] The concentration of deep-level acceptor impurities in the compensation layer is greater than the concentration of deep-level acceptor impurities in the gallium nitride substrate.

[0027] Preferably, the semiconductor structure layer includes a buffer layer, the buffer layer being made of the same material as the compensation layer; the step of heat-treating the first gallium nitride substrate and introducing a growth source to form the gallium nitride substrate and the compensation layer includes:

[0028] Hydrogen gas is introduced into the growth chamber to heat-treat the first gallium nitride substrate, causing the first gallium nitride substrate to gradually decompose from the surface and enrich the deep-level acceptor impurities on the surface of the remaining part of the first gallium nitride substrate, thereby obtaining a second gallium nitride substrate with the deep-level acceptor impurities enriched on the surface.

[0029] The growth source is introduced into the growth cavity to form the gallium nitride substrate, the compensation layer, and the buffer layer, which are stacked sequentially.

[0030] Preferably, the step of introducing the growth source into the growth cavity to form the gallium nitride substrate, the compensation layer, and the buffer layer stacked sequentially includes:

[0031] The growth source is introduced into the growth cavity so that the deep-level acceptor impurities on the surface of the second gallium nitride substrate form the compensation layer with the growth source, and the second gallium nitride substrate is transformed into the gallium nitride substrate.

[0032] The growth source is continued to be introduced into the growth chamber to form the buffer layer on the compensation layer;

[0033] The thickness of the compensation layer is 20nm to 60nm, and / or the sum of the thicknesses of the buffer layer and the compensation layer is 80nm to 120nm.

[0034] Preferably, the growth source includes a gallium source and a nitrogen source, and the preparation of the buffer layer includes:

[0035] The buffer layer is deposited by introducing a nitrogen source with a flow rate of 1500-2000 sccm, a gallium source with a flow rate of 50-100 sccm, and a carrier gas with a flow rate of 2000-3000 sccm at a temperature of 1050℃~1100℃.

[0036] Preferably, the deep-level acceptor impurity is an Fe impurity, and the fabrication process of the first gallium nitride substrate is as follows:

[0037] Under conditions of 1000℃~1050℃, a nitrogen source with a flow rate of 1000ml / min~1100ml / min, a chlorine source with a flow rate of 50ml / min~55ml / min, and a doped iron source with a flow rate of 100ml / min~120ml / min are introduced into the reaction chamber to prepare the first gallium nitride substrate.

[0038] The catalytic introduction time is 20 min to 200 min, and the Fe impurity concentration in the first gallium nitride substrate is 5 × 10⁻⁶. 17 cm -3 ~1×10 19 cm -3 .

[0039] Preferably, in the heat treatment process, the heat treatment temperature is 850℃~1100℃;

[0040] And / or, the semiconductor structure layer further includes a channel layer and a barrier layer, wherein the semiconductor structure layer is grown on the substrate whose surface is enriched with deep-level acceptor impurities, specifically including:

[0041] The channel layer and the barrier layer are sequentially formed on the buffer layer, thereby forming the semiconductor structure layer;

[0042] And / or, the method further includes:

[0043] A source electrode, a drain electrode, and a gate electrode are formed on the semiconductor structure layer.

[0044] Preferably, the channel layer is made of GaN;

[0045] Under conditions of 1100℃~1150℃ and 80Torr~100Torr, a gallium source and a nitrogen source are introduced into the reaction chamber to deposit a channel layer with a thickness of 0.8-2.5μm on the buffer layer;

[0046] And / or, the material of the barrier layer includes Al. x Ga 1-x N, 0.1 ≤ x ≤ 0.15;

[0047] Under conditions of temperature of 1060℃~1100℃ and pressure of 60Torr~80Torr, a gallium source, an aluminum source and a nitrogen source are introduced into the reaction chamber to deposit a barrier layer with a thickness of 100-300nm on the channel layer.

[0048] And / or, the formation of the source electrode, drain electrode, and gate electrode on the semiconductor structure layer includes:

[0049] The semiconductor structure layer is etched to form a groove with a depth of 15nm-30nm;

[0050] A first dielectric layer with a thickness of 2-8 nm and a second dielectric layer with a thickness of 2-10 nm are sequentially deposited on the inner wall and bottom of the groove to obtain a dielectric layer;

[0051] A passivation layer with a thickness of 80nm-150nm is deposited on the surface of the semiconductor structure layer that is not covered by the dielectric layer; a portion of the passivation layer is etched to expose the semiconductor structure layer, forming a drain region and a source region;

[0052] The gate electrode is deposited on the dielectric layer, and the source electrode and the drain electrode are deposited in the source region and the drain region, respectively; wherein the source electrode and the drain electrode are spaced apart.

[0053] In summary, the above-described technical solutions conceived in this invention can achieve the following beneficial effects:

[0054] (1) This invention provides a gallium nitride electronic device, wherein the gallium nitride substrate has shallow-level donor impurities and deep-level acceptor impurities, and the deep-level acceptor impurities are metal impurities; by introducing metal impurities into the gallium nitride substrate to form a metal-doped gallium nitride substrate, the background carrier concentration is compensated by utilizing the characteristic that metal ions are deeply attached to the principal level, thereby compensating for the concentration of impurity atoms adsorbed on the surface of the gallium nitride substrate, especially the concentration of Si atoms, which effectively solves the problems of excessive carbon concentration and carbon atoms occupying nitrogen sites to form deep-level traps in traditional carbon doping methods, resulting in serious leakage current and low output power of high electron mobility transistor devices based on gallium nitride, thus improving the quality of gallium nitride electronic devices.

[0055] (2) The present invention provides a method for fabricating gallium nitride electronic devices, providing a first gallium nitride substrate having shallow-level donor impurities and deep-level acceptor impurities, wherein the deep-level acceptor impurities are metallic impurities. The first gallium nitride substrate is heat-treated and a growth source is introduced to cause the metallic impurities to thermally decompose at high temperature and remain on the substrate surface, thereby achieving effective compensation of Si, avoiding many challenges brought about by carbon doping, simplifying the fabrication process, and solving the problems of complex process and high cost of traditional carbon doping methods. Attached Figure Description

[0056] Figure 1 This is a schematic diagram illustrating the relationship between Si impurity concentration and structural depth provided in an embodiment of the present invention;

[0057] Figure 2 This is a schematic diagram of the structure of a gallium nitride electronic device provided in an embodiment of the present invention;

[0058] Figure 3A flowchart illustrating the fabrication method of gallium nitride electronic devices provided in this embodiment of the invention;

[0059] Figure 4 This is a schematic diagram of the device structure after the buffer layer is prepared according to the preparation method of this invention.

[0060] Figure 5 This is a schematic diagram of the device structure after the channel layer is fabricated according to the fabrication method of this invention.

[0061] Figure 6 This is a schematic diagram of the device structure after the barrier layer is fabricated according to the fabrication method of this invention.

[0062] Figure 7 This is a schematic diagram illustrating the relationship between Fe impurity concentration and structural depth after in-situ heat treatment and without in-situ heat treatment, provided as an embodiment of the present invention.

[0063] Explanation of reference numerals in the attached figures: 1 is gallium nitride substrate, 2 is compensation layer, 3 is semiconductor structure layer, 31 is buffer layer, 32 is channel layer, 33 is barrier layer, 34 is dielectric layer, 341 is first dielectric layer, 342 is second dielectric layer, 35 is passivation layer, 4 is source electrode, 5 is drain electrode, and 6 is gate electrode. Detailed Implementation

[0064] In view of the shortcomings of the prior art, the inventors of this invention, through long-term research and extensive practice, have proposed the technical solution of this invention. The following will further explain and illustrate this technical solution, its implementation process, and its principles.

[0065] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and therefore the scope of protection of the invention is not limited to the specific embodiments disclosed below.

[0066] Furthermore, in the description of this invention, it should be understood that the terms "upper," "lower," "inner," "outer," "horizontal," "vertical," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0067] In the description of this specification, the references to terms such as "an embodiment," "a particular embodiment," or "the embodiment" indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0068] See Figure 1 , Figure 1 This is a schematic diagram illustrating the relationship between Si impurity concentration and structural depth, provided in an embodiment of the present invention. Figure 1 The relationship between Si impurity concentration and structure depth is shown. The depth of the protrusions corresponds to the position of the substrate interface. It can be seen that the Si impurity concentration at the substrate interface can reach a maximum of 5E19 cm⁻¹. 3 This high Si impurity concentration significantly reduces the performance of gallium nitride electronic devices. Therefore, how to effectively reduce the concentration of impurity atoms (especially Si atoms) adsorbed on the surface of gallium nitride substrates and improve the performance of GaN-based high electron mobility transistor devices is an urgent technical problem to be solved.

[0069] The first aspect of this invention provides a gallium nitride electronic device. Please refer to [link / reference needed]. Figure 2 , Figure 2 This is a schematic diagram of the structure of a gallium nitride electronic device provided in an embodiment of the present invention. The gallium nitride electronic device includes a gallium nitride substrate 1 and a semiconductor structure layer 3 disposed on the gallium nitride substrate 1.

[0070] The gallium nitride substrate 1 contains shallow-level donor impurities and deep-level acceptor impurities. The deep-level acceptor impurities are used to compensate for the shallow-level donor impurities, and the deep-level acceptor impurities are metallic impurities. A compensation layer 2 is disposed at the interface between the gallium nitride substrate 1 and the semiconductor structure layer 3. The concentration of deep-level acceptor impurities in the compensation layer 2 is greater than the concentration of deep-level acceptor impurities in the gallium nitride substrate 1.

[0071] By using deep-level acceptor impurities to compensate for shallow-level donor impurities, the problem of excessive carbon concentration and deep-level traps formed by carbon atoms occupying nitrogen sites, which leads to severe leakage current and low output power in gallium nitride-based high electron mobility transistors, is effectively solved by traditional carbon doping methods, thus improving the quality of gallium nitride electronic devices.

[0072] Preferably, the melting point of the deep-level acceptor impurity is greater than the decomposition temperature of GaN.

[0073] Preferably, the deep-level acceptor impurity is an Fe impurity, a Ni impurity, or a Mn impurity; the Fe impurity concentration in the gallium nitride substrate 1 is 5 × 10⁻⁶. 17 cm -3~1×10 19 cm -3 The Fe impurity concentration in compensation layer 2 is 5 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 The Fe impurity concentration in gallium nitride substrate 1 is, for example, 5 × 10⁻⁶. 17 cm -3 6×10 17 cm -3 7×10 17 cm -3 8×10 17 cm -3 9×10 17 cm -3 1×10 18 cm -3 2×10 18 cm -3 3×10 18 cm -3 4×10 18 cm -3 5×10 18 cm -3 6×10 18 cm -3 7×10 18 cm -3 8×10 18 cm -3 9×10 18 cm -3 Or 1×10 19 cm -3 The Fe impurity concentration in compensation layer 2 is, for example, 5 × 10⁻⁶. 18 cm -3 6×10 18 cm -3 7×10 18 cm -3 8×10 18 cm -3 9×10 18 cm -3 1×10 19 cm -3 2×10 19 cm -3 3×10 19 cm -3 4×10 19 cm -3 Or 5×10 19 cm -3 .

[0074] Furthermore, the thickness of the compensation layer 2 is 20nm to 60nm, and the formation temperature is 850℃ to 1100℃. Preferably, the thickness of the compensation layer 2 is, for example, 20nm, 30nm, 40nm, 50nm or 60nm, and the formation temperature of the compensation layer 2 is, for example, 850℃, 900℃, 950℃, 1000℃, 1050℃ or 1100℃.

[0075] Furthermore, such as Figure 2 As shown, the semiconductor structure layer 3 includes a buffer layer 31, a channel layer 32, and a barrier layer 33 sequentially disposed along the direction away from the gallium nitride substrate 1, and the barrier layer 33 has a groove. The semiconductor structure layer 3 also includes a dielectric layer 34 and a passivation layer 35, the dielectric layer 34 being disposed on the inner wall and bottom of the groove, and the passivation layer 35 being disposed on the barrier layer 33.

[0076] The gallium nitride electronic device also includes a source electrode 4, a drain electrode 5, and a gate electrode 6. The gate electrode 6 is covered by a dielectric layer 34. The source electrode 4 and the drain electrode 5 are disposed on the side of the barrier layer 33 away from the gallium nitride substrate 1 and are spaced apart.

[0077] Furthermore, the buffer layer 31 and the channel layer 32 are made of GaN, and the barrier layer 33 is made of AlGaN. More preferably, the barrier layer is made of Al... x Ga 1-x N, 0.1 ≤ x ≤ 0.15. Buffer layer 31 is, for example, a GaN buffer layer; channel layer 32 is, for example, a GaN channel layer; and barrier layer 33 is, for example, Al. x Ga 1-x The N-barrier layer, channel layer 32, and barrier layer 33 form a heterojunction structure Al. x Ga 1-x N / GaN, Al x Ga 1-x The N / GaN heterojunction structure generates a high concentration of two-dimensional electron gas through spontaneous polarization and piezoelectric polarization, giving gallium nitride electronic devices advantages such as high current density, low on-resistance, and high power density.

[0078] Furthermore, the sum of the thicknesses of the buffer layer 31 and the compensation layer 2 is 80 nm to 120 nm. The thickness of the channel layer 32 is 0.8 μm to 2.5 μm. The thickness of the barrier layer 33 is 100 nm to 300 nm. Preferably, the thickness of the compensation layer 2 is, for example, 30 nm, the thickness of the buffer layer 31 is, for example, 60 nm, the thickness of the channel layer 32 is, for example, 0.8 μm, 1.0 μm, 1.2 μm, 1.4 μm, 1.6 μm, 1.8 μm, 2.0 μm, 2.2 μm or 2.5 μm, and the thickness of the barrier layer 33 is, for example, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm or 300 nm.

[0079] A second aspect of this invention provides a method for fabricating gallium nitride electronic devices, used for fabricating... Figure 2 Gallium nitride electronic devices in the illustrated embodiments. Please refer to... Figure 3 The preparation method includes steps S100-S300.

[0080] Step S100: A first gallium nitride substrate is provided; wherein the first gallium nitride substrate has shallow-level donor impurities and deep-level acceptor impurities, and the deep-level acceptor impurities are metallic impurities, which are used to compensate for the shallow-level donor impurities.

[0081] In this embodiment, a metal-doped gallium nitride substrate is selected when fabricating gallium nitride electronic devices (such as GaN-based HEMT structures). Metal-doped gallium nitride substrates offer the following advantages when forming GaN-based HEMT structures: The metal, acting as an acceptor impurity, can compensate for the background electron concentration in GaN, making the GaN material exhibit semi-insulating properties and thus increasing the substrate resistivity. This is crucial for HEMT devices because a high-resistivity substrate reduces leakage current, improving device performance and reliability. Furthermore, metal doping can improve the high-frequency characteristics of the device, making it more suitable for high-frequency, high-power devices.

[0082] In step S200, the first gallium nitride substrate is heat-treated and a growth source is introduced to form a gallium nitride substrate and a compensation layer, wherein the concentration of deep-level acceptor impurities in the compensation layer is greater than the concentration of deep-level acceptor impurities in the gallium nitride substrate.

[0083] Step S300: A semiconductor structure layer is formed on the compensation layer.

[0084] Under conditions of 1000℃~1050℃, a nitrogen source with a flow rate of 1000ml / min~1100ml / min, a chlorine source with a flow rate of 50ml / min~55ml / min, and a doped iron source with a flow rate of 100ml / min~120ml / min are introduced into the reaction chamber to prepare a first gallium nitride substrate, wherein the deep-level acceptor impurity in the first gallium nitride substrate is an Fe impurity. For example, the temperature can be 1000℃, 1010℃, 1020℃, 1030℃, 1040℃, or 1050℃; the nitrogen source can be NH3, and the flow rate of the nitrogen source can be 1000ml / min, 1010ml / min, 1020ml / min, 1030ml / min, 1040ml / min, 1050ml / min, 1060ml / min, 1070ml / min, 1080ml / min, 1090ml / min, or 1100ml / min; the chlorine source can be HCl. The flow rate of the source can be 50 ml / min, 51 ml / min, 52 ml / min, 53 ml / min, 54 ml / min or 55 ml / min; the iron doping source can be ferrocene, and the flow rate of the iron doping source can be 100 ml / min, 102 ml / min, 104 ml / min, 106 ml / min, 108 ml / min, 110 ml / min, 112 ml / min, 114 ml / min, 116 ml / min, 118 ml / min or 120 ml / min.

[0085] Furthermore, the introduction time of the nitrogen source, chlorine source, and doped iron source is 20 min to 200 min, and the Fe impurity concentration of the first gallium nitride substrate is 5 × 10⁻⁶. 17 cm- 3 ~1×10 19 cm- 3 For example, the inlet time can be 20 min, 40 min, 60 min, 80 min, 100 min, 120 min, 140 min, 160 min, 180 min, or 200 min.

[0086] In one embodiment, the preparation process of the first gallium nitride substrate is described using Fe impurity as an example. Specifically, the first gallium nitride substrate is prepared through the following steps S101-S103.

[0087] Step S101: Place the cleaned sapphire substrate into an HVPE furnace to generate a GaN substrate.

[0088] The GaN substrate is a gallium nitride substrate without Fe doping. Preferably, the layer thickness of the GaN substrate is controlled in the range of 1 μm to 5 μm, for example, the thickness of the generated GaN substrate is 1 μm, 2 μm, 3 μm, 2 μm, 4 μm or 5 μm.

[0089] In step S102, ferrocene carrier gas, ammonia and hydrogen chloride are introduced into the HVPE furnace at a temperature of 1000℃~1050℃ to generate iron-doped GaN single crystal wafers.

[0090] The flow rate of ferrocene was 100 ml / min to 120 ml / min, the flow rate of ammonia was 1000 ml / min to 1100 ml / min, and the flow rate of hydrogen chloride was 50 ml / min to 55 ml / min. Furthermore, the three gases were introduced for a total of 20 to 200 minutes.

[0091] Step S103: The sapphire substrate in the iron-doped GaN single crystal wafer is peeled off to obtain a first gallium nitride substrate doped with Fe impurities.

[0092] After growth is complete, the GaN single wafer is cooled and removed. The sapphire substrate is then removed from the GaN single wafer by peeling, yielding a first gallium nitride substrate doped with Fe impurities. This first gallium nitride substrate is a semi-insulating GaN single wafer. Preferably, the Fe doping concentration in the obtained first gallium nitride substrate is in the range of 5 × 10⁻⁶. 17 cm- 3 ~1×10 19 cm- 3 For example, 1×10 18 cm- 3 .

[0093] Preferably, the semiconductor structure layer includes a buffer layer, and the material of the buffer layer is the same as that of the compensation layer. Step S200 involves heat-treating the first gallium nitride substrate and introducing a growth source to form the gallium nitride substrate and the compensation layer, including the following steps S201-S202.

[0094] Step S201: Hydrogen gas is introduced into the growth chamber to heat-treat the first gallium nitride substrate, causing the first gallium nitride substrate to gradually decompose from the surface and enrich the surface of the remaining part of the first gallium nitride substrate with deep level acceptor impurities, thereby obtaining a second gallium nitride substrate with surface enriched with deep level acceptor impurities.

[0095] Preferably, when heat-treating the first gallium nitride substrate, the heat treatment temperature is 850℃~1100℃, and the heat treatment time is 10-600s. For example, the heat treatment temperature is 850℃, 900℃, 950℃, 1000℃, 1050℃ or 1100℃, and the heat treatment time is 10s, 20s, 50s, 100s, 2000s or 600s.

[0096] Step S202: A growth source is introduced into the growth cavity to form a gallium nitride substrate, a compensation layer, and a buffer layer that are stacked sequentially.

[0097] Preferably, step S202 includes: introducing a growth source into the growth cavity so that the deep-level acceptor impurities on the surface of the second gallium nitride substrate form a compensation layer with the growth source, and transforming the second gallium nitride substrate into a gallium nitride substrate; and continuing to introduce a growth source into the growth cavity to form a buffer layer on the compensation layer. More preferably, the thickness of the compensation layer is 20 nm to 60 nm, and the sum of the thicknesses of the buffer layer and the compensation layer is 80 nm to 120 nm.

[0098] Preferably, the preparation of the buffer layer includes: introducing a nitrogen source with a flow rate of 1500-2000 sccm, a gallium source with a flow rate of 50-100 sccm, and a carrier gas with a flow rate of 2000-3000 sccm at a temperature of 1050℃~1100℃ to deposit the buffer layer.

[0099] In this embodiment, instead of using a complex MOCVD deposition process to form the compensation layer, a simpler process can be employed. A buffer layer formed on the compensation layer improves the interfacial bonding between the channel layer and the gallium nitride substrate. After step S200, the resulting structure comprising the gallium nitride substrate 1, the compensation layer 2, and the buffer layer 31 is as follows: Figure 4 As shown.

[0100] As a specific embodiment, the compensation layer is formed by in-situ thermal decomposition, which is simple and easy to operate. Taking Fe impurities as the deep-level acceptor impurities in the gallium nitride substrate as an example, the specific implementation process of step S200 is explained, including the following steps 1-3.

[0101] Step 1: Place the first gallium nitride substrate into the MOCVD equipment.

[0102] Step 2: Hydrogen gas is introduced into the MOCVD equipment, and the MOCVD equipment is heated to a temperature between 850°C and 1100°C. The first gallium nitride substrate undergoes in-situ thermal decomposition in a hydrogen atmosphere, and the remaining Fe remains on the substrate surface after decomposition.

[0103] Specifically, before depositing the buffer layer using MOCVD, only hydrogen gas is introduced into the MOCVD equipment to heat it to a temperature between 850°C and 1100°C. The first gallium nitride substrate is then heated in situ under a hydrogen atmosphere. Through heating, GaN decomposes into metallic gallium and nitrogen gas. The decomposition chemical formula is as follows:

[0104] 2GaN(S)=2Ga(g)+N2(g)

[0105] A hydrogen atmosphere can prevent the oxidation of GaN and doped Fe impurities.

[0106] It is important to note that the heating temperature should not exceed 1100℃, as this accelerates the decomposition of gallium nitride (GaN), potentially causing the majority of the Fe-doped first GaN substrate to decompose. At heating temperatures between 850℃ and 1100℃, decomposition begins at the surface of the first GaN substrate, effectively preventing its complete decomposition. The decomposition process extends downwards from the surface, releasing nitrogen gas. The remaining metallic gallium, being liquid at high temperatures, slides off the Fe-doped first GaN substrate. Since the Fe impurities are uniformly distributed throughout the first GaN substrate, and Fe has a melting point above 1500℃ and a volatilization temperature above 2700℃, the Fe within the GaN material, due to its low saturated vapor pressure, remains on the surface of the remaining portion of the first GaN substrate, resulting in a second GaN substrate with Fe impurities enriched on its surface.

[0107] Step 3: Introduce gallium and nitrogen sources into the MOCVD equipment to deposit a buffer layer, and retain Fe on the substrate surface to form a compensation layer.

[0108] Taking GaN as an example for the buffer layer material, step 3 is explained as follows: After in-situ decomposition at high temperature for 50 seconds, gallium and nitrogen sources are introduced into the MOCVD equipment to deposit and form a GaN buffer layer. Although the remaining Fe after decomposition in step 2 is not a thin layer structure that completely covers the gallium nitride substrate, Fe impurities are enriched on the substrate surface after decomposition. Therefore, when depositing the GaN buffer layer (denoted as GaN buffer layer), a Fe-enriched compensation layer will be formed at the interface between the substrate and the GaN buffer layer.

[0109] The GaN buffer layer is formed in an MOCVD equipment using MOCVD technology. Preferably, the GaN buffer layer is deposited using a gas mixture at a temperature of 1050℃~1100℃, an ammonia flow rate of 1500sccm~2000sccm, a gallium source flow rate of 50sccm~100sccm, and a hydrogen flow rate of 2000sccm~3000sccm.

[0110] It should be noted that at temperatures between 1050℃ and 1100℃, although some GaN will decompose, the deposition rate is greater than the decomposition rate, resulting in an increasing deposition thickness and ultimately forming a GaN buffer layer. This preparation method does not require complex carbon doping processes; an Fe-enriched compensation layer can be formed during the GaN buffer layer formation process.

[0111] The above method does not require a complex C doping process; the Fe-enriched compensation layer can be formed during the formation of the buffer layer.

[0112] Preferably, the semiconductor structure layer further includes a channel layer and a barrier layer. The semiconductor structure layer is grown on a substrate with deep-level acceptor impurities on its surface. Specifically, it includes forming a channel layer and a barrier layer sequentially on a buffer layer to form the semiconductor structure layer.

[0113] More preferably, the channel layer is made of GaN. The specific process of forming the channel layer on the buffer layer is as follows: under the conditions of a temperature of 1100℃~1150℃ and a pressure of 80Torr~100Torr, a gallium source and a nitrogen source are introduced into the reaction chamber to deposit a channel layer with a thickness of 0.8-2.5μm on the buffer layer.

[0114] Further preferred materials for the barrier layer include Al. x Ga 1-x N, 0.1≤x≤0.15. The specific process of forming a barrier layer on the channel layer is as follows: under the conditions of temperature of 1060℃~1100℃ and pressure of 60Torr~80Torr, gallium source, aluminum source and nitrogen source are introduced into the reaction chamber to deposit a barrier layer with a thickness of 100-300nm on the channel layer.

[0115] Taking GaN as the material for both the buffer layer and the channel layer and AlGaN as the material for the barrier layer, the specific implementation process of step S300 is explained, which includes the following steps S301-S302.

[0116] Step S301: Continue to form a GaN channel layer on the GaN buffer layer using MOCVD technology.

[0117] To improve the quality of the formed GaN channel layer, the vapor deposition temperature can be increased. For example, in this embodiment, triethylgallium and high-purity ammonia are used as the gallium source and nitrogen source, respectively. At a temperature of 1100℃~1150℃ and a pressure of 80Torr~100Torr, a GaN channel layer with a thickness of 0.8μm~2.5μm is deposited on the GaN buffer layer using MOCVD. After this step, the resulting structure, comprising a gallium nitride substrate 1, a compensation layer 2, a buffer layer 31, and a channel layer 32, is as follows: Figure 5 As shown.

[0118] Step S302: Prepare an AlGaN barrier layer on the GaN channel layer.

[0119] In the AlGaN barrier layer, the Al content is between 10 mol% and 15 mol%. For example, the Al in the AlGaN barrier layer can be Al... 0.1 Ga 0.9 N or Al 0.15 Ga 0.85 For ease of writing, a specific content of N is abbreviated as Al. x Ga 1-x N, 0.1 ≤ x ≤ 0.15. The resulting Al x Ga 1-x The N-barrier layer and the GaN channel layer form a heterojunction structure Al x Ga 1-x NGaN, Al x Ga 1-x The N / GaN heterojunction structure generates a high concentration of two-dimensional electron gas through spontaneous polarization and piezoelectric polarization, giving gallium nitride electronic devices advantages such as high current density, low on-resistance, and high power density.

[0120] Specifically, triethylgallium, trimethylaluminum, and high-purity ammonia were used as gallium, aluminum, and nitrogen sources, respectively, to lower the formation temperature. Under conditions of 1060℃–1100℃ and 60 Torr–80 Torr, an Al layer with a thickness of 100 nm–300 nm was deposited on the GaN channel layer using MOCVD. x Ga 1-x N-type barrier layer. After this step, the resulting structure includes a gallium nitride substrate 1, a compensation layer 2, a buffer layer 31, a channel layer 32, and a barrier layer 33 as shown below. Figure 6 As shown.

[0121] Preferably, the above preparation method further includes step S400: forming a source electrode, a drain electrode and a gate electrode on the semiconductor structure layer.

[0122] More preferably, step S400 includes steps S410-S440.

[0123] Step S410: Etch the semiconductor structure layer to form a groove with a depth of 15nm-30nm.

[0124] For example, a combination of photolithography and dry etching can be used to etch the barrier layer in a semiconductor structure to form a trench with a depth of 15nm-30nm. For instance, the trench depth can be 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, 21nm, 22nm, 23nm, 24nm, 25nm, 26nm, 27nm, 28nm, 29nm, or 30nm.

[0125] Step S420, as follows Figure 2 As shown, a first dielectric layer 341 with a thickness of 2-8 nm and a second dielectric layer 342 with a thickness of 2-10 nm are sequentially deposited on the inner wall and bottom of the groove to obtain dielectric layer 34.

[0126] The first dielectric layer 341 is, for example, an aluminum oxide (Al2O3) layer, and the second dielectric layer 342 is, for example, a hafnium dioxide (HfO2) layer. The first dielectric layer 341 and the second dielectric layer 342 form a double-layer gate dielectric layer (i.e., dielectric layer 34). Specifically, in step S420, for example, an atomic layer deposition process is used, which can form a relatively dense aluminum oxide layer and a hafnium dioxide layer. The thickness of the aluminum oxide layer is, for example, 2 nm to 8 nm, and the thickness of the hafnium dioxide layer is, for example, 2 nm to 10 nm, forming a double-layer gate dielectric layer.

[0127] Step S430: Deposit a passivation layer with a thickness of 80nm-150nm on the surface of the semiconductor structure layer that is not covered by the dielectric layer; etch a portion of the passivation layer to expose the semiconductor structure layer, forming a drain region and a source region.

[0128] The passivation layer can be made of materials such as SiO2 or SiN, and its thickness can be 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm or 150nm.

[0129] Step S440: Deposit a gate electrode on the dielectric layer, and deposit a source electrode and a drain electrode in the source region and the drain region, respectively; wherein the source electrode and the drain electrode are spaced apart.

[0130] In the source region, drain region, and gate recess region, Ti / Al / Ni / Au metal combination or alloy material thereof is deposited by electron beam evaporation or sputtering process to form the source electrode, drain electrode, and gate electrode.

[0131] The technical solution of the present invention will be further described in detail below with reference to several preferred embodiments and accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Test methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions.

[0132] Example 1

[0133] The method for fabricating a gallium nitride electronic device proposed in this embodiment includes the following steps.

[0134] Step 1: At a temperature of 1000℃, a nitrogen source at a flow rate of 1000 ml / min, a chlorine source at a flow rate of 50 ml / min, and a doped iron source at a flow rate of 100 ml / min are introduced into the reaction chamber for 20 min to prepare the first gallium nitride substrate.

[0135] The first gallium nitride substrate contains Fe and Si impurities. The Fe impurities are used to compensate for the Si impurities. The concentration of Fe impurities in the first gallium nitride substrate is 5 × 10⁻⁶. 17 cm- 3 .

[0136] Step 2: Heat-treat the first gallium nitride substrate and introduce a growth source to form a stacked gallium nitride substrate, compensation layer and buffer layer.

[0137] S21: Hydrogen gas is introduced into the growth chamber to heat-treat the first gallium nitride substrate, causing the first gallium nitride substrate to gradually decompose from the surface and enrich Fe impurities on the surface of the remaining part of the first gallium nitride substrate, thereby obtaining a second gallium nitride substrate with Fe impurities enriched on the surface.

[0138] S22: A growth source is introduced into the growth chamber to form a gallium nitride substrate, a compensation layer, and a buffer layer that are stacked sequentially.

[0139] S221: At a temperature of 1050℃, a nitrogen source with a flow rate of 1500 sccm, a gallium source with a flow rate of 50 sccm, and a carrier gas with a flow rate of 2000 sccm are introduced into the growth chamber so that the Fe impurities on the surface of the second gallium nitride substrate form a compensation layer with a thickness of 20 nm with the nitrogen source and the gallium source, and the second gallium nitride substrate is transformed into a gallium nitride substrate.

[0140] S222: At a temperature of 1050℃, nitrogen source with a flow rate of 1500 sccm, gallium source with a flow rate of 50 sccm, and carrier gas with a flow rate of 2000 sccm are continuously introduced into the growth chamber to form a buffer layer with a thickness of 60 nm on the compensation layer.

[0141] Step 3: Form a channel layer and a barrier layer sequentially on the buffer layer to form a semiconductor structure layer.

[0142] S31: Under conditions of 1100℃ and 80 Torr, a gallium source and a nitrogen source are introduced into the reaction chamber to deposit a channel layer with a thickness of 0.8 μm on the buffer layer.

[0143] S32: Under conditions of 1060℃ and 60 Torr, gallium, aluminum, and nitrogen sources are introduced into the reaction chamber to deposit a 200nm thick Al material on the channel layer. 0.1 Ga 0.9 The barrier layer of N.

[0144] Step 4: Form the source electrode, drain electrode, and gate electrode on the semiconductor structure layer.

[0145] S41: Etch the semiconductor structure layer to form a trench with a depth of 15nm.

[0146] S42: A first dielectric layer with a thickness of 2nm and a second dielectric layer with a thickness of 2nm are sequentially deposited on the inner wall and bottom of the groove to obtain a dielectric layer.

[0147] S43: Deposit a passivation layer with a thickness of 80 nm on the surface of the semiconductor structure layer that is not covered by the dielectric layer; etch a portion of the passivation layer to expose the semiconductor structure layer, forming the drain region and the source region.

[0148] S44: Deposit a gate electrode on the dielectric layer, and deposit a source electrode and a drain electrode in the source region and the drain region, respectively; wherein the source electrode and the drain electrode are spaced apart.

[0149] During the formation and storage of gallium nitride substrates, Si impurities accumulate on the substrate surface. During in-situ thermal decomposition and deposition to form a buffer layer, Si impurities are present in the Fe compensation layer due to the high melting point of Si. Since Si is a shallow-level donor impurity and Fe is a deep-level acceptor impurity, the deep-level characteristics of Fe compensate for the background carrier concentration, thereby compensating for the concentration of Si impurity atoms adsorbed on the surface of the gallium nitride substrate.

[0150] Comparative Example 1-1

[0151] The method for fabricating a gallium nitride electronic device proposed in this comparative example is basically the same as that in Example 1, except that the first gallium nitride substrate prepared there is no Fe impurity.

[0152] Examples 1-2

[0153] The method for preparing a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 1, except that the heating temperature in steps S221 and S222 is 700°C.

[0154] Examples 1-3

[0155] The method for preparing a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 1, except that the heating temperature in steps S221 and S222 is 1200℃.

[0156] Examples 1-4

[0157] The method for fabricating a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 1, except that the Fe impurity concentration of the first gallium nitride substrate prepared in step 1 is 4 × 10⁻⁶.17 cm- 3 .

[0158] Examples 1-5

[0159] The method for fabricating a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 1, except that the concentration of Fe impurities in the first gallium nitride substrate prepared in step 1 is 2 × 10⁻⁶. 19 cm- 3 .

[0160] The performance characterization results of the gallium nitride electronic devices prepared in Example 1 and Comparative Examples 1-1 to 1-5 are shown in Table 1.

[0161] Table 1

[0162] project Output power Example 1 6W / mm Comparative Example 1-1 4.8W / mm Examples 1-2 5.7W / mm Examples 1-3 5.9W / mm Examples 1-4 5.8W / mm Examples 1-5 5.6W / mm

[0163] Example 2

[0164] The method for fabricating a gallium nitride electronic device proposed in this embodiment includes the following steps.

[0165] Step 1: At a temperature of 1020℃, a nitrogen source at a flow rate of 1050 ml / min, a chlorine source at a flow rate of 52 ml / min, and a doped iron source at a flow rate of 110 ml / min are introduced into the reaction chamber for a period of 100 min to prepare the first gallium nitride substrate.

[0166] The first gallium nitride substrate contains Fe impurities and shallow-level donor impurities. The Fe impurities are used to compensate for the shallow-level donor impurities. The concentration of Fe impurities in the first gallium nitride substrate is 5 × 10⁻⁶. 18 cm- 3 .

[0167] Step 2: Heat-treat the first gallium nitride substrate and introduce a growth source to form a stacked gallium nitride substrate, compensation layer and buffer layer.

[0168] S21: Hydrogen gas is introduced into the growth chamber to heat-treat the first gallium nitride substrate, causing the first gallium nitride substrate to gradually decompose from the surface and enrich Fe impurities on the surface of the remaining part of the first gallium nitride substrate, thereby obtaining a second gallium nitride substrate with Fe impurities enriched on the surface.

[0169] S22: A growth source is introduced into the growth chamber to form a gallium nitride substrate, a compensation layer, and a buffer layer that are stacked sequentially.

[0170] S221: At a temperature of 1070℃, a nitrogen source with a flow rate of 1700 sccm, a gallium source with a flow rate of 80 sccm, and a carrier gas with a flow rate of 2500 sccm are introduced into the growth chamber so that the Fe impurities on the surface of the second gallium nitride substrate form a compensation layer with a thickness of 40 nm with the nitrogen source and the gallium source, and the second gallium nitride substrate is transformed into a gallium nitride substrate.

[0171] S222: At a temperature of 1070℃, nitrogen source with a flow rate of 1700 sccm, gallium source with a flow rate of 80 sccm, and carrier gas with a flow rate of 2500 sccm are continuously introduced into the growth chamber to form a buffer layer with a thickness of 60 nm on the compensation layer.

[0172] Step 3: Form a channel layer and a barrier layer sequentially on the buffer layer to form a semiconductor structure layer.

[0173] S31: Under conditions of 1125℃ and 90 Torr, a gallium source and a nitrogen source are introduced into the reaction chamber to deposit a channel layer with a thickness of 1.5 μm on the buffer layer.

[0174] S32: Under conditions of 1080℃ and 70 Torr, gallium, aluminum, and nitrogen sources are introduced into the reaction chamber to deposit a 200nm thick Al material on the channel layer. 0.12 Ga 0.88 The barrier layer of N.

[0175] Step 4: Form the source electrode, drain electrode, and gate electrode on the semiconductor structure layer.

[0176] S41: Etch the semiconductor structure layer to form a trench with a depth of 22nm;

[0177] S42: A first dielectric layer with a thickness of 5 nm and a second dielectric layer with a thickness of 6 nm are sequentially deposited on the inner wall and bottom of the groove to obtain a dielectric layer;

[0178] S43: Deposit a passivation layer with a thickness of 115 nm on the surface of the semiconductor structure layer that is not covered by the dielectric layer; etch a portion of the passivation layer to expose the semiconductor structure layer, forming the drain region and the source region.

[0179] S44: Deposit a gate electrode on the dielectric layer, and deposit a source electrode and a drain electrode in the source region and the drain region, respectively; wherein the source electrode and the drain electrode are spaced apart.

[0180] Comparative Example 2-1

[0181] The method for preparing a gallium nitride electronic device proposed in this comparative example is basically the same as that in Example 2, except that the first gallium nitride substrate prepared there is no Fe impurity.

[0182] Example 2-2

[0183] The method for preparing a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 2, except that the heating temperature in steps S221 and S222 is 700°C.

[0184] Example 2-3

[0185] The method for preparing a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 2, except that the heating temperature in steps S221 and S222 is 1200℃.

[0186] Examples 2-4

[0187] The method for fabricating a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 2, except that the Fe impurity concentration of the first gallium nitride substrate prepared in step 1 is 4 × 10⁻⁶. 17 cm- 3 .

[0188] Examples 2-5

[0189] The method for fabricating a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 2, except that the Fe impurity concentration of the first gallium nitride substrate prepared in step 1 is 2 × 10⁻⁶. 19 cm- 3 .

[0190] The performance characterization results of the gallium nitride electronic devices prepared in Example 2 and Comparative Examples 2-1 to 2-5 are shown in Table 2.

[0191] Table 2

[0192] project Output power Example 2 10W / mm Comparative Example 2-1 8.4W / mm Example 2-2 9.8W / mm Example 2-3 9.6W / mm Examples 2-4 9.7W / mm Examples 2-5 9.5W / mm

[0193] Example 3

[0194] The method for fabricating a gallium nitride electronic device proposed in this embodiment includes the following steps.

[0195] Step 1: At a temperature of 1050℃, a nitrogen source at a flow rate of 1100 ml / min, a chlorine source at a flow rate of 55 ml / min, and a doped iron source at a flow rate of 120 ml / min are introduced into the reaction chamber for a period of 200 min to prepare the first gallium nitride substrate.

[0196] The first gallium nitride substrate contains Fe impurities and shallow-level donor impurities. The Fe impurities are used to compensate for the shallow-level donor impurities. The concentration of Fe impurities in the first gallium nitride substrate is 1 × 10⁻⁶. 19 cm- 3 .

[0197] Step 2: Heat-treat the first gallium nitride substrate and introduce a growth source to form a stacked gallium nitride substrate, compensation layer and buffer layer.

[0198] S21: Hydrogen gas is introduced into the growth chamber to heat-treat the first gallium nitride substrate, causing the first gallium nitride substrate to gradually decompose from the surface and enrich Fe impurities on the surface of the remaining part of the first gallium nitride substrate, thereby obtaining a second gallium nitride substrate with Fe impurities enriched on the surface.

[0199] S22: A growth source is introduced into the growth chamber to form a gallium nitride substrate, a compensation layer, and a buffer layer that are stacked sequentially.

[0200] S221: At a temperature of 1100℃, a nitrogen source with a flow rate of 2000 sccm, a gallium source with a flow rate of 100 sccm, and a carrier gas with a flow rate of 3000 sccm are introduced into the growth chamber so that the Fe impurities on the surface of the second gallium nitride substrate form a compensation layer with a thickness of 60 nm with the nitrogen source and the gallium source, and the second gallium nitride substrate is transformed into a gallium nitride substrate.

[0201] S222: At a temperature of 1100℃, nitrogen source with a flow rate of 2000 sccm, gallium source with a flow rate of 100 sccm, and carrier gas with a flow rate of 3000 sccm are continuously introduced into the growth chamber to form a buffer layer with a thickness of 60 nm on the compensation layer.

[0202] Step 3: Form a channel layer and a barrier layer sequentially on the buffer layer to form a semiconductor structure layer.

[0203] S31: Under conditions of 1150℃ and 100 Torr, a gallium source and a nitrogen source are introduced into the reaction chamber to deposit a channel layer with a thickness of 2.5 μm on the buffer layer.

[0204] S32: Under conditions of 1100℃ and 80 Torr, gallium, aluminum, and nitrogen sources are introduced into the reaction chamber to deposit a 300nm thick Al material on the channel layer. 0.15 Ga 0.85 The barrier layer of N.

[0205] Step 4: Form the source electrode, drain electrode, and gate electrode on the semiconductor structure layer.

[0206] S41: Etch the semiconductor structure layer to form a trench with a depth of 30nm;

[0207] S42: A first dielectric layer with a thickness of 8 nm and a second dielectric layer with a thickness of 10 nm are sequentially deposited on the inner wall and bottom of the groove to obtain a dielectric layer;

[0208] S43: Deposit a passivation layer with a thickness of 150 nm on the surface of the semiconductor structure layer that is not covered by the dielectric layer; etch a portion of the passivation layer to expose the semiconductor structure layer, forming the drain region and the source region.

[0209] S44: Deposit a gate electrode on the dielectric layer, and deposit a source electrode and a drain electrode in the source region and the drain region, respectively; wherein the source electrode and the drain electrode are spaced apart.

[0210] Comparative Example 3-1

[0211] The method for preparing a gallium nitride electronic device presented in this comparative example is basically the same as that in Example 3, except that the first gallium nitride substrate prepared there is no Fe impurity.

[0212] Example 3-2

[0213] The method for preparing a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 3, except that the heating temperature in steps S221 and S222 is 700°C.

[0214] Example 3-3

[0215] The method for preparing a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 3, except that the heating temperature in steps S221 and S222 is 1200℃.

[0216] Examples 3-4

[0217] The method for fabricating a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 3, except that the Fe impurity concentration of the first gallium nitride substrate prepared in step 1 is 4 × 10⁻⁶. 17 cm- 3 .

[0218] Examples 3-5

[0219] The method for fabricating a gallium nitride electronic device proposed in this embodiment is basically the same as that in Embodiment 3, except that the concentration of Fe impurities in the first gallium nitride substrate prepared in step 1 is 2 × 10⁻⁶. 19 cm- 3 .

[0220] Comparative Examples 3-6

[0221] The method for fabricating a gallium nitride electronic device proposed in this comparative example is basically the same as that in Example 3, except that step S21 is not included in step 2, that is, the first gallium nitride substrate is not subjected to heat treatment.

[0222] The performance characterization results of the gallium nitride electronic devices prepared in Example 3 and Comparative Examples 3-1 to 3-6 are shown in Table 3.

[0223] Table 3

[0224] project Output power Example 3 15W / mm Comparative Example 3-1 13.8W / mm Example 3-2 14.7W / mm Example 3-3 14.9W / mm Examples 3-4 14.5W / mm Examples 3-5 14.6W / mm Comparative Examples 3-6 13.2W / mm

[0225] The comparison results of Example 3 and Comparative Examples 3-6 are as follows: Figure 7 As shown. Figure 7 This shows the relationship between Fe impurity concentration and structural depth after in-situ heat treatment and without in-situ heat treatment. Figure 7 As can be seen, after in-situ heat treatment, the concentration of Fe impurities on the surface of the gallium nitride substrate increased by nearly an order of magnitude. In-situ heat treatment alone can meet the preparation requirements well, without the need for more complex processes.

[0226] Combining Tables 1, 2, and 3, the following conclusions can be drawn. Compared to gallium nitride electronic devices using undoped gallium nitride substrates, the gallium nitride electronic devices using Fe-doped gallium nitride substrates in this application achieve a significant increase in output power, with an improvement of up to 25%; and 5×10 17 cm- 3 ~1×10 19 cm- 3 Within a certain range, the higher the Fe doping concentration, the higher the output power of gallium nitride electronic devices; when the Fe doping concentration is higher than 1×10⁻⁶, the higher the output power of the devices. 19 cm- 3 or less than 5×10 17 cm- 3 This can lead to a decrease in the output power of the prepared gallium nitride electronic devices. When heating gallium nitride substrates in a hydrogen atmosphere: both excessively high and excessively low heating temperatures will result in a decrease in the output power of the prepared gallium nitride electronic devices; the highest output power of gallium nitride electronic devices is obtained when the heating temperature is in the range of 850℃ to 1100℃.

[0227] This invention provides a gallium nitride (GaN) electronic device and its fabrication method. Addressing the problem that reducing the concentration of impurity atoms adsorbed on the surface of the gallium nitride substrate leads to severe leakage current and low output power in existing GaN HEMT devices, this invention proposes a method that introduces metal impurities onto the surface of the gallium nitride substrate to form a metal-doped gallium nitride substrate, instead of carbon doping. This method utilizes Fe... 3+ / Fe 2+The characteristics of the main energy level are used to compensate for the background carrier concentration, thereby compensating for the concentration of impurity atoms, especially Si atoms, adsorbed on the surface of the gallium nitride substrate, thus solving the problems existing in the prior art. Furthermore, in-situ heating (heating temperature controlled at 850-1100℃) can be used to thermally decompose the metal-doped gallium nitride substrate in a hydrogen atmosphere, causing the metal impurities to decompose at high temperature and remain on the substrate surface, achieving effective compensation for Si, avoiding many challenges brought about by carbon doping, and thus simplifying the fabrication process.

[0228] The gallium nitride electronic device fabrication method provided in this invention effectively improves the electrical performance at the interface, is simple and easy to implement, and has low cost. It solves the problem of parasitic conductive channels caused by Si impurities. It avoids the limitations of traditional surface treatment methods (cleaning) and provides a more effective impurity compensation scheme, offering a new approach to improving the performance of GaN-based HEMT devices.

[0229] It should be understood that the above embodiments are merely illustrative of the technical concept and features of the present invention, and are intended to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be construed as limiting the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.

Claims

1. A gallium nitride electronic device, comprising a gallium nitride substrate and a semiconductor structure layer disposed on the gallium nitride substrate; characterized in that: The surface of the gallium nitride substrate has shallow-level donor impurities and deep-level acceptor impurities. The deep-level acceptor impurities are used to compensate for the concentration of shallow-level donor impurities adsorbed on the surface of the gallium nitride substrate. The deep-level acceptor impurities are metallic impurities introduced into the surface of the gallium nitride substrate through doping. The deep-level acceptor impurities are Fe impurities, Ni impurities, or Mn impurities. The shallow-level donor impurities are Si impurities. A compensation layer is provided at the interface between the gallium nitride substrate and the semiconductor structure layer. The concentration of deep-level acceptor impurities in the compensation layer is greater than the concentration of deep-level acceptor impurities in the gallium nitride substrate. The thickness of the compensation layer is 20 nm to 60 nm.

2. The gallium nitride electronic device according to claim 1, characterized in that, The melting point of the deep-level acceptor impurity is greater than the decomposition temperature of gallium nitride. And / or, the material of the compensation layer includes GaN; And / or, the concentration of Fe impurities in the gallium nitride substrate is 5 × 10⁻⁶. 17 cm -3 ~1×10 19 cm -3 ; And / or, the concentration of Fe impurities in the compensation layer is 5 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 ; And / or, the formation temperature of the compensation layer is 850℃~1100℃.

3. The gallium nitride electronic device according to claim 1, characterized in that, The semiconductor structure layer includes a buffer layer, a channel layer, and a barrier layer sequentially disposed along a direction away from the gallium nitride substrate, wherein the barrier layer has a groove; The semiconductor structure layer further includes a dielectric layer and a passivation layer. The dielectric layer is disposed on the inner wall and bottom of the groove, and the passivation layer is disposed on the barrier layer. The gallium nitride electronic device further includes a source electrode, a drain electrode, and a gate electrode, wherein the gate electrode covers the dielectric layer; the source electrode and the drain electrode are disposed on the side of the barrier layer away from the gallium nitride substrate and are spaced apart. The buffer layer and the channel layer are made of GaN; and / or the barrier layer is made of AlGaN; and / or the sum of the thicknesses of the buffer layer and the compensation layer is 80nm~120nm.

4. A method for fabricating a gallium nitride electronic device, characterized in that, include: A first gallium nitride (GaN) substrate is provided; wherein the surface of the first GaN substrate has shallow-level donor impurities and deep-level acceptor impurities, and the deep-level acceptor impurities are metallic impurities, which are used to compensate for the concentration of shallow-level donor impurities adsorbed on the surface of the GaN substrate, and the deep-level acceptor impurities are introduced into the surface of the GaN substrate by doping; the deep-level acceptor impurities are Fe impurities, Ni impurities, or Mn impurities; and the shallow-level donor impurities are Si impurities; The first gallium nitride substrate is heat-treated and a growth source is introduced to form a gallium nitride substrate and a compensation layer. A semiconductor structure layer is formed on the compensation layer; The concentration of deep-level acceptor impurities in the compensation layer is greater than that in the gallium nitride substrate; the thickness of the compensation layer is 20 nm to 60 nm.

5. The preparation method according to claim 4, characterized in that, The semiconductor structure layer includes a buffer layer, the buffer layer being made of the same material as the compensation layer; the step of heat-treating the first gallium nitride substrate and introducing a growth source to form the gallium nitride substrate and the compensation layer includes: Hydrogen gas is introduced into the growth chamber to heat-treat the first gallium nitride substrate, causing the first gallium nitride substrate to gradually decompose from the surface and enrich the deep-level acceptor impurities on the surface of the remaining part of the first gallium nitride substrate, thereby obtaining a second gallium nitride substrate with the deep-level acceptor impurities enriched on the surface. The growth source is introduced into the growth cavity to form the gallium nitride substrate, the compensation layer, and the buffer layer, which are stacked sequentially.

6. The preparation method according to claim 5, characterized in that, The step of introducing the growth source into the growth cavity to form the gallium nitride substrate, the compensation layer, and the buffer layer stacked sequentially includes: The growth source is introduced into the growth cavity so that the deep-level acceptor impurities on the surface of the second gallium nitride substrate form the compensation layer with the growth source, and the second gallium nitride substrate is transformed into the gallium nitride substrate. The growth source is continued to be introduced into the growth chamber to form the buffer layer on the compensation layer; The combined thickness of the buffer layer and the compensation layer is 80nm~120nm.

7. The preparation method according to claim 6, characterized in that, The growth source includes a gallium source and a nitrogen source, and the preparation of the buffer layer includes: The buffer layer is deposited by introducing a nitrogen source with a flow rate of 1500-2000 sccm, a gallium source with a flow rate of 50-100 sccm, and a carrier gas with a flow rate of 2000-3000 sccm at a temperature of 1050℃~1100℃.

8. The preparation method according to claim 4, characterized in that, The deep-level acceptor impurity is an Fe impurity, and the fabrication process of the first gallium nitride substrate is as follows: Under the condition of 1000℃~1050℃, a nitrogen source with a flow rate of 1000ml / min~1100ml / min, a chlorine source with a flow rate of 50ml / min~55ml / min, and a doped iron source with a flow rate of 100ml / min~120ml / min are introduced into the reaction chamber to prepare the first gallium nitride substrate. The catalytic injection time is 20 min to 200 min, and the Fe impurity concentration in the first gallium nitride substrate is 5 × 10⁻⁶. 17 cm -3 ~1×10 19 cm -3 .

9. The preparation method according to claim 5, characterized in that, In the heat treatment process, the heat treatment temperature is 850℃~1100℃; And / or, the semiconductor structure layer further includes a channel layer and a barrier layer, wherein the semiconductor structure layer is grown on the substrate whose surface is enriched with deep-level acceptor impurities, specifically including: The channel layer and the barrier layer are sequentially formed on the buffer layer, thereby forming the semiconductor structure layer; And / or, the method further includes: A source electrode, a drain electrode, and a gate electrode are formed on the semiconductor structure layer.

10. The preparation method according to claim 9, characterized in that, The channel layer is made of GaN; Under conditions of 1100℃~1150℃ and 80Torr~100Torr, a gallium source and a nitrogen source are introduced into the reaction chamber to deposit a channel layer with a thickness of 0.8-2.5μm on the buffer layer. And / or, the material of the barrier layer includes Al. x Ga 1-x N, 0.1 ≤ x ≤ 0.15; Under conditions of temperature of 1060℃~1100℃ and pressure of 60Torr~80Torr, a gallium source, an aluminum source and a nitrogen source are introduced into the reaction chamber to deposit a barrier layer with a thickness of 100-300nm on the channel layer. And / or, the formation of the source electrode, drain electrode, and gate electrode on the semiconductor structure layer includes: The semiconductor structure layer is etched to form a groove with a depth of 15nm-30nm; A first dielectric layer with a thickness of 2-8 nm and a second dielectric layer with a thickness of 2-10 nm are sequentially deposited on the inner wall and bottom of the groove to obtain a dielectric layer; A passivation layer with a thickness of 80nm-150nm is deposited on the surface of the semiconductor structure layer that is not covered by the dielectric layer; a portion of the passivation layer is etched to expose the semiconductor structure layer, forming a drain region and a source region; The gate electrode is deposited on the dielectric layer, and the source electrode and the drain electrode are deposited in the source region and the drain region, respectively; wherein the source electrode and the drain electrode are spaced apart.