Self-adaptive color-changing device based on viologen derivative electrolyte as well as preparation method and application of self-adaptive color-changing device

By using a color-changing device combining 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine with zinc and platinum electrodes, the problems of poor cycle stability and dependence on electrical energy are solved, realizing the fast response and large light modulation of the adaptive color-changing device, which is suitable for energy-saving buildings and intelligent windows for transportation.

CN120848075APending Publication Date: 2025-10-28UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511077561.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-08-01
Publication Date
2025-10-28

AI Technical Summary

Technical Problem

Existing color-changing devices using 4,4′-bipyridine and its derivatives as electrochromic materials suffer from poor cycle stability, dependence on electrical energy, and slow response speed, which limits their application range.

Method used

Using 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine as electrochromic materials, combined with zinc and platinum electrodes, the inherent potential difference between transparent conductive glass/zinc and transparent conductive glass/platinum drives interfacial charge transfer, achieving adaptive coloring and fading.

Benefits of technology

It enables rapid and autonomous adjustment of coloring and fading without the need for an external power supply, and features a fast response speed and a large light modulation amplitude, thus expanding its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120848075A_ABST
    Figure CN120848075A_ABST
Patent Text Reader

Abstract

The invention relates to a self-adaptive color-changing device based on viologen derivative electrolyte and a preparation method and application of the self-adaptive color-changing device, the color-changing device comprises a color-changing device cavity and a built-in electrochromic solution, the color-changing device cavity comprises an electrode frame, and a first transparent conductive substrate and a second transparent conductive substrate which are arranged on the two sides of the electrode frame; the electrochromic solution comprises a 4, 4 '-bipyridine derivative, zinc chloride and hydrochloric acid; the 4, 4 '-dipyridyl derivative is selected from 1-butyl-4, 4'-dipyridyl or 1-butyl-1 '-(2-propenyl)-4, 4'-dipyridyl, and the structural formula of the 4, 4 '-dipyridyl derivative is shown in the description. Compared with the prior art, the color-changing device can achieve self-coloring and color fading without being powered on, has high response speed and large light modulation amplitude, and can be applied to energy-saving buildings, traffic intelligent windows and related fields of the energy-saving buildings, the traffic intelligent windows and the related fields of the energy-saving buildings and the traffic intelligent windows.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials technology and relates to an adaptive color-changing device based on viologen derivative electrolyte, its preparation method and application; in particular, it relates to an adaptive color-changing device based on 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine electrolyte, its preparation method and application. Background Technology

[0002] Smart windows are energy-saving devices whose light transmittance can be reversibly adjusted via an external power source. They are primarily used in construction, transportation, and aerospace, significantly reducing energy consumption and contributing to global carbon neutrality goals. However, electrochromic smart windows, characterized by rapid response, large light modulation, and excellent controllability, typically require an external power source, which greatly limits their energy-saving effects and application scope. Therefore, a novel smart window that requires no external power input is a pressing issue.

[0003] Integrating active metal electrodes into electrochromic devices can reduce their dependence on external power sources. Therefore, electrochromic devices incorporating aluminum, zinc, and magnesium anodes have become an attractive platform for realizing self-powered electrochromic devices, where the fading of Prussian blue and the coloring of tungsten oxide can be achieved rapidly by connecting to a metal anode. However, fading Prussian blue and coloring tungsten oxide typically require a slow oxidation process to return to their initial state. Compared to inorganic electrochromic materials that rely on redox reactions of metal ions or protons, small organic electrochromic molecules offer a superior alternative. 4,4′-bipyridine and its derivatives, as important small organic molecule electrochromic materials, have been extensively studied. However, in existing technologies, bis(3-hydroxyethyl)violin dibromide exhibits poor cycling stability and slow response in electrochromic devices, and also suffers from dependence on electrical energy. Summary of the Invention

[0004] The purpose of this invention is to provide an adaptive color-changing device based on viologen derivative electrolytes, its preparation method, and its application. Using 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine as the electrochromic material, an adaptive color-changing device is obtained. This effectively solves the problems of poor cycle stability and dependence on electrical energy caused by using 4,4′-bipyridine and its derivatives as electrochromic materials in the prior art. The resulting color-changing device can achieve autonomous control of coloring and fading without power, exhibiting a certain degree of adaptability, and has a fast response speed and a large light modulation amplitude. It can be applied to energy-saving buildings and intelligent windows for transportation and related fields.

[0005] The objective of this invention can be achieved through the following technical solutions:

[0006] A first aspect of the present invention provides a color-changing device, comprising:

[0007] The color-changing device cavity includes an electrode frame and a first transparent conductive substrate and a second transparent conductive substrate on both sides of the electrode frame; and...

[0008] An electrochromic solution, disposed in the cavity of a color-changing device, comprises a 4,4′-bipyridine derivative, zinc chloride, and hydrochloric acid; wherein the 4,4′-bipyridine derivative is selected from 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine.

[0009] In some specific embodiments, the first transparent conductive substrate is fluorine-doped tin oxide (FTO) conductive glass; the second transparent conductive substrate is platinum-plated FTO conductive glass.

[0010] In some specific embodiments, the electrode frame is selected from one of zinc frames, aluminum frames, or magnesium frames.

[0011] In some specific embodiments, the concentration of the 4,4′-bipyridine derivative in the electrochromic solution is 4–10 g / L; the concentration of zinc chloride is 0.8–1.2 mol·L⁻¹. -1 The concentration of hydrochloric acid is 0.1–0.8 mol·L⁻¹. -1 .

[0012] In some specific embodiments, the electrochromic solution further includes potassium chloride, sodium chloride, or potassium sulfate.

[0013] A second aspect of the present invention provides a method for preparing the color-changing device as described above, comprising:

[0014] Prepare an electrochromic solution containing a 4,4′-bipyridine derivative, zinc chloride, and hydrochloric acid;

[0015] The electrode frame is assembled with the first transparent conductive substrate and the second transparent conductive substrate to form a color-changing device cavity;

[0016] An electrochromic solution is injected into the cavity of the color-changing device to obtain the color-changing device.

[0017] In some specific embodiments, when the 4,4′-bipyridine derivative is 1-butyl-4,4′-bipyridine, the preparation method includes:

[0018] 1-Iodobutane and 4,4′-bipyridine were mixed in an acetonitrile solution and stirred at 60–80 °C. The mixture was filtered, and the filtrate was added to diethyl ether to precipitate the precipitate. The precipitate was then dried to obtain the final product.

[0019] The mass ratio of 1-iodobutane to 4,4′-bipyridine is (3-4):3.

[0020] In some specific embodiments, when the 4,4′-bipyridine derivative is 1-butyl-1′-(2-propenyl)-4,4′-bipyridine, the preparation method includes:

[0021] 1-Iodobutane and 4,4′-bipyridine were mixed in an acetonitrile solution at a mass ratio of (3-4):3, stirred at 60-80°C, filtered, and the filtrate was added to diethyl ether to precipitate and dried to obtain 1-butyl-4,4′-bipyridine.

[0022] 1-Butyl-4,4′-bipyridine and 3-chloropropene were mixed in acetonitrile and stirred at 80°C. The precipitate was collected and dried to obtain 1-Butyl-1′-(2-propenyl)-4,4′-bipyridine.

[0023] The mass ratio of 1-butyl-4,4′-bipyridine to 3-chloropropene is 1:(1-3).

[0024] In some specific embodiments, the second transparent conductive substrate is platinum-plated FTO conductive glass, and the preparation method includes: coating a platinum source solution onto the surface of the FTO conductive glass and annealing it.

[0025] In some specific embodiments, the concentration of the platinum source solution is 4–6 mmol·L⁻¹. -1 In the annealing process, the processing temperature is 350-400℃, the processing time is 10-20 minutes, and the processing atmosphere is air.

[0026] In some specific embodiments, the electrode frame and the first transparent conductive substrate, and the electrode frame and the second transparent conductive substrate are bonded together to form a color-changing device cavity.

[0027] A third aspect of the present invention provides an application of the color-changing device as described above, including: using the color-changing device to manufacture a smart window or a display.

[0028] The color-changing device based on viologen derivative electrolyte and zinc and platinum electrodes obtained by the above preparation method of the present invention can achieve adaptive coloring and fading without external voltage, and has a fast response speed and a large light modulation amplitude, showing good application prospects in smart windows or displays.

[0029] Compared with the prior art, the present invention has the following characteristics:

[0030] (1) The viologen derivative electrolyte-based zinc and platinum electrode-containing color-changing device adopts a three-electrode structure of transparent conductive glass, active and inert metals, which can achieve rapid self-coloring and fading without an external power supply, thus overcoming the disadvantage of electrochromic devices being dependent on electrical energy and expanding the application range. The spontaneous coloring and fading of the viologen derivative adsorbed on the transparent conductive glass substrate are achieved by interfacial charge transfer driven by the inherent potential difference between the transparent conductive glass / zinc and the transparent conductive glass / platinum, respectively. Without an external power supply, an ultra-low transmittance of 0.2% and a maximum light modulation amplitude of 71.3% can be achieved at 550 nm within 7.5 s.

[0031] (2) The color-changing electrolyte based on viologen derivative of the present invention has a high transmittance.

[0032] (3) The color-changing device based on viologen derivative electrolyte with zinc and platinum electrodes of the present invention can also achieve rapid coloring and fading under certain external voltage conditions, reducing the consumption of electrical energy and increasing the application range. Attached Figure Description

[0033] Figure 1 This is a schematic diagram of the color-changing device based on a zinc- and platinum-containing electrode using a 1-butyl-4,4′-bipyridine electrolyte in Example 1.

[0034] Figure 2 These are photographs of the faded state (a) and colored state (b) of the color-changing device based on zinc and platinum electrodes with 1-butyl-4,4′-bipyridine electrolyte in Example 1.

[0035] Figure 3 The transmittance curves for the colored and faded states of the color-changing device based on viologen derivative electrolyte with zinc and platinum electrodes in Example 1 are shown.

[0036] Figure 4 The image shows the response time curve of the color-changing device based on a viologen derivative electrolyte with zinc and platinum electrodes in Example 1. Figure 5 The image shows the cycle stability curve of the color-changing device based on viologen derivative electrolyte with zinc and platinum electrodes in Example 1 under energized conditions. Detailed Implementation

[0037] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0038] The types of metal electrodes and viologen derivative electrolytes used in color-changing devices based on zinc and platinum electrodes are all considered equivalent substitutions and are included within the scope of protection of this invention, provided that no other changes, modifications, substitutions, combinations, or simplifications are made without departing from the spirit and principle of this invention.

[0039] The following are more detailed implementation examples, which further illustrate the technical solution of the present invention and the technical effects that can be obtained.

[0040] In the following examples, the preparation method of 1-butyl-4,4′-bipyridine includes: firstly, mixing 3.5 g of 1-iodobutane and 3 g of 4,4′-bipyridine in 10 mL of acetonitrile solution and stirring at 60 °C for 24 h. The resulting product is filtered and then precipitated in diethyl ether. The obtained 1-butyl-4,4′-bipyridine is dried to obtain an orange compound, which is 1-butyl-4,4′-bipyridine.

[0041] The preparation method of 1-butyl-1′-(2-propenyl)-4,4′-bipyridine includes: dissolving 1 g of 1-butyl-4,4′-bipyridine in 25 mL of acetonitrile, adding 2 g of 3-chloropropene, stirring at 80 °C for 48 h, the resulting mixture forms a brown precipitate, which is collected, washed with acetonitrile, and dried to obtain 1-butyl-1′-(2-propenyl)-4,4′-bipyridine.

[0042] The synthesized samples are 1-butyl-4,4′-bipyridine and 1-butyl-1′-(2-propenyl)-4,4′-bipyridine, with the following structural formulas:

[0043] 1-Butyl-4,4′-Bipyridine:

[0044]

[0045] 1-Butyl-1′-(2-Propylene)-4,4′-Bipyridine:

[0046]

[0047] Example 1

[0048] A color-changing device based on a zinc and platinum electrode containing a 1-butyl-4,4′-bipyridine electrolyte, capable of self-coloring and fading, is prepared by the following steps:

[0049] (1) Dissolve 0.04 g of 1-butyl-4,4′-bipyridine in 5 mL of deionized water;

[0050] (2) Add 0.68 g of zinc chloride and 0.21 mL of concentrated hydrochloric acid to the solution obtained in step (1), stir for 10 min, and then sonicate for 10 min to prepare a solution containing 1 mol·L⁻¹ -1 Zinc chloride and 0.5 mol·L -1 A mixed solution of hydrochloric acid;

[0051] (3) First, for 1.5×4cm 2 The zinc sheet is pickled, alcohol-washed, and ultrasonically treated to remove surface oxides. Then, it is cut into zinc frames with an inner width of 1.3 cm, a length of 3.8 cm, and a thickness of 0.05 cm to serve as zinc electrodes.

[0052] (4) Dissolve 103.6 mg of chloroplatinic acid hexahydrate in 40 mL of isopropanol to prepare a solution with a concentration of 0.005 mol·L⁻¹. -1 The precursor solution of chloroplatinic acid hexahydrate was prepared by spin-coating 500 μL of the precursor solution evenly onto a 5×5 cm plate pre-cleaned with deionized water and ethanol. 2 Platinum-plated FTO conductive glass electrodes were obtained by annealing them in air at 380°C for 15 min on FTO conductive glass.

[0053] (5) Place 2.5×5cm 2 The FTO conductive glass 1, double-sided adhesive 2 (3M double-sided adhesive) with a width of 5mm and a thickness of 1mm, a zinc frame 3, and platinum-plated FTO glass 4 are assembled together to obtain a color-changing device cavity containing zinc and platinum electrodes, such as... Figure 1 As shown;

[0054] (6) The mixed solution obtained in step (2) is injected into the cavity of the color-changing device containing zinc and platinum electrodes to obtain a color-changing device that can self-color and fade based on zinc and platinum electrodes containing 1-butyl-4,4′-bipyridine electrolyte.

[0055] A schematic diagram of the color-changing device based on 1-butyl-4,4′-bipyridine electrolyte and zinc and platinum electrodes prepared in this embodiment is shown below. Figure 1 As shown, the addition of a metal electrode as a third electrode enables the electrochromic smart window to break free from its dependence on electrical energy.

[0056] Figure 2 These are photographs of a color-changing device containing a zinc- and platinum-platinum electrode with a 1-butyl-4,4′-bipyridine electrolyte, in both colored and faded states. The device is in the colored state when the FTO conductive glass is connected to the zinc electrode, and in the faded state when the FTO conductive glass is disconnected from the zinc electrode and connected to platinum-plated FTO conductive glass.

[0057] The transmittance curves for coloring and fading of a color-changing device with zinc and platinum electrodes containing 1-butyl-4,4′-bipyridine electrolyte are shown below. Figure 3As shown, the light modulation amplitude at 550 nm wavelength was 71.3% when tested using a UV-Vis-NIR spectrophotometer in the wavelength range of 400–1000 nm.

[0058] Figure 4 The figure shows the response time curve of the device. As can be seen from the figure, when the zinc frame is connected to the FTO conductive glass, the device rapidly turns purple. When the FTO conductive glass is disconnected from the zinc frame and connected to the platinum-plated FTO conductive glass, the device changes from purple to colorless. The coloring time of the device is 7.2 s, and the fading time is 5.2 s. Figure 5 The device's cycle stability curve shows that it can maintain a relatively large optical modulation amplitude for about 750 seconds.

[0059] Example 2

[0060] A color-changing device based on a zinc and platinum electrode containing a 1-butyl-4,4′-bipyridine electrolyte, capable of self-coloring and fading, is prepared by the following steps:

[0061] (1) 0.04 g of 1-butyl-1′-(2-propenyl)-4,4′-bipyridine was dissolved in 5 mL of deionized water;

[0062] (2) Add 0.68 g of zinc chloride and 0.21 mL of concentrated hydrochloric acid to the solution obtained in step (1), stir for 10 min, and then sonicate for 10 min to prepare a solution containing 1 mol·L⁻¹ -1 Zinc chloride and 0.5 mol·L -1 hydrochloric acid solution;

[0063] (3) First, for 1.5×4cm 2 The zinc sheet is pickled, alcohol-washed, and ultrasonically treated to remove surface oxides. Then, it is cut into zinc frames with an inner width of 1.3 cm, a length of 3.8 cm, and a thickness of 0.05 cm to serve as zinc electrodes.

[0064] (4) Dissolve 103.6 mg of chloroplatinic acid hexahydrate in 40 mL of isopropanol to prepare a solution with a concentration of 0.005 mol·L⁻¹. -1 The precursor solution of chloroplatinic acid hexahydrate was prepared by spin-coating 500 μL of the precursor solution evenly onto a 5×5 cm plate pre-cleaned with deionized water and ethanol. 2 Platinum-plated FTO conductive glass electrodes were obtained by annealing them in air at 380°C for 15 min on FTO conductive glass.

[0065] (5) Place 2.5×5cm 2 The FTO conductive glass, 3M double-sided adhesive with a width of 5mm and a thickness of 1mm, zinc frame and platinum-plated FTO glass are assembled together to obtain the cavity of the color-changing device containing zinc and platinum electrodes.

[0066] (6) The mixed solution obtained in step (2) is injected into the cavity of the color-changing device containing zinc and platinum electrodes to obtain a color-changing device that can self-color and fade based on the zinc and platinum electrodes containing viologen derivative electrolyte.

[0067] Example 3

[0068] A color-changing device based on a zinc and platinum electrode containing a 1-butyl-4,4′-bipyridine electrolyte, capable of self-coloring and fading, is prepared by the following steps:

[0069] (1) Dissolve 0.04 g of 1-butyl-4,4′-bipyridine in 5 mL of deionized water;

[0070] (2) Add 0.3 g of zinc chloride and 0.5 mL of concentrated hydrochloric acid to the solution obtained in step (1) to obtain 0.4 mol·L⁻¹ -1 Zinc chloride and 1.09 mol·L -1 A mixed solution of hydrochloric acid was stirred for 10 minutes and then sonicated for 10 minutes to obtain an acidic electrolyte solution with electrochromic properties.

[0071] (3) First, for 1.5×4cm 2 The zinc sheet is pickled, alcohol-washed, and ultrasonically treated to remove surface oxides. Then, it is cut into zinc frames with an inner width of 1.3 cm, a length of 3.8 cm, and a thickness of 0.05 cm to serve as zinc electrodes.

[0072] (4) Dissolve 103.6 mg of chloroplatinic acid hexahydrate in 40 mL of isopropanol to prepare a solution with a concentration of 0.005 mol·L⁻¹. -1 The precursor solution of chloroplatinic acid hexahydrate was prepared by spin-coating 500 μL of the precursor solution evenly onto a 5×5 cm plate pre-cleaned with deionized water and ethanol. 2 Platinum-plated FTO conductive glass electrodes were obtained by annealing them in air at 380°C for 15 min on FTO conductive glass.

[0073] (5) Place 2.5×5cm 2 The FTO conductive glass, 3M double-sided adhesive with a width of 5mm and a thickness of 1mm, zinc frame and platinum-plated FTO glass are assembled together to obtain the cavity of the color-changing device containing zinc and platinum electrodes.

[0074] (6) The mixed solution obtained in step (2) is injected into the cavity of the color-changing device containing zinc and platinum electrodes to obtain a color-changing device that can self-color and fade based on the zinc and platinum electrodes containing viologen derivative electrolyte.

[0075] Example 4

[0076] A color-changing device based on a zinc and platinum electrode containing a 1-butyl-4,4′-bipyridine electrolyte, capable of self-coloring and fading, is prepared by the following steps:

[0077] (1) Dissolve 0.04 g of 1-butyl-4,4′-bipyridine in 5 mL of deionized water;

[0078] (2) Add 0.37 g zinc chloride and 0.21 mL concentrated hydrochloric acid to the solution obtained in step (1), stir for 10 min, and then sonicate for 10 min to prepare a solution containing 1 mol·L⁻¹ -1 Zinc chloride and 0.5 mol·L -1 A mixed solution of hydrochloric acid;

[0079] (3) First, for 1.5×4cm 2 The magnesium sheet was acid-washed, alcohol-washed, and ultrasonically treated to remove surface oxides. Then, it was cut into magnesium frames with an inner width of 1.3 cm, a length of 3.8 cm, and a thickness of 0.05 cm to serve as magnesium electrodes.

[0080] (4) Dissolve 103.6 mg of chloroplatinic acid hexahydrate in 40 mL of isopropanol to prepare a solution with a concentration of 0.005 mol·L⁻¹. -1 The precursor solution of chloroplatinic acid hexahydrate was prepared by spin-coating 500 μL of the precursor solution evenly onto a 5×5 cm plate pre-cleaned with deionized water and ethanol. 2 Platinum-plated FTO conductive glass electrodes were obtained by annealing them in air at 380°C for 15 min on FTO conductive glass.

[0081] (5) Place 2.5×5cm 2 The FTO conductive glass, 3M double-sided adhesive with a width of 5mm and a thickness of 1mm, magnesium frame and platinum-plated FTO glass are assembled together to obtain the color-changing device cavity containing magnesium and platinum electrodes.

[0082] (6) The mixed solution obtained in step (2) is injected into the cavity of the color-changing device containing magnesium and platinum electrodes to obtain an adaptive color-changing device based on viologen derivative electrolyte containing magnesium and platinum electrodes.

[0083] In summary, this invention provides a color-changing device based on zinc and platinum electrodes using 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine electrolytes. By combining the zinc anode and platinum cathode with an electrolyte containing viologen derivatives, this strategy of combining different active metals with electrochromic materials to achieve self-coloring and fading functions provides a new direction for developing more energy-efficient technologies.

[0084] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A color-changing device, characterized in that, include: The color-changing device cavity includes an electrode frame and a first transparent conductive substrate and a second transparent conductive substrate on both sides of the electrode frame; as well as, An electrochromic solution, disposed in the cavity of a color-changing device, comprises a 4,4′-bipyridine derivative, zinc chloride, and hydrochloric acid; wherein the 4,4′-bipyridine derivative is selected from 1-butyl-4,4′-bipyridine or 1-butyl-1′-(2-propenyl)-4,4′-bipyridine.

2. The color-changing device according to claim 1, characterized in that, The first transparent conductive substrate is fluorine-doped tin oxide conductive glass; the second transparent conductive substrate is platinum-plated fluorine-doped tin oxide conductive glass.

3. The color-changing device according to claim 1, characterized in that, The electrode frame is selected from one of zinc, aluminum or magnesium frames.

4. The color-changing device according to claim 1, characterized in that, In the electrochromic solution, the concentration of the 4,4′-bipyridine derivative is 4–10 g / L; the concentration of zinc chloride is 0.8–1.2 mol·L⁻¹. -1 The concentration of hydrochloric acid is 0.1–0.8 mol·L⁻¹. -1 .

5. A method for preparing a color-changing device as described in any one of claims 1 to 4, characterized in that, The method includes: Prepare an electrochromic solution containing a 4,4′-bipyridine derivative, zinc chloride, and hydrochloric acid; The electrode frame is assembled with the first transparent conductive substrate and the second transparent conductive substrate to form a color-changing device cavity; An electrochromic solution is injected into the cavity of the color-changing device to obtain the color-changing device.

6. The method for preparing the color-changing device according to claim 5, characterized in that, When the 4,4′-bipyridine derivative is 1-butyl-4,4′-bipyridine, the preparation method includes: 1-Iodobutane and 4,4′-bipyridine were mixed in an acetonitrile solution, stirred at 60–80 °C, filtered, and the filtrate was added to diethyl ether to precipitate the mixture. The precipitate was then dried to obtain the final product. The mass ratio of 1-iodobutane to 4,4′-bipyridine is (3-4):

3.

7. The method for preparing the color-changing device according to claim 5, characterized in that, When the 4,4′-bipyridine derivative is 1-butyl-1′-(2-propenyl)-4,4′-bipyridine, the preparation method includes: 1-Iodobutane and 4,4′-bipyridine were mixed in an acetonitrile solution at a mass ratio of (3-4):3, stirred at 60-80°C, filtered, and the filtrate was added to diethyl ether to precipitate and dried to obtain 1-butyl-4,4′-bipyridine. 1-Butyl-4,4′-bipyridine and 3-chloropropene were mixed in acetonitrile and stirred at 80°C. The precipitate was collected and dried to obtain 1-Butyl-1′-(2-propenyl)-4,4′-bipyridine. The mass ratio of 1-butyl-4,4′-bipyridine to 3-chloropropene is 1:(1-3).

8. The method for preparing the color-changing device according to claim 5, characterized in that, The second transparent conductive substrate is platinum-plated FTO conductive glass, and the preparation method includes: coating a platinum source solution onto the surface of FTO conductive glass and annealing it. The concentration of the platinum source solution is 4–6 mmol·L⁻¹. -1 In the annealing process, the processing temperature is 350-400℃, the processing time is 10-20 minutes, and the processing atmosphere is air.

9. The method for preparing the color-changing device according to claim 8, characterized in that, The electrode frame is bonded to the first transparent conductive substrate and the second transparent conductive substrate to form a color-changing device cavity.

10. An application of the color-changing device as described in any one of claims 1 to 4, characterized in that, The color-changing device is used to manufacture smart windows or displays.