High-stability methanol fuel catalyst and preparation method thereof
By combining TiO2@Al2O3 core-shell support and mesoporous SiO2 shell, the stability and anti-sintering problems of existing methanol fuel catalysts are solved, achieving high-efficiency methanol conversion and anti-poisoning capabilities, and possessing reversible regeneration characteristics.
Patent Information
- Application Number
- CN202510980323.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-16
- Publication Date
- 2025-10-17
- Estimated Expiration
- 2045-07-16
AI Technical Summary
Existing methanol fuel catalysts have significant bottlenecks in terms of long-term operational stability and anti-sintering properties. In particular, metal nanoparticles are prone to aggregation under high temperature and dynamic operating conditions, and the high-temperature phase transformation of the support leads to a sharp drop in specific surface area. Alloying is costly and difficult to scale up.
A mesoporous SiO2 shell was prepared by combining a TiO2@Al2O3 core-shell carrier, block copolymer P123, 3-aminopropyltriethoxysilane, H2PtCl6·6H2O, ascorbic acid and ethylenediamine through weak acid precipitation-calcination. Platinum atoms were anchored to the pore wall surface in the form of N2O2 or O4. Multiple interface modulations were combined to suppress the migration and aggregation of platinum atoms.
The catalyst achieves stability and anti-poisoning ability in the methanol conversion environment, has reversible regeneration characteristics, reduces the risk of platinum atom migration and sintering, and improves catalytic activity and anti-carbon deposition performance.
Smart Images

Figure CN120790139A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the field of fuel catalysts, in particular to a high-stability methanol fuel catalyst and a preparation method thereof. BACKGROUND
[0002] As a liquid hydrogen carrier, the efficient catalytic conversion of methanol is the key to hydrogen energy economy and portable energy systems. Existing catalysts are mainly divided into two categories: methanol reforming catalysts, mainly Cu / ZnO / Al2O3, Pd / ZnO or Pt-based catalysts, which produce hydrogen through methanol steam reforming (MSR) or partial oxidation (POX); DMFC anode catalysts, represented by PtRu / C, which directly catalyze the electrochemical oxidation of methanol. Although the above-mentioned catalysts have achieved industrial application, there are significant bottlenecks in long-term operation stability, and the core problems are concentrated in the sintering and aggregation of active components: high-temperature structural instability: at the reforming reaction temperature (200-350℃), Cu, Pt and other metal nanoparticles undergo Ostwald ripening due to surface energy minimization, resulting in significant increase in particle size (such as Cu / ZnO-Al2O3, which significantly reduces activity after 500 hours of operation at 300℃). The high-temperature phase transition of the carrier (such as γ-Al2O3) to α-Al2O3 causes a sharp decrease in specific surface area, accelerating metal migration and aggregation. Poor tolerance to dynamic conditions: temperature cycling stress (such as 50℃ to 300℃ cycling) caused by frequent start-stop of vehicle-mounted or backup power supply repeatedly damages the metal-carrier interface, particles detach from anchor sites and aggregate. Limitations of anti-sintering strategies: structural additives (such as MgO, ZrO2): only delay the sintering rate, but cannot inhibit long-term thermodynamic-driven deactivation. Alloying (such as PtRu) is costly for noble metals, and Ru is easily dissolved at the anode potential; and the preparation process of core-shell structure (such as underpotential deposition) is complex, difficult to scale up, and the shell layer has insufficient thermal stability. Therefore, it is extremely necessary to develop a methanol fuel catalyst with high anti-sintering property, active site accessibility and scalability. SUMMARY
[0003] In view of the defects of the prior art, the purpose of the present application is to provide a high-stability methanol fuel catalyst and a preparation method thereof.
[0004] The technical effects of the present application are realized by the following technical scheme: a high-stability methanol fuel catalyst, which comprises the following components: TiO2@Al2O3 core-shell carrier, block copolymer P123, 3-aminopropyl triethoxysilane, H2PtCl6·6H2O, ascorbic acid, ethylenediamine and tetraethyl orthosilicate.
[0005] Preferably, the preparation of the TiO2@Al2O3 core-shell carrier comprises the following steps: S1: TiOSO4 and polyethylene glycol are added to deionized water, ammonia water and H2SO4 solution are added dropwise to adjust pH to 3-3.5, the temperature is increased to 70-90℃, 500 rpm stirring reaction for 3-5h, 60℃ standing for 10-16h, centrifugation, 0.05M oxalic acid solution and deionized water repeated washing 3 times, -50℃ vacuum freeze drying for 24h, then calcination treatment at 400℃ for 2-4h, to obtain anatase TiO2 nanospheres; S2: Al(OC3H7)3 is added to anhydrous ethanol, then acetylacetone is added to inhibit hydrolysis, stirring until complete dissolution to obtain solution A; the anatase TiO2 nanospheres of step S1 are ultrasonically dispersed in anhydrous ethanol to obtain a 20wt% suspension B; S3: Solution A of step S2 is slowly added dropwise to suspension B at 60℃ at a speed of 1mL / min, slowly drop 0.1M ammonia water in ethanol solution, control pH to neutral, after the dropwise addition of solution A, stirring for 2-3h, centrifugation, filtration, 70℃ aging treatment for 12-16h, heating to 300℃ at a rate of 2℃ / min, holding for 1-2h, heating to 500℃ at a rate of 1℃ / min, holding for 2-4h, to obtain TiO2@Al2O3 core-shell carrier; Preferably, in step S1, the amount ratio of TiOSO4, polyethylene glycol and deionized water is 0.1mol:18-24g:350-450mL; Preferably, in step S2, the amount ratio of Al(OC3H7)3, anhydrous ethanol and acetylacetone is 0.1mol:400-500mL:0.2-0.25mol; Preferably, in step S3, the volume amount ratio of solution A and suspension B is 2:1; Preferably, another aspect of the present application provides a preparation method of a high-stability methanol fuel catalyst, specifically comprising the following steps: S101: TiO2@Al2O3 core-shell carrier is added to toluene, 3-aminopropyl triethoxysilane is added dropwise, under nitrogen atmosphere, reflux treatment at 100-120℃ for 5-8h, ethanol is repeatedly washed to remove 3-aminopropyl triethoxysilane, vacuum drying at 60℃ for 16-24h, to obtain an aminated carrier; S102: Block copolymer P123 is added to 0.5M HCl solution, stirring at 40℃ until clear, then tetraethyl orthosilicate is slowly added dropwise at a speed of 0.5-1mL / min, stirring at 40℃ for 2h to form silicic acid oligomers, then the aminated carrier of step S101 is added, ultrasonic treatment to disperse uniformly, reaction at 60-80℃ for 24-48h, cooling and filtration, drying at 60℃ for 2-4h, gradient calcination to remove the template, to obtain a mesoporous carrier; S103: adding H2PtCl6·6H2O and ethylenediamine into anhydrous ethanol, stirring and dissolving uniformly, then adding ascorbic acid and the mesoporous carrier prepared in step S102, ultrasonic / vacuum impregnation treatment, freeze-drying, then stage temperature rising calcination, to obtain the catalyst; Preferably, in step S101, the ratio of the use amount of the TiO2@Al2O3 core-shell carrier, toluene and 3-aminopropyl triethoxysilane is 1g:15-20mL:0.1-0.15mL; Preferably, in step S102, the ratio of the use amount of the block copolymer P123, HCl solution, the aminated carrier and tetraethyl orthosilicate is 0.1-0.15g:2-3mL:1g:0.2-0.3mL; Preferably, in step S102, the ultrasonic treatment parameters are: 100-150W, 40kHz, time 20-40min; Preferably, in step S102, the gradient calcination parameters are: under nitrogen atmosphere, 300℃ for 1.5-2.5h at a speed of 2℃ / min, and 500℃ for 2-4h at a speed of 1℃ / min; Preferably, in step S103, the ratio of the use amount of the H2PtCl6·6H2O, ethylenediamine, ascorbic acid, anhydrous ethanol and mesoporous carrier is 0.01-0.012g:0.008-0.01g:0.015-0.02g:5-6mL:1g; Preferably, in step S103, the ultrasonic / vacuum impregnation treatment parameters are: temperature 50℃, 200-300W, 40kHz, treatment for 3-5h, then-0.1MPa vacuum, treatment for 1-3h; Preferably, in step S103, the freeze-drying parameters are: pre-freezing at-80℃ under vacuum for 2h, and vacuum freeze-drying at-50℃ for 24h; Preferably, in step S103, the stage temperature rising calcination parameters are: under nitrogen atmosphere, 150℃ for 1-1.5h at a speed of 2℃ / min, and 320℃ for 1-2h at a speed of 1℃ / min; under nitrogen atmosphere containing 5% hydrogen, 200-220℃ for 1-2h, and rapid cooling to room temperature.
[0006] The beneficial effects of the present application are as follows: The present application obtains anatase TiO2 core under weak acid precipitation-calcination condition, and coats the core with a layer of γ-Al2O3 by mild hydrolysis-dehydration method, so as to introduce oxygen vacancy electron pool and Lewis acid site barrier into a single particle at the same time. TiO2 can provide electrons for subsequent step-by-step oxidation-dehydrogenation of methanol molecules, and dense Al2O3 helps to isolate the core from the erosion of acidic medium, and provides weak acid coordination sites for reactants. 3-aminopropyl triethoxysilane condensed by toluene reflux can build a relatively uniform -NH2 brush layer on the outer surface; the organic layer is basically removed in the subsequent inert atmosphere calcination, leaving only dense ≡Si-OH end groups. Since the ethylenediamine complexing solution is weakly alkaline, part of the ≡Si-OH is deprotonated to SiO - during the impregnation process, and then coordinates with the planar [Pt(en)2] 2+ , so that the platinum atom is anchored to the pore wall surface in the N2O2 or O4 mode. The mesoporous SiO2 shell grows in situ through acid-catalyzed hydrolysis-condensation induced by block copolymer P123; the template can be completely removed by calcination in an atmosphere at 450-500°C, and the channels still maintain a high degree of order, ensuring smooth diffusion of reactants and products and providing spatial confinement for platinum active centers. The ligand removal stage is preferably first pyrolyzed at 200-250°C in a nitrogen atmosphere to crack most of the organic skeleton, and then oxidized at a low oxygen partial pressure for a short time to remove residual carbon, followed by reduction in H2 / N2 mixed gas to restore the metal or low-valence state of platinum. Although this temperature range is not sufficient to produce a complete TiO X coating, limited electron migration has already lowered the d-band center of platinum, which helps to weaken the Pt-CO bond and thus reduce the poisoning of intermediates. In long-range reactions, strong coordination-bridge bonds and weak electronic coupling together inhibit the migration and aggregation of platinum atoms; the straight pore channels provided by the mesoporous shell reduce the risk of product retention and local overheating, and also act as a certain buffer during mechanical oscillation or temperature fluctuations. When the catalyst activity decreases due to running time, the surface oxygen vacancies and pore cleanliness can be restored by low-temperature hydrogen or mild air reprocessing; once carbon deposition occurs, it can also be cleaned online with moderate gas-liquid flushing. In summary, after hierarchical structure design and multiple interface regulation, the catalyst exhibits relatively stable activity, certain anti-poisoning ability, and reversible regeneration characteristics in the methanol conversion environment.
[0007] Specific mechanism, the application firstly through the weak acid hydrolysis, TiOSO4 is decomposed by water to generate metatitanic acid gel TiO(OH)2, and H2SO4 is released; the sulfuric acid in the solution is then neutralized by ammonia water, (NH4)2SO4 by-product is produced, and the pH of the system is adjusted to the range suitable for precipitation. The obtained TiO(OH)2 is converted into anatase TiO2 nanometer core after calcination and dehydration. Then, aluminum isopropoxide is gradually hydrolyzed in the buffer coordinated by acetylacetone, Al(OH)3 is first formed, then AlOOH is obtained by low-temperature dehydration, and finally the dehydration and phase transition are completed at about 500°C, and a dense and stable γ-Al2O3 shell layer is constructed. Then, 3-aminopropyltriethoxysilane is condensed with the outer layer hydroxyl to introduce a uniformly distributed -NH2 functional brush on the surface of the particle, providing controllable coordination sites for the subsequent noble metal complex. Through the acid-catalyzed hydrolysis-condensation reaction of tetraethyl orthosilicate, a mesoporous SiO2 shell is in-situ grown on the outer surface; after the removal of the template agent, regular straight pores are left, laying a spatial foundation for the diffusion of the reactants and the anchoring of monatomic platinum. In the loading stage, platinum chlorate first forms a planar four-coordinated [Pt(en)2] 2+ complex with ethylenediamine; the complex is coordinated with the surface -NH2 / deprotonated SiO - sites, and the platinum atom is embedded in the N2O2 planar environment and fixed by bridging two Si-O bonds. After the removal of the organic ligand by heating in an inert atmosphere, the platinum is partially oxidized to a positive state under mild oxygen conditions to form a monatomic site of (≡Si-O)2Pt δ+ , and the Si-O bridge around it still remains, which can inhibit metal migration at a higher temperature. Finally, the platinum can be regulated to a Pt 0 / δ⁺ coexistence state with metal characteristics through low-temperature hydrogen reduction, and the Pt-O-Si anchoring skeleton remains unchanged, providing a long-acting and anti-sintering active center for the electro-thermal conversion reaction of methanol. BRIEF DESCRIPTION OF DRAWINGS
[0008] In order to more clearly illustrate the technical solutions of the present application or the prior art, the following will briefly introduce the drawings needed to be used in the embodiments or prior art description. Obviously, the drawings in the following description are only a part of the present application, and other drawings can also be obtained by those skilled in the art without any creative effort.
[0009] Figure 1 is a methanol conversion rate test result graph of the catalyst prepared in examples 1-3 and comparative examples 1-3 of the present application; Figure 2 is a CO by-product ratio test result graph of the catalyst prepared in examples 1-3 and comparative examples 1-3 of the present application; Figure 3is a carbon deposition resistance and regeneration test result diagram of the catalyst prepared in Example 3 and Comparative Examples 1-3 of the present application; Figure 4 is a SEM scanning electron microscope diagram of the TiO2@Al2O3 core-shell carrier prepared in Example 3 of the present application. DETAILED DESCRIPTION
[0010] The technical solutions of the present application will be described clearly and completely below in combination with the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative labor fall within the scope of protection of the present application. It should be noted that, unless otherwise specified, the raw materials involved in the present application are purchased through conventional commercial channels.
[0011] Example 1: A high-stability methanol fuel catalyst, which comprises the following components: TiO2@Al2O3 core-shell carrier, block copolymer P123, 3-aminopropyltriethoxysilane, H2PtCl6·6H2O, ascorbic acid, ethylenediamine and tetraethyl orthosilicate.
[0012] 1. The preparation of the TiO2@Al2O3 core-shell carrier comprises the following steps: S1: 0.1 mol of TiOSO4 and 18 g of polyethylene glycol are added to 350 mL of deionized water, an ammonia water and H2SO4 solution are added dropwise to adjust the pH to 3.5, the temperature is increased to 90°C, and the reaction is stirred at 500 rpm for 3 h, 60°C for 10 h, centrifuged, washed with 0.05 M oxalic acid solution and deionized water for 3 times, vacuum freeze-dried at -50°C for 24 h, and then calcined at 400°C for 4 h to obtain anatase TiO2 nanospheres; S2: 0.1 mol of Al(OC3H7)3 is added to 400 mL of anhydrous ethanol, and then 0.2 mol of acetylacetone is added to inhibit hydrolysis, and the mixture is stirred until complete dissolution to obtain solution A; 20 g of anatase TiO2 nanospheres from step S1 are ultrasonically dispersed in 100 mL of anhydrous ethanol to obtain a 20 wt% suspension B; S3: 200 mL of solution A from step S2 is slowly added dropwise to 100 mL of suspension B at 60°C at a speed of 1 mL / min, a 0.1 M ammonia water ethanol solution is slowly added dropwise, the pH is controlled to be neutral, the solution A is stirred for 2 h after the addition is completed, centrifuged, filtered, aged at 70°C for 12 h, heated to 300°C at a speed of 2°C / min, and kept for 2 h, heated to 500°C at a speed of 1°C / min, and kept for 4 h to obtain the TiO2@Al2O3 core-shell carrier; 2. The preparation of the high-stability methanol fuel catalyst comprises the following steps: S101: 10 g TiO2@Al2O3core-shell support was added into 150 mL toluene, 1 mL 3- aminopropyltriethoxysilane was added dropwise, and the mixture was treated under reflux at 120 °C for 5 h under nitrogen atmosphere. The 3-aminopropyltriethoxysilane was removed by repeated washing with ethanol, and the mixture was vacuum dried at 60 °C for 24 h to obtain an aminated support; S102: 1 g block copolymer P123 was added into 20 mL 0.5 M HCl solution, and stirred at 40 °C until clear. Then 2 mL tetraethyl orthosilicate was added dropwise at a rate of 1 mL / min, and the mixture was stirred at 40 °C for 2 h to form silicic acid oligomers. Then 10 g of the aminated support prepared in step S101 was added, and the mixture was ultrasonically treated at 100 W and 40 kHz for 40 min to disperse uniformly. The mixture was reacted at 60 °C for 48 h, cooled and filtered, and dried at 60 °C for 4 h. The mixture was treated at 300 °C for 1.5 h at a rate of 2 °C / min under nitrogen atmosphere, and then treated at 500 °C for 2 h at a rate of 1 °C / min to remove the template to obtain a mesoporous support; S103: 0.1 g H2PtCl6·6H2O and 0.08 g ethylenediamine were added into 50 mL anhydrous ethanol, and the mixture was stirred to dissolve uniformly. Then 0.15 g ascorbic acid and 10 g of the mesoporous support prepared in step S102 were added, and the mixture was treated at 50 °C for 5 h at 200 W and 40 kHz. Then the mixture was treated at -0.1 MPa vacuum for 1 h, pre-frozen at -80 °C for 2 h, and vacuum freeze-dried at -50 °C for 24 h. Then the mixture was treated at 150 °C for 1 h at a rate of 2 °C / min under nitrogen atmosphere, and then treated at 320 °C for 1 h at a rate of 1 °C / min. The mixture was treated at 200 °C for 2 h under a nitrogen atmosphere containing 5% hydrogen, and then quickly cooled to room temperature to obtain a catalyst.
[0013] Example 2: A high-stability methanol fuel catalyst, which comprises the following components: TiO2@Al2O3core-shell support, block copolymer P123, 3-aminopropyltriethoxysilane, H2PtCl6·6H2O, ascorbic acid, ethylenediamine, and tetraethyl orthosilicate.
[0014] 1. Preparation of TiO2@Al2O3core-shell support includes the following steps: S1: 0.1 mol TiOSO4and 20 g polyethylene glycol were added into 400 mL deionized water, and the pH was adjusted to 3 by adding ammonia water and H2SO4solution. The temperature was increased to 70 °C, and the mixture was stirred at 500 rpm for 5 h. The mixture was allowed to stand at 60 °C for 16 h, and then centrifuged. The mixture was repeatedly washed with 0.05 M oxalic acid solution and deionized water for 3 times, and then vacuum freeze-dried at -50 °C for 24 h. Then the mixture was calcined at 400 °C for 3 h to obtain anatase TiO2nanospheres; S2: 0.1 mol Al(OC3H7)3 was added into 450 mL anhydrous ethanol, then 0.22 mol acetylacetone was added to inhibit hydrolysis, and stirring was performed until complete dissolution to obtain solution A; 20 g anatase TiO2 nanospheres of step S1 were ultrasonically dispersed in 100 mL anhydrous ethanol to obtain 20 wt% suspension B; S3: 200 mL solution A of step S2 was slowly added into 100 mL suspension B at 60°C at a speed of 1 mL / min, a 0.1 M ammonia water ethanol solution was slowly added at a concentration of 0.1 M, the pH was controlled to be neutral, after the addition of solution A was completed, stirring was performed for 3 h, centrifugation was performed, filtration was performed, 70°C aging treatment was performed for 16 h, the temperature was increased to 300°C at a speed of 2°C / min and maintained for 1.5 h, the temperature was increased to 500°C at a speed of 1°C / min and maintained for 3 h to obtain TiO2@Al2O3 core-shell carrier; 2. Preparation of high-stability methanol fuel catalyst includes the following steps: S101: 10 g TiO2@Al2O3 core-shell carrier was added into 180 mL toluene, 1.2 mL 3-aminopropyltriethoxysilane was added dropwise, 100°C reflux treatment was performed for 8 h under a nitrogen atmosphere, ethanol was repeatedly washed to remove 3-aminopropyltriethoxysilane, and 60°C vacuum drying was performed for 16 h to obtain an aminated carrier; S102: 1.2 g block copolymer P123 was added into 25 mL 0.5 M HCl solution, stirring was performed at 40°C until clear, then 2.5 mL tetraethyl orthosilicate was slowly added dropwise at a speed of 0.8 mL / min, 40°C stirring treatment was performed for 2 h to form silicic acid oligomers, then 10 g aminated carrier of step S101 was added, ultrasonic treatment was performed at 130 W, 40 kHz for 20 min, uniform dispersion was obtained, 80°C reaction was performed for 24 h, cooling and filtration were performed, and 60°C drying was performed for 2 h, and the obtained mesoporous carrier was obtained by treating at 300°C at a speed of 2°C / min for 2.5 h under a nitrogen atmosphere, and treating at 500°C at a speed of 1°C / min for 4 h to remove the template; S103: 0.11 g H2PtCl6·6H2O and 0.09 g ethylenediamine were added into 55 mL anhydrous ethanol, stirring was performed until complete dissolution, then 0.18 g ascorbic acid and 10 g mesoporous carrier prepared in step S102 were added, treatment was performed at 50°C for 3 h at 300 W and 40 kHz, then-0.1 MPa vacuum treatment was performed for 3 h, -80°C vacuum pre-freezing was performed for 2 h, -50°C vacuum freeze-drying was performed for 24 h, then the temperature was increased to 150°C at a speed of 2°C / min under a nitrogen atmosphere for 1.5 h, and the temperature was increased to 320°C at a speed of 1°C / min for 2 h; treatment was performed at 220°C for 1 h under a nitrogen atmosphere containing 5% hydrogen, and rapid cooling to room temperature was performed to obtain a catalyst.
[0015] Example 3: A high-stability methanol fuel catalyst, the composition of which comprises the following components: TiO2@Al2O3core-shell carrier, block copolymer P123, 3-aminopropyl triethoxysilane, H2PtCl6·6H2O, ascorbic acid, ethylenediamine, and tetraethyl orthosilicate.
[0016] 1. Preparation of the TiO2@Al2O3core-shell carrier comprises the following steps: S1: 0.1 mol of TiOSO4 and 24 g of polyethylene glycol are added to 450 mL of deionized water, an ammonia water and H2SO4 solution are added dropwise to adjust the pH to 3.2, the temperature is raised to 80°C, and the reaction is stirred at 500 rpm for 4 h, 60°C for 12 h, centrifuged, washed with 0.05 M oxalic acid solution and deionized water for 3 times, vacuum freeze-dried at -50°C for 24 h, and then calcined at 400°C for 2 h to obtain anatase TiO2nanospheres; S2: 0.1 mol of Al(OC3H7)3 is added to 500 mL of anhydrous ethanol, and then 0.25 mol of acetylacetone is added to inhibit hydrolysis, and the mixture is stirred until complete dissolution to obtain solution A; 20 g of anatase TiO2nanospheres from step S1 are ultrasonically dispersed in 100 mL of anhydrous ethanol to obtain a 20 wt% suspension B; S3: 200 mL of solution A from step S2 is slowly added dropwise to 100 mL of suspension B at 60°C at a rate of 1 mL / min, a 0.1 M ammonia water in ethanol solution is slowly added dropwise, the pH is controlled to be neutral, the solution A is added dropwise for 2.5 h after the addition is completed, centrifuged, filtered, aged at 70°C for 14 h, heated to 300°C at a rate of 2°C / min, and held for 1 h, heated to 500°C at a rate of 1°C / min, and held for 2 h to obtain a TiO2@Al2O3core-shell carrier; 2. Preparation of the high-stability methanol fuel catalyst comprises the following steps: S101: 10 g of TiO2@Al2O3core-shell carrier is added to 200 mL of toluene, 1.5 mL of 3-aminopropyl triethoxysilane is added dropwise, and the mixture is refluxed at 110°C under a nitrogen atmosphere for 6 h, the 3-aminopropyl triethoxysilane is removed by repeated washing with ethanol, and the mixture is vacuum dried at 60°C for 18 h to obtain an aminated carrier; S102: 1.5 g of block copolymer P123 was added to 30 mL of 0.5 M HCl solution, stirred at 40°C until clear, then 3 mL of tetraethyl orthosilicate was slowly added at a rate of 0.5 mL / min, stirred at 40°C for 2 h to form a silicic acid oligomer, then 10 g of the amino carrier prepared in step S101 was added, ultrasonically treated at 150 W, 40 kHz for 30 min, uniformly dispersed, reacted at 70°C for 36 h, cooled and filtered, dried at 60°C for 3 h, treated at 300°C at a rate of 2°C / min for 2 h under a nitrogen atmosphere, and treated at 500°C at a rate of 1°C / min for 3 h to remove the template to obtain a mesoporous carrier; S103: 0.12 g of H2PtCl6·6H2O and 0.1 g of ethylenediamine were added to 60 mL of anhydrous ethanol, stirred to dissolve uniformly, then 0.02 g of ascorbic acid and 10 g of the mesoporous carrier prepared in step S102 were added, treated at 250 W, 40 kHz for 4 h at a temperature of 50°C, then treated at -0.1 MPa vacuum for 2 h, pre-frozen at -80°C for 2 h under vacuum, and freeze-dried at -50°C under vacuum for 24 h, then treated at 150°C at a rate of 2°C / min for 1.2 h and treated at 320°C at a rate of 1°C / min for 1.5 h under a nitrogen atmosphere containing 5% hydrogen, and treated at 210°C for 1.5 h under a nitrogen atmosphere containing 5% hydrogen, and rapidly cooled to room temperature to obtain a catalyst.
[0017] Comparative Example 1: The operating procedure parameters of Comparative Example 1 and Example 3 were basically the same, the main difference being that CTAB was used instead of block copolymer P123 in Comparative Example 1.
[0018] Comparative Example 2: The operating procedure parameters of Comparative Example 2 and Example 3 were basically the same, the main difference being that all operations in step S102 were removed in Comparative Example 2, i.e., the growth of mesoporous SiO2 was removed.
[0019] Comparative Example 3: The operating procedure parameters of Comparative Example 3 and Example 3 were basically the same, the main difference being that a TiO2 carrier was directly used instead of a TiO2@Al2O3 core-shell carrier in Comparative Example 3.
[0020] Performance test: Methanol vapor reforming test: 200 mg of the catalyst prepared in Examples 1-3 and Comparative Examples 1-3 was placed in a catalytic bed, 5 vol% H2 / N2 mixed gas was introduced at a rate of 50 mL / min, the temperature was raised to 220°C at a rate of 10°C / min, and the temperature was maintained for 1 h, and then the remaining hydrogen was replaced by switching to pure N2 at a rate of 50 mL / min; then, under normal pressure, methanol was introduced at a rate of 0.04 mL / min, deionized water was introduced at a rate of 0.034 mL / min, and nitrogen was introduced at a rate of 30 mL / min, the reaction temperature was 240°C, the methanol conversion rate (%) = (molar flow of methanol entering the reactor - molar flow of unreacted methanol leaving the reactor) / molar flow of methanol entering the reactor x 100%; the CO byproduct ratio (%) = molar flow of CO in the outlet gas / (molar flow of CO2 in the outlet gas + molar flow of CO in the outlet gas) x 100%, three sets of parallel samples were set for each test, the results were averaged, the results were rounded to one decimal place, and the results are shown in Figure 1 and Figure 2 .
[0021] From Figure 1 and Figure 2 It can be seen from the results that the catalyst prepared in the application has excellent performance in methanol conversion, and has a lower CO byproduct ratio, and overall has excellent catalytic performance compared to the comparative examples; from the results of Comparative Example 1 and Example 3, the methanol conversion rate decreases and the CO byproduct ratio increases, which may be due to the fact that CTAB often forms smaller pores of 2-3 nm, and the residual chlorine in the template easily corrodes the carrier, resulting in partial pore blockage; the decrease in order degree and the increase in diffusion resistance result in a slight decrease in conversion rate; the increase in pore wall defects makes the local high temperature area prone to dehydration to generate CO; from the results of Comparative Example 2 and Example 3, the methanol conversion rate decreases significantly and the CO byproduct ratio increases significantly, which may be due to the fact that the lack of SiO2 leads to a significant decrease in specific surface area, limited Pt dispersion and partial sintering; the lack of SiO - anchor points, insufficient Pt-O-Al / Ti anchoring, and decreased CO removal efficiency; the lack of pores leads to product retention and increased side reactions; from the results of Comparative Example 3 and Example 3, the methanol conversion rate decreases significantly and the CO byproduct ratio increases significantly, which may be due to the fact that only TiO2 carriers are used without the barrier of γ-Al2O3, TiO2 is more easily partially reduced in a high-temperature methanol / water atmosphere, and Pt and TiO2 form weaker SMSI; the decrease in Lewis acid sites makes CO removal dependent on a single Pt site, and both the conversion rate and the CO2 selectivity are impaired; the lack of outer layer confinement leads to more significant Pt sintering and hard carbon formation.
[0022] Acidic cycle stability test: 100 mg of catalyst prepared in Example 3 and Comparative Examples 1-3 was placed in 50 mL of 0.5 M H2SO4 solution, stirred at 50 °C for 12 h, 10 mL of the suspension was taken (labeled the 1st cycle supernatant), filtered through a 0.22 µm PES filter membrane into an ICP sample bottle, the filter residue was washed with 30 mL of deionized water until the filtrate was neutral; vacuum dried at 60 °C for 4 h, the mass of the residue was measured as m1; the dried catalyst was re- placed into fresh 50 mL of 0.5 M H2SO4 solution, and the treatment was repeated for 3 cycles; the element loss percentage (%) of each cycle = (the concentration of element i in the filtrate of the nth cycle x the total volume of the filtrate) / (the mass of the catalyst before the first cycle x the theoretical mass fraction of element i in the catalyst) x 100%, three parallel samples were set for each test, the results were averaged and rounded to two decimal places, and the results are shown in Table 1 (the percentage is based on the element content measured by ICP total digestion for the first time as 100%; ND indicates that the element itself does not exist in the sample).
[0023] Table 1. Catalyst cycle stability test results
[0024] From the results in Table 1, it can be seen that the catalyst prepared in the application has only a small amount of Ti, Al and Pt loss after multiple cycles, and the overall stability is significantly better than that of each comparative sample; from the results of Comparative Example 1 and Example 3, it can be seen that the pore size is reduced and residual Cl - corrodes the wall surface, and the acid penetrates faster; the defects in the pore wall not only accelerate the dissolution of Al 3+ in the γ-Al2O3 layer, but also weaken the coordination of Pt and SiO - , thereby causing the loss rates of Al and Pt to increase simultaneously; from the results of Comparative Example 2 and Example 3, it can be seen that the mesoporous SiO2 shell is removed, and Al2O3 is directly exposed to strong acid H2SO4, resulting in continuous hydrolysis-dissolution; acid etching proceeds inward to the TiO2 interface, resulting in a significant increase in the loss of Ti and Pt, and the Pt-O-Al bond is particularly fragile due to the lack of SiO - anchoring; from the results of Comparative Example 3 and Example 3, it can be seen that the Al2O3 barrier is missing, and the acid can directly etch the TiO2 surface layer, at this time Pt is mainly fixed by weak electroadsorption or TiO2-x SMSI effect, and has the lowest acid desorption resistance, showing the largest element loss.
[0025] Anti-carbon deposition and regeneration test: after the methanol reforming reaction, 20vol% CH3OH / 80vol% N2 (anhydrous) is continuously introduced at 300°C (5°C / min heating) for 4h to make the channel easy to generate polymeric carbon; then switch to 5vol% O2 / N2 mixed gas, 240°C for 1h; then 5vol% H2 / N2 mixed gas, 220°C for 30min; repeat the methanol vapor reforming conversion rate test before and after regeneration, calculate the retention rate (%) = steady-state conversion rate after regeneration / initial steady-state conversion rate x 100%, set three parallel samples for each test, take the average value, the result is rounded to one decimal place, and the result is shown in Figure 3 .
[0026] From Figure 3 The results show that the catalyst prepared by the application has excellent anti-carbon deposition and regeneration performance; from the results of Comparative Example 1 and Example 3, it can be seen that CTAB is substituted for P123, the pore size is smaller and the distribution is uneven, and part of the hard carbon is not completely oxidized; Cl - residues cause local Pt sintering, and the activity slightly decreases after regeneration; from the results of Comparative Example 2 and Example 3, it can be seen that the mesoporous SiO2 shell is removed, and the mesoporous confinement is lacking, Pt agglomeration and carbon deposition occur synchronously; the Al2O3 surface carbon layer is thick and difficult to completely remove during oxidation, and the activity recovery is limited; from the results of Comparative Example 3 and Example 3, it can be seen that the Al2O3 barrier is missing, the acid-base sites are insufficient, and Pt exists in the form of large particles, which easily generates a dense carbon skin in dry methanol at 300°C; although part of the carbon is removed by regeneration oxidation, Pt has been significantly sintered, and the activity loss is the largest.
[0027] Spectrum test: take the TiO2@Al2O3 core-shell carrier sample prepared in Example 3, and perform SEM scanning electron microscope test, and the results are shown in Figure 4 .
[0028] From Figure 4 The results show that the particles in the picture are basically near-spherical or subspherical, and it is difficult to obtain such regular and independent spherical aggregates at this scale by simply sintering TiO2; the surface of each sphere is composed of small protrusions, which has a typical orange peel or raspberry texture; this nanometer roughness conforms to the grain assembly texture produced by the hydrolysis and dehydration shrinkage of γ-Al2O3, and the TiO2 core is still shown as an overall gray scale at this magnification, indicating that the shell particles have hidden the core details from the electron beam signal; the surface of the number of spheres is continuous and has no obvious collapse, indicating that the outer Al2O3 and the inner core shrinkage match well; if the shell layer is only physically adsorbed or partially coated, cracks or flaky peeling often occur after calcination.
[0029] While embodiments of the application have been shown and described, it is to be understood that the embodiments described are merely exemplary of the principles and application of the present application. Numerous modifications and adaptions can be effected without departing from the spirit and scope of the present application, which is not limited to the exact construction and arrangement described. It is intended, therefore, to cover all modifications and adaptions that fall within the scope of the claims and their equivalents.
Claims
1. A high-stability methanol fuel catalyst, characterized in that: The composition includes the following components: TiO2@Al2O3 core-shell carrier, block copolymer P123, 3-aminopropyltriethoxysilane, H2PtCl6·6H2O, ascorbic acid, ethylenediamine and ethyl orthosilicate.
2. A high-stability methanol fuel catalyst according to claim 1, characterized in that: The preparation of the TiO2@Al2O3 core-shell carrier comprises the following steps: S1: Add TiOSO4 and polyethylene glycol to deionized water, add ammonia water and H2SO4 solution to adjust the pH, increase the temperature, stir the reaction, let it stand, centrifuge, repeatedly wash with oxalic acid solution and deionized water, freeze-dry in vacuum, and then calcine to obtain anatase TiO2 nanospheres; S2: Add Al(OC3H7)3 to anhydrous ethanol, then add acetylacetone to inhibit hydrolysis, and stir until completely dissolved to obtain solution A; ultrasonically disperse the anatase TiO2 nanospheres from step S1 in anhydrous ethanol to obtain suspension B; S3: Slowly add solution A from step S2 dropwise to suspension B, and simultaneously slowly add an ethanol solution of aqueous ammonia to control the pH to be neutral. After the addition of solution A is completed, stir, centrifuge, filter, age, heat and keep warm, and then heat and keep warm again to obtain a TiO2@Al2O3 core-shell carrier.
3. A high-stability methanol fuel catalyst according to claim 2, characterized in that: In step S1, the ratio of the amount of TiOSO4, polyethylene glycol and deionized water is 0.1 mol: 18-24 g: 350-450 mL.
4. A high-stability methanol fuel catalyst according to claim 3, characterized in that: In step S2, the ratio of the amount of Al(OC3H7)3, anhydrous ethanol and acetylacetone is 0.1 mol:400-500 mL:0.2-0.25 mol; in step S3, the volume ratio of the solution A and the suspension B is 2:
1.
5. A method for preparing a high-stability methanol fuel catalyst according to any one of claims 1 to 4, characterized in that: The specific steps include: S101: Add the TiO2@Al2O3 core-shell carrier to toluene, add 3-aminopropyltriethoxysilane dropwise, reflux under nitrogen atmosphere, repeatedly wash with ethanol to remove 3-aminopropyltriethoxysilane, and vacuum dry to obtain an amino carrier; S102: Add the block copolymer P123 to the HCl solution and stir until it is clear. Then, slowly add tetraethyl orthosilicate dropwise and stir to form silicic acid oligomers. Then, add the amino support prepared in step S101 and perform ultrasonic treatment to disperse the solution uniformly. Then, heat the solution to react, cool and filter, dry, and perform gradient calcination to remove the template to obtain a mesoporous support. S103: Add H2PtCl6·6H2O and ethylenediamine to anhydrous ethanol, stir and dissolve evenly, then add ascorbic acid and the mesoporous support prepared in step S102, perform ultrasonic / vacuum impregnation treatment, freeze-dry, and then calcine in stages to obtain a catalyst.
6. A method for preparing a high-stability methanol fuel catalyst according to claim 5, characterized in that: In step S101, the ratio of the amount of the TiO2@Al2O3 core-shell carrier, toluene and 3-aminopropyltriethoxysilane is 1 g:15-20 mL:0.1-0.15 mL.
7. A method for preparing a high-stability methanol fuel catalyst according to claim 6, characterized in that: In step S102 , the ratio of the block copolymer P123, HCl solution, amino carrier and tetraethyl orthosilicate is 0.1-0.15 g:2-3 mL:1 g:0.2-0.3 mL.
8. A method for preparing a high-stability methanol fuel catalyst according to claim 7, characterized in that: In step S102, the ultrasonic treatment parameters are: 100-150W, 40kHz, and time 20-40min; The gradient calcination parameters are: in a nitrogen atmosphere, treating at 300° C. at a rate of 2° C. / min for 1.5 to 2.5 hours, and heating to 500° C. at a rate of 1° C. / min for 2 to 4 hours.
9. A method for preparing a high-stability methanol fuel catalyst according to claim 8, characterized in that: In step S103, the ratio of the amount of H2PtCl6·6H2O, ethylenediamine, ascorbic acid, anhydrous ethanol and mesoporous carrier is 0.01-0.012 g: 0.008-0.01 g: 0.015-0.02 g: 5-6 mL: 1 g; the ultrasonic / vacuum immersion treatment parameters are: temperature 50°C, 200-300 W, 40 kHz, treatment for 3-5 hours, then -0.1 MPa vacuum, treatment for 1-3 hours.
10. A method for preparing a high-stability methanol fuel catalyst according to claim 9, characterized in that: In step S103, the freeze-drying parameters are: vacuum pre-freezing at -80°C for 2 hours, vacuum freeze-drying at -50°C for 24 hours; the staged temperature rising calcination parameters are: in a nitrogen atmosphere, heating to 150°C at a rate of 2°C / min for 1-1.5 hours, heating to 320°C at a rate of 1°C / min for 1-2 hours; in a nitrogen atmosphere containing 5% hydrogen, heating at 200-220°C for 1-2 hours, and rapidly cooling to room temperature.
Citation Information
Patent Citations
Acidity-controllable core-shell type platinum based catalyst and preparation and application thereof
CN106824175A
Fe2O3-loaded Al2O3 / SiO2@TiO2 porous core-shell sphere adsorbent as well as preparation method and application thereof
CN113019311A
Propane dehydrogenation catalyst with SiO2-Al2O3 yolk-eggshell structure loaded multi-element complex phosphoric acid metal system and preparation method thereof
CN117339613A
Platinum-based molecular sieve catalyst stabilized by soft template modified bimetallic auxiliary agent and preparation method and application of platinum-based molecular sieve catalyst
CN118491557A
Preparation method of mesoporous gamma-Al2O3-coated TiO2 core-shell structure catalyst for carbonyl sulfide hydrolysis
CN119186652A
Cited By
Wear-resistant and weather-resistant printing ink and preparation method thereof
CN121628429A