A multilayer encapsulation material and encapsulation method for solid-state batteries

By using multi-layer encapsulation materials and plasma activation treatment, the problems of electrode expansion and low thermal management efficiency in all-solid-state batteries during cycle use have been solved, thereby improving the structural stability, thermal management performance and environmental tolerance of the battery, and ensuring the long-term safety and reliability of the battery.

CN120784529BActive Publication Date: 2026-11-17ZHONGSHAN BASD CHEM TECH CO LTD +5
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510988862.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-07-17
Publication Date
2026-11-17
Estimated Expiration
2045-07-17

AI Technical Summary

Technical Problem

During cycling, all-solid-state batteries suffer from structural deformation due to electrode expansion, separation of electrodes from current collectors, reaction between encapsulation materials and electrolytes, and internal gas generation. These issues affect the battery's cycle performance and safety. Furthermore, their low thermal management efficiency and poor environmental tolerance result in a fragile and easily cracked battery structure, limiting their performance improvement and industrialization process.

Method used

A multi-layer encapsulation structure consisting of a silicone-bonded base layer, a polyurethane buffer layer, and a polyurea protective layer is adopted. The interface bonding is enhanced through plasma activation treatment to construct a gradient functional layer, thereby achieving a synergistic improvement in mechanical buffering, thermal conduction, and chemical protection.

Benefits of technology

It significantly improves the battery's structural stability, thermal management performance, and environmental tolerance, reduces the risk of internal short circuits, extends battery life, and enhances battery reliability in harsh environments such as high temperature and high humidity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application discloses a multilayer encapsulation material and encapsulation method for solid-state batteries. The multilayer encapsulation material includes a silicone bonding base layer, which is coated onto the outer surface of the solid-state battery by a spraying process, with a thickness of 50-100 μm; a polyurethane buffer layer, which is coated onto the outer surface of the silicone bonding base layer after plasma activation treatment and thinning, with a thickness of 2-6 mm; and a polyurea protective layer, which is wrapped around the outside of the polyurethane buffer layer, with a thickness of 0.5-1.5 mm. This application focuses on the synergistic effect of silicone, polyurethane and polyurea composite materials to solve the three core problems in the field of solid-state battery encapsulation: insufficient structural stability, low thermal management efficiency and poor environmental tolerance. Through material modification, structural gradient optimization and process innovation, the mechanical buffering, thermal conductivity and chemical protection of the battery encapsulation layer are synergistically improved, thereby improving the safety, energy density and cycle life of solid-state batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of all-solid-state battery packaging technology, and in particular to a multilayer packaging material and packaging method for solid-state batteries. Background Technology

[0002] Solid-state batteries, by using solid electrolytes instead of traditional liquid electrolytes, effectively avoid the risks of electrolyte leakage, volatilization, and combustion, thus improving the intrinsic safety of the battery. However, solid-state batteries still face multiple technical challenges in application. During battery cycling, the electrode materials repeatedly expand, which can lead to delamination between the electrodes and current collectors, causing deformation of the internal electrode structure, electrode pulverization, and increased contact resistance, significantly affecting the battery's cycle performance and lifespan. Therefore, a certain amount of elastic pressure needs to be introduced before battery molding to effectively alleviate the electrode expansion problem and solve the capacity decay problem caused by cycling. Simultaneously, the electrolyte and electrode materials inside the battery may react chemically with the encapsulation material, leading to swelling, corrosion, or cracking of the encapsulation material. This not only affects the encapsulation effect but may also cause serious safety hazards such as internal short circuits, greatly reducing the battery's reliability and lifespan. Furthermore, during charging and discharging, a certain amount of gas is generated inside the solid-state battery, causing an increase in internal pressure. This requires the encapsulation material to have good high-pressure resistance to prevent deformation or cracking of the battery casing and ensure the integrity and safety of the battery structure. Solid-state batteries also exhibit brittleness, making them prone to cracking during volume expansion and contraction cycles. When significant pressure is applied to the cell, dimensional differences between the positive electrode, solid electrolyte membrane, and negative electrode create interlayer porosity, leading to electrode breakage and short circuits. Simultaneously, these dimensional differences generate shear stress at the electrode edges, causing edge tearing and penetration of the solid electrolyte layer, resulting in structural defects and further exacerbating short circuits, severely impacting electrochemical performance. Furthermore, during heat sealing of the encapsulation material at high temperatures, moisture in the resin film constituting the substrate layer rapidly vaporizes. Even after cooling, moisture may remain between resin film layers, affecting encapsulation quality. These technical challenges severely restrict the performance improvement and industrialization of solid-state batteries. Summary of the Invention

[0003] This application provides a multilayer encapsulation material and method for solid-state batteries. It constructs a gradient functional layer consisting of a silicone bonding base layer, a polyurethane buffer layer, and a polyurea protective layer through material modification. This achieves a structurally optimized composite structure with a 50-100μm silicone bonding layer, a 2-6mm polyurethane buffer layer, and a 0.5-1.5mm polyurea protective layer. Furthermore, it employs innovative process technology, introducing plasma activation treatment to enhance interfacial bonding. This systematically solves the problems of insufficient structural stability (effectively mitigating delamination and pulverization caused by electrode cyclic expansion through the gradient buffer structure), low thermal management efficiency (significantly improving interfacial thermal conductivity through multilayer synergistic design), and poor environmental tolerance in the field of solid-state battery encapsulation (comprehensively blocking electrolyte corrosion and gas permeation through material modification). It achieves a synergistic improvement and balanced optimization of the mechanical buffering, thermal conductivity, and chemical protection of the battery encapsulation layer, providing a reliable guarantee for the long-term stable operation of all-solid-state batteries. The technical solution provided in this application is as follows: On one hand, this application provides a multilayer encapsulation material for solid-state batteries, comprising: A silicone bonding base layer is sprayed and coated onto the outer surface of the solid-state battery, with a thickness of 50-100μm. A polyurethane buffer layer is applied to the outer surface of the silicone bonding base layer after it has been thinned by plasma activation treatment, and the thickness of the layer is 2-6 mm. A polyurea protective layer, with a thickness of 0.5-1.5 mm, is wrapped around the outside of the polyurethane buffer layer.

[0004] In one exemplary embodiment, the silicone-bonded base layer is composed of silicone containing silica microspheres, wherein the content of the silica microspheres is 2-4% of the total mass of the silicone, and their particle size is 20-60 μm, pore size is 10-21 nm, and specific surface area is 170-260 m² / g.

[0005] In one exemplary embodiment, the polyurethane buffer layer comprises a combination of polyether polyols, polymethylene polyphenyl isocyanates, a catalyst, and a blowing agent.

[0006] In one exemplary embodiment, the polyurethane buffer layer further comprises thermally conductive ceramic particles, wherein the thermally conductive ceramic particles are selected from one or more materials selected from alumina, aluminum nitride, boron nitride, beryllium oxide, zinc oxide, titanium dioxide, and magnesium dioxide.

[0007] In one exemplary embodiment, the thermally conductive ceramic particle material comprises boron nitride and aluminum oxide, wherein the content of boron nitride is 1-4% and the content of aluminum oxide is 1-2%; and the lateral dimension of the boron nitride nanosheets is 0.5-2.5 μm.

[0008] On the other hand, this application also provides a solid-state battery packaging method, including: Silicone containing 2-4% silica microspheres is atomized and sprayed onto the outer surface of the solid-state battery to form a silicone bonding base layer; The silicone bonding substrate is thinned by plasma activation treatment, with a thinning thickness of 2-21 μm. Polyurethane is foamed and thermocured on the thinned silicone-bonded base layer to form a polyurethane buffer layer; A polyurea protective layer is formed by spraying polyurea onto the outside of the polyurethane buffer layer.

[0009] In one exemplary embodiment, the silica microspheres have a particle size of 20-60 μm, and the thickness is reduced by 0.2-0.3 times the particle size of the silica microspheres. After thinning, the surface roughness Ra of the silicone bonding substrate is 1.0-1.5 μm.

[0010] In one exemplary embodiment, the atomization pressure of the silicone containing 2-4% silica microspheres during the spraying process is 0.3-0.6MPa, and the droplet size of the silicone containing 2-4% silica microspheres after atomization is <50μm. The spraying distance between the spray gun and the surface of the solid-state battery is 150-250mm.

[0011] In one exemplary embodiment, the plasma activation treatment uses a 2-(5:1) Ar / O2 mixture, a power of 250-350W, and a treatment time of 10-25s.

[0012] In one exemplary embodiment, the polyurethane foam mixing pressure is 10-15 MPa, the material temperature is 25-30°C, the mold temperature is 40-50°C, and the curing time is 8-15 min.

[0013] By adopting the above technical solution, the solid-state battery multilayer encapsulation material and encapsulation method provided in this application have the following beneficial effects: 1. Significantly improve structural stability: By constructing a gradient functional layer of silicone bonding base layer / polyurethane buffer layer / polyurea protective layer, and optimizing the design of a composite structure of 50-100μm silicone bonding layer, 2-6mm polyurethane buffer layer and 0.5-1.5mm polyurea protective layer, the peeling and pulverization phenomenon caused by electrode cyclic expansion is effectively alleviated, the structural integrity of the battery in long-term charge and discharge cycles is greatly improved, and the battery life is extended.

[0014] 2. Optimize thermal management performance: Enhance the synergy of interfacial thermal conduction through multi-layer collaborative design, significantly improve the thermal conduction efficiency of the encapsulation material, improve the internal heat distribution of the solid-state battery, reduce thermal stress accumulation, and improve the thermal stability of the battery under high-rate charge and discharge conditions, thereby enhancing the safety and reliability of the battery.

[0015] 3. Enhanced environmental resistance: Plasma activation treatment enhances interfacial bonding, and material modification gives the encapsulation layer excellent chemical corrosion resistance. It can completely block electrolyte penetration and gas diffusion, effectively prevent swelling, corrosion or cracking of the encapsulation material, avoid battery performance degradation caused by environmental factors, and improve the long-term stability of the battery under complex working conditions.

[0016] 4. Achieve synergistic performance optimization: Through the organic combination of material modification, structural optimization and process innovation, the encapsulation layer simultaneously possesses excellent mechanical buffering, efficient thermal conductivity and outstanding chemical protection, solving the problem of insufficient single performance of traditional encapsulation materials, providing all-round protection for all-solid-state batteries and significantly improving the overall performance of the battery.

[0017] 5. Ensure long-term stable operation of the battery: The multi-layer packaging structure can effectively alleviate electrode expansion, block corrosive media, withstand high-pressure environments, reduce the risk of internal short circuits, and improve the reliability of the battery in harsh environments such as high temperature and high humidity, providing reliable technical support for the industrial application of all-solid-state batteries. Detailed Implementation

[0018] The technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0019] For the terms defined below, unless a different definition is given elsewhere in the claims or this specification, these definitions shall apply. All numerical values, whether explicitly indicated or not, are defined herein as being modified by the term "about." The term "about" generally refers to a range of numerical values ​​that a person skilled in the art would consider equivalent to the stated values ​​to produce substantially the same properties, functions, results, etc. A range of numerical values ​​indicated by a low value and a high value is defined as including all numerical values ​​included within that range and all subranges included within that range.

[0020] It should be noted that the terms "first," "second," etc., used in the specification and claims of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion.

[0021] This application provides a solid-state battery multilayer encapsulation material, comprising: A silicone bonding base layer is sprayed and coated onto the outer surface of the solid-state battery, with a thickness of 50-100μm. A polyurethane buffer layer, with a thickness of 2-6mm, is wrapped around the outer surface of the silicone bonding base layer after it has been thinned by plasma activation treatment. A polyurea protective layer, wrapped around the outside of the polyurethane buffer layer, has a thickness of 0.5-1.5 mm.

[0022] Specifically, material gradient optimization can improve encapsulation reliability. Among these, silicone-bonded base layers have significant advantages as direct contact layers: Firstly, the siloxane skeleton itself exhibits strong inertness to most chemicals (including acids, alkalis, salts, and polar solvents). Its low-reactivity groups (saturated alkyl or aryl groups such as methyl or phenyl) and saturated chemical structure are less likely to react with active components such as lithium metal compared to the ester and urea bonds of polyurethane / polyurea. This effectively avoids the breakage of C=O or CO bonds caused by the strong reducing properties of lithium metal, as well as the generation of amine molecules or CO2 gas due to high-temperature chain scission. This avoids issues such as the reaction of polar groups (-NH-) with Li2S to form Li-NS compounds. Meanwhile, silica gel exhibits stable electrochemical performance, is more resistant to oxidation under high voltage, does not decompose to produce gas, does not react with lithium metal or lithium-intercalated anodes, and does not trigger the decomposition of sulfide electrolytes, thus significantly reducing the risks of corrosion, gas generation, short circuits, swelling, and rupture. Furthermore, the spraying process allows silica gel to be uniformly sprayed onto the surface of the solid-state battery in a non-contact manner as atomized micron-sized droplets. This avoids damage to the brittle solid-state electrolyte or thin electrodes without the need for pressurization or high-temperature heating. Additionally, the low-viscosity silica gel before atomization is subjected to shear force... With its drastically reduced viscosity, silicone can penetrate like water into the gaps between electrode particles, interlayer interface defects, and pores caused by dimensional differences between the positive and negative electrodes and the solid electrolyte membrane. This allows for bubble-free filling by expelling air. The silicone component in the gaps not only provides microscopic elastic buffering but also reduces the possibility of the battery extending from the gaps as the starting point for cracks. Furthermore, compared to liquid polymer wetting, which is difficult to fully fill the defects of microporous structures, spraying can achieve thin-layer application of silicone. Moreover, silicone has a lower curing shrinkage rate than materials such as polyurethane and polyurea. The thin-layer design further reduces the risk of curing shrinkage cracking the interface or creating new pores. At the same time, silicone's resistance to high and low temperatures (-50~200℃) and resistance to damp heat can maintain the bonding strength throughout the battery's entire life cycle, avoiding sealing failure caused by aging and cracking. The elastic thin layer formed by it is tightly bonded to the solid-state battery, providing excellent elastic buffering performance. In addition, pure silicone, as an excellent electrical insulator, has extremely low ionic conductivity, further reducing the possibility of the encapsulation material itself acting as an ion transport path or causing leakage. Together with the outer polyurethane buffer layer and polyurea protective layer, it achieves a balanced optimization of mechanical buffering, thermal conductivity, and chemical protection.

[0023] In one exemplary embodiment, the silicone-bonded base layer is composed of silicone containing silica microspheres, wherein the silica microspheres comprise 2-4% of the total mass of the silicone, have a particle size of 20-60 μm, a pore size of 10-21 nm, and a specific surface area of ​​170-260 m² / g. The mesoporous structure introduced by the silica microspheres provides highly efficient adsorption capacity, effectively adsorbing gases generated during the charging and discharging of solid-state batteries and the volume changes caused by repeated electrode expansion. This provides ample buffer space for gas release and mechanical deformation, improving the stability of the encapsulation material-electrode interface and reducing the generation of interfacial porosity and cracks. Simultaneously, the introduction of silica microspheres reduces the content of organic groups in the silicone, enhancing the overall chemical inertness of the material and improving its resistance to electrolyte corrosion and chemical reactions. Furthermore, the soft elasticity of the silicone matrix and the rigidity of the silica microspheres complement each other, constructing multiple mechanical buffering mechanisms at the interface. This ensures close contact between the encapsulation material and the electrode while effectively absorbing and dispersing mechanical stress, further enhancing interfacial stability.

[0024] In one exemplary embodiment, the polyurethane buffer layer comprises a combination of polyether polyols, polymethylene polyphenyl isocyanates, a catalyst, and a blowing agent. Specifically, the blowing agent is selected from at least one of pentane, HFC-245fa, HFO-1234yf, HFO-1233zd, R600 / R600a, and R290 as an environmentally friendly blowing agent. A high-density urethane foam structure is constructed by combining the polyether polyol and polymethylene polyphenyl isocyanates under catalytic reaction conditions, achieving precise control of the foam density within the range of 80-200 kg / m³. Its dense microstructure with a closed-cell rate >90% reduces the thermal conductivity to ≤23 mW / (m·K), improving mechanical cushioning performance.

[0025] In one exemplary embodiment, the polyurethane buffer layer further comprises thermally conductive ceramic particles, wherein the thermally conductive ceramic particles are selected from one or more materials selected from alumina, aluminum nitride, boron nitride, beryllium oxide, zinc oxide, titanium dioxide, and magnesium dioxide. By uniformly dispersing highly thermally conductive ceramic particles in the polymer matrix, an efficient heat conduction network is constructed, which can effectively disperse the local heat generated during battery charging and discharging, prevent excessive temperature gradients caused by heat accumulation, and thus improve the overall thermal management efficiency of the battery. At the same time, the introduction of these highly thermally conductive ceramic particles significantly improves the intrinsic thermal conductivity of the polyurethane buffer layer and enhances the dielectric strength of the material through the particle filling effect, providing a buffer protection layer for solid-state batteries with both excellent thermal conductivity and electrical insulation properties, effectively solving the problems of heat accumulation and electric field concentration inside the battery.

[0026] In one exemplary embodiment, the thermally conductive ceramic particle material includes boron nitride and aluminum oxide, wherein the content of boron nitride is 1-4% and the content of aluminum oxide is 1-2%; and the lateral size of the boron nitride nanosheets is 0.5-2.5 μm. This composite thermal conductivity system uses boron nitride as the main framework material, leveraging its extremely high thermal conductivity, excellent insulation, and lubrication properties to construct a highly efficient heat conduction network. Simultaneously, alumina is used to fill the gaps between the boron nitride flake particles, utilizing the cost-effectiveness of alumina while effectively supporting the main framework material, thus improving the overall thermal conductivity of the polyurethane buffer layer. Specifically, the existing preparation process results in alumina particles exhibiting a wide distribution, allowing for a denser packing structure of large and small particles (large spheres + small spheres). The two work synergistically to construct a continuous thermal conductivity pathway, significantly shortening the heat conduction path within the polymer matrix. Furthermore, the nano-boron nitride flakes and nano-alumina particles form a multi-layered physical barrier. This increases the electron flow path and makes water and gas diffusion more tortuous, significantly improving the polyurethane layer's water vapor permeability and electrical insulation properties. It also promotes uniform heat distribution within the material, effectively preventing localized overheating and achieving a uniform heat distribution effect. This allows the composite system to quickly reach a temperature equilibrium state, reducing the internal temperature gradient and improving the thermal management efficiency and long-term reliability of solid-state batteries during charging and discharging.

[0027] This application also provides a solid-state battery packaging method, including: Silicone containing 2-4% silica microspheres is atomized and sprayed onto the outer surface of the solid-state battery to form a silicone bonding base layer; Plasma activation treatment was used to thin the silicone bonding substrate, with a reduction thickness of 2-21 μm. Polyurethane is foamed and thermocured on a thinned silicone-bonded substrate to form a polyurethane buffer layer. A polyurea protective layer is formed by spraying polyurea onto the outside of the polyurethane buffer layer.

[0028] Specifically, atomized spraying technology is used to uniformly coat the outer surface of the solid-state battery with functionalized liquid silicone (including liquid silicone, addition-curing silicone, or condensation-curing silicone, etc., suitable for spraying) containing 2-4% silica microspheres, forming a silicone bonding base layer with a thickness of 50-100μm. This spraying technology forms micron-sized droplets and sprays them onto the battery surface in a non-contact manner, without the need for pressurization or high-temperature heating of the substrate, effectively avoiding damage to the brittle solid electrolyte or thin electrodes. At the same time, the viscosity of the low-viscosity silicone drops sharply under the atomization shear force, allowing it to penetrate like water into the gaps between electrode particles, interlayer interface defects, and micron-sized pores caused by size differences between the positive and negative electrodes and the solid electrolyte film, thus expelling air. Achieving bubble-free filling not only provides a microscopic elastic buffer for the battery but also reduces the risk of crack propagation caused by gaps. Compared to traditional impregnation processes, spraying allows for the application of thinner silicone layers (50-100μm), and the curing shrinkage rate of silicone is lower than that of materials such as polyurethane and polyurea. The thin-layer design further reduces the risk of interfacial tearing or the formation of new voids due to curing shrinkage. By precisely controlling the thickness and surface roughness of this silicone layer, not only is the interfacial bonding strength with the polyurethane buffer layer enhanced, avoiding poor bonding or chemical reaction problems, but an effective barrier is also formed to prevent internal material reactions, gas generation, or crack propagation, achieving effective isolation between the internal and external environments and enabling operation even during frequent battery deformation. (e.g., maintaining stable barrier performance during charge-discharge cycles); further, plasma activation treatment is used to selectively thin the silicone bonding base layer (thinning thickness precisely controlled within the range of 2-21 μm). Through the dual effects of surface activation and thinning, the interfacial bonding strength with the polyurethane buffer layer is improved, reducing the risk of delamination; subsequently, liquid polyurethane raw materials with excellent flowability are used for foaming and thermosetting, achieving uniform encapsulation while fully wetting the battery surface, providing excellent bonding strength; the polyurethane buffer layer, with its compression resilience, high elastic modulus, and high elongation at break characteristics, can effectively resist external impacts and adapt to the deformation caused by the drastic expansion of the electrodes and battery charge-discharge cycles, maintaining stable sealing pressure over a long period of time. The polyurethane buffer layer, with a thickness of 2-6mm, achieves a balance between buffering forces and uniform heat diffusion, effectively mitigating battery expansion and preventing heat accumulation. Finally, a 0.5-1.5mm thick polyurea protective layer is applied using a spraying process. This polyurea protective layer has excellent weather resistance (stable operation within the range of -40℃ to 120℃), high impact resistance (tensile strength ≥25MPa), and good barrier properties, effectively isolating moisture and chemical corrosion. This reduces the risk of short circuits in the battery cell and prevents moisture from penetrating into the polyurethane foam layer. This constructs a multi-layered encapsulation system from micro-buffering to macro-protection, comprehensively improving the structural stability, environmental adaptability, and safety performance of solid-state batteries.

[0029] In one exemplary embodiment, the silica microspheres have a particle size of 20-60 μm, and the thickness is reduced by 0.2-0.3 times the particle size of the silica microspheres. After thinning, the surface roughness Ra of the silicone bonded substrate is 1.0-1.5 μm. By precisely controlling the plasma activation thinning process, the surface of the silicone-bonded substrate is thinned to a thickness range of 0.2-0.3 times the particle size of silica microspheres (i.e., 4-18 μm), resulting in a surface roughness Ra of 1.0-1.5 μm for the thinned silicone layer. This thinning process exposes some silica microspheres on the surface, forming rigid particles of suitable height. These rigid particles of porous silica microspheres undergo multiple physical interactions with the polyurethane foam, including penetration, bonding, and mechanical interlocking, forming a strong anchoring effect. In particular, the thinned interface region forms a three-phase interwoven composite structure of silicone (soft matrix), porous silica microspheres (rigid particles), and polyurethane (elastomer), constructing an overlapping interface transition region from soft to hard. This structural design not only enhances the interfacial bonding force but also effectively disperses stress concentration through the rigid-flexible interface transition, significantly reducing the risk of cracking at the interface and providing a reliable guarantee for the structural stability of the battery during long-term cycling.

[0030] In one exemplary embodiment, the atomization pressure of the silicone containing 2-4% silica microspheres during spraying is 0.3-0.6 MPa, resulting in a droplet size of <50 μm after atomization. By precisely controlling the spraying process parameters and setting the atomization pressure of the silicone containing 2-4% silica microspheres to 0.3-0.6 MPa, the droplet size of the atomized silicone is controlled within the range of less than 50 μm. This optimized atomization parameter ensures that the droplets have a suitable size distribution and kinetic energy, guaranteeing both uniform atomization effect and optimal performance. Stability also gives the droplets sufficient penetrability, allowing them to effectively penetrate the gaps between electrode particles, interlayer interface defects, and micron-sized pores (including micropore structures) caused by size differences between the positive and negative electrodes and the solid electrolyte membrane, achieving comprehensive and sufficient filling. Small-diameter droplets exhibit stronger surface tension and wettability during spraying, enabling them to closely conform to the substrate contour and effectively expel air to form a bubble-free filling effect. At the same time, the micron-sized droplets match the internal microstructure of the battery, achieving uniform coverage at the microscale without damaging the brittle solid electrolyte and thin electrodes.

[0031] The spraying distance between the spray gun and the solid-state battery surface is 150-250mm. This appropriate spraying distance ensures that the atomized silicone droplets have suitable flight time and diffusion space, allowing the droplets to be evenly distributed on the battery surface. This improves the uniformity of the coating layer and avoids the problem of the film being too thin or incomplete coverage due to excessive distance. At the same time, this distance range effectively prevents liquid flow rebound and splashing, and controls the droplet impact force within an appropriate range. This ensures that sufficient kinetic energy penetrates into the gaps between electrode particles, interlayer interface defects, and micron-level pores caused by size differences between the positive and negative electrodes and the solid electrolyte film, while avoiding mechanical damage to the brittle solid electrolyte and thin electrodes.

[0032] In one exemplary embodiment, the plasma activation treatment uses a 2-(5:1) Ar / O2 mixture, with a power of 250-350W and a treatment time of 10-25s. Preferably, the Ar / O2 mixture ratio is 4:1, the power is 300W, and the treatment time is 30s. Using high-purity argon as the main carrier gas ensures stable plasma excitation. The introduction of trace amounts of oxygen can precisely etch low-activity saturated alkyl functional groups such as methyl or phenyl groups on the silicone surface without over-oxidizing and damaging the silicone bulk structure. At the same time, a certain number of polar groups (such as hydroxyl and carboxyl groups) can be controllably generated, improving the chemical activity of the silicone surface. The power range of 250-350W ensures that the plasma density reaches the optimal balance point, which not only ensures sufficient energy density for surface chemical modification but also avoids over-etching and thermal damage caused by high power. The precise treatment time of 10-25s achieves the optimal match between surface modification and structural integrity, resulting in a uniform micro-rough structure on the silicone surface while avoiding material degradation caused by long-term treatment.

[0033] In one exemplary embodiment, the polyurethane foam mixing pressure is 10-15 MPa, the material temperature is 25-30°C, the mold temperature is 40-50°C, and the curing time is 8-15 min. Specifically, the foam mixing pressure is preferably 13 MPa. High-pressure mixing ensures sufficient contact and rapid reaction between the combined polyether polyol and the polymethylene polyphenyl isocyanate. Precise control of the material temperature and mold temperature optimizes the foaming reaction kinetics, promoting uniform and dense cell structure. The short curing cycle of 8-15 min ensures full cross-linking of the urethane molecular chains while improving production efficiency.

[0034] The following detailed description of examples of the present invention is exemplary and is used only to explain the present invention, and should not be construed as limiting the present invention.

[0035] Example 1 A multilayer encapsulation material for solid-state batteries comprises a silicone bonding base layer, a polyurethane buffer layer, and a polyurea protective layer sequentially coated on the outer surface of the solid-state battery. The silicone bonding base layer has a thickness of 78 μm and uses silicone containing silica microspheres as the matrix, with 2.6% by mass of boron nitride (nanofibers with a lateral dimension of 2.1 μm) and 1.7% by mass of alumina added. The silica microspheres account for 3.5% of the total mass of the silicone, with a particle size of 46 μm, a pore size of 16.5 nm, and a specific surface area of ​​235 m² / g. The polyurethane buffer layer has a thickness of 3.5 mm and uses a combination of polyether polyol, polymethylene polyphenyl isocyanate, triethylenediamine, and stannous octoate catalyst, as well as pentane, HFC-245fa, HFO-1234yf, HFO-1233ZD, R600 / R600a, and R290 as foaming agents. The polyurea protective layer has a thickness of 1.2 mm and uses commercially available polyurea products that meet performance requirements.

[0036] A solid-state battery encapsulation method comprises the following steps: First, silicone containing 3.5% silica microspheres is atomized and sprayed onto the outer surface of the solid-state battery to form a silicone bonding base layer. During the spraying process, the atomization pressure is controlled at 0.45 MPa, and the droplet size of the atomized silicone coating is controlled below 50 μm. The spraying distance between the spray gun and the solid-state battery surface is set to 210 mm. Subsequently, plasma activation treatment is performed using an Ar / O2 mixed gas (volume ratio 2:3) at a power of 310 W for 14 s, thinning the silicone bonding base layer by 15 μm, resulting in a surface roughness Ra of 1.2 μm. Next, polyurethane is foamed and thermocured on the thinned silicone bonding base layer to form a polyurethane buffer layer. The high pressure of the polyurethane foaming mixture is 13 MPa, the material temperature is 26 °C, the mold temperature is 45 °C, and the curing time is 10 min. Finally, polyurea is sprayed onto the outside of the polyurethane buffer layer to form a polyurea protective layer, completing the encapsulation.

[0037] Example 2 The solid-state battery multilayer encapsulation material of Example 1 differs in that boron nitride and aluminum oxide are not added to the silicone bonding layer.

[0038] Example 3 The solid-state battery multilayer encapsulation material of Example 1 is similar, except that the mass percentage of silica microspheres is 1.1% of the total mass of silicone.

[0039] Example 4 The solid-state battery multilayer encapsulation material of Example 1 is similar, except that the particle size of the silica microspheres is 13 μm.

[0040] Example 5 The solid-state battery encapsulation method of Example 1 is similar, except that the atomization pressure during the silicone atomization spraying process is 0.25 MPa.

[0041] Example 6 The solid-state battery encapsulation method of Example 1 is similar, except that the spraying distance between the spray gun and the surface of the solid-state battery is 305mm.

[0042] Example 7 The solid-state battery packaging method of Example 1 is similar, except that the power of the plasma activation treatment is 170W and the treatment time is 40s.

[0043] Comparative Example 1 Referring to the solid-state battery multilayer encapsulation material of Example 1, the difference is that the encapsulation material does not contain a silicone bonding base layer, and a polyurethane buffer layer and a polyurea protective layer are directly coated on the outer surface of the solid-state battery in sequence.

[0044] Comparative Example 2 The solid-state battery multilayer encapsulation material of Example 1 is similar, except that the thickness of the silicone bonding base layer is 34 μm.

[0045] Comparative Example 3 The solid-state battery encapsulation method of Example 1 differs in that the silicone bonding substrate does not contain silica microspheres.

[0046] Comparative Example 4 The solid-state battery encapsulation method of Example 1 is different in that the silicone bonding base layer is not thinned.

[0047] Test case The encapsulated solid-state batteries prepared in Examples 1-7 and Comparative Examples 1-4 were characterized, including mechanical integrity, barrier performance, thermal stability, interfacial bonding strength, surface roughness, electrochemical performance, and shock resistance of the buffer layer. Mechanical integrity was assessed by observing for defects such as expansion, bulging, or delamination of the electrodes after 100 charge cycles to verify the stability of the electrode structure during long-term charge-discharge. Barrier performance was characterized by two indicators: oxygen permeability (OTR ≤ 0.01 cm³ / (m²·day·atm)) and water vapor permeability (WVTR ≤ 0.05 g / (m²·day)), measured using the isobaric method / differential pressure method and the electrolytic method / infrared detection method, respectively, to ensure the stability of the battery's internal environment. Thermal stability was tested using a thermogravimetric analyzer (TGA) at 150°C. The following parameters were assessed: material quality changes to evaluate high-temperature resistance; interfacial bonding strength was determined by peel test to measure the peel force between the silicone bonding base layer and the battery casing (≥5 N / cm) to ensure interface firmness; surface roughness was measured using a surface profilometer to detect the Ra value (≤1.5 μm) of the silicone bonding base layer surface after plasma treatment to optimize coating adhesion; electrochemical performance was evaluated by the capacity retention rate (≥95%) after 100 charge-discharge cycles at 1C to assess battery cycle life; and the impact resistance of the buffer layer was verified by testing the surface of the polyurethane buffer layer for cracking at 5J impact energy. The results of mechanical integrity characterization are detailed in Table 1, barrier performance characterization in Table 2, thermal stability (mass change at 150℃) characterization in Table 3, interfacial bonding strength characterization in Table 4, surface roughness (Ra / μm) characterization in Table 5, electrochemical performance characterization in Table 6, and buffer layer impact resistance characterization in Table 7.

[0048] Table 1 Mechanical Integrity Test Results

[0049] Table 2 Barrier Performance Test Results

[0050] Table 3 Thermal stability test results

[0051] Table 4. Results of interfacial bonding strength test

[0052] Table 5 Surface roughness test results

[0053] Table 6 Electrochemical performance test results

[0054] Table 7. Impact Resistance Test Results of the Buffer Layer

[0055] Based on the test results of Examples 1-7 and Comparative Examples 1-4, it can be seen that Example 1 exhibits the best performance in mechanical integrity, barrier properties, thermal stability, interfacial bonding strength, surface roughness, electrochemical performance, and impact resistance of the buffer layer. After 100 cycles, the structure remains intact, with an oxygen permeability of only 0.0012 cm³ / (m²·day·atm), a water vapor permeability of 0.028 g / (m²·day), a mass change of only 0.24% at 150℃, a peel strength of 8.2 N / cm, a surface roughness Ra of only 0.89 μm, a capacity retention of 99.4%, and no damage after a 5J impact. When the silicone bonding layer lacks boron nitride and alumina (Example 2), reduces the proportion of silica microspheres (Example 3), or reduces the particle size (Example 4), all properties deteriorate to varying degrees (e.g., slight cracking of mechanical integrity, and an OTR (Optical Time Tolerance) increase to 0.0036 - 0.0041). While reducing atomizing pressure (Example 5), increasing spraying distance (Example 6), or adjusting plasma treatment parameters (Example 7) did not cause serious defects, some indicators such as barrier performance and interfacial bonding strength were slightly inferior to Example 1. Comparative Example 1, due to the complete elimination of the silicone bonding base layer, exhibited the worst performance, with severe cracking, an OTR as high as 0.0123 cm³ / (m²·day·atm), and a peel force of only 4.5 N / cm. Comparative Examples 2-4, due to the thinning of the base layer (Comparative Example 2), the absence of silica microspheres (Comparative Example 3), or the lack of thinning treatment (Comparative Example 4), showed significant deterioration in various performance aspects, especially in mechanical integrity and barrier performance. This verifies that the material composition (boron nitride / alumina additive), structural parameters (silica microsphere ratio / particle size), and preparation process (atomizing pressure / spraying distance / plasma treatment) of the silicone bonding base layer are key factors determining the encapsulation effect, and their optimized combination can improve the long-term stability and safety of solid-state batteries.

Claims

1. A multilayer encapsulation material for solid-state batteries, characterized in that, include: A silicone bonding base layer is sprayed and coated onto the outer surface of the solid-state battery, with a thickness of 50-100μm. A polyurethane buffer layer is wrapped around the outer surface of the silicone bonding base layer after it has been thinned by plasma activation treatment, and its thickness is 2-6mm; wherein, the plasma activation treatment uses a 2-(5:1) Ar / O2 mixed gas, the power is 250-350W, and the treatment time is 10-25s; A polyurea protective layer, wrapped around the outside of the polyurethane buffer layer, has a thickness of 0.5-1.5 mm; The silicone bonding base layer is composed of silicone containing silica microspheres, wherein the content of the silica microspheres is 2-4% of the total mass of the silicone, and their particle size is 20-60 μm, pore size is 10-21 nm, and specific surface area is 170-260 m². 2 / g; The thickness of the silicone bonding base layer is reduced by 0.2-0.3 times the particle size of the silica microspheres, and the surface roughness Ra of the thinned silicone bonding base layer is 1.0-1.5 μm; The polyurethane buffer layer comprises thermally conductive ceramic particles, the thermally conductive ceramic particle material comprising boron nitride and alumina, wherein the content of boron nitride is 1-4% and the content of alumina is 1-2%; and the lateral dimension of the boron nitride nanosheets is 0.5-2.5 μm.

2. The multilayer encapsulation material according to claim 1, characterized in that, The polyurethane buffer layer also includes a combination of polyether polyols, polymethylene polyphenyl isocyanates, catalysts, and foaming agents.

3. A solid-state battery encapsulation method, used to prepare the solid-state battery multilayer encapsulation material according to any one of claims 1-2, characterized in that, include: Silicone containing 2-4% silica microspheres is atomized and sprayed onto the outer surface of the solid-state battery to form a silicone bonding base layer; The silicone bonding substrate is thinned by plasma activation treatment, with a thinning thickness of 2-21 μm. Polyurethane is foamed and thermocured on the thinned silicone-bonded base layer to form a polyurethane buffer layer; A polyurea protective layer is formed by spraying polyurea onto the outside of the polyurethane buffer layer.

4. The packaging method according to claim 3, characterized in that, The silica gel containing 2-4% silica microspheres has an atomization pressure of 0.3-0.6MPa during the spraying process, and the droplet size of the silica gel containing 2-4% silica microspheres after atomization is <50μm. The spraying distance between the spray gun and the surface of the solid-state battery is 150-250mm.

5. The packaging method according to claim 3, characterized in that, The polyurethane foam mixing pressure is 10-15 MPa, the material temperature is 25-30℃, the mold temperature is 40-50℃, and the curing time is 8-15 min.

Citation Information

Patent Citations

  • Material with high heat conductivity coefficient sprayed or soaked on surface of battery shell

    CN111799531A

  • Single battery and battery module

    CN217788559U

  • Bonding of polyurethane to silicone rubber

    US4312693A