Woven hole abrasive cloth and preparation method thereof

CN120755805APending Publication Date: 2025-10-10ZIBO RIKEN MT COATED ABRASIVES
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511057826.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-30
Publication Date
2025-10-10

AI Technical Summary

Technical Problem

Traditional abrasive cloth has technical bottlenecks such as dust clogging, poor heat dissipation, and workpiece burns during the grinding process. Existing improvement methods lead to problems such as dust accumulation, high production energy consumption, increased VOC emissions, and poor grinding performance.

Method used

The composite structure of substrate layer, base adhesive layer, abrasive layer and top adhesive layer is adopted. The substrate layer forms through-holes. The holes and micropores work together, combined with epoxy adhesive and specific abrasive to form an effective dust removal and adsorption path, enhance air circulation, reduce dust and increase cutting volume.

Benefits of technology

Effectively reduce dust volume, increase cutting capacity, reduce workpiece burns and scratches, simplify production processes, and reduce energy consumption and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005524901970000071
    Figure BDA0005524901970000071
  • Figure HDA0005524901980000011
    Figure HDA0005524901980000011
  • Figure HDA0005524901980000012
    Figure HDA0005524901980000012
Patent Text Reader

Abstract

The invention relates to the technical field of abrasive cloth, in particular to woven abrasive cloth and a preparation method thereof. Comprising a base material layer, a bottom adhesive layer, an abrasive material layer and a composite adhesive layer, the base material layer is formed by weaving fibers and forms pore channels penetrating through the base material layer, and the pore channels are parallel to the thickness direction of the base material layer. The base material layer is formed by weaving fibers and forms the pore channels penetrating through the base material layer, and the pore channels are parallel to the thickness direction of the base material layer, so that the problems of burn rate and scratch of a workpiece can be effectively solved; the hole diameter of the hole channels is 2-6 mm, the porosity is 20-60%, and the dust amount in the polishing process can be effectively reduced by matching with micropores formed among the fibers, and meanwhile the cutting amount is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of abrasive cloth, and in particular to a woven abrasive cloth and a preparation method thereof. Background Art

[0002] Traditional emery cloth faces three major technical bottlenecks during the grinding process: dust clogging, poor heat dissipation, and workpiece burns. Currently, air permeability is mainly improved by adding a backing fleece layer or punching, but this leads to the following defects: conventional backing fleece lacks a systematic dust exhaust channel and relies solely on post-punching. The insufficient porosity causes dust accumulation to be more than three times that of the embodiment; multi-layer substrates require adhesive bonding, increasing production energy consumption and VOC emissions; existing paper-based emery cloth is too hard and aggravates scratches, while cloth-based emery cloth is soft but has poor grinding performance. In addition, high grinding temperatures can easily cause workpiece burns, seriously affecting processing quality.

[0003] Chinese invention patent CN108608343B discloses a manufacturing process for ceramic corundum abrasive cloth. The process includes the following steps: Step 1: producing the grey cloth; Step 2: obtaining the raw cloth; Step 3: stretching and shaping; Step 4: backfilling; Step 5: frontfilling; Step 6: applying primer; Step 7: electrostatic sanding; Step 8: pre-drying; Step 9: gluing; Step 10: drying; Step 11: curing; and Step 12: bending. The abrasive cloth produced by this method uses ceramic corundum in its abrasive layer, which effectively increases the cloth's grinding life and provides excellent cutting force. However, it does not address technical issues such as dust clogging, poor heat dissipation, and workpiece burns. Summary of the Invention

[0004] The first aspect of the present invention provides a woven abrasive cloth, comprising a substrate layer, a base glue layer, an abrasive layer and a double glue layer that are compositely connected in sequence; the substrate layer is woven from fibers and forms channels that penetrate the substrate layer, and the channels are parallel to the thickness direction of the substrate layer.

[0005] The pore size of the pores is 2-6 mm, and the porosity is 20-60%.

[0006] Optionally, the pore size of the pores is 2-4 mm, and the porosity is 20-50%.

[0007] Micropores are formed between the fibers in the substrate layer, and the diameter of the micropores is 10-100 μm.

[0008] The pores have a diameter of 2-6mm and a porosity of 20-60%. Combined with the micropores formed between the fibers, they effectively reduce dust production during the grinding process while increasing stock removal. The pores serve as the primary dust removal pathway, utilizing the centrifugal force generated by high-speed rotation during grinding to eject coarse grinding debris. The micropores serve as a secondary adsorption pathway, adsorbing fine dust particles <10μm through a capillary network formed by the interwoven warp yarns. The high surface energy of the micropores effectively prevents dust from escaping. The pores and micropores work together to generate a dynamic airflow circulation enhancement effect: as the substrate heats and expands during grinding, the expansion of the macropores increases air convection, forming a closed-loop airflow that draws in cool air and discharges hot dust.

[0009] Further research found that by controlling the pore size of the micropores to 10-100μm, the cutting amount can be increased while maintaining the mechanical properties of the gauze. This may be because the epoxy glue forms a certain differential phase between the micropores, avoiding excessive stress at the pore connections caused by excessive porosity.

[0010] The base adhesive layer is prepared from epoxy adhesive.

[0011] Optionally, the raw materials for preparing the epoxy adhesive include epoxy resin with an epoxy equivalent weight of 170-200 g / eq.

[0012] Optionally, the epoxy resin includes bisphenol A epoxy resin.

[0013] Optionally, the epoxy resin has an epoxy equivalent weight of 176-184 g / eq, model NPEL-127E, and is purchased from Nan Ya, Taiwan, China.

[0014] The epoxy adhesive further comprises an epoxy resin curing agent and an epoxy diluent.

[0015] The epoxy resin curing agent includes one or more of ethylenediamine, diethylenetriamine and polyamide among aliphatic polyamines.

[0016] The epoxy diluent includes one or more of butanone, n-butanol, toluene, alkylene glycidyl ether, and trimethylolpropane triglycidyl ether.

[0017] The abrasive layer is composed of abrasives that meet the following parameters: average particle size 150-450 mesh, Mohs hardness ≥ 8.5, specific gravity 1.53-1.99 g / cm 3 .

[0018] The abrasive includes at least one of brown corundum, single crystal corundum, white corundum, calcined corundum and silicon carbide.

[0019] The glue solution raw material of the sizing layer comprises, by weight parts, phenolic resin 80-120 parts, urea-formaldehyde resin 10-30 parts, amino resin 10-30 parts, filler 10-50 parts, defoaming agent 0.1-2 parts, leveling agent 0.1-2 parts, water-based color paste 0.5-3 parts, and water 1-10 parts.

[0020] The weight ratio of the phenolic resin, urea-formaldehyde resin and amino resin is 10:(1-3):(1-3).

[0021] The viscosity of the phenolic resin at 25 DEG C is 1000-1500 mPa s.

[0022] Optionally, the viscosity of the phenolic resin at 25 DEG C is 1100-1300 mPa s.

[0023] The viscosity of the urea-formaldehyde resin at 25 DEG C is 200-500 mPa s.

[0024] Optionally, the viscosity of the urea-formaldehyde resin at 25 DEG C is 200-400 mPa s.

[0025] The viscosity of the amino resin at 25 DEG C is 600-1000 mPa s.

[0026] Optionally, the viscosity of the amino resin at 25 DEG C is 700-1000 mPa s.

[0027] The leveling agent comprises octyl polymethylsiloxane.

[0028] The filler comprises at least one of calcium carbonate, wollastonite, kaolin, titanium white powder and sepiolite.

[0029] The second aspect of the application provides a preparation method of the woven hole abrasive cloth, comprising the following steps: coating epoxy glue on a substrate layer to form a primer layer; implanting abrasive on the primer layer to bond with the primer layer to form an abrasive layer; and coating glue solution of a sizing layer on the abrasive layer to obtain the woven hole abrasive cloth after solidification.

[0030] Advantages

[0031] 1. The substrate layer is woven by fibers and forms channels penetrating through the substrate layer, and the channels are parallel to the thickness direction of the substrate layer, which can effectively solve the problem of workpiece burn rate and scratches.

[0032] 2. The channel has a pore size of 2-6 mm and a porosity of 20-60%, and cooperates with the micropores formed between the fibers to effectively reduce the amount of dust in the polishing process and improve the cutting amount.

[0033] 3. By controlling the pore size of the micropores to be 10-100 μm, the cutting amount can be improved while the mechanical properties of the gauze are maintained.

[0034] 4. By limiting the glue liquid raw materials and composition of the double-layer glue, the number of scratches and the degree of clogging can be effectively reduced.

[0035] 5. The preparation method of the present invention is simple and can be used for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is the front side of the woven abrasive cloth prepared in Example 1 (with the adhesive layer on top).

[0037] Figure 2 This is the back side of the woven abrasive cloth prepared in Example 1 (the substrate layer is on top). DETAILED DESCRIPTION

[0038] Example 1

[0039] A woven abrasive cloth consists of a base layer (100g mesh polyester backing cloth, purchased from Zhangjiagang Yuxing Warp Knitting Mesh Cloth Factory), a base rubber layer, an abrasive layer and a double rubber layer that are connected in sequence; the base layer is woven from fibers and forms channels that penetrate the base layer, and the channels are parallel to the thickness direction of the base layer.

[0040] The pore diameter of the pore channel is 3 mm, and the porosity is 30%.

[0041] Micropores are formed between the fibers in the substrate layer, and the pore diameter of the micropores is 50 μm.

[0042] The base adhesive layer is made from epoxy adhesive; the raw materials for preparing the epoxy adhesive are, by weight, 100 parts of epoxy resin, 25 parts of epoxy resin curing agent (ethylenediamine), and 5 parts of epoxy resin diluent (toluene: butanone weight ratio = 1:1). The epoxy resin has an epoxy equivalent weight of 176-184 g / eq and is model NPEL-127E, purchased from Nan Ya in Taiwan, China.

[0043] The abrasive layer is composed of abrasive (single crystal corundum) that meets the following parameters: average particle size 180 mesh, Mohs hardness ≥ 8.5, specific gravity 1.53-1.99 g / cm 3 , purity ≥97wt%, iron oxide content ≤0.2wt%, purchased from Zhengzhou Xinrui Wear-Resistant Materials Co., Ltd.

[0044] The raw materials of the adhesive liquid of the adhesive layer are as follows by weight: 100 parts of phenolic resin, 10 parts of urea-formaldehyde resin, 30 parts of amino resin, 40 parts of filler (calcium carbonate and titanium dioxide are mixed in a mass ratio of 3:1), 0.5 parts of defoaming agent (tributyl phosphate), 0.5 parts of leveling agent (octyl polymethylsiloxane), 1.5 parts of water-based color paste and 5.5 parts of water.

[0045] Among them, phenolic resin: PR-G-350, purchased from Nantong Sumitomo Bakelite Co., Ltd., has a viscosity of 1250 mPa·s at 25°C; urea-formaldehyde resin: urea-formaldehyde resin 801104A, purchased from Taier Adhesive (Guangdong) Co., Ltd., has a viscosity of 280 mPa·s at 25°C; amino resin has a viscosity of 800 mPa·s at 25°C, purchased from Foshan Wengkaier Trading Co., Ltd., model CYMEL385.

[0046] A method for preparing a woven abrasive cloth comprises the following steps: applying epoxy glue on a base material layer to form a base glue layer; implanting abrasives on the base glue layer by an electrostatic sand implanting machine, bonding the abrasives to the base glue layer to form an abrasive layer; applying glue of a secondary glue layer on the abrasive layer, drying and solidifying the glue, and then cutting the glue cloth to obtain a woven abrasive cloth. Figure 1 As shown, the back side Figure 2 shown.

[0047] Example 2

[0048] A woven abrasive cloth consists of a base layer (100g mesh polyester backing cloth, purchased from Zhangjiagang Yuxing Warp Knitting Mesh Cloth Factory), a base rubber layer, an abrasive layer and a double rubber layer that are connected in sequence; the base layer is woven from fibers and forms channels that penetrate the base layer, and the channels are parallel to the thickness direction of the base layer.

[0049] The pore diameter of the pore channel is 3 mm, and the porosity is 30%.

[0050] Micropores are formed between the fibers in the substrate layer, and the pore diameter of the micropores is 50 μm.

[0051] The base adhesive layer is made from epoxy adhesive; the raw materials for preparing the epoxy adhesive are, by weight, 100 parts epoxy resin, 80 parts epoxy resin curing agent (polyamide), and 5 parts epoxy resin diluent (n-butanol: butanone weight ratio = 1:1). The epoxy resin has an epoxy equivalent weight of 176-184 g / eq and is model NPEL-127E, purchased from Nan Ya in Taiwan, China.

[0052] The abrasive layer is composed of abrasive (calcined corundum) that meets the following parameters: average particle size 180 mesh, Mohs hardness ≥ 8.5, specific gravity 1.53-1.99 g / cm 3 , purity ≥97wt%, iron oxide content ≤0.2wt%, purchased from Zhengzhou Xinrui Wear-Resistant Materials Co., Ltd.

[0053] The raw materials of the adhesive liquid of the adhesive layer are as follows by weight: 100 parts of phenolic resin, 20 parts of urea-formaldehyde resin, 20 parts of amino resin, 30 parts of filler (calcined kaolin), 0.5 parts of defoaming agent (tributyl phosphate), 0.5 parts of leveling agent (octyl polymethylsiloxane), 1.5 parts of water-based color paste and 5.5 parts of water.

[0054] Among them, phenolic resin: WL-1808 was purchased from Puyang Weilin Technology Co., Ltd., with a viscosity of 1200 mPa·s at 25°C; urea-formaldehyde resin: urea-formaldehyde resin 801104A was purchased from Taier Adhesive (Guangdong) Co., Ltd., with a viscosity of 280 mPa·s at 25°C; amino resin has a viscosity of 800 mPa·s at 25°C, purchased from Foshan Wengkaier Trading Co., Ltd., model CYMEL385.

[0055] A preparation method of woven abrasive cloth comprises the following steps: coating epoxy glue on a base material layer to form a base glue layer; implanting abrasives on the base glue layer by an electrostatic sand implanting machine, bonding the abrasives to the base glue layer to form an abrasive layer; coating the abrasive layer with glue liquid of a secondary glue layer, drying and curing the glue liquid, and then cutting the glue cloth to obtain the woven abrasive cloth.

[0056] Example 3

[0057] A woven abrasive cloth consists of a base layer (100g mesh polyester backing cloth, purchased from Zhangjiagang Yuxing Warp Knitting Mesh Cloth Factory), a base rubber layer, an abrasive layer and a double rubber layer that are connected in sequence; the base layer is woven from fibers and forms channels that penetrate the base layer, and the channels are parallel to the thickness direction of the base layer.

[0058] The pore diameter of the pore channel is 3 mm, and the porosity is 30%.

[0059] Micropores are formed between the fibers in the substrate layer, and the pore diameter of the micropores is 50 μm.

[0060] The base adhesive layer was prepared from epoxy adhesive; the raw materials for preparing the epoxy adhesive were, by weight, 100 parts of epoxy resin, 25 parts of epoxy resin curing agent (diethylenetriamine), and 5 parts of epoxy resin diluent (trimethylolpropane triglycidyl ether). The epoxy resin, with an epoxy equivalent weight of 176-184 g / eq and model number NPEL-127E, was purchased from Nan Ya in Taiwan, China.

[0061] The abrasive layer is composed of abrasive (brown corundum) that meets the following parameters: average particle size 180 mesh, Mohs hardness ≥ 8.5, specific gravity 1.53-1.99 g / cm 3 , purity ≥97wt%, iron oxide content ≤0.2wt%, purchased from Zhengzhou Xinrui Wear-Resistant Materials Co., Ltd.

[0062] The raw materials of the adhesive liquid of the adhesive layer are as follows by weight: 100 parts of phenolic resin, 30 parts of urea-formaldehyde resin, 10 parts of amino resin, 30 parts of filler (kaolin and titanium dioxide mixed in a mass ratio of 3:1), 0.5 parts of defoaming agent (tributyl phosphate), 0.5 parts of leveling agent (octyl polymethylsiloxane), 1 part of water-based color paste and 6 parts of water.

[0063] Among them, phenolic resin: PR-G-350, purchased from Nantong Sumitomo Bakelite Co., Ltd., has a viscosity of 1250 mPa·s at 25°C; urea-formaldehyde resin: urea-formaldehyde resin 801104A, purchased from Taier Adhesive (Guangdong) Co., Ltd., has a viscosity of 280 mPa·s at 25°C; amino resin has a viscosity of 800 mPa·s at 25°C, purchased from Foshan Wengkaier Trading Co., Ltd., model CYMEL385.

[0064] A preparation method of woven abrasive cloth comprises the following steps: coating epoxy glue on a base material layer to form a base glue layer; implanting abrasives on the base glue layer by an electrostatic sand implanting machine, bonding the abrasives to the base glue layer to form an abrasive layer; coating the abrasive layer with glue liquid of a secondary glue layer, drying and curing the glue liquid, and then cutting the glue cloth to obtain the woven abrasive cloth.

[0065] Comparative Example 1

[0066] The specific implementation is the same as Example 1; the difference is that the substrate layer (without pores) in Comparative Example 1: 100g polyester back fleece, purchased from Zhangjiagang Yuxing Warp Knitting Mesh Fabric Factory.

[0067] Comparative Example 2

[0068] The specific embodiment is the same as Example 1; the difference is that the substrate layer in Comparative Example 2 is a paper base (RF-110g blue latex paper purchased from Ahlstrom, France)

[0069] Comparative Example 3

[0070] The specific implementation is the same as Example 1; the difference is that the substrate layer in Comparative Example 3 is a cloth base (pure cotton cloth base, RMC-515K, purchased from Henan Jurui Abrasives Co., Ltd.).

[0071] Performance testing methods

[0072] The abrasive cloths in the examples and comparative examples were subjected to the following performance tests, and the test data are listed in Table 1.

[0073] 1. Grinding Performance Test: Grind the above discs at a fixed speed and pressure on a car repair putty plate. The grinding effect is determined by the amount of grinding performed per unit time. The grinding amount is measured in grams; the greater the grinding amount, the better the grinding effect.

[0074] 2. Dust Collection Test: After grinding, the machine is left in a closed space for a fixed period of time. The dust collected is then weighed to determine the dust collection effect. The lighter the weight, the better the dust collection effect. Dust collection is measured in grams for grinders with suction function.

[0075] 3. Sand surface anti-clogging test: After grinding, observe the sand surface for clogging by putty powder. The less surface clogging, the better the anti-clogging effect. Sand surface clogging degree: The percentage of sand surface clogging to surface area.

[0076] 4. Comparative analysis of energy saving and environmental protection: Compared with similar back velvet products produced by traditional technology, the energy saving and environmental protection effects are analyzed from the perspective of saved production links and materials.

[0077] 5. Scratch test: After grinding, measure the average scratch value Ra and the maximum scratch value Rz of the ground material. The smaller the value, the smaller the scratch.

[0078] 6. Workpiece Burn Rate: After the test, observe the burn rate of the stainless steel workpiece being ground at 10,000 rpm. Ten burns are counted as a group. The fewer burns, the better the effect. The test is graded from 0 to 10, with 0 representing no burns, indicating the best burn prevention effect; 10 represents irreparable burns, indicating the worst effect.

[0079] Performance test data

[0080] Table 1

[0081]

[0082] Comparative Example 1 is a similar commercially available velvet-coated abrasive product. Unlike the examples, this product lacks mesh-like velvet bases, lacking the micropores and larger diamond-shaped and circular channels on the surface. Instead, it features a few holes punched in later. Comparative testing revealed that this product produced three times more dust and had abrasive surface clogging than the examples. Comparative Example 2 is a similar commercially available velvet-coated abrasive product. Unlike the examples, this product uses a paper base as the base for the primer, with the velvet cloth attached to the back. This product exhibited poor flexibility, with scratches exceeding 30% of those observed in the examples. Comparative Example 3 is a similar commercially available velvet-coated abrasive product. Unlike the examples, this product uses a cloth base as the base for the primer, with the velvet cloth attached to the back. This product exhibited better flexibility, but exhibited over 20% lower abrasive removal than the examples.

[0083] Comparative Example 1 includes an additional punching step, which wastes raw materials and increases labor and material resources. Comparative Examples 2 and 3 are similar commercially available suede-backed coated abrasive products. They differ from the examples in that the cloth / paper base serves as the base for the primer coating, and the suede backing is adhered to the back of the cloth / paper base. These Comparative Examples 2 and 3 waste the cloth / paper base, and the adhesive and diluent used in the bonding process between the cloth / paper base and the suede backing contribute to environmental pollution and are not environmentally friendly.

Claims

1. A woven abrasive cloth, characterized in that: It includes a substrate layer, a base adhesive layer, an abrasive layer and a double adhesive layer which are compositely connected in sequence; the substrate layer is woven from fibers and forms channels that penetrate the substrate layer, and the direction of the channels is parallel to the thickness direction of the substrate layer.

2. The woven abrasive cloth according to claim 1, characterized in that: The pore size of the pores is 2-6 mm, and the porosity is 20-60%.

3. The woven abrasive cloth according to claim 2, characterized in that: Micropores are formed between the fibers in the substrate layer, and the diameter of the micropores is 10-100 μm.

4. The woven abrasive cloth according to claim 1 or 3, characterized in that: The base adhesive layer is prepared from epoxy adhesive.

5. The woven abrasive cloth according to claim 4, characterized in that: The raw materials for preparing the epoxy adhesive include epoxy resin with an epoxy equivalent weight of 170-200 g / eq.

6. The perforated abrasive cloth according to claim 5, characterized in that: The abrasive layer is composed of abrasives that meet the following parameters: average particle size 150-450 mesh, Mohs hardness ≥ 8.5, specific gravity 1.53-1.99 g / cm 3 .

7. The perforated abrasive cloth according to claim 6, characterized in that: The adhesive liquid raw materials of the adhesive layer include, by weight, 80-120 parts of phenolic resin, 10-30 parts of urea-formaldehyde resin, 10-30 parts of amino resin, 10-50 parts of filler, 0.1-2 parts of defoaming agent, 0.1-2 parts of leveling agent, 0.5-3 parts of water-based color paste and 1-10 parts of water.

8. The perforated abrasive cloth according to claim 7, characterized in that: The weight ratio of the phenolic resin, the urea-formaldehyde resin and the amino resin is 10:(1-3):(1-3).

9. The perforated abrasive cloth according to claim 7, characterized in that: The filler includes at least one of calcium carbonate, wollastonite, kaolin, titanium dioxide, and sepiolite.

10. A method for preparing the perforated abrasive cloth according to any one of claims 7 to 9, characterized in that: The following steps are involved: The epoxy adhesive is coated on the base material layer to form a base adhesive layer; an abrasive is implanted on the base adhesive layer and bonded to the base adhesive layer to form an abrasive layer; the adhesive liquid of the secondary adhesive layer is coated on the abrasive layer and cured to obtain a woven abrasive cloth.

Citation Information

Patent Citations

  • A manufacturing process for ceramic corundum abrasive cloth

    CN108608343B