Bridge I-shaped girder full penetration fillet weld welding process window determination method
By using computer finite element simulation and digital control thermal/mechanical simulation, the welding process window for the full penetration fillet weld of the main beam of the bridge I-shaped structure was determined, which solved the problem of difficulty in determining welding parameters in the existing technology, and realized efficient and stable selection of welding parameters to ensure the full penetration of the weld and the requirements for low-temperature impact toughness.
Patent Information
- Application Number
- CN202510944947.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-07-09
- Publication Date
- 2025-11-04
AI Technical Summary
Existing technologies require numerous combination trials to determine the welding process window for full penetration fillet welds on the main beams of bridges, and cannot determine specific welding parameters. This makes it impossible to guarantee full penetration of the weld and low-temperature impact toughness requirements of the heat-affected zone when welding parameters are changed.
By using computer finite element simulation and digital control thermal/mechanical simulation, the minimum and maximum values of welding heat input are determined. Combined with historical experience data of welding methods, the parameter ranges of welding current, voltage, and speed are deduced, and welding processes are developed to guide the welding of full penetration fillet welds.
Quickly determine the full penetration high-efficiency welding process window for different steel plate materials and thicknesses, reduce combination trial experiments, ensure full penetration of weld and low-temperature impact toughness requirements of weld heat-affected zone, and improve welding production efficiency and pass rate.
Smart Images

Figure CN120893244A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of bridge welding technology, specifically a method for determining the welding process window for full penetration fillet welds on I-shaped main beams of bridges. Background Technology
[0002] For the I-beam main girder of the steel bridge (web plate thickness 10-20mm), during the full penetration welding of fillet welds, the web plate is not beveled, and the root pass is not cleaned before welding the back side. Single-wire submerged arc welding or double-wire submerged arc welding with double-sided single-pass high heat input is used. When using this welding method, the welding process window needs to be determined to ensure the weld's full penetration and mechanical properties. The magnitude of the welding heat input directly affects the weld's fusion depth and the mechanical properties of the heat-affected zone (mainly the low-temperature impact toughness of the heat-affected zone). The lower limit (minimum value) of the welding heat input must meet the weld's full penetration requirement, and the upper limit (maximum value) must meet the design requirements for the weld's mechanical properties (mainly the low-temperature impact toughness of the heat-affected zone).
[0003] If the welding heat input is less than the lower limit, the weld penetration will be insufficient, failing to achieve full penetration welding and thus not meeting the Class I qualification requirement for ultrasonic testing of full penetration welds in steel bridges. Currently, most bridge steel plates are delivered in the thermomechanically rolled (TMCP) condition. TMCP steel plates are sensitive to heat input, have a narrow welding process window, and the welding process window varies significantly between different steel grades. Excessive welding heat input can cause many problems to the weld heat-affected zone (HAZ), such as: significant local grain coarsening in the HAZ, a sharp increase in the tendency for coarse grains to become embrittled; increased size of acicular and blocky ferrite, significant coarsening of granular bainite, increased MA (Mao Island) component content, which is blocky and unevenly distributed at grain boundaries and within grains. The blocky MA component acts as a crack initiation source; the higher its content and the larger its size, the easier it is to generate cracks, resulting in very low low-temperature impact toughness; and a reduction in the number of large-angle grain boundaries, reducing the number of units that effectively hinder crack propagation, significantly decreasing the low-temperature impact toughness of the HAZ. Therefore, it is necessary to strictly control the upper limit of welding heat input to ensure the mechanical properties of the welding heat-affected zone.
[0004] Currently, the welding process window for the full penetration main weld of the I-beam of steel bridge is mostly determined by combining and trying different methods based on past engineering experience. For example, for a certain steel grade and plate thickness, different welding methods (such as single-wire submerged arc welding and double-wire submerged arc welding), welding current, voltage, welding speed, welding torch offset angle, etc. are used to combine multiple parameters. Then, multiple sets of test pieces are welded. After parameter combination, the number of welding tests is huge, which consumes a lot of manpower, material resources and time. Then, the parameter combination that can ensure full penetration of the weld and qualified low-temperature impact toughness of the heat-affected zone is selected as the process parameters for welding production.
[0005] If the steel grade, plate thickness, or both change, a new round of combination trials is required. Furthermore, this method cannot determine the specific fusion depth of the welds on both sides, the overlap of the welds, or the margin of error for the selected welding parameters. In other words, the welding process window (wire quantity, current, voltage, welding speed, welding heat input, etc.) is a set of specific values, not a range, which greatly complicates welding operations. Changes in welding parameters will affect the weld penetration and the low-temperature impact toughness of the heat-affected zone. For example, a decrease in welding heat input or a change in the welding torch angle will make it impossible to guarantee that the weld meets the full penetration requirement; conversely, an increase in welding heat input will make it impossible to guarantee that the low-temperature impact toughness of the heat-affected zone meets the requirements.
[0006] For example, the invention patent application with publication number CN118218726A, entitled "An Efficient Welding Process for T-Type Full Penetration Fillet Welds with Thicker Web Plates," uses this traditional combined trial method to determine welding parameters. These welding parameters are only applicable to efficient welding processes for T-type full penetration fillet welds with specific materials and plate thicknesses. If the steel grade, plate thickness, or both are changed, the process may no longer be applicable, requiring a large number of combined experiments to determine the welding parameters, which has significant limitations. Summary of the Invention
[0007] The purpose of this invention is to provide a method for determining the welding process window of full penetration fillet welds for I-beams of bridges, so as to solve the problems mentioned in the background art.
[0008] To achieve the above objectives, the present invention provides the following technical solution:
[0009] A method for determining the welding process window for full penetration fillet welds on I-beams of bridges includes:
[0010] S1. Determine the minimum welding heat input and welding torch offset angle range of the I-shaped main beam through computer finite element simulation, i.e., the lower limit of the welding process window.
[0011] S2. The maximum value of welding heat input for the I-shaped main beam is determined by digital control thermal / mechanical simulation, which is the upper limit of the welding process window;
[0012] S3. Based on the lower limit of the welding process window in step S1 and the upper limit of the welding process window in step S2, determine the range of the welding process window, select the corresponding welding method, and according to the selected welding method and the determined welding heat input range and welding torch offset angle, combined with the historical welding experience data corresponding to the welding method, deduce the parameter range of welding current, welding voltage and welding speed according to the welding heat input formula, and compile the welding process to guide the welding of full penetration fillet welds of the I-shaped main beam.
[0013] As a further aspect of the present invention, the specific process of step S1 is as follows: using computer finite element simulation software, geometric modeling, determination of the thermophysical property parameters of the material, mathematical modeling of the heat source model, heat source verification of the T-joint of the I-shaped main beam, simulation calculation of the temperature field and stress field, and numerical simulation results and analysis are performed in sequence to complete the finite element simulation. The influence of welding heat input and welding torch offset angle on the penetration depth and angular deformation of the T-joint is simulated. By calculating the penetration depth and overlap of the welds on both sides, under the premise of meeting the full penetration requirements of welds of various plate thicknesses and the overlap of welds on both sides not less than 3mm, the lower limit of the welding process window for various web plate thickness combination fillet welds is determined, namely the minimum value of welding heat input and the range of welding torch offset angle.
[0014] As a further aspect of the present invention, the numerical simulation results and analysis specifically include: analysis of the weld depth of the T-joint, analysis of the temperature field simulation results, analysis of the stress field simulation results, and analysis of the angular deformation results.
[0015] As a further aspect of the present invention, the specific process of step S2 is as follows: the influence of welding heat input on the microstructure and properties of the coarse-grained heat-affected zone of various steel grades is simulated using a Gleeble-3500 digital control thermal / mechanical simulation testing machine. Specifically, the thermal cycling process experienced by the coarse-grained heat-affected zone of various steel grades under various welding heat input conditions is simulated respectively.
[0016] Metallographic specimens and standard impact specimens were prepared for the samples after thermal cycling, and the effects of various welding heat input conditions on the microstructure and properties of the coarse-grained heat-affected zone of the steel were compared and studied.
[0017] The morphology of various samples was observed under an optical microscope, and EBSD observation was performed under a scanning electron microscope equipped with EBSD function to obtain microstructures with various orientations. The low-temperature impact energy of the coarse-grained heat-affected zone of the sample was tested under an impact testing machine.
[0018] The low-temperature impact energy of the coarse-grained heat-affected zone of the sample was statistically analyzed, and the maximum heat input value that meets the requirements of the low-temperature impact energy of the coarse-grained heat-affected zone was selected as the maximum allowable heat input value for a certain steel grade, which is the upper limit of the welding process window.
[0019] As a further aspect of the present invention, in step S2: when selecting the maximum heat input condition, the microstructure requirements that the sample needs to meet are as follows: the original austenite grain size is less than 100 μm, the microstructure is a mixture of lath ferrite, granular bainite and polygonal ferrite, and the proportion of microstructure orientation difference angle > 15° is more than 20%.
[0020] As a further aspect of the present invention, the welding heat input formula in step S3 is specifically as follows:
[0021]
[0022] Where Q represents the welding heat input; k represents the thermal efficiency, which is 1 for submerged arc welding; U is the welding voltage; I is the welding current; and v is the welding speed.
[0023] Compared with the prior art, the beneficial effects of the present invention are: the method of the present invention can quickly determine the full penetration high-efficiency welding process window for different steel plate materials and different web thicknesses (10-20mm), and select welding parameters within the determined welding process window range for welding, which can ensure both the full penetration requirement of the weld and the low-temperature impact toughness requirement of the heat-affected zone, avoid a large number of combined welding tests, and save costs and time for the manufacturer. Attached Figure Description
[0024] Figure 1 This is an analysis diagram of the weld penetration on both sides of the T-joint in this invention;
[0025] Figure 2 This is an analysis diagram of the deformation results of the T-joint angle in this invention;
[0026] Figure 3 This is a micrograph of the tissue morphology and microstructure of the sample used in this invention.
[0027] Figure 4 This is a cross-sectional view of the 1R10 I-shaped main beam in this invention. Detailed Implementation
[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] Please see Figures 1-4 A method for determining the welding process window for full penetration fillet welds on the main beam of a bridge, comprising:
[0030] S1. Determine the minimum welding heat input and welding torch offset angle range of the I-shaped main beam through computer finite element simulation, i.e., the lower limit of the welding process window.
[0031] S2. The maximum value of welding heat input for the I-shaped main beam is determined by digital control thermal / mechanical simulation, which is the upper limit of the welding process window;
[0032] S3. Based on the lower limit of the welding process window in step S1 and the upper limit of the welding process window in step S2, determine the range of the welding process window, select the corresponding welding method, and according to the selected welding method and the determined welding heat input range and welding torch offset angle, combined with the historical welding experience data corresponding to the welding method, deduce the parameter range of welding current, welding voltage and welding speed according to the welding heat input formula, and compile the welding process to guide the welding of full penetration fillet welds of the I-shaped main beam.
[0033] As a specific solution, step S1 involves the following steps: using the finite element simulation software SYSWELD, geometric modeling, determination of material thermophysical property parameters, mathematical modeling of the heat source model, heat source verification of the T-joint of the I-shaped main beam, simulation calculation of temperature and stress fields, and analysis of numerical simulation results are performed sequentially to complete the finite element simulation. This simulation simulates the influence of welding heat input and welding torch offset angle on the penetration depth and angular deformation of the T-joint. By calculating the penetration depth and overlap of the welds on both sides, and under the premise of meeting the full penetration requirements for welds of various plate thicknesses and ensuring that the overlap of the welds on both sides is not less than 3mm, the lower limit of the welding process window for fillet welds of various web plate thickness combinations (e.g., web plate thickness 10-20mm) is determined, i.e., the minimum welding heat input and the range of welding torch offset angle. Through these constraints, a certain margin is provided in the lower limit of the welding process window, ensuring full penetration of the weld even if there are deviations in heat input or welding torch angle during welding production.
[0034] Specifically, the numerical simulation results and analyses include: analysis of the weld depth of the T-joint, analysis of the temperature field simulation results, analysis of the stress field simulation results, and analysis of the angular deformation results.
[0035] For main beam steel plates with yield strengths of 345, 370, and 420 MPa, all are of the same steel type, and their thermophysical properties are basically the same. In the finite element simulation, the influence of steel type change on the weld penetration of the T-joint can be disregarded. Only three factors with a significant impact on the weld penetration of the T-joint are selected as variables: web thickness (10, 12, 14, 16, 18, and 20 mm respectively), welding heat input (40, 50, 60, 70, and 80 KJ / cm respectively), and welding torch offset angle (38° and 45° with the cover plate respectively). Figure 1 As shown, it is an analysis diagram of the weld penetration on both sides of the T-joint, as follows. Figure 2 As shown, it is an analysis diagram of the deformation results of the T-type joint angle.
[0036] As a specific solution, the specific process of step S2 is as follows: The influence of welding heat input on the microstructure and properties of the coarse-grained heat-affected zone (CGHAZ) of various steel grades is simulated using a Gleeble-3500 digital control thermal / mechanical simulation testing machine. The microstructure and composition of different plate thicknesses (12-20mm range) of the same steel grade are basically the same, so the influence of plate thickness can be ignored. Only two factors that have a large influence on the microstructure and properties of the coarse-grained heat-affected zone (CGHAZ) are selected as variables to simulate the thermal cycle process experienced by the coarse-grained heat-affected zone of various steel grades with yield strength (e.g., 345, 370, 420MPa grade) under various welding heat input conditions (e.g., 40, 50, 60, 70, 80KJ / cm).
[0037] Specifically, the sample plate thickness was selected as 18 mm, and longitudinal samples were taken from steel plates of different steel grades. The sample size was 10.5X10.5X80 mm. The heat transfer model of the HAZ software package Rykalin-2D was used to generate thermal cycle curves simulating different welding heat inputs (40, 50, 60, 70, 80 KJ / cm). The curves were then imported into the Gleeble-3500 digital control thermal / mechanical simulation test machine to simulate the thermal cycle process experienced by the coarse-grained heat-affected zone (CGHAZ).
[0038] Metallographic specimens and standard impact specimens were prepared for the samples after thermal cycling, and the effects of various welding heat input conditions on the microstructure and properties of the coarse-grained heat-affected zone (CGHAZ) of the steel were compared and studied.
[0039] The tissue morphology of various samples was observed under an optical microscope, and EBSD observation was performed under a scanning electron microscope equipped with EBSD function to obtain microstructures with various tissue orientations, such as... Figure 3 As shown, the low-temperature impact energy of the coarse-grained heat-affected zone (CGHAZ) of the specimen was tested under an impact testing machine.
[0040] The low-temperature impact energy of the coarse-grained heat-affected zone (CGHAZ) of the sample was statistically analyzed. The maximum heat input value that meets the low-temperature impact energy requirement of the coarse-grained heat-affected zone (CGHAZ) was selected as the maximum allowable heat input value for a certain steel grade, which is the upper limit of the welding process window.
[0041] In step S2, when selecting the maximum heat input condition, the microstructure requirements that the sample needs to meet are as follows: the original austenite grain size is less than 100 μm, the microstructure is a mixture of lath ferrite, granular bainite and polygonal ferrite, and the proportion of microstructure orientation difference angle > 15° is more than 20%.
[0042] As a specific approach, based on the lower limit of the welding process window in step S1 and the upper limit of the welding process window in step S2, the range of the welding process window is determined, and the corresponding welding method (such as single-wire submerged arc welding or double-wire submerged arc welding) is selected. According to the selected welding method and the determined welding heat input range and welding torch offset angle, combined with the historical welding experience data corresponding to the welding method (for example, the common heat input for single-wire submerged arc welding is generally 30-50 KJ / cm, and the common heat input for double-wire submerged arc welding is 50-100 KJ / cm), the parameter ranges of welding current, welding voltage and welding speed are derived by reversing the welding heat input formula, and the welding process is compiled to guide the welding of full penetration fillet welds on the I-shaped main beam.
[0043] Specifically, the welding heat input formula in step S3 is as follows:
[0044]
[0045] Where Q represents the welding heat input; k represents the thermal efficiency, which is 1 for submerged arc welding; U is the welding voltage; I is the welding current; and v is the welding speed.
[0046] The method of this invention only requires computer finite element simulation and thermophysical simulation experiments to determine the efficient full penetration welding process window for steel bridge I-beams with multiple steel grades and web plate thicknesses. The selected process window meets the full penetration requirement and has an appropriate margin, with a lap of more than 3mm on both sides of the weld. It can meet the requirement of Level I qualification for ultrasonic testing of full penetration welds during large-scale welding production, and the first-pass qualification rate of welds reaches more than 98%. Welding procedure qualification tests are conducted on typical cases. For example, for Q420MD with a web plate thickness of 18mm, welding test plates are welded using welding parameters within the welding process window. The -20℃ impact energy of the weld heat-affected zone of the weld test plate meets the standard requirements, and other mechanical properties also meet the requirements.
[0047] Traditional methods for determining the welding process window for full penetration fillet welds on main beams of bridges typically employ a combination trial approach to determine welding parameters. This involves combining multiple parameters such as the number of welding wires (e.g., single-wire submerged arc welding and double-wire submerged arc welding), welding current, voltage, welding speed, and welding torch offset angle for different steel grades (bridge steel plates with yield strengths of 345, 370, and 420 MPa), different plate thicknesses (web plate thickness of 10–20 mm), and different welding currents, voltages, welding speeds, and welding torch offset angles. This results in a large number of welding tests after parameter combinations, often requiring at least several thousand sets of combined tests before the results of the technical solution of this invention can be obtained.
[0048] The method of this invention can avoid a large number of parameter combination experiments, reduce the consumption of manpower, material resources and time, and at the same time, it has high process stability, is applicable to a wide range of steel types, and is suitable for determining the full penetration high-efficiency welding process window for steel bridge I-beams with web plate thickness of 10-20mm. The first-time flaw detection pass rate of welds is high, and the mechanical properties of the weld heat-affected zone meet the requirements.
[0049] As a specific case, the welding condition of the full penetration fillet weld of the I-beam numbered 1R10 and the results of the tensile and impact tests of the full penetration fillet weld are shown in Tables 1 and 2 below. The cross-sectional view of the 1R10 I-beam is shown below. Figure 4 As shown.
[0050] Table 1: Welding status of full penetration fillet welds
[0051]
[0052] Table 2: Results of tensile and impact tests on full penetration fillet welds
[0053]
[0054]
[0055] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
Claims
1. A method for determining the welding process window for full penetration fillet welds on I-beams of bridges, characterized in that, include: S1. Determine the minimum welding heat input and welding torch offset angle range of the I-shaped main beam through computer finite element simulation, i.e., the lower limit of the welding process window. S2. The maximum value of welding heat input for the I-shaped main beam is determined by digital control thermal / mechanical simulation, which is the upper limit of the welding process window; S3. Based on the lower limit of the welding process window in step S1 and the upper limit of the welding process window in step S2, determine the range of the welding process window, select the corresponding welding method, and according to the selected welding method and the determined welding heat input range and welding torch offset angle, combined with the historical welding experience data corresponding to the welding method, deduce the parameter range of welding current, welding voltage and welding speed according to the welding heat input formula, and compile the welding process to guide the welding of full penetration fillet welds of the I-shaped main beam.
2. The method for determining the welding process window for full penetration fillet welds of I-beams in bridges according to claim 1, characterized in that, The specific process of step S1 is as follows: using computer finite element simulation software, geometric modeling, determination of material thermophysical property parameters, mathematical modeling of heat source model, heat source verification of T-joint of I-shaped main beam, simulation calculation of temperature field and stress field, and numerical simulation results and analysis are performed in sequence to complete the finite element simulation. The influence of welding heat input and welding torch offset angle on the penetration and angular deformation of T-joint is simulated. By calculating the penetration of welds on both sides and the overlap of welds on both sides, under the premise of meeting the full penetration requirements of welds of various plate thicknesses and the overlap of welds on both sides not less than 3mm, the lower limit of the welding process window for various web plate thickness combination fillet welds is determined, that is, the minimum value of welding heat input and the range of welding torch offset angle.
3. The method for determining the welding process window for full penetration fillet welds of I-beams in bridges according to claim 2, characterized in that, The numerical simulation results and analyses specifically include: analysis of the weld depth of the T-joint, analysis of the temperature field simulation results, analysis of the stress field simulation results, and analysis of the angular deformation results.
4. The method for determining the welding process window for full penetration fillet welds of I-beams in bridges according to claim 2, characterized in that, The specific process of step S2 is as follows: the influence of welding heat input on the microstructure and properties of the coarse-grained heat-affected zone of various steel grades is simulated using a Gleeble-3500 digital control thermal / mechanical simulation testing machine. Specifically, the thermal cycling process experienced by the coarse-grained heat-affected zone of various steel grades with different yield strengths is simulated under various welding heat input conditions. Metallographic specimens and standard impact specimens were prepared for the samples after thermal cycling, and the effects of various welding heat input conditions on the microstructure and properties of the coarse-grained heat-affected zone of the steel were compared and studied. The morphology of various samples was observed under an optical microscope, and EBSD observation was performed under a scanning electron microscope equipped with EBSD function to obtain microstructures with various orientations. The low-temperature impact energy of the coarse-grained heat-affected zone of the sample was tested under an impact testing machine. The low-temperature impact energy of the coarse-grained heat-affected zone of the sample was statistically analyzed, and the maximum heat input value that meets the requirements of the low-temperature impact energy of the coarse-grained heat-affected zone was selected as the maximum allowable heat input value for a certain steel grade, which is the upper limit of the welding process window.
5. The method for determining the welding process window for full penetration fillet welds of I-beams in bridges according to claim 4, characterized in that, In step S2: when selecting the maximum heat input conditions, the microstructure requirements that the sample needs to meet are as follows: the original austenite grain size is less than 100 μm, the microstructure is a mixture of lath ferrite, granular bainite and polygonal ferrite, and the proportion of microstructure orientation difference angle > 15° is more than 20%.
6. The method for determining the welding process window for full penetration fillet welds of bridge I-beams according to claim 5, characterized in that, The welding heat input formula in step S3 is as follows: Where Q represents welding heat input; k represents thermal efficiency; U is welding voltage; I is welding current; and v is welding speed.
Citation Information
Patent Citations
Efficient welding process for T-shaped penetration fillet weld of thick web
CN118218726A