Pearl viscose composite fiber long-acting antibacterial fabric and chemical additive-free process

By combining the synergistic innovation of the porous sheath slow-release antibacterial mechanism of pearl viscose composite fiber with the physical enhancement of honeycomb structure, the problems of biosafety and functional durability of existing antibacterial fabrics have been solved, realizing pearl viscose composite fiber fabrics with high-efficiency antibacterial properties and environmentally friendly production.

CN120840190APending Publication Date: 2025-10-28SHANGHAI COOL BING KURE BRAND MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510990710.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-07-17
Publication Date
2025-10-28

AI Technical Summary

Technical Problem

Existing antibacterial fabrics rely on chemical antibacterial agents, which have defects in biosafety and insufficient functional durability. Chemical auxiliaries need to be added during the production process, resulting in environmental burden.

Method used

By employing the synergistic innovation of the porous skin slow-release antibacterial mechanism of pearl viscose composite fiber and the physical trapping effect of honeycomb structure, pearl viscose composite fiber fabric is prepared through a three-layer composite structure without chemical additives. This includes the fine weaving and hot-melt bonding of the front antibacterial layer, the reverse skin-friendly layer and the middle moisture-wicking layer.

Benefits of technology

It achieves a breakthrough in antibacterial durability, biosafety, and user comfort without the addition of any chemical additives throughout the entire process. The antibacterial rate is still ≥96.7% after 50 washes, reducing production costs by 23.5% and carbon emissions by 39.5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120840190A_ABST
    Figure CN120840190A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of functional textile materials, and discloses a pearl viscose composite fiber long-acting antibacterial fabric and a chemical additive-free process. Through the cooperation of a porous cortex layer slow-release antibacterial mechanism of the pearl viscose fibers and physical trapping synergism of a honeycomb structure, under the condition that no chemical additive is added in the whole process, synchronous breakthrough of antibacterial durability, biological safety and taking comfort is achieved, meanwhile, the production cost is reduced, and the production efficiency is improved. The contradiction that the safety risk and the function attenuation of the traditional antibacterial fabric are irreconcilable is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional textile materials technology, specifically to a pearl viscose composite fiber long-lasting antibacterial fabric and a chemical-free auxiliary agent process. Background Technology

[0002] Current antibacterial fabrics mainly rely on chemical technologies such as silver ions, organic quaternary ammonium salts, and nano zinc oxide. Silver ions pose a risk of heavy metal leaching (exceeding the standard rate >23%, leaching amount >100ppm), which can lead to cumulative toxicity in the human body; organic quaternary ammonium salts experience a decrease in antibacterial rate of >65% after 20 washes and induce microbial resistance; nano zinc oxide decomposes rapidly under ultraviolet radiation, with an outdoor lifespan of less than 3 months, severely limiting functional durability.

[0003] The aforementioned technologies, relying on chemical antibacterial agents, generally suffer from biosafety defects (heavy metal leaching, induced drug resistance) and insufficient functional durability (washing / light exposure failure). Furthermore, the production process requires the addition of chemical auxiliaries, exacerbating the environmental burden. The industry urgently needs to develop a safe fabric based on a physical antibacterial mechanism, washable, and without any chemical additives throughout the entire process, to overcome the irreconcilable contradiction between safety risks and functional degradation in existing technologies. Therefore, a long-lasting antibacterial fabric made of pearl viscose composite fiber and a chemical-free process are proposed. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention provides a long-lasting antibacterial fabric made of pearl viscose composite fiber and a chemical-free process to solve the problems in the prior art.

[0005] To achieve the above objectives, the present invention provides the following technical solution:

[0006] Firstly, a pearl viscose composite fiber long-lasting antibacterial fabric includes a three-layer composite structure:

[0007] Front antibacterial layer: formed by a honeycomb raised structure woven from blended yarn using a double needle bed warp knitting machine, with a honeycomb diameter of 0.5mm±0.05 and a depth of 0.2mm. The blended yarn includes cotton fiber, Tencel fiber, polyester fiber and pearl viscose composite fiber.

[0008] The reverse skin-friendly layer is woven from modal spandex core-spun yarn using a weft-insertion method to form a double-ribbed groove structure. The groove width is 80μm, the depth is 50μm, and the groove density is 80-120 grooves / cm. 2 ;

[0009] Intermediate moisture-wicking layer: Located between the front antibacterial layer and the back skin-friendly layer, it is made of polyester filaments orthogonally woven mesh structure with a warp density of 420 threads / 10cm, a weft density of 380 threads / 10cm, and a mesh pore size of 50μm±5.

[0010] Preferably, the blended yarn composition of the front antibacterial layer is 25wt%-35wt% cotton fiber, 25wt%-35wt% Tencel fiber, 15wt%-25wt% polyester fiber, and 15wt%-25wt% pearl viscose composite fiber.

[0011] Preferably, the modal spandex core-spun yarn of the reverse skin-friendly layer uses 40D spandex filament as the core yarn and is wrapped with 60S modal yarn, with a composition ratio of 90wt%-94wt% modal fiber and 6wt%-10wt% spandex.

[0012] Preferably, the polyester filament fineness of the intermediate moisture-wicking layer is 0.4D-0.6D.

[0013] Secondly, a chemical-free process for preparing a pearl viscose composite fiber long-lasting antibacterial fabric includes the following steps:

[0014] Front antibacterial layer: Based on the front antibacterial layer material described in claim 2, it is woven from 60S blended yarn through a 28G double needle bed warp knitting machine. The needles of the double needle bed warp knitting machine move according to the padding yarn digital "2-3 / 1-0 / 1-2 / 3-4", and the loop depth is 3.4mm-3.6mm, forming a honeycomb structure front antibacterial layer.

[0015] Intermediate moisture-wicking layer: Based on the intermediate moisture-wicking layer material described in claim 4, a mesh is woven by introducing weft yarns at a speed of 600rpm-700rpm using an air-jet loom (main nozzle pressure 0.3MPa-0.4MPa), and then heat-fused and bonded to the front antibacterial layer, with interlayer misalignment ≤0.1mm;

[0016] Reverse skin-friendly layer: Based on the reverse skin-friendly layer material described in claim 3, a double needle bed warp knitting machine is used, with the rear needle bed fully threaded with modal spandex core-spun yarn and the front needle bed intermittently threaded with the same type of modal spandex core-spun yarn (1 thread and 1 gap), forming a double-threaded groove structure through weft insertion movement, and then thermally bonded to the intermediate moisture-wicking layer.

[0017] Preferably, the pearl viscose composite fiber in the front antibacterial layer is prepared by the following steps:

[0018] 1-micron aragonite-type pearl powder (CaCO3 content ≥95%, particle size D50=1.0±0.2μm) was modified with silane coupling agent KH-550 to obtain modified pearl powder. The amount of silane coupling agent added was 1.5-2% of the pearl powder mass.

[0019] Modified pearl powder was dispersed at 5-8 wt% in viscose spinning solution (α-cellulose ≥92%), and homogenized under high pressure of 45-55 MPa for 3 cycles to make the particle size distribution of the modified pearl powder dispersed phase D90 ≤ 2 μm.

[0020] The homogenized pearl powder / viscose dispersion was extruded through a spinneret using wet spinning technology and then fed into a coagulation bath containing 10% H2SO4 + 15% Na2SO4 at a draw ratio of 1:3.2 to obtain pearl viscose composite fibers with a porous skin structure.

[0021] Preferably, the intermediate moisture-wicking layer is treated with 1000W plasma for 55-65 seconds after spinning to achieve permanent water repellency.

[0022] Preferably, after spinning, the antibacterial layer on the front side is cyclically set for 30-40 seconds using hot air at 122℃, overfeed rate +8%, and wind speed of 8m / s.

[0023] Preferably, after spinning, the reverse skin-friendly layer is fixed by infrared radiation at 175°C for 10-14 seconds (wavelength 3.5μm) to instantly lock in its elasticity.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] This invention achieves a breakthrough in antibacterial durability, biocompatibility, and wearing comfort simultaneously by combining the slow-release antibacterial mechanism of the porous outer layer of pearl viscose fiber with the enhanced physical trapping effect of the honeycomb structure, all without the addition of any chemical additives. At the same time, it reduces production costs and completely resolves the irreconcilable contradiction between the safety risks and functional degradation of traditional antibacterial fabrics.

[0026] Other features and advantages of the invention will be set forth in the description which follows, and will be apparent in part from the description, or may be learned by practicing the invention. The objects and other advantages of the invention may be realized and obtained by means of the structures pointed out in the description, claims and drawings. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the three-layer composite structure of the pearl viscose composite fiber long-lasting antibacterial fabric of the present invention.

[0028] Figure 2 This is an electron microscope image showing the multi-level micro / nano structure characteristics of the pearl powder of this invention;

[0029] Figure 3 This is an electron micrograph of the synergistic antibacterial mechanism of the pearl fiber / honeycomb structure of the present invention. Detailed Implementation

[0030] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] Please see Figures 1-3 The present invention discloses a pearl viscose composite fiber long-lasting antibacterial fabric and a chemical-free auxiliary agent process, comprising the following:

[0032] 1. Preparation of pearl viscose composite fiber

[0033] 1) Raw material screening and pretreatment:

[0034] Pearl powder treatment:

[0035] Raw material screening: X-ray diffraction (XRD, Rigaku SmartLab) was used to verify aragonite-type pearl powder, and batches with CaCO3 content ≥98% were screened.

[0036] Particle size control: Pearl powder with D50 = 1.0 ± 0.2 μm was sorted by a laser particle size analyzer (Malvern Mastersizer 3000).

[0037] Surface modification:

[0038] The selected aragonite-type pearl powder was modified using silane coupling agent KH-550 to obtain modified pearl powder. The amount of silane coupling agent added was 1.5-2% of the pearl powder mass.

[0039] KH-550 silane coupling agent forms Si-O-Ca bonds on the surface of pearl powder, enhancing the interfacial bonding force with adhesive.

[0040] 2) Preparation of pearl powder / viscose dispersion system

[0041] Raw material selection: Select viscose spinning solution with α-cellulose ≥ 92%.

[0042] High-pressure homogenization process:

[0043] Modified pearl powder was added to viscose spinning solution at a ratio of 6 wt%.

[0044] Modified pearl powder and viscose spinning solution were circulated three times in a 50MPa high-pressure homogenizer.

[0045] The particle size distribution of the modified pearl powder dispersion phase is D90≤2μm.

[0046] High-pressure shearing force breaks down pearl powder agglomerates, ensuring the fluidity of the spinning solution and the uniform distribution of pearl powder in the fiber.

[0047] 3) Wet spinning forming

[0048] The homogenized pearl powder / viscose dispersion was extruded through a spinneret using wet spinning technology.

[0049] The extruded spinneret is solidified in a coagulation bath containing 10% H2SO4 + 15% Na2SO4 at a draw ratio of 1:3.2 to obtain pearl viscose composite fiber with a porous skin structure.

[0050] The porous cortex structure of pearl viscose composite fibers was analyzed, and EDS verification showed that when the Ca enrichment was ≥10 at%, the Ca content in sweat was high. 2+ Sustained release ≥120 mg / L (ICP-OES assay);

[0051] The specific surface area of ​​the pearl viscose composite fiber was measured to be ≥15m² using the BET method. 2 / g.

[0052] Porous cortex accelerates Ca 2+ The pearl powder in the blended yarn is exposed at a rate of ≥65%, allowing it to directly contact bacteria and improve antibacterial efficiency.

[0053] 2. Three-layer antibacterial fabric weaving

[0054] 1) Front antibacterial layer: honeycomb structure fabric

[0055] Element Proportion effect cotton fiber 30wt% Enhanced moisture absorption Tencel fiber 30wt% Improve flexibility polyester fiber 20wt% Increase structural strength Pearl viscose fiber 20wt% Core antibacterial function

[0056] It is woven from 60S blended yarn (30wt% cotton fiber + 30wt% Tencel fiber + 20wt% polyester fiber + 20wt% pearl viscose fiber) using a 28G double needle bed warp knitting machine. The front antibacterial layer has a honeycomb raised structure (0.5mm ± 0.05mm honeycomb diameter and 0.2mm depth) using padding yarn digital 2-3 / 1-0 / 1-2 / 3-4 (GB1 comb bar) and a loop depth of 3.5mm.

[0057] Pearl powder is concentrated on the inner wall of the honeycomb cell, and SEM shows that it accounts for ≥70%;

[0058] The honeycomb-shaped protrusion structure mechanically locks in bacteria. High-speed photography was used to verify the difference between fabrics with and without the honeycomb-shaped protrusion structure. The results showed that the fabric with the honeycomb-shaped protrusion structure could extend the contact time to 42.7 minutes, thereby improving the sterilization effect.

[0059] Front antibacterial layer shaping:

[0060] A hot air tenter frame is used with 122℃ hot air, an overfeed rate of +8%, and an air speed of 8m / s to circulate and shape the antibacterial layer on the front of the honeycomb raised structure for 30-40 seconds to stabilize the honeycomb structure.

[0061] 2) Intermediate moisture-wicking layer: mesh structure fabrication

[0062] Raw material: 0.5D ultrafine polyester filament.

[0063] Weaving process:

[0064] An air-jet loom is used, with a set machine speed of 650 rpm, a main nozzle pressure of 0.35 MPa, a warp density of 420 ends / 10 cm, and a weft density of 380 ends / 10 cm.

[0065] An air-jet loom introduces weft yarns to weave an intermediate moisture-wicking layer with a mesh structure of 50μm±5 mesh apertures.

[0066] Plasma water-repellent treatment:

[0067] A plasma system was used to treat the middle moisture-wicking layer of the mesh structure with 1000W plasma for 60 seconds, making the contact angle of the middle moisture-wicking layer >130°, achieving permanent water repellency, blocking sweat back seepage, and protecting the activity of pearl powder. After washing the fabric 50 times, SEM showed that the pearl powder activity retention rate was still 95.2% and the antibacterial rate was still ≥96.7%.

[0068] Orthogonal mesh for rapid moisture wicking (capillary effect), water-repellent treatment to prevent sweat backflow and protect pearl activity.

[0069] 3) Reverse skin-friendly layer: grooved structure weave

[0070] Preparation of core-spun yarn:

[0071] The core yarn is made of 40D spandex, and the outer yarn is made of 60S modal yarn. The modal yarn is wrapped around the core yarn in a ratio of 92wt%:8wt% through a core-spun process to form modal spandex core-spun yarn.

[0072] Double-groove weaving:

[0073] Using a double-needle-bed warp knitting machine, modal spandex core-spun yarn is fully threaded onto the back needle bed, while modal spandex core-spun yarn is threaded 1-1-open onto the front needle bed. Through weft insertion, a double-ribbed groove structure is formed, with grooves 80μm wide and 50μm deep, and a groove density of 98 grooves / cm². 2 .

[0074] The grooved structure accelerates sweat diffusion; tested according to GB / T 12704.2 standard, the measured moisture permeability is ≥13000g / m². 2 / 24h.

[0075] Reverse skin-friendly layer shaping:

[0076] An infrared radiation setting machine is used to set the skin-friendly layer on the reverse side of the double-threaded groove structure for 12 seconds (wavelength 3.5μm) with infrared radiation at 175℃, instantly locking its elasticity.

[0077] 3. Interlayer bonding and finishing

[0078] 1) Hot melt adhesive composite

[0079] The antibacterial layer on the front and the moisture-wicking layer in the middle are first laminated using a hot press laminating machine, with an interlayer misalignment of ≤0.1mm.

[0080] The antibacterial front layer / moisture-wicking middle layer is then laminated with the skin-friendly layer to form a pearl viscose composite fiber long-lasting antibacterial fabric.

[0081] Example:

[0082] Taking Staphylococcus aureus as an example, according to GB / T 20944.3, the antibacterial rate of this pearl viscose composite fiber long-lasting antibacterial fabric can reach ≥95%, and no heavy metals or other pollutants were detected.

[0083] This invention utilizes the porous outer layer of pearl fibers to slowly release antibacterial (Ca) 2+ The synergistic innovation of ≥120mg / L and honeycomb structure physical enhancement (contact area ↑229%) achieves an antibacterial rate of ≥96.7% after 50 washes without any chemical additives, while reducing production costs by 23.5% and carbon emissions by 39.5%, completely breaking through the dilemma of safety risks and functional degradation of traditional antibacterial fabrics.

Claims

1. A pearl viscose composite fiber long-lasting antibacterial fabric, characterized in that, Includes a three-layer composite structure: Front antibacterial layer: formed by a honeycomb raised structure woven from blended yarn using a double needle bed warp knitting machine, with a honeycomb diameter of 0.5mm±0.05 and a depth of 0.2mm. The blended yarn includes cotton fiber, Tencel fiber, polyester fiber and pearl viscose composite fiber. The reverse skin-friendly layer is woven from modal spandex core-spun yarn using a weft-insertion method to form a double-ribbed groove structure. The groove width is 80μm, the depth is 50μm, and the groove density is 80-120 grooves / cm. 2 ; Intermediate moisture-wicking layer: Located between the front antibacterial layer and the back skin-friendly layer, it is made of polyester filaments orthogonally woven mesh structure with a warp density of 420 threads / 10cm, a weft density of 380 threads / 10cm, and a mesh pore size of 50μm±5.

2. The pearl viscose composite fiber long-lasting antibacterial fabric according to claim 1, characterized in that, The blended yarn composition of the front antibacterial layer is 25wt%-35wt% cotton fiber, 25wt%-35wt% Tencel fiber, 15wt%-25wt% polyester fiber, and 15wt%-25wt% pearl viscose composite fiber.

3. The pearl viscose composite fiber long-lasting antibacterial fabric according to claim 1, characterized in that, The reverse skin-friendly layer's modal spandex core-spun yarn uses 40D spandex filament as the core yarn and is wrapped with 60S modal yarn, with a composition ratio of 90wt%-94wt% modal fiber and 6wt%-10wt% spandex.

4. The pearl viscose composite fiber long-lasting antibacterial fabric according to claim 1, characterized in that, The polyester filament fineness of the intermediate moisture-wicking layer is 0.4D-0.6D.

5. A chemical-free process for a pearl viscose composite fiber long-lasting antibacterial fabric, characterized in that, The process for preparing the fabric according to claims 1-4 includes the following steps: Front antibacterial layer: Based on the front antibacterial layer material described in claim 2, it is woven from 60S blended yarn using a 28G double needle bed warp knitting machine. The needles of the double needle bed warp knitting machine move according to the padding yarn digital "2-3 / 1-0 / 1-2 / 3-4", and the loop depth is 3.4mm-3.6mm, forming a honeycomb structure front antibacterial layer. Intermediate moisture-wicking layer: Based on the intermediate moisture-wicking layer material described in claim 4, a mesh is woven by introducing weft yarns at a speed of 600rpm-700rpm using an air-jet loom (main nozzle pressure 0.3MPa-0.4MPa), and then heat-fused and bonded to the front antibacterial layer, with interlayer misalignment ≤0.1mm; Reverse skin-friendly layer: Based on the reverse skin-friendly layer material described in claim 3, a double needle bed warp knitting machine is used, with the rear needle bed fully threaded with modal spandex core-spun yarn and the front needle bed intermittently threaded with the same type of modal spandex core-spun yarn (1 thread and 1 gap), forming a double-threaded groove structure through weft insertion movement, and then thermally bonded to the intermediate moisture-wicking layer.

6. The chemical-free process for a pearl viscose composite fiber long-lasting antibacterial fabric according to claim 5, characterized in that, The pearl adhesive composite fiber in the front antibacterial layer is prepared through the following steps: 1-micron aragonite-type pearl powder (CaCO3 content ≥95%, particle size D50=1.0±0.2μm) was modified with silane coupling agent KH-550 to obtain modified pearl powder. The amount of silane coupling agent added was 1.5-2% of the pearl powder mass. Modified pearl powder was dispersed at 5-8 wt% in viscose spinning solution (α-cellulose ≥92%), and homogenized under high pressure of 45-55 MPa for 3 cycles to make the particle size distribution of the modified pearl powder dispersed phase D90 ≤ 2 μm. The homogenized pearl powder / viscose dispersion was extruded through a spinneret using wet spinning technology and then fed into a coagulation bath containing 10% H2SO4 + 15% Na2SO4 at a draw ratio of 1:3.2 to obtain pearl viscose composite fibers with a porous skin structure.

7. The chemical-free process for a pearl viscose composite fiber long-lasting antibacterial fabric according to claim 5, characterized in that, After spinning, the intermediate moisture-wicking layer is treated with 1000W plasma for 55-65 seconds to achieve permanent water repellency.

8. The chemical-free process for a pearl viscose composite fiber long-lasting antibacterial fabric according to claim 5, characterized in that, After spinning, the antibacterial layer on the front is circulated and set for 30-40 seconds using hot air at 122℃, overfeed rate +8%, and wind speed of 8m / s.

9. The chemical-free process for a pearl viscose composite fiber long-lasting antibacterial fabric according to claim 5, characterized in that, After spinning, the reverse skin-friendly layer is fixed by infrared radiation at 175°C for 10-14 seconds (wavelength 3.5μm) to instantly lock in its elasticity.