Cold-rolled high-temperature-oxidation-resistant hot-formed steel and preparation method thereof

By adding Cr and V elements to cold-rolled high-temperature oxidation-resistant hot-formed steel with low silicon content to form a dense oxide layer, the problem of oxidation and decarburization of hot-formed steel at high temperatures is solved, achieving high strength and oxidation resistance, and meeting the requirements of automotive lightweighting.

CN120830052APending Publication Date: 2025-10-24HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510924081.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-04
Publication Date
2025-10-24

AI Technical Summary

Technical Problem

Existing hot-formed steel is prone to oxidation and surface decarburization under high-temperature conditions, which affects its performance. It is also costly or poses a risk of cracking, making it difficult to meet the comprehensive performance requirements of high strength and oxidation resistance.

Method used

It uses cold-rolled high-temperature oxidation-resistant hot-formed steel with low silicon content, and forms a dense oxide layer by adding elements such as Cr and V. Combined with precise heat treatment process, a continuous dense oxide layer is formed, avoiding shot peening and allowing for direct coating.

Benefits of technology

It achieves excellent oxidation resistance at high temperatures, a smooth surface that requires no shot peening, high strength and high toughness, reduces energy consumption and costs, and meets the lightweight requirements of automobiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120830052A_ABST
    Figure CN120830052A_ABST
Patent Text Reader

Abstract

The invention relates to cold-rolled high-temperature-oxidation-resistant hot-formed steel and a preparation method thereof, and belongs to the technical field of steel and iron materials. The hot forming steel comprises the following chemical components in percentage by mass: 0.18 to 0.24 percent of C, 0.3 to 0.6 percent of Si, 0.8 to 1.3 percent of Mn, 2.5 to 5.2 percent of Cr, 0.03 to 0.07 percent of Ti, 0.025 to 0.05 percent of Al, 0.03 to 0.15 percent of V and the balance of Fe and inevitable impurities. Through alloying and thermoforming treatment processes, the obtained thermoformed steel has good oxidation resistance, meanwhile, an extremely thin oxide layer with excellent adhesion is generated on the surface of a component, shot blasting treatment is not needed after the thermoforming process, direct coating can be achieved, the content of Si in the steel grade is low, the influence on welding in the production process is avoided, and the production efficiency is improved. The comprehensive performance of high strength, high toughness and high-temperature oxidation resistance is realized.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The application belongs to the technical field of steel materials, and relates to a cold-rolled high-temperature oxidation-resistant hot forming steel and a preparation method thereof. BACKGROUND

[0002] Under the background of the global automobile industry's pursuit of lightweight and fuel efficiency improvement, the demand for high-strength steel materials for automobile bodies is increasingly urgent. However, with the increase of strength, the forming performance is significantly reduced. Directly processing forming by hot stamping forming solves the problem of easy cracking and large springback of ultra-high-strength steel cold stamping sheet, and improves the condition of simple shape of parts made of cold stamping high-strength steel sheet. The hot stamping forming technology is formed in the austenite phase zone under high temperature conditions, has small springback, is suitable for manufacturing complex structure parts, improves the part precision, and through the subsequent pressure holding quenching process, an ultra-high-strength steel part with uniform martensite structure can be obtained, effectively simplifying the design of vehicle body structure and parts, reducing the energy consumption and carbon emission of automobiles, and conforming to the green development road.

[0003] At present, there are mainly two kinds of hot forming steels in the market, namely, uncoated hot forming steel and plated hot forming steel. The uncoated hot forming steel does not adopt other treatment methods in the hot forming process, and has the characteristics of simple production process and low cost. However, oxidation easily occurs under the high temperature condition of hot forming, and decarburization appears on the surface, which affects the performance of the steel material. Meanwhile, shot blasting treatment is needed after hot forming, and the surface quality is poor, which affects the subsequent coating performance; the plated hot forming steel applies one or more metal plating layers on the surface of the steel material to provide additional protection and improve certain properties. Common plated hot forming steels include aluminum-silicon plating layer and zinc-based plating layer, which can effectively prevent surface decarburization and oxidation during steel heating process, and eliminate the subsequent shot blasting process. However, due to the patent restriction of aluminum-silicon plating layer, the cost of hot forming steel applying aluminum-silicon plating layer is high, and the zinc-based plating layer hot forming steel may appear liquid metal embrittlement (LME) during high temperature heating, which increases the risk of cracks generated in the forming process, and the common hydrogen embrittlement of hot forming steel also causes great limitation to the mass application of the material.

[0004] Patent application with publication number CN116949360A discloses a thin slab continuous casting and rolling 2000MPa grade high strength and plasticity oxidation resistant hot forming steel and its production method, its composition is like: C: 0.3%~0.4%, Mn: 1.0%~1.6%, Cr: 1.5~3.0%, Si: 1.0~2.0%, V: 0%~0.2%, the rest is Fe and inevitable impurity elements, by adding Cr, Si, improve the oxidation resistance effect of product surface in hot forming process, but high content of Si leads to the appearance of steel plate difficult to remove surface oxide scale, affect the welding process; Patent application with publication number CN117265225A discloses a hot forming steel with super strong oxidation resistance and its preparation method, by adding a certain content of rare earth elements (Ce, Y) combined with hot forming process improvement, promote the formation of very thin and dense structure of the oxidation layer on the surface of the steel plate, solve the mold wear problem caused by the falling of the oxidation layer, avoid the subsequent shot blasting treatment, can be directly coated, but the addition of rare earth elements increases the cost of steel, and the content of rare earth elements is difficult to control, which leads to unstable performance of steel and blocking of water gap in continuous casting process, affecting the product quality and industrial production. SUMMARY

[0005] To solve the above technical problems, the present application provides a cold-rolled high-temperature oxidation-resistant hot forming steel and a preparation method thereof. The obtained hot forming steel has good oxidation resistance and produces an extremely thin oxidation layer with excellent adhesion on the surface of the component. After the hot forming process, shot blasting treatment is not required, and direct coating is possible. The Si content in the steel grade is low, avoiding the impact on welding during production, and achieving high strength, high toughness, and comprehensive performance of high-temperature oxidation resistance.

[0006] To achieve the above-mentioned purposes, the technical solution adopted by the present application is as follows:

[0007] A cold-rolled high-temperature oxidation-resistant hot forming steel, the chemical composition and mass percentage are as follows: C: 0.18~0.24%, Si: 0.3~0.6%, Mn: 0.8~1.3%, Cr: 2.5~5.2%, Ti: 0.03~0.07%, Al: 0.025~0.05%, V: 0.03~0.15%, the balance is Fe and inevitable impurities.

[0008] Further, after simulating stamping forming, the hot forming steel forms a continuous and dense oxidation layer with a thickness of 3~4μm.

[0009] Further, after the hot forming process, the yield strength is ≥1100Pa, the tensile strength is ≥1500MPa, the total elongation is ≥7.0%, and the strength plasticity product is ≥11.8GPa%.

[0010] In another aspect, the present application also provides a production method of the cold-rolled high-temperature oxidation-resistant hot forming steel, which comprises vacuum melting, forging, hot rolling, acid rolling, continuous annealing, and hot forming processes.

[0011] In the hot forming process, the steel plate is heated to 870-930 DEG C, and held for 3-8 min to completely austenitize the steel plate; then stamping forming is performed; pressure holding rapid cooling quenching is performed, and the cooling rate is controlled to be 15-200 DEG C / s, so that the austenite is transformed into martensite, and the hot forming part is obtained by directly coating without shot blasting.

[0012] Further, in the forging process, the open forging temperature is 1100-1150 DEG C, and the finish forging temperature is 880-910 DEG C.

[0013] Further, in the hot rolling process, the open rolling temperature is 1100-1150 DEG C, and the finish rolling temperature is 880-900 DEG C.

[0014] Further, in the acid rolling process, the cold rolling reduction is controlled to be 40-70%, and the cold-rolled steel plate with a thickness of 1.0-2.4 mm is obtained.

[0015] Further, in the continuous annealing process, the cold-rolled steel plate is heated to 810-840 DEG C at a heating rate of 5-10 DEG C / s, held for 180-350 s, slowly cooled to 650 DEG C at a cooling rate of 8-11.88 DEG C / s, then rapidly cooled to 400-420 DEG C at a cooling rate of ≥28.75 DEG C / s, aged for 450-600 s to 380-400 DEG C, and then finally cooled to 150 DEG C at a cooling rate of 1.77-2.27 DEG C / s.

[0016] The mechanism and effect of the control of the content of each chemical component in the hot forming steel are as follows:

[0017] C: Carbon can improve the strength of the steel, affect the hardenability of the steel, form martensite in the quenching process, obtain higher strength and hardness, and ensure that the content of carbon element is ≥0.18% in order to obtain high-strength hot forming steel. When the content of carbon element is too high, the hydrogen brittleness sensitivity of the steel is increased, and the toughness of the steel is reduced. The content of carbon should not be more than 0.24%.

[0018] Si: Silicon can inhibit the precipitation of carbide, improve the toughness and plasticity of the steel, and reduce the generation of the oxide layer on the surface of the steel plate and improve the adhesion of the oxide layer. In the heating process, a thin oxide layer is formed on the surface of the steel, which can hinder the diffusion of oxygen elements and metal ions, and reduce the generation of loose oxide layer on the surface of the steel. In actual production, the enrichment of silicon in the near-surface layer leads to obvious surface decarburization in the welding process, reduces the strength of the part, and greatly affects the weldability of the on-site production. Lower silicon content is used to improve the adhesion of the surface oxide layer without causing a large amount of segregation in the near-surface layer.

[0019] Cr: Chromium as one of the core elements of the present application is the key element to make the steel have good high-temperature oxidation resistance. When the chromium content is ≥0.2%, a dense Cr2O3 oxidation layer can be generated on the surface of the steel; in addition, chromium can improve the hardenability of the steel, and solid solution in austenite improves the stability of austenite, which is beneficial to obtain full martensite structure during quenching. The present application realizes the regulation of the oxidation behavior of the steel under high temperature conditions by adding a large amount of chromium element, and enhances the high-temperature oxidation resistance. Because excessive chromium addition will reduce the brittleness and toughness, the corrosion resistance of the steel will change unexpectedly, therefore the chromium content is specified to 2.5-5.2%.

[0020] V: Vanadium can improve the strength of the steel, refine the grain, and improve the thermal stability and hardenability of the steel. Vanadium can effectively improve the hardenability of the steel, so that the steel obtains uniform martensite structure during quenching, thereby improving the overall performance of the steel, and in hot forming steel, vanadium can generate VC as a hydrogen trap to hinder the diffusion of hydrogen elements in the steel matrix, thereby reducing the influence of hydrogen embrittlement. Excessive vanadium will lead to reduced plasticity and increased brittleness of the steel, so the total content of vanadium is not more than 0.15%.

[0021] The beneficial effects produced by the above technical scheme are as follows:

[0022] (1) The high-temperature oxidation resistant hot forming steel provided by the present application is a cold rolled product compared with the existing coating-free hot forming steel product, the surface roughness of the steel plate is low, the waviness is relatively stable, and under the same thickness conditions, the developed steel has stronger mechanical properties, which can realize the replacement of traditional hot forming steel by thin gauge plate;

[0023] (2) The high-temperature oxidation resistant hot forming steel provided by the present application can realize rapid induction heating or infrared heating compared with the existing aluminum-silicon coated hot forming steel without coating, which reduces the heating and holding time in the hot forming process, reduces energy consumption, improves efficiency, reduces cost, and meets the application of industrial production;

[0024] (3) The high-temperature oxidation resistant hot forming steel provided by the present application adds an appropriate amount of Cr element to improve the high-temperature oxidation resistance of the steel plate, the oxidation weight gain rate per unit area of the steel plate at the surface layer is ≤0.1 g / (m 2· h), the oxidation layer thickness is <4 μm, and the oxidation resistance grade reaches level 1. After holding in the hot forming process, the steel can be directly formed in the atmosphere without protection, and after forming, there is no oxidation skin falling off, and no shot blasting treatment is needed, and the steel can be directly coated;

[0025] (4) The oxidation resistant coating-free hot forming steel provided by the present application adds vanadium (V) element to form carbide as a hydrogen trap in the steel matrix, which avoids the problem of hydrogen embrittlement of hot forming steel and improves the product quality; and refines the steel structure, so that the product has excellent comprehensive performance;

[0026] (5) The high-temperature oxidation-resistant hot forming steel provided by the application also has excellent mechanical properties, and after heat forming treatment, the yield strength is greater than or equal to 1100 MPa, the tensile strength is greater than or equal to 1500 MPa, the elongation is greater than or equal to 7%, and the product of strength and plasticity is greater than or equal to 11.8 GPa · .

[0027] The hot forming steel of the application realizes the self-protection function in a high-temperature environment through alloying and heat treatment processes, thereby avoiding the performance degradation of traditional hot forming steel in the high-temperature oxidation process. In the application, a high proportion of chromium (Cr) element is added to the base steel to form a dense and stable oxidation layer during austenitizing, effectively isolating the contact between the steel and oxygen; the silicon (Si) element content is reduced to reduce surface decarburization and reduce welding problems; vanadium (V) element is added to refine the material organization and reduce the hydrogen embrittlement of the hot forming steel. By precisely controlling the heating temperature, holding time and cooling rate in the heat treatment process, the microstructure of the steel is optimized, and the mechanical properties are improved. The hot forming steel of the application can still maintain high strength and good plasticity without relying on external coating, can improve the environmental adaptability and service life of the material, and meets the demand of the automobile industry for high-strength, lightweight materials. And has the advantages of low production cost and simple manufacturing process. BRIEF DESCRIPTION OF DRAWINGS

[0028] Figure 1 is the continuous annealing process curve diagram of the application;

[0029] Figure 2 is the metallographic structure diagram of the hot-rolled slab of Example 4 of the application;

[0030] Figure 3 is the metallographic structure diagram of the hot-formed slab of the cold-rolled plate of Example 4;

[0031] Figure 4 is the stress-strain curve diagram of the A50 tensile sample of the hot-formed slab of Example 4;

[0032] Figure 5 is the cross-section oxidation layer thickness diagram of the hot-formed slab of Example 4. DETAILED DESCRIPTION

[0033] The application will be further described in detail below in combination with specific embodiments.

[0034] Examples 1-8

[0035] The production method of the cold-rolled high-temperature oxidation-resistant hot forming steel of the application includes vacuum melting, forging, hot rolling, acid rolling, continuous annealing and hot forming processes. The specific steps are as follows:

[0036] (1) Vacuum melting process: ingredients are prepared according to target composition, raw materials are smelted in a vacuum induction furnace and cast, impurity element content is strictly controlled during smelting, and sampling test composition is performed before tapping to adjust to target composition;

[0037] (2) Forging process: the ingot is heated to 1200-1250℃ in an electric resistance furnace, homogenized for 2 hours, then forged, the open forging temperature is 1100-1150℃, the finish forging temperature is 880-910℃, and a long blank is obtained after forging;

[0038] (3) Hot rolling process: the forged long blank is heated to 1200-1250℃ and homogenized for 1 hour, then hot rolled, the open rolling temperature is 1100-1150℃, and the finish rolling temperature is 880-900℃, to obtain a hot rolled coil with a thickness of 3.5mm;

[0039] (4) Pickling process: the hot rolled coil is subjected to tension and correction pickling, then subjected to multi-pass cold rolling by cold rolling rollers, the cold rolling reduction is controlled at 40-60%, to obtain a cold rolled steel plate with a thickness of 1.0-2.4mm;

[0040] (5) Continuous annealing process: under a nitrogen protective atmosphere, the cold rolled steel plate is heated to 810-840℃ at a rate of 5-10℃ / s, homogenized for 180-350s, slowly cooled to 650℃ at a rate of 8-11.88℃ / s, then rapidly cooled to 400-420℃ at a rate of ≥28.75℃ / s, aged for 450-600s to 380-400℃, and finally cooled to 150℃ at a rate of 1.77-2.27℃ / s.

[0041] (6) Hot forming process: the hot stamping forming steel plate is heated to 870-930℃ and homogenized for 3-8min, after the steel plate is completely austenitized, it is sent to a stamping die with a cooling system for pressure quenching, the cooling rate is controlled at 50-200℃ / s to convert austenite to martensite, and a hot formed steel part is obtained.

[0042] The process parameter settings of each embodiment are shown in Tables 1-3, the chemical composition of the hot forming steel is shown in Table 4, the surface state parameters of the cold rolled plate after annealing are shown in Table 5, and the mechanical properties, oxide layer thickness and weight gain of the steel plate after hot forming are shown in Table 6.

[0043] Table 1: Forging and hot rolling process parameters of each embodiment

[0044]

[0045] Table 2: Annealing process parameters of each embodiment

[0046]

[0047] Table 3 Parameters of pickling and hot forming processes in various embodiments

[0048]

[0049]

[0050] Table 4 Chemical composition of hot-formed steel in various embodiments (mass percentage, %)

[0051] Example C Si Mn Cr V Al Ti 1 0.19 0.60 1.30 5.20 0.03 0.025 0.03 2 0.20 0.55 1.23 4.46 0.05 0.026 0.03 3 0.24 0.51 1.12 4.02 0.04 0.033 0.04 4 0.23 0.41 1.11 3.51 0.09 0.035 0.05 5 0.22 0.51 0.83 3.04 0.13 0.048 0.05 6 0.22 0.32 0.80 2.50 0.07 0.047 0.06 7 0.18 0.30 0.85 3.52 0.15 0.050 0.07 8 0.21 0.43 0.91 2.87 0.067 0.048 0.07

[0052] Table 5 Surface state parameters of each embodiment before thermoforming

[0053] Example Roughness Ra / pm Waviness Wsa / pm Infrared absorption / % Permeability / p 1 2.1 0.23 73 716 2 2.0 0.22 72 825 3 2.3 0.25 72 782 4 1.98 0.28 87 790 5 2.1 0.27 78 830 6 1.94 0.25 83 769 7 1.89 0.24 85 839 8 1.85 0.22 72 780

[0054] Table 6 Mechanical properties, oxide layer thickness and weight gain of steel plates after hot forming in each embodiment

[0055]

[0056] Depend on Figure 2 It can be seen that the metallographic structure of the hot-rolled steel plate of the present invention is ferrite + pearlite structure. Figure 3 It can be seen that the metallographic structure of the cold-rolled sheet after hot forming is a martensite structure.

[0057] Depend on Figure 4 It can be seen that the stress-strain curve of the slab after thermoforming of the present invention has higher strength and larger elongation.

[0058] Depend on Figure 5 It can be seen that after the simulated flat die quenching, the steel plate of the present invention has a continuous and complete oxide layer with a thickness of 3.61 μm, and has excellent high-temperature oxidation resistance.

Claims

1. A cold-rolled, high-temperature oxidation-resistant hot-formed steel, characterized in that, The chemical composition and mass percentage content are as follows: C: 0.18-0.24%, Si: 0.3-0.6%, Mn: 0.8-1.3%, Cr: 2.5-5.2%, Ti: 0.03-0.07%, Al: 0.025-0.05%, V: 0.03-0.15%, and the balance of Fe and inevitable impurities.

2. - Cold rolled high temperature oxidation resistant press hardening steel according to claim 1, characterized in that, After the hot forming steel is simulated stamping forming, a continuous and dense oxide layer is formed, and the thickness is 3-4 microns.

3. - Cold rolled high temperature oxidation resistant press hardening steel according to claim 2, characterized in that, After the hot forming process, the yield strength is greater than or equal to 1100 Pa, the tensile strength is greater than or equal to 1500 MPa, the total elongation is greater than or equal to 7.0%, and the strength plastic product is greater than or equal to 11.8 GPa%.

4. Process for the production of a cold rolled temperature resistant hot formed steel according to any one of claims 1 to 3, characterized in that, The hot forming process comprises vacuum melting, forging, hot rolling, acid rolling, continuous annealing, and hot forming processes. In the hot forming process, the steel plate is heated to 870-930 DEG C, and the temperature is kept for 3-8 minutes to make the steel plate completely austenitic, then stamping forming is carried out, and the pressure is kept and rapidly cooled to quench, the cooling speed is controlled to be 15-200 DEG C / s, the austenite is converted into martensite, and the hot forming parts are obtained by directly coating without shot blasting.

5. Process for the production of a cold rolled temperature resistant oxidizable hot formed steel according to claim 4, characterized in that, In the forging process, the open forging temperature is 1100-1150 DEG C, and the final forging temperature is 880-910 DEG C.

6. Process for the production of a cold rolled temperature resistant oxidizable hot formed steel according to claim 5, characterized in that, In the hot rolling process, the open rolling temperature is 1100-1150 DEG C, and the final rolling temperature is 880-900 DEG C.

7. Process for the production of a cold rolled temperature resistant oxidizable hot formed steel according to claim 6, characterized in that, In the acid rolling process, the cold rolling reduction is controlled to be 40-70%, and the cold rolled steel plate with a thickness of 1.0-2.4 mm is obtained.

8. Process for the production of a cold rolled temperature resistant oxidizable hot formed steel according to claim 7, characterized in that, In the continuous annealing process, the cold rolled steel plate is heated to 810-840 DEG C at a speed of 5-10 DEG C / s, kept for 180-350 s, slowly cooled to 650 DEG C at a speed of 8-11.88 DEG C / s, then rapidly cooled to 400-420 DEG C at a speed of greater than or equal to 28.75 DEG C / s, aged for 450-600 s to 380-400 DEG C, and finally cooled to 150 DEG C at a speed of 1.77-2.27 DEG C / s.

Citation Information

Patent Citations

  • Thin slab continuous casting and rolling 2000MPa-grade high-strength plastic anti-oxidation hot forming steel and production method thereof

    CN116949360A

  • Hot forming steel with super-strong oxidation resistance and preparation method of hot forming steel

    CN117265225A