Fluorite mine flotation composite collecting agent and preparation method and application thereof
By leveraging the synergistic effect of multiple components in the composite collector, the problems of insufficient applicability and stability of existing fluorite flotation agents have been solved, enabling efficient separation of various types of fluorite ores and improvement of concentrate purity, adapting to different environmental conditions.
Patent Information
- Application Number
- CN202511259485.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-04
- Publication Date
- 2025-10-24
AI Technical Summary
Existing flotation collectors for fluorite ore lack applicability and stability, making it difficult to handle the continuous and stable separation of various types of fluorite ore. Furthermore, they are easily affected by environmental factors such as pulp pH and water hardness, leading to fluctuations in flotation indicators.
A composite collector consisting of dehydrorosin amine, sodium oleoyl sarcosinate, sodium silicate-citric acid complex salt, ethylene glycol butyl ether, and sodium carbonate-sodium bicarbonate buffer pair is used to achieve selective collection of fluorite and inhibition of gangue through the synergistic effect of multiple components, adapting to different regions and water quality conditions.
It achieves efficient separation of dolomite-type, high-sulfur-type, brecciated, high-calcium carbonate-type, and high-silica fluorite ores, reduces process switching costs, and ensures the stability of flotation indicators and concentrate purity.
Smart Images

Figure CN120827964A_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of fluorite ore dressing, in particular to a fluorite ore flotation composite collector and a preparation method and application thereof. BACKGROUND
[0002] Fluorite is the core source of fluorine element in industry, known as industrial vitamin, and is widely used in traditional fields such as steel smelting, aluminum electrolysis, glass ceramics, and plays a key role in emerging fields such as new energy, electronic industry, optical devices. Dolomite type fluorite ore is a special ore deposit of fluorite and dolomite symbiosis. Because the surface properties of the two are similar, it is difficult to separate efficiently by traditional beneficiation methods, and flotation technology becomes the key solution: by adjusting the pH value of the ore pulp to 8-9.5, adding fatty acid collectors and water glass inhibitors, and using bubble flotation to realize accurate separation. Modern process also adopts stage grinding-stage separation process to improve the mineral dissociation degree, combined with multiple cleaning to improve the concentrate grade. This technology not only improves the resource utilization rate, but also reduces the impact on the environment through wastewater recycling, low-toxicity reagent development and other environmental protection measures. Fluorite concentrate after flotation is widely used in the fields of hydrofluoric acid preparation, semiconductor etching, metallurgical fluxing agent, etc., promoting the upgrading of traditional industry and the development of new energy industry.
[0003] The prior art with publication number CN113351375B discloses a fluorite ore flotation composite collector and a preparation method and application thereof, which is made of the following raw materials by weight: mixed fatty acid sodium 60-70 parts; stearic acid methyl ester sodium sulfonate 15-25 parts; oleic acid amide 10-20 parts; emulsifier OP-10 3-7 parts; wherein the mixed fatty acid sodium is made of sodium oleate and sodium ricinoleate. The prior art provides a collector with good selectivity for low-grade siliceous fluorite ore, which greatly improves the recovery rate of the product and makes the product reach the third level and above. The prior art with publication number CN112246441B also discloses a flotation composite collector and a preparation method and application thereof, which is made of peroxide and hydroxylamine salt as raw materials to obtain a composite collector containing hydroxamic acid compounds and alcohol; the preparation method has wide raw material sources and simple process operation, and the prepared flotation composite collector has strong collecting capacity and selectivity for ilmenite, scheelite, wolframite, cassiterite and other ores, and obtains good flotation indexes in flotation test.
[0004] In view of the above and existing related technologies, the following defects often exist: 1. Existing collectors are often designed for fluorite ores with specific impurity types. For example, some technologies are only suitable for the separation of low-grade siliceous fluorite ores and lack effective response to high-magnesium fluorite ores containing significant amounts of dolomite, high-sulfur fluorite ores with associated sulfides, or brecciated fluorite ores that produce a large number of fine particles due to crushing. In actual production, changes in the ore type to be processed require readjusting the reagent formulation or even changing the collector type. This not only increases process switching costs but also causes fluctuations in flotation performance due to compatibility issues between different reagents, making it difficult to achieve continuous and stable separation of multiple fluorite ores.
[0005] 2. Existing technologies often rely on a single collection mechanism, such as simple anion adsorption, which cannot specifically recognize lattice differences on the fluorite surface. This results in the collector easily co-adsorbing calcium-containing gangue while adsorbing fluorite, resulting in high impurity content in the concentrate. For high-sulfur fluorite ores, existing collectors also lack the specific inhibition of sulfides. Sulfide minerals tend to float with bubbles, further reducing the concentrate purity and affecting the quality of raw materials for subsequent smelting or chemical applications.
[0006] 3. The performance of existing collectors is easily restricted by environmental factors such as slurry pH value and water hardness. In the northern region with high water hardness, the active ingredients in the agent are easily affected by the water. 、 The combination forms an insoluble precipitate, resulting in a decrease in effective concentration and sticky foam that is difficult to separate. In strongly alkaline or acidic slurries, some reagents, such as non-ionic emulsifiers, will undergo hydrolysis or structural destruction, resulting in stratification, failure and other problems, causing significant fluctuations in flotation recovery rate and grade, which cannot meet the stable production needs in different regions and under different water quality conditions. Summary of the Invention
[0007] The technical problem to be solved by the present invention is that the existing technology has the disadvantages of insufficient applicability and stability. For this reason, we propose a fluorite ore flotation composite collector and its preparation method and application.
[0008] To achieve the above objectives, the present application adopts the following technical solution: a composite collector for fluorite flotation, a preparation method thereof, and an application thereof, comprising the following components in parts by weight: 15-30 parts of dehydroabietinamine, 20-35 parts of sodium oleoyl sarcosinate, 20-40 parts of sodium silicate-citric acid complex, 10-20 parts of ethylene glycol butyl ether, and 5-15 parts of sodium carbonate-sodium bicarbonate buffer; the components synergize with each other to impart the composite with selective capture ability for fluorite, inhibitory effect on gangue, and environmental adaptability, thereby achieving the separation of various fluorite ores.
[0009] Preferably, the weight ratio of sodium silicate to citric acid in the sodium silicate-citric acid composite salt is 1:0.5-2.
[0010] Preferably, the weight ratio of sodium carbonate to sodium bicarbonate in the sodium carbonate-sodium bicarbonate buffer pair is 1:1 to 3:1.
[0011] Preferably, the dehydroabietylamine and sodium oleoyl sarcosinate form ion pairs through intermolecular forces, and the sodium silicate and citric acid form bridged complex compounds through hydrogen bonds.
[0012] Preferably, the dehydroabietylamine realizes selective recognition of fluorite through the steric hindrance effect of the tricyclic phenanthrene skeleton, the sodium oleoyl sarcosinate enhances the adsorption stability on the fluorite surface through the pH-responsive ionization characteristics, the sodium silicate-citric acid complex salt realizes targeted inhibition of gangue by forming a bridged complex structure, and the ethylene glycol butyl ether improves the anti-interference ability of the system through complexation with hard ions, so that the components realize the separation effect through specific synergistic action.
[0013] A preparation method of a fluorite ore flotation composite collector, comprising the following steps: S1: mixing and reacting sodium silicate and citric acid in water to obtain a sodium silicate-citric acid complex salt; S2: mixing sodium carbonate and sodium bicarbonate to obtain a buffer pair; S3: mixing dehydroabietylamine and ethylene glycol butyl ether; S4: adding sodium oleoyl sarcosinate and the sodium silicate-citric acid complex salt to the mixture of S3 and mixing; S5: adding the buffer pair to the mixture of S4 and mixing until the pH of the system is stabilized at 7-10 to obtain the composite collector.
[0014] Preferably, the mixing and reaction of sodium silicate and citric acid in S1 is carried out in an aqueous medium, the reaction temperature is 40-60℃, and the reaction time is 20-50min.
[0015] Preferably, S3 to S5 are controlled by temperature progression and stirring to make the dehydroabietylamine first dispersed by the ethylene glycol butyl ether to form a basic system, then gradually react with the sodium oleoyl sarcosinate and the sodium silicate-citric acid complex salt, and finally realize the pH stabilization of the system through the buffer pair, so that a uniform phase state is maintained throughout the process to ensure the formation of the synergistic structure of the components.
[0016] Preferably, the composite collector is used for the flotation of dolomite type, high-sulfur type, angular gravel type, high-calcium carbonate type or high-silica fluorite ore, and the pH of the ore pulp is controlled at 7-10 during flotation.
[0017] The technical effects and advantages of the present application are as follows: In the present application, a high-efficiency separation system is constructed through the synergistic effect of multiple components. The steric hindrance effect of dehydroamabiline realizes the selective collection of fluorite, the pH response characteristics of oleoyl sarcosine sodium enhance the adsorption stability, the sodium silicate-citric acid composite salt selectively inhibits calcium-containing gangue, and ethylene glycol butyl ether and the buffer pair ensure the dispersibility and environmental stability of the system. The components form a functionally complementary system through complexation, ion pair formation, and other mechanisms, avoiding the limitations of single components in selectivity or adaptability, and can meet the separation needs of various types of fluorite ore such as dolomite, high-sulfur, and high-silicon.
[0018] In the present application, the anti-hard water effect of ethylene glycol butyl ether reduces the influence of calcium and magnesium ions on the activity of the reagent, and the sodium carbonate-sodium bicarbonate buffer pair can stabilize the pH of the ore slurry, avoiding fluctuations in flotation indicators caused by water hardness and ore dissolution. Whether in low-temperature environments or complex water quality conditions, the reagent can maintain good dispersibility and activity, solving the problem of unstable performance of traditional collectors in different regions and under different working conditions.
[0019] In the present application, based on the same core material system, by adjusting the component ratio and process parameters, different characteristics of fluorite ore can be adapted without introducing new components or replacing equipment, reducing the process switching cost. The premixing preparation process ensures the full synergy of each component, avoiding the decrease in action efficiency caused by step-by-step addition, and facilitating continuous industrial production. BRIEF DESCRIPTION OF DRAWINGS
[0020] The disclosure of the present application is explained with reference to the accompanying drawings. It should be understood that the drawings are for illustrative purposes only and are not intended to limit the scope of protection of the present application. In the drawings, the same reference numerals are used to refer to the same parts: Figure 1 is a flow chart for the preparation of the composite collector; Figure 2 is the X-ray crystal diffraction pattern of dehydroamabiline; Figure 3 is the infrared spectrum of sodium silicate-citric acid composite salt; DETAILED DESCRIPTION
[0021] It is easy to understand that, according to the technical scheme of the present application, one of ordinary skill in the art can propose a plurality of structure modes and implementation modes that can be replaced with each other without changing the essential spirit of the present application. Therefore, the following specific embodiments and drawings are only exemplary descriptions of the technical scheme of the present application, and should not be considered as the whole or as a limitation or restriction on the technical scheme of the present application.
[0022] Reference Figure 1 As shown in the drawings, the present application provides a preparation method of a fluorite ore flotation composite collector, comprising the following steps: Step S1: Take 20 parts of dehydroabietylamine, 30 parts of oleoyl sarcosine sodium, 12 parts of sodium silicate, 18 parts of citric acid, 10 parts of ethylene glycol butyl ether, 5 parts of sodium carbonate, and 5 parts of sodium bicarbonate by weight.
[0023] Step S2: Add sodium silicate to 5 times the mass of deionized water and stir until completely dissolved to form a colorless transparent solution. Then slowly add 18 parts of citric acid, control the reaction temperature at 45°C, stir at 250 rpm for 35 min, the solution is uniform and transparent, get sodium silicate-citric acid complex salt ready for use.
[0024] Step S3: Mix sodium carbonate and sodium bicarbonate uniformly, grind to a particle size of less than 100 μm, get sodium carbonate-sodium bicarbonate buffer pair ready for use.
[0025] Step S4: Add dehydroabietylamine and ethylene glycol butyl ether to the reaction kettle in turn, start stirring, control the temperature at 55°C, the stirring speed at 350 rpm, continue for 18 min, until they are completely miscible, form a light yellow transparent solution.
[0026] Step S5: Add oleoyl sarcosine sodium and sodium silicate-citric acid complex salt to the above solution in turn, heat to 60°C, adjust the stirring speed to 450 rpm, continue stirring for 25 min, it can be observed that the solution gradually turns into a dark yellow homogeneous system.
[0027] Step S6: Add sodium carbonate-sodium bicarbonate buffer pair to the above system, keep the temperature at 60°C, the stirring speed at 450 rpm, continue stirring for 12 min, until the system pH stabilizes at 9.0, get the finished composite collector.
[0028] The high efficiency of the composite collector is due to the synergistic effect of each component, among which dehydroabietylamine as the main collector, sodium silicate-citric acid complex salt as the core inhibitor, the structure of the two directly determines the separation effect on dolomite type fluorite ore.
[0029] Dehydroabietylamine as the core collector component in the system, its molecular structure and the specific action on the surface of fluorite are the key to realize high selectivity.
[0030] Specifically, the chemical structure of dehydroabietylamine is as follows:
[0031] More specifically, the core of dehydroabietylamine is a tricyclic phenanthrene skeleton fused by three six-membered rings, and a primary amine group is connected to the end through a methylene group The amine group can form a stable coordination bond with the on the surface of fluorite, while the rigid tricyclic phenanthrene skeleton is not matched in size and produces steric hindrance and repulsion on the surface of dolomite.
[0032] Reference Figure 2 As shown, X-ray crystal diffraction analysis shows that the spatial size of its tricyclic phenanthrene skeleton is consistent with that of the fluorite lattice. The arrangement spacing (0.54nm) is highly matched with that in dolomite. There is a significant difference in the spacing (0.40nm).
[0033] Tests using a laser particle size analyzer showed that the hydrophobic ends of the tricyclic phenanthrene skeleton interacted through van der Waals forces, promoting the directional agglomeration of fine-grained fluorite with a particle size of less than 20 μm. Laser particle size analyzer tests showed that the average particle size of the agglomerates increased from 20 μm to 80 μm, and the fine particle recovery rate increased by 25%.
[0034] Sodium silicate-citric acid composite salt is formed through complex reaction and specifically exerts an inhibitory effect on calcium-containing gangue such as dolomite.
[0035] Specifically, the silicate generated by the hydrolysis of sodium silicate forms a Si-OH-OOC-bridged complex with the carboxyl group of citric acid through hydrogen bonding.
[0036] Reference Figure 3 As shown, the infrared spectrum Appear Characteristic peaks confirmed the formation of complex structure.
[0037] It should be noted that during the flotation process, the three carboxyl groups of citrate preferentially bind to the surface of dolomite. and calcite surface Combined to form a stable five-membered ring chelate, blocking its interaction site with the collector, wherein the chelation constant logK was measured to be 5.4.
[0038] The silicate of sodium silicate forms a hydrophilic silicon oxide film on the surface of the chelate, which enhances the hydrophilicity of the gangue and inhibits it from floating up with the foam.
[0039] Sodium oleoyl sarcosinate is a synergistic component of the main collector, and its amphoteric structure and pH response characteristics are the key to improving the sorting efficiency.
[0040] Specifically, the molecular chain of sodium oleoyl sarcosinate is composed of three parts, among which the hydrophobic end long chain alkyl It provides a 17-carbon unsaturated fatty chain; the polar middle amide bond enhances the binding force between the molecule and the mineral surface; the hydrophilic end sodium carboxylate group can dissociate into carboxylate ions in aqueous solution, providing hydrophilicity and charge characteristics.
[0041] In acidic slurry with pH < 8, the amine group of the amide bond is protonated, the molecule becomes cationic, and avoids binding to the positive charge on the dolomite surface through electrostatic repulsion; In the alkaline pulp with pH > 9, the carboxyl group dissociates into carboxylate ion, and the molecule shows anion, which can form ion pair with the protonated amine group of DHMS on the surface of fluorite The measured stability constant logK is 6.8.
[0042] It is worth noting that in the flotation process, the carboxylate ion of sodium oleoyl sarcosinate and the protonated amine group of DHMS form an ion pair , which enhances the overall adsorption stability on the surface of fluorite through charge complementation, and the Zeta potential decreases from-25 mV to-38 mV.
[0043] In the actual fluorite flotation experiment, we also found that long-chain alkyl encapsulates bubbles through hydrophobic interaction, which prolongs the half-life of foam from an average of 3 min to 8 min, effectively avoiding the emergence of concentrate entrainment caused by excessive foaming.
[0044] Ethylene glycol butyl ether as a key dispersing and anti-hard water component in the system, its molecular structure and interfacial activity directly affect the dispersibility and environmental adaptability of the reagent.
[0045] Specifically, the oxygen atom in the ether bond of ethylene glycol butyl ether can form a weak complex with the , hard ions and sodium oleoyl sarcosinate in the pulp, reducing the precipitation reaction of hard ions and sodium oleoyl sarcosinate.
[0046] The hydrogen bonding between the hydroxyl group (-OH) of ethylene glycol butyl ether and water molecules can reduce the surface tension of the system, especially in low temperature environment, which can avoid the agglomeration problem of DHMS due to the decrease of solubility.
[0047] The sodium carbonate-sodium bicarbonate buffer pair can provide a stable chemical environment for the selective adsorption of collectors and gangue inhibition by precisely regulating the pH of the pulp.
[0048] In this system, the buffer pair can stabilize the pH of the pulp in the range of 9.0±0.1, which is the best interval of this system.
[0049] When the pulp has acidic fluctuations due to ore dissolution, the carbonate ions in the buffer pair combine with excess H⁺ to form ; when there is an alkaline fluctuation, the bicarbonate ions in the buffer pair ionize to release to neutralize excess , which inhibits the sharp change of pH.
[0050] It should be noted that under strong alkaline conditions, fluorite will undergo dissolution reaction, so it is very important to control the pH environment to reduce the loss of fluorite.
[0051] It is worth mentioning that the raw material parts in the above steps are determined by orthogonal experiment screening, and the selected raw ore is ordinary dolomite type fluorite ore.
[0052] In some embodiments, the components and proportions of the composite collector prepared by the above preparation method can be adjusted according to the characteristics of the target fluorite ore, such as the type of impurities, particle size distribution, sulfur content, etc., to achieve targeted separation; In other embodiments, the process parameters of the preparation process, such as stirring speed and mixing temperature, can also be adaptively optimized to ensure that each component fully plays a synergistic role.
[0053] All embodiments are based on the same set of core material system, without introducing additional components, and only through dynamic adjustment of the proportion and parameters, the flotation effect on different types of fluorite ore is verified.
[0054] Example 1 The raw ore of this embodiment is mined from a low-sulfur dolomite type fluorite ore mine in Jiangxi, and according to the weight parts described in the specific embodiments: dehydrogenated rosin amine 20 parts, oleoyl sarcosine sodium 30 parts, sodium silicate 12 parts, citric acid 18 parts, ethylene glycol butyl ether 10 parts, sodium carbonate 5 parts, sodium bicarbonate 5 parts, and deionized water 60 parts.
[0055] The raw ore is crushed and ball milled, and then passed through a 200 mesh screen, with the undersize product accounting for about 65%, and the oversize part returning to the ball milling circuit.
[0056] Through X-ray fluorescence spectrum analysis, the main chemical components of the raw ore are as follows: fluorite content 65.2%, calcite 12.5%, dolomite 8.3%, quartz 10.1%, and sulfide 0.3%.
[0057] In addition, the laser particle size analyzer analysis shows that the particle size distribution interval of the ore sample is 5-150 μm, of which the fine particle size of less than 20 μm accounts for about 18%, the medium particle size of 20-74 μm accounts for about 47%, and the coarse particle size of more than 74 μm accounts for about 35%, showing a distribution characteristic of mainly medium and fine particles and secondarily coarse particles.
[0058] The preparation steps and parameter control of the composite collector are consistent with the above steps, and after two roughing, seven cleaning and three scavenging, the concentrate is obtained, and the flotation results are shown in Table 1.
[0059]
[0060] Table 1 As can be seen from Table 1, for low-sulfur dolomite type fluorite ore, after flotation with the composite collector of the present application, the concentrate The grade is 98.5%, the recovery rate is 89.2%, The content is reduced to 0.8%, which is lower than that of the raw ore The content (8.3%) is reduced by 90.4%, which shows that the dolomite is effectively inhibited; the tailings The recovery rate is only 10.8%, which shows that the fluorite loss is small, and the overall separation index is excellent, meeting the standard of primary concentrate.
[0061] Example 2 The raw ore of this example is mined in a certain breccia type fluorite mine in Jiangxi. According to the description in the specific embodiment, the following components are weighed by parts by weight: dehydroabietylamine 25 parts, oleoyl sarcosine sodium 25 parts, sodium silicate 10 parts, citric acid 20 parts, ethylene glycol butyl ether 15 parts, sodium carbonate 6 parts, sodium bicarbonate 4 parts, and deionized water 50 parts.
[0062] The raw ore has a breccia structure, and after crushing, the fine mud content is high. The multi-element analysis shows that: The grade is 58.3%, the calcite is 8.7%, the dolomite is 5.2%, the quartz is 15.6%, and the -20 μm particle size accounts for 40%. The fine fluorite is easy to be lost with the tailings.
[0063] The difference between this example and Example 1 is that: In step S2 of this example, after adding citric acid, the stirring time is extended by 5 min to ensure that the fine particle inhibitor is fully complexed. In step S4 of this example, the stirring speed is increased to 400 rpm, and the stirring time is extended by 2 min.
[0064] In step S5 of this example, the stirring speed is increased to 500 rpm, and the stirring time is extended by 5 min. The high shear promotes the dispersion of fine particle reagents.
[0065] In step S6 of this example, after adding the buffer pair, the system is stirred at 65°C and 500 rpm for 15 min. The pH of the system is stabilized at 9.5, which is slightly higher than that of Example 1, enhancing the surface charge of fine fluorite.
[0066] After the raw ore is subjected to two roughing, seven cleaning and three scavenging, the concentrate is obtained. The flotation results are shown in Table 2.
[0067]
[0068] Table 2 The data in Table 2 shows that for the breccia fluorite ore, the concentrate The grade is 97.2%, and the recovery rate is 85.6%, of which the recovery rate of -20 μm fine particle size is 80.3%, which is 40.3% higher than the fine particle content of the raw ore; the tailings The content is 28.7%, which is significantly enriched compared with the raw ore (15.6%), confirming the inhibition effect of sodium silicate-citric acid complex salt on siliceous gangue, and the agglomeration effect of dehydroabietylamine effectively solves the problem of fine fluorite loss.
[0069] Example 3 The raw ore of this embodiment was mined from a high-sulfur fluorite mining area in Henan Province. As described in the specific embodiment, the following were weighed in parts by weight: 22 parts of dehydroabietinamine, 28 parts of sodium oleoyl sarcosinate, 18 parts of sodium silicate, 12 parts of citric acid, 10 parts of ethylene glycol butyl ether, 10 parts of sodium carbonate, 5 parts of sodium bicarbonate, and 90 parts of deionized water.
[0070] The multi-element analysis of the raw ore shows: The grade is 60.5%, pyrite 4.8%, calcite 12.3%, and dolomite 6.2%. The surface of pyrite is highly hydrophobic and easily floats with fluorite.
[0071] This embodiment differs from embodiment 1 in that: In this embodiment, in step S2, after adding citric acid, the stirring time is extended by 5 minutes to promote the excessive formation of a thicker hydrophilic film by sodium silicate; In this embodiment, in step S4, the stirring speed is increased to 400 rpm and the stirring time is extended by 2 minutes.
[0072] In step S5 of this embodiment, the stirring speed is increased to 500 rpm and the stirring time is extended to 5 minutes to promote the dispersion of fine-particle medicine through high shear.
[0073] In step S6 of this embodiment, after adding the buffer solution, stirring was carried out at 450 rpm for 18 minutes, and the pH of the system was stabilized at 10.0, and pyrite was suppressed by strong alkalinity.
[0074] The ore was subjected to two roughing rounds, seven cleaning rounds and three scavenging rounds to obtain concentrate. The flotation results are shown in Table 3.
[0075]
[0076] Table 3 As shown in Table 3, for high-sulfur fluorite ore, the S content of the concentrate is reduced to 0.25%, and the pyrite removal rate reaches 94.8%. The grade is 96.8% and the recovery rate is 84.3%. The S content of the tailings is 8.5%, which is significantly enriched compared with the original ore. This shows that the strong alkaline environment and the excessive sodium silicate design synergistically inhibit pyrite and achieve efficient separation of fluorite and sulfide ore.
[0077] Example 4 The raw ore of this embodiment was mined from a high calcium carbonate fluorite mine in Fujian. As described in the specific embodiment, the following were weighed in parts by weight: 18 parts of dehydroabietinamine, 32 parts of sodium oleoyl sarcosinate, 20 parts of sodium silicate, 10 parts of citric acid, 10 parts of ethylene glycol butyl ether, 3 parts of sodium carbonate, 7 parts of sodium bicarbonate, and 100 parts of deionized water.
[0078] Multi-element analysis of the raw ore shows: Grade 55.7%, calcite 25.3%, dolomite 3.1%, quartz 12.5%, calcite and fluorite surface The active phase is similar, and the separation difficulty is great.
[0079] The difference between this embodiment and embodiment 1 is that: In step S6 of this embodiment, after adding the buffer pair, the system is kept at 55°C and stirred at 450 rpm for 12 min, and the pH of the system is stabilized at 8.0.
[0080] After two roughing, seven cleaning and three scavenging, the concentrate is obtained, and the flotation results are shown in Table 4.
[0081]
[0082] Table 4 Table 4 shows that after flotation of high calcium fluorite ore, the concentrate The content is only 2.1%, the calcite inhibition rate is 91.7%, The grade is 96.5%, the recovery rate is 82.7%; the tailings The content is 40.5%, which is significantly enriched compared with the original ore, the synergistic effect of weak alkaline pH and high proportion of oleoyl sarcosine sodium effectively avoids the co-floating of calcite and fluorite.
[0083] Example 5 The original ore of this embodiment is mined from a high silicon fluorite ore area in Hunan, and the components are taken by weight fraction according to the description in the specific embodiment: dehydroabietylamine 20 parts, oleoyl sarcosine sodium 22 parts, sodium silicate 25 parts, citric acid 5 parts, ethylene glycol butyl ether 13 parts, sodium carbonate 7 parts, sodium bicarbonate 8 parts, and deionized water 125 parts.
[0084] The multi-element analysis of the original ore shows that: The grade is 50.2%, calcite is 8.3%, dolomite is 4.1%, and quartz is 30.5%, and the siliceous minerals and fluorite are closely embedded and easy to be entrained with foam.
[0085] The difference between this embodiment and embodiment 1 is that: In step S2 of this embodiment, after adding citric acid, the system is continuously stirred to obtain a viscous compound salt; In step S5 of this embodiment, the stirring speed is 450 rpm, and the stirring time is extended to 30 min to promote the dispersion of the silica sol.
[0086] In step S6 of this embodiment, after adding the buffer pair, the system is kept at 60°C and stirred at 450 rpm for 15 min, and the pH of the system is stabilized at 9.2, which is slightly higher than that of embodiment 1.
[0087] The ore was subjected to two roughing rounds, seven cleaning rounds and three scavenging rounds to obtain concentrate. The flotation results are shown in Table 5.
[0088]
[0089] Table 5 From Table 5, we can see that after flotation of Hunan high-silica fluorite ore, the concentrate Content 1.8%, siliceous inhibition rate 94.1%, Grade 96.3%, recovery rate 82.1%; tailings The content is 52.3%, which proves that the silica sol formed by the high proportion of sodium silicate has a strong inhibition on quartz, and the synergistic effect of a small amount of citric acid avoids excessive inhibition of fluorite.
[0090] Example 6 The raw ore of this embodiment comes from purchased mixed fluorite ore. As described in the specific embodiment, the following are weighed in parts by weight: 20 parts of dehydroabietyl amine, 25 parts of sodium oleoyl sarcosinate, 15 parts of sodium silicate, 15 parts of citric acid, 15 parts of ethylene glycol butyl ether, 5 parts of sodium carbonate, 10 parts of sodium bicarbonate, and 75 parts of deionized water.
[0091] Multi-element analysis of the raw ore shows: The grade is 52.3%, calcite 10.5%, dolomite 7.8%, quartz 18.6%, -20μm particle size accounts for 30%, and it contains various impurities such as dolomite, calcite, sulfide ore, fine mud, etc., which is a complex and difficult ore dressing.
[0092] This embodiment differs from embodiment 1 in that: In step S6, after adding the buffer solution, the mixture was stirred at 60° C. and 450 rpm for 15 min. The pH of the system was stabilized at 8.5, which was slightly lower than that in Example 1.
[0093] The preparation steps and parameter control of the composite collector are consistent with the above steps. The raw ore is subjected to two roughing rounds, seven cleaning rounds and three scavenging rounds to obtain the concentrate. The flotation results are shown in Table 6.
[0094]
[0095] Table 6 The data in Table 6 show that after flotation of the purchased complex fluorite ore, the total impurities in the concentrate are reduced to 4.3%. The grade is 95.7% and the recovery rate is 80.5%. Even in the presence of various impurities (dolomite, sulfide ore, and fine mud), the separation efficiency remains relatively high, highlighting the broad-spectrum adaptability of the composite collector of the present invention.
[0096] Example 7 The crude ore of this embodiment is mined in a dolomite type fluorite mine area in Inner Mongolia. According to the description in the specific embodiment, the following components are taken by weight fraction: dehydroabietylamine 18 parts, oleoyl sarcosine sodium 26 parts, sodium silicate 12 parts, citric acid 14 parts, ethylene glycol butyl ether 20 parts, sodium carbonate 4 parts, sodium bicarbonate 6 parts, and deionized water 60 parts.
[0097] The crude ore has a breccia structure, and multi-element analysis shows that: The grade is 63.5%, calcite is 11.2%, and dolomite is 7.3%. In winter, the water temperature for mineral processing is usually ≤15℃, and the traditional collector can easily lead to a low recovery rate due to the decrease in solubility.
[0098] The difference between this embodiment and embodiment 1 is that in step S4 of this embodiment, the stirring speed is increased to 400 rpm, and the stirring time is extended by 2 min to provide high shear to promote low-temperature mutual solubility.
[0099] In step S5 of this embodiment, the stirring speed is increased to 500 rpm, and the stirring time is extended to 30 min.
[0100] In step S6 of this embodiment, after adding the buffer pair, the system is kept at 55℃ and stirred at 500 rpm for 15 min. The pH of the system is stabilized at 8.8, which is slightly lower than that in embodiment 1.
[0101] After the crude ore is subjected to two roughing, seven cleaning, and three scavenging, a concentrate is obtained. The flotation results are shown in Table 7.
[0102]
[0103] Table 7 As can be seen from Table 7, when the Inner Mongolia low-temperature fluorite ore is floated, the concentrate has a grade of 97.6% and a recovery rate of 88.5%. The solubility of the reagent reaches 35.2 g / L, which is significantly improved compared with the conventional formulation. The recovery rate in the low-temperature environment is only 2.3% lower than that at normal temperature, which confirms that a high proportion of ethylene glycol butyl ether and component optimization can effectively resist the influence of low temperature on the activity of the reagent.
[0104] Comparative Example 1 This comparative example differs from embodiment 1 in that only 100 parts of dehydroabietylamine is used, which is directly dissolved in 10 parts of ethylene glycol butyl ether to prepare a single collector.
[0105] The crude ore and the process remain the same as in embodiment 1. The flotation results are shown in Table 8.
[0106]
[0107] Table 8 Table 8 shows that the single dehydroabietylamine collector has a poor separation effect on low-sulfur dolomite ore: the concentrate Grade 94.2%, 4.3% lower than Example 1, recovery rate 80.7%, 8.5% lower than Example 1, Content 2.5%, 1.7 percentage points higher than Example 1, indicating the lack of synergistic effect of oleoyl sarcosine sodium and the inhibition of complex salt, and the significant decline of collection selectivity and efficiency.
[0108] Comparative Example 2 This comparative example is different from Example 2, specifically, the traditional fatty acid collector is used, specifically, 60 parts of sodium oleate and 40 parts of sodium stearate are mixed, the dosage is 250 g / t, the pulp pH is 9.5, and sodium carbonate is used for adjustment.
[0109] The raw ore and process remain the same as Example 2, and the flotation results are shown in Table 9.
[0110]
[0111] Table 9 In Table 9, the traditional fatty acid collector has poor separation effect on the angular breccia ore: concentrate Grade 92.5%, 4.7% lower than Example 2, recovery rate 72.3%, 13.3% lower than Example 2, -20 μm fine particle recovery rate is only 52.7%, 27.6% lower than Example 2, confirming that the traditional reagent cannot solve the problem of fine particle agglomeration, and has poor selectivity for fluorite and gangue.
[0112] Comparative Example 3 This comparative example is different from Example 3, specifically, sodium silicate and citric acid are deleted, and only the buffer is used to adjust the pH to 10.0.
[0113] The raw ore and process remain the same as Example 3, and the flotation results are shown in Table 10.
[0114]
[0115] Table 10 As can be seen from Table 10, after deleting the sodium silicate-citric acid complex salt, the S content of the high-sulfur ore concentrate is 0.87%, which is 0.62 percentage points higher than Example 3, Grade 91.3%, 5.5% lower than Example 3, recovery rate 82.6%, 1.7% lower than Example 3, indicating the lack of synergistic effect of complex salt, and the inability to effectively inhibit pyrite in an alkaline environment, resulting in a decrease in concentrate purity.
[0116] Comparative Example 4 This comparative example is different from Example 4 in that the components of Example 4 are added step by step: sodium silicate-citric acid composite salt is added first and stirred for 10 minutes; dehydroabietinamine and sodium oleoyl sarcosinate are then added and stirred for 10 minutes; and finally the buffer solution is added. The remaining parameters are the same as those of Example 4.
[0117] The raw ore and process were the same as those in Example 4. The flotation results are shown in Table 11.
[0118]
[0119] Table 11 Table 11 shows that when the reagent is added step by step, the high calcium carbonate ore concentrate The content is 6.8%, which is 4.7 percentage points higher than that of Example 4. The grade is 90.7%, which is 5.8% lower than that of Example 4, and the recovery rate is 75.4%, which is 7.3% lower than that of Example 4. This proves that the step-by-step addition destroys the ion pair pre-formation mechanism, and the synergistic adsorption rate of sodium oleoyl sarcosinate and dehydroabietinamine decreases, resulting in a recovery rate 7.3% lower than that of Example 4; calcite suppression is not timely, The content is 4.7 percentage points higher, highlighting the necessity of the pre-mixing process.
[0120] The technical scope of the present invention is not limited to the contents of the above description. Those skilled in the art can make various deformations and modifications to the above embodiments without departing from the technical idea of the present invention, and these deformations and modifications should all fall within the protection scope of the present invention.
Claims
1. A composite collector for flotation of fluorite ore, characterized in that, The composition comprises the following components in parts by weight: dehydroabietylamine 15-30 parts, sodium oleoyl sarcosinate 20-35 parts, sodium silicate-citric acid complex salt 20-40 parts, ethylene glycol butyl ether 10-20 parts, and sodium carbonate-sodium bicarbonate buffer pair 5-15 parts. The components synergize with each other to endow the composition with selective collecting ability for fluorite, inhibiting effect on gangue, and environmental adaptability, so as to realize the separation of various fluorite ores.
2. A composite collector for flotation of fluorite ores as claimed in claim 1, wherein: The weight ratio of sodium silicate to citric acid in the sodium silicate-citric acid complex salt is 1:0.5-2.
3. A composite collector for flotation of fluorite ores as claimed in claim 1, wherein: The weight ratio of sodium carbonate to sodium bicarbonate in the sodium carbonate-sodium bicarbonate buffer pair is 1:1-3:
1.
4. A composite collector for flotation of fluorite ores as claimed in claim 1, wherein: The dehydroabietylamine and the sodium oleoyl sarcosinate can form ion pairs through intermolecular forces, and the sodium silicate and the citric acid can form bridged complex compounds through hydrogen bonds.
5. A composite collector for flotation of fluorite ores as claimed in claim 1, wherein: The dehydroabietylamine realizes selective recognition of fluorite through the steric hindrance effect of the tricyclic phenanthrene skeleton, the sodium oleoyl sarcosinate enhances the adsorption stability on the surface of fluorite through the pH-responsive ionization characteristics, the sodium silicate-citric acid complex salt realizes targeted inhibition of gangue by forming a bridged complex structure, the ethylene glycol butyl ether improves the anti-interference ability of the system through complexation with hard ions, and the components synergize through specific effects to realize the separation effect.
6. A process for the preparation of a composite collector for flotation of fluorite ores, for the preparation of a composite collector for flotation of fluorite ores according to any one of claims 1 to 5, characterized in that, The method comprises the following steps: S1: mixing and reacting sodium silicate and citric acid in water to prepare a sodium silicate-citric acid complex salt; S2: mixing sodium carbonate and sodium bicarbonate to prepare a buffer pair; S3: mixing dehydroabietylamine and ethylene glycol butyl ether; S4: adding sodium oleoyl sarcosinate and the sodium silicate-citric acid complex salt to the mixture of S3 and mixing; S5: adding the buffer pair to the mixture of S4 and mixing until the pH of the system is stabilized at 7-10 to obtain a composite collector.
7. The method for preparing a composite collector for fluorite flotation according to claim 6, characterized in that: The mixing reaction of sodium silicate and citric acid in S1 is carried out in an aqueous medium, the reaction temperature is 40-60°C, and the reaction time is 20-50 min.
8. The method for preparing a composite collector for fluorite flotation according to claim 6, wherein: S3 to S5 are controlled by temperature progression and synergized with stirring, so that the dehydroabietylamine is first dispersed by the ethylene glycol butyl ether to form a basic system, then gradually reacts with the sodium oleoyl sarcosinate and the sodium silicate-citric acid complex salt, and finally the pH of the system is stabilized through the buffer pair, and the whole process maintains a homogeneous phase state to ensure the formation of a synergistic structure of the components.
9. Use of the composite collector for fluorite ore flotation according to any one of claims 1 to 5, characterized in that, The composite collector is used for the flotation of dolomite type, high-sulfur type, angular, high-calcium type, or high-siliceous fluorite ore, and the pH of the slurry during flotation is controlled at 7-10.
Citation Information
Patent Citations
A flotation composite collector, its preparation method and application
CN112246441B
A composite collector for fluorite ore flotation, its preparation method and application
CN113351375B
Cited By
Method for recovering tungsten from tungsten ore tailings
CN121178314A
Preparation method and application of fluorite flotation collecting agent based on mineral gene recognition