Method for preparing silicon-carbon composite negative electrode material by using porous carbon airflow fine powder
By using binders containing petroleum asphalt and other components to treat porous carbon gas stream fine powder, a stable conductive carbon network is formed, which solves the problem of recycling porous carbon fine powder and improves the electrochemical performance and yield of silicon-carbon composite materials.
Patent Information
- Application Number
- CN202511393659.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-28
- Publication Date
- 2025-10-31
- Estimated Expiration
- 2045-09-28
AI Technical Summary
Existing technologies are unable to effectively process the fine powder generated by porous carbon gas flow mills, resulting in material loss and poor electrochemical performance. Traditional binders cannot effectively coat and bind ultrafine particles, affecting the rate performance of silicon-carbon composite anode materials.
By using binders with specific components, including petroleum asphalt, polyamic acid solution, cellulose nanofibers, epoxy silane coupling agents, and metal catalysts, a stable conductive carbon network is formed through curing, pyrolysis, and activation processes, thereby improving electrochemical performance.
This technology enables the efficient recycling of porous carbon gas stream fine powder, significantly improves the rate performance of silicon-carbon composite materials, and reduces production costs.
Smart Images

Figure CN120878767A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery anode material technology, specifically relating to a method for preparing silicon-carbon composite anode materials using porous carbon gas stream powder. Background Technology
[0002] In the preparation process of silicon-carbon composite anode materials, porous carbon needs to undergo silane vapor deposition. Before deposition, the porous carbon needs to be crushed to the target particle size range using an air jet mill. This process generates fine powder with a particle size ≤2μm. Currently, carbon material activation technology struggles to effectively handle this fine powder generated by air jet milling, primarily due to the performance limitations of existing activation equipment. The main equipment used in porous carbon activation processes is a rotary activation furnace, one of the core components of which is a metal filter unit. The minimum pore size of existing metal filter element preparation technology is approximately 10μm, while the average particle size of the fine powder from air jet milling is far lower than this value, generally not exceeding 2μm. If a rotary furnace is directly used to activate this fine powder, most of the material will be lost through the filter element pores. Furthermore, during subsequent electrode slurry and sintering processes, the ultrafine air jet powder is easily lost with the solvent or airflow. Furthermore, in the subsequent electrode slurry preparation and sintering processes, ultrafine powders are easily carried away by solvents or airflows, resulting in material loss; it is also not advisable to directly reuse such fine powders for silane deposition to prepare silicon-carbon composite materials, as they are prone to agglomeration during slurry preparation, affecting the uniformity of the slurry and the electrochemical performance of the final electrode.
[0003] Therefore, to effectively reuse porous carbon gas stream fine powder, it is necessary to pretreat it with a binder, followed by pyrolysis and activation, and finally obtain a silicon-carbon composite material that meets electrochemical requirements through silane deposition. However, commonly used binders are not suitable for this type of fine powder. Due to its extremely small particle size, large specific surface area, and high surface energy, the fine powder easily agglomerates into hard lumps that are difficult to deagglomerate, requiring a large amount of binder to cover the particle surface and form a stable bonding system. Excessive binder dosage not only clogs the material pores but also negatively affects electrochemical behavior. On the other hand, the preform after bonding and curing still needs to undergo high-temperature pyrolysis and activation. The carbon skeleton constructed by traditional bonding systems has low strength and is difficult to meet mechanical performance requirements. The cured precursor needs to be crushed and sieved to obtain particles in the target particle size range of 30–100 mesh. If the bonding strength is insufficient, the yield of the finished product in this particle size range will be significantly reduced.
[0004] Furthermore, the wide particle size distribution of airflow fines, typically spanning a span of SPAN ≥ 3, further complicates their utilization. Typical processes aim for uniform particle size and good dispersibility to produce stable products. An ideal binder must not only coat ultrafine particles to reduce loss but also possess sufficient binding strength to bind larger particles. Under current technological conditions, the secondary utilization of airflow fines is extremely challenging, and no publicly available literature reports a suitable binding system for this type of material.
[0005] An ideal binder for porous carbon gas stream fine powder should possess the following characteristics: low addition amount, high bond strength, and the ability to effectively coat and bond fine powder with high specific surface area; good dispersibility, allowing for thorough wetting of particle surfaces; a controllable and uniform carbonization process after curing, forming a carbon network structure with good conductivity and certain mechanical strength; and without blocking the original pores of porous carbon. Our research group has attempted to use conventional PVDF and SBR / CMC systems, but both have encountered problems such as insufficient bonding force, pore blockage, or poor strength of the carbonized structure.
[0006] The inventor's previous patent CN202511113420.5 disclosed a method for preparing porous carbon through the secondary utilization of porous carbon gas stream powder. This method employs a self-made binding system to form a multi-level porous carbon structure, improving the electrochemical performance of the material. The binder includes thermosetting phenolic resin, epoxy silane coupling agent, and fumed silica. This patent addresses the shortcomings of conventional binders in terms of poor utilization efficiency of gas stream powder. However, the carbon substances formed by the added binder during subsequent sintering do not improve lithium-ion transport efficiency, particularly as they do not form a conductive network. This is crucial for the contact between fine particles, resulting in poor electrochemical performance of the resulting silicon-carbon composite anode material, especially in rate performance. The inventor previously attempted to directly add conductive carbon substances, such as carbon nanotubes and graphene, to the binder. However, while this improved the conductivity of the product, it reduced the binding performance and increased the loss rate during the separation of 30-100 mesh particles. Furthermore, carbon nanotubes and graphene are relatively expensive. These combined factors increase costs and make the method unsuitable for industrial production. Summary of the Invention
[0007] To address the shortcomings of existing technologies where the small-particle-size gas stream powder generated during porous carbon production processes is difficult to recycle and reuse, and where the recycled powder, when used as raw material to prepare porous carbon and subsequently silicon-carbon composite anode materials, exhibits poor electrochemical performance, particularly rate performance, this invention proposes a method for preparing silicon-carbon composite anode materials using porous carbon gas stream powder. This invention employs a binder with specific components, which significantly improves the electrochemical performance of the resulting silicon-carbon composite anode material without affecting its bonding properties. Specifically, this invention achieves the above objectives through the following technical solutions.
[0008] A method for preparing silicon-carbon composite anode materials using porous carbon gas stream powder includes the following steps: (S1) The porous carbon gas flow fine powder and the binder are mixed at a mass ratio of 100:12-18, and then the mixture is cured to obtain the precursor; the binder includes the following raw materials: petroleum asphalt, polyamic acid solution, cellulose nanofibers (CNF), epoxy silane coupling agent alcohol aqueous solution, nickel dicene and / or nickel acetylacetonate, toluene; (S2) After the precursor is crushed and screened, it is pyrolyzed and carbonized in an inert atmosphere to obtain pyrolytic carbon. (S3) Under an activating atmosphere, pyrolytic carbon is activated to obtain porous carbon materials; (S4) Silane deposition is performed on porous carbon to obtain silicon-carbon composite anode material.
[0009] Compared to the inventor's previous patent CN202511113420.5, the changes in this invention are primarily in that the main carbon source of the binder is changed to petroleum asphalt, which is more widely available and cheaper. Compared to thermosetting phenolic resin, it is easier to soften and can effectively wet and coat ultrafine air-flow powder. Furthermore, under the action of ferrocene / nickel, a conductive carbon network with a graphite structure can be generated in situ during pyrolysis. Secondly, this invention no longer uses epoxy silane coupling agents and fumed silica. The previous patent technology used epoxy silane coupling agents and fumed silica, which together could form a stable cross-linked network, increasing the binder's skeletal stabilization effect on the air-flow powder. However, after the reaction and cross-linking, electrochemically inert Si-O-Si is formed, which hinders electron transport, increases the overall impedance of the composite material, and leads to poor rate performance. In addition, although the formed skeleton has good mechanical properties, it is brittle, which will lead to a decrease in the yield of 30-100 mesh target particles in subsequent crushing and screening. To overcome the drawbacks of epoxy silane coupling agents and fumed silica, this invention employs cellulose nanofibers, which have a large aspect ratio and abundant hydroxyl groups on their surface, enabling them to form a stable network structure with epoxy silane coupling agents. While carbon nanotubes can also be used, they are expensive, and the inventors found that the bonding performance of the binder is inferior to that of cellulose nanofibers after their addition. The binder of this invention also incorporates nickel dicene and / or nickel acetylacetonate, providing a certain catalytic ability to promote the transformation of asphalt into graphitized carbon during subsequent pyrolysis, thereby improving the electrochemical performance of the composite material. Using the above-mentioned compounded binder, this invention can further reduce the amount of binder required.
[0010] Further, the softening point of the petroleum asphalt is 40-60℃; the intrinsic viscosity of the polyamic acid is 1.5-1.9 dL / g; the diameter of the cellulose nanofibers is 20-40 nm and the length is 200-500 nm; the epoxy silane coupling agent is selected from at least one of 3-glycidyl etheroxypropyltrimethoxysilane (KH-560), 3-(2,3-epoxypropoxy)propyltriethoxysilane (KH-561), and 3-(2,3-epoxypropoxy)propylmethyldimethoxysilane (KH-563); the solid content of the epoxy silane coupling agent alcohol aqueous solution is 30-40%, the alcohol is at least one of methanol, ethanol, and isopropanol, and the solvent of the alcohol aqueous solution is an alcohol-water mixture in a volume ratio of 4-7:1.
[0011] Furthermore, the polyamic acid solution is obtained by polycondensation of dianhydride monomer and diamine monomer in a polar aprotic solvent at a molar ratio of 1:0.8-1.2, preferably with a molar ratio of dianhydride monomer to diamine monomer of 1:0.9-1.1, more preferably with a molar ratio of 1:0.95-1.05, such as 1:1; the solid content of the polyamic acid solution is 20-30%.
[0012] Further, the dianhydride monomer is selected from at least one of pyromellitic dianhydride, biphenyl dianhydride, oxydiphthalic anhydride, and naphthalenecyclodianhydride; the diamine monomer is selected from at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, p-phenylenediamine, m-phenylenediamine, 4,4'-bis(4-aminophenoxy)diphenyl sulfone, and 4,4'-diamino-2,2'-dimethylbiphenyl.
[0013] Furthermore, the polyamic acid is prepared by a method comprising the following steps: under an inert atmosphere, dianhydride monomer and diamine monomer are fed into a polar aprotic solvent and reacted at 10-25°C to obtain a polyamic acid solution.
[0014] Furthermore, the inert atmosphere is nitrogen and / or argon, and the polar aprotic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethyl sulfoxide; the amount of polar aprotic solvent added is such that the solid content of the polyamic acid solution is 20-30%.
[0015] Further, the binder comprises the following raw materials in parts by weight: 4-6 parts petroleum asphalt, 1.6-2.1 parts polyamic acid solution, 0.05-0.08 parts cellulose nanofibers (CNF), 0.5-0.8 parts epoxy silane coupling agent alcohol aqueous solution, 0.01-0.02 parts nickel dicene and / or nickel acetylacetonate, and 10 parts toluene.
[0016] Further, in step (S1), the porous carbon airflow powder fine powder has a Dv50 ≤ 2 μm and a span ≤ 4. The porous carbon airflow powder fine powder originates from fine powder with a particle size ≤ 2 μm produced during the porous carbon preparation process using an airflow mill to control the particle size of the material. The span (SPAN) reflects the particle size distribution and is calculated according to the following formula: SPAN = (Dv90 - Dv10) / Dv50 The meanings of Dv90, Dv50, and Dv10 are well-known in the art, representing the diameters of particles located at 90%, 50%, and 10% of the volume when arranged in ascending order of diameter. The porous carbon airflow fine powder has a small particle size (Dv50 ≤ 2 μm) and a wide particle size distribution (span ≥ 3). Typically, a wide particle size distribution leads to uneven particle packing density and low tap density, a problem that needs to be overcome in secondary particle processing. However, the inventors unexpectedly discovered that this wide distribution characteristic actually translates into a unique advantage when processing airflow fine powder using a binder: smaller particles can effectively fill the gaps between larger particles, resulting in more compact secondary particles and reducing the amount of binder required. The core of this invention is the use of a combination of cellulose nanofibers (CNCs) and an epoxy silane coupling agent. CNF has a large aspect ratio, and after uniform mixing with binder and air-jet fine powder, it forms a stable three-dimensional network under the action of epoxy coupling agent. Furthermore, the epoxy coupling agent reacts with the oxygen-containing groups of petroleum asphalt, significantly improving the affinity between CNF and petroleum asphalt and preventing phase separation. CNF and petroleum asphalt, catalyzed by nickel dicene and / or nickel acetylacetonate, facilitate the graphitization of carbon layers. The inventors also found that using other metals, such as ferrocene and platinum acetylacetonate compounds, did not yield satisfactory results, and the electrochemical performance of the resulting silicon-carbon composite material was not excellent.
[0017] This invention utilizes a binder with specific components and proportions to achieve efficient coating and bonding of ultrafine porous carbon stream powder (Dv50≤2μm) at relatively low addition levels, forming structurally stable secondary particles. The improved binder exhibits excellent flow characteristics during the curing stage, effectively wetting and uniformly coating the fine powder particles. During subsequent pyrolysis and carbonization, it is controllably transformed into a carbon skeleton with a certain degree of conductivity. Compared to traditional binders, such as conventional thermosetting resins, which have high carbonization shrinkage rates and generate structural stress leading to easy skeleton collapse, resulting in low yields when sieved at specific particle sizes (e.g., 30-100 mesh), the binder of this invention, through a specific curing-synergistic carbonization mechanism, achieves stable particle bonding while ultimately forming a highly stable carbon network structure compatible with porous carbon.
[0018] There are no particular restrictions on the mixing method of porous carbon airflow powder binder, as long as it can be mixed evenly, such as a high-speed mixer.
[0019] Further, in step (S2), the crushing and screening process controls the particle size to 30-100 mesh; the inert atmosphere is nitrogen and / or argon; the pyrolysis carbonization process conditions are 600-800℃; and the pyrolysis time is 5-10 hours. If the binder performance is poor, the yield will be very low during the crushing and screening process in step S2.
[0020] Further, in step (S3), the activation atmosphere includes at least one of carbon dioxide and water vapor, the activation temperature is 900-1100℃, and the activation time is 10-24h.
[0021] Further, in step (S4), the silane is selected from at least one of silane, disilane, dichlorosilane, and trichlorosilane. The amount of silane gas introduced is such that the mass percentage of Si in the silicon-carbon composite material is between 40-60%, preferably between 45-55%. Preferably, a carrier gas is also introduced when the silane is introduced, and the carrier gas is selected from at least one of nitrogen and argon. The volume ratio of silane to carrier gas is 1:1-10, preferably 1:1-5. The temperature for silane deposition is 450-600°C.
[0022] This invention provides a method for preparing silicon-carbon composite anode materials using porous carbon gas flow powder. Utilizing a binder of specific composition, the method not only binds and solidifies the ultrafine gas flow powder with a wide particle size distribution into a stable solidified structure, achieving a high yield during crushing and sieving, but also significantly improves the rate performance of the resulting silicon-carbon composite material at low cost without affecting the bonding performance. This invention also recycles and reuses the gas flow powder generated during the porous carbon preparation process, which is difficult to effectively utilize in existing technologies. The preparation process is simple, requires no expensive equipment or reagents, and the resulting silicon-carbon composite material exhibits excellent electrochemical performance, comparable to silicon-carbon composite anode materials prepared using conventional porous carbon processes. Attached Figure Description
[0023] Figure 1 This is a particle size distribution diagram of the porous carbon product obtained in Example 1; Figure 2 This is a photograph of the precursor obtained in Example 1; Figure 3 This is a SEM image of the porous carbon obtained in Example 1. Detailed Implementation
[0024] To more clearly illustrate the technical solutions mentioned in this invention, examples will be provided below. Obviously, this invention is not limited to these examples.
[0025] The petroleum asphalt was sourced from PetroChina, grade 70#, with a softening point of 47.6℃; the cellulose nanofibers were purchased from Nanjing Tianlu Nanotechnology Co., Ltd., with a diameter of 30-40 nm and a length of approximately 400 nm; the porous carbon gas stream fine powder was sourced from Beijing Yijin New Energy Technology Co., Ltd., with a Dv50 of 1.929 μm and a span (SPAN) of 3.9. The particle size distribution is shown in [reference needed]. Figure 1 .
[0026] Preparation Example 1 Pyromellitic dianhydride, 4,4'-diaminodiphenyl ether, and p-phenylenediamine were added to DMF in a molar ratio of 1:0.6:0.4 and reacted at room temperature for 12 h to obtain a polyamic acid solution with a solid content of 21.6% and an intrinsic viscosity of 1.82 dL / g.
[0027] Preparation Example 2 Biphenyltetracarboxylic dianhydride, 4,4'-diaminodiphenyl ether, and p-phenylenediamine were added to DMF in a molar ratio of 1:0.8:0.2 and reacted at room temperature for 12 hours to obtain a polyamic acid solution with a solid content of 24.7% and an intrinsic viscosity of 1.78 dL / g.
[0028] Example 1 (S1) 10 kg toluene, 4 kg petroleum asphalt, 2.1 kg of polyamic acid solution prepared in Example 1, 0.05 kg cellulose nanofibers, 0.5 kg of an alcohol-water solution of silane coupling agent KH-560 with a solid content of 30% (the solvent is a mixture of ethanol and water in a volume ratio of 7:1), and 0.01 kg nickel dicene are mixed evenly as a binder; porous carbon air jet powder and binder are mixed evenly in a high-speed mixer at a mass ratio of 100:18, and the mixture is cured at 120°C for 24 h; the precursor is obtained. Figure 2 The image shows a photograph of the precursor obtained in Example 1. It can be seen that the surface is dense, achieving a good bonding effect.
[0029] (S2) The precursor is crushed and sieved to select particles of suitable size of 30-100 mesh, and the mass ratio of 30-100 mesh particles to the precursor is calculated. The mass ratio of 30-100 mesh particles can be used to evaluate the bonding performance of the binder. The higher the mass ratio, the better the bonding performance and the higher the yield. Under nitrogen atmosphere, the carbon is pyrolyzed at 800℃ for 5 hours to obtain pyrolyzed carbon. (S3) Pyrolytic carbon is activated at 980℃ for 12 hours in a steam atmosphere to obtain porous carbon; Figure 3 This is a SEM image of the porous carbon obtained in step S3 of Example 1.
[0030] (S4) Porous carbon is added to a fluidized bed reactor, and a mixture of silane and nitrogen in a volume ratio of 1:3 is introduced. Silicon deposition is carried out at 500°C, and nano-silicon is deposited into the pores of the porous carbon. After cooling, a silicon-carbon composite anode material is obtained, in which the mass ratio of Si is 46% (in subsequent examples and comparative examples, the amount of silane introduced is based on the mass ratio of Si in the silicon-carbon composite material of the product being 46%).
[0031] Example 2 (S1) Mix 10 kg toluene, 6 kg petroleum asphalt, 1.6 kg of polyamic acid solution prepared in Example 2, 0.08 kg cellulose nanofibers, 0.8 kg of an alcohol-water solution of silane coupling agent KH-560 with a solid content of 30% (the solvent is a mixture of ethanol and water in a volume ratio of 4:1), and 0.02 kg nickel acetylacetone evenly as a binder; mix the porous carbon air jet powder and the binder evenly in a high-speed mixer at a mass ratio of 100:12, and carry out the curing reaction at 120°C for 24 h; to obtain the precursor.
[0032] Steps (S2) to (S4) are the same as in Example 1.
[0033] Example 3 (S1) Mix 10 kg toluene, 5 kg petroleum asphalt, 1.8 kg of polyamic acid solution prepared in Example 2, 0.07 kg cellulose nanofibers, 0.6 kg of an alcohol-water solution of silane coupling agent KH-560 with a solid content of 30% (the solvent is a mixture of ethanol and water in a volume ratio of 7:1), and 0.02 kg nickel acetylacetone evenly as a binder; mix the porous carbon air jet powder and the binder evenly in a high-speed mixer at a mass ratio of 100:15, and carry out the curing reaction at 120°C for 24 h; to obtain the precursor.
[0034] Steps (S2) to (S4) are the same as in Example 1.
[0035] Comparative Example 1 Other conditions and operations are the same as in Example 1. The difference is that in step (S1), the binder is thermosetting phenolic resin Y606 diluted with water to a solid content of 45%, and the porous carbon gas fine powder and binder are in a mass ratio of 100:18. If the amount of binder is too small, the yield of 30-100 mesh particles will be too low.
[0036] Comparative Example 2 The other conditions and operations are the same as in Example 1, except that in step (S1), the binder is replaced with a mixture of 10 kg toluene and 6 kg petroleum asphalt.
[0037] Comparative Example 3 The other conditions and operations are the same as in Example 1, except that nickel dicene is not added to the binder in step (S1).
[0038] Comparative Example 4 The other conditions and operations are the same as in Example 1, except that cellulose nanofibers are not added to the binder in step (S1).
[0039] Application examples The yield can be understood as the percentage of 30-100 mesh particles in step S2, and the bonding performance of the binder is evaluated. Electrochemical performance was tested as follows: The silicon-carbon composite materials obtained in the embodiments and comparative examples of this invention were assembled into batteries, and their electrochemical performance was verified. The electrochemical performance test was conducted as follows: The assembled button batteries were tested on a Blue Electric system with a test voltage of 0.005-1.5V. The positive electrode material of the button battery was lithium foil, the negative electrode was silicon-carbon composite material, the conductive agent Super P and the binder polyacrylic acid were composed in a mass ratio of 86:7:7, the separator was a double-layer PP / PE, and the electrolyte was 1 mol / L LiPF6 (its solvent was a mixture of diethyl carbonate, dimethyl carbonate, and ethylene carbonate in a volume ratio of 1:1:1). The test results are shown in Table 1.
[0040] Table 1 Adhesive performance test .
[0041] As shown in Table 1, this invention utilizes a binder with specific components to simultaneously achieve effective bonding of porous carbon gas stream fine powder for its secondary utilization, and also improves the electrochemical performance of the resulting silicon-carbon composite material, especially its rate performance. The utilization process of porous carbon gas stream fine powder using this invention is simple, and the raw materials are inexpensive and readily available, making it a promising candidate for industrial application.
Claims
1. A method for preparing silicon-carbon composite anode materials using porous carbon gas stream powder, characterized in that, Includes the following steps: (S1) The porous carbon gas flow fine powder and the binder are mixed at a mass ratio of 100:12-18, and then the mixture is cured to obtain the precursor; the binder includes the following raw materials: petroleum asphalt, polyamic acid solution, cellulose nanofibers, epoxy silane coupling agent alcohol aqueous solution, nickel dicene and / or nickel acetylacetonate, toluene; (S2) After the precursor is crushed and screened, it is pyrolyzed and carbonized in an inert atmosphere to obtain pyrolytic carbon. (S3) Under an activating atmosphere, pyrolytic carbon is activated to obtain porous carbon materials; (S4) Silane deposition is performed on porous carbon to obtain silicon-carbon composite anode material.
2. The preparation method according to claim 1, characterized in that, The softening point of the petroleum asphalt is 40-60℃; and / or The intrinsic viscosity of polyamic acid is 1.5-1.9 dL / g; and / or The cellulose nanofibers have a diameter of 20-40 nm and a length of 200-500 nm; and / or The epoxy silane coupling agent is selected from at least one of 3-glycidyl etheroxypropyltrimethoxysilane, 3-(2,3-epoxypropoxy)propyltriethoxysilane, and 3-(2,3-epoxypropoxy)propylmethyldimethoxysilane; the solid content of the epoxy silane coupling agent in an alcoholic aqueous solution is 30-40%.
3. The preparation method according to claim 1, characterized in that, The polyamic acid solution is obtained by polycondensation of dianhydride monomer and diamine monomer in a polar aprotic solvent at a molar ratio of 1:0.8-1.
2.
4. The preparation method according to claim 1, characterized in that, The solid content of the polyamic acid solution is 20-30%.
5. The preparation method according to claim 3, characterized in that, The dianhydride monomer is selected from at least one of pyromellitic dianhydride, biphenyl dianhydride, oxydiphthalic anhydride, and naphthalenecyclodianhydride; the diamine monomer is selected from at least one of 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, p-phenylenediamine, m-phenylenediamine, 4,4'-bis(4-aminophenoxy)diphenyl sulfone, and 4,4'-diamino-2,2'-dimethylbiphenyl.
6. The preparation method according to claim 3, characterized in that, The polyamic acid is prepared by a method including the following steps: under an inert atmosphere, dianhydride monomer and diamine monomer are fed into a polar aprotic solvent and reacted at 10-25°C to obtain a polyamic acid solution.
7. The preparation method according to claim 6, characterized in that, The inert atmosphere is nitrogen and / or argon, and the polar aprotic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, and dimethyl sulfoxide; the amount of polar aprotic solvent added is such that the solid content of the polyamic acid solution is 20-30%.
8. The preparation method according to claim 1, characterized in that, The binder comprises the following raw materials in parts by weight: 4-6 parts petroleum asphalt, 1.6-2.1 parts polyamic acid solution, 0.05-0.08 parts cellulose nanofibers, 0.5-0.8 parts epoxy silane coupling agent alcohol aqueous solution, 0.01-0.02 parts nickel dicene and / or nickel acetylacetonate, and 10 parts toluene.
9. The preparation method according to claim 3, characterized in that, In step (S1), the porous carbon gas flow powder fine powder has a Dv50 ≤ 2 μm and a span ≤ 4.
10. The preparation method according to claim 3, characterized in that, In step (S2), the crushing and screening process controls the particle size to be 30-100 mesh; the inert atmosphere is nitrogen and / or argon; the pyrolysis carbonization process conditions are 600-800℃, and the pyrolysis time is 5-10h; and / or In step (S3), the activation atmosphere includes at least one of carbon dioxide and water vapor, the activation temperature is 900-1100℃, and the activation time is 10-24h; and / or In step (S4), the silane is selected from at least one of silane, silane, dichlorosilane, and trichlorosilane. The amount of silane gas introduced is such that the mass ratio of Si in the silicon-carbon composite material is between 40-60%, preferably between 45-55%. The temperature during silane deposition is 450-600℃.
Citation Information
Patent Citations
Preparation method for composite cathode material of lithium ion battery
CN102646818A
Silicon-carbon composite negative electrode material for enhancing structural stability by using one-dimensional material and preparation method of silicon-carbon composite negative electrode material
CN118658996A
Preparation method of composite porous carbon beneficial to silicon deposition and silicon-carbon composite negative electrode
CN119637871A
Preparation method of aerogel spherical porous carbon, preparation method of aerogel spherical silicon carbon negative electrode material and battery
CN119735206A
Silicon carbon material and preparation method thereof, secondary battery and electronic device
CN119920885A