A method for predicting whether chipping will occur in engineered wood panels

By milling grooves on the surface of engineered wood panels and measuring the height of serrated defects, the problem of predicting edge chipping in engineered wood panel production was solved, enabling rapid and accurate quality control and avoiding economic losses and quality problems.

CN120985765BActive Publication Date: 2026-11-10INST OF WOOD INDUDTRY CHINESE ACAD OF FORESTRY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410631314.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2026-11-10
Estimated Expiration
2044-05-21

AI Technical Summary

Technical Problem

Existing technologies cannot predict edge chipping during the production of engineered wood panels, leading to defects such as curling, burrs, breakage, and peeling during use or cutting, which affect the appearance quality of finished products and cause customer complaints and economic losses.

Method used

Milling grooves are performed on the surface of the artificial board. The presence of serrated defects on the side of the decorative layer of the milled groove is observed, and the maximum height of the serrated defects is measured. A threshold (0.5 mm) is set to determine whether the board has a risk of edge chipping.

Benefits of technology

It enables rapid and accurate prediction of edge chipping during the production of engineered wood panels, avoiding finished product quality defects, customer complaints and economic losses, and reducing production costs and resource waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN120985765B_ABST
    Figure CN120985765B_ABST
Patent Text Reader

Abstract

This invention relates to a method for predicting edge chipping in engineered wood products, comprising: firstly, milling a "U"-shaped groove on the surface of the engineered wood product; then observing whether there are serrated defects on the side edge of the decorative layer next to the groove after milling; if so, measuring the maximum height of the serrated defect (i.e., the maximum length perpendicular to the groove direction, from the junction of the groove and the decorative layer to the outer edge of the serrated defect). If the maximum height of the serrated defect is ≥0.5mm, it indicates that the engineered wood product is unqualified and will chip during use and sawing. This invention provides accurate and rapid prediction results, quickly detecting edge chipping defects in the same batch of products using only small samples; it avoids lawsuits regarding product quality and economic losses caused by product quality issues; moreover, the equipment used in this invention is simple, being standard production and processing equipment for engineered wood product manufacturers, reducing testing costs and production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for quality inspection of engineered wood products, and more particularly to a method for detecting edge chipping in engineered wood products, belonging to the field of engineered wood manufacturing. Background Technology

[0002] Currently, engineered wood panels on the market are manufactured through processes such as pressing, molding, and curing. Commonly used types include particleboard, medium-density fiberboard (MDF), blockboard (plywood), plywood, and decorative engineered wood panels such as fire-resistant boards. When engineered wood panels are used to make furniture, uneven cut surfaces, curling, and rough edges can occur during the cutting process due to the inherent properties of the wood itself, as well as the influence of cutting tools and speed. In particular, the edge-trimming process can easily cause serrated defects on the surface of decorative panels, i.e., chipping.

[0003] Customized home furnishing products are assembled from engineered wood panels through sawing, edge banding, drilling, and assembly. Edge chipping is a cosmetic defect that occurs during the sawing process of engineered wood panels, resulting in curling, burrs, breakage, or peeling at the cut edge. Edge chipping is a quality defect of engineered wood panels; high-quality engineered wood panels will not exhibit these defects. When edge chipping occurs during panel sawing, this cosmetic defect is irreparable, affecting not only the aesthetics of the customized home furnishing product but also creating a defect in the finished wooden furniture product (GB / T 3324 "General Technical Conditions for Wooden Furniture" stipulates that the veneer, edge banding, and edge binding of panels should not exhibit delamination, bubbling, or cracking, further leading to losses for furniture manufacturers and users).

[0004] Edge chipping refers to the unevenness, curling, burrs, breakage, and peeling that occurs on the cut surface of engineered wood panels during the cutting process, due to inherent characteristics of the panel itself, as well as the effects of cutting tools and speed. During use, the edges of the panel may begin to shed particles, crack, or break, severely impacting its lifespan and aesthetics. There are many reasons for edge chipping: it may be related to the material itself; it may be related to the manufacturing process; and it may be related to the storage environment.

[0005] Edge chipping in engineered wood panels is caused by a variety of factors. Given the current level of process control in engineered wood panel production, edge chipping has a certain degree of randomness; that is, it is not particularly related to product type or raw materials. Edge chipping often occurs within the same batch of products, and its presence is only discovered after the purchase order contract between the engineered wood panel user (i.e., customer, such as furniture manufacturers or users) and the engineered wood panel producer takes effect. This can lead to issues such as delayed delivery, customer complaints, and financial disputes; or even property damage or more serious economic losses.

[0006] If chipping or cracking occurs during sawing or use of the engineered wood panels after a furniture manufacturer signs a customer order, it means that the entire batch of engineered wood panels has the same problem. Re-producing the panels would not only delay the order and generate customer complaints, but also result in significant economic losses. However, if chipping or cracking could be predicted during the engineered wood panel production process, these problems could be avoided.

[0007] However, to date, the standards for engineered wood products, such as GB / T 15102-2017 "Impregnated Paper-faced Fiberboard and Particleboard", GB / T 34722-2017 "Impregnated Paper-faced Plywood and Blockboard", and GB / T 17657-2022 "Test Methods for Physical and Chemical Properties of Engineered Wood Products and Decorated Engineered Wood Products", do not include test methods for edge chipping of the boards.

[0008] Because current standards for engineered wood products lack methods for predicting and detecting edge chipping, chipping is often only discovered after a customer places an order and the product has passed inspection according to existing standards and entered into production (i.e., custom furniture making, board cutting). By then, the board has already been used, and replacing it at the last minute will cause order delays and financial losses for the customer. In other words, because edge chipping is unpredictable, it cannot be stipulated in the sales agreement; revisions are only made after problems arise, leading to delays in order delivery and resulting in economic losses.

[0009] Therefore, there is an urgent need to develop a method that can predict whether chipping will occur in engineered wood products during the production process. After repeated experiments, the inventors have creatively developed a method for predicting and identifying chipping performance of engineered wood products. This method can effectively predict chipping, avoid customer complaints caused by chipping in wooden furniture products, and avoid production delays and production losses caused by chipping. Summary of the Invention

[0010] The purpose of this invention is to address the issue of edge chipping defects in existing engineered wood products, a technical problem that can only be discovered by users during use or cutting after the products are delivered. This leads to defects such as curling, burrs, breakage, and peeling during use, further resulting in defects in the appearance of finished products, consumer disputes, work delays, and production losses. This invention provides a method to predict whether edge chipping will occur in engineered wood products during production. The method involves milling a sample board and observing whether there are serrated defects on the side of the milled groove's decorative layer, as well as measuring the maximum height h of the serrated defects. This accurately predicts and judges whether edge chipping will occur in the produced engineered wood products, reducing quality defects, consumer disputes, work delays, production losses, and economic losses in the finished engineered wood products.

[0011] To achieve the objectives of this invention, one aspect of this invention provides a method for predicting whether chipping will occur in engineered wood panels, comprising: firstly, milling grooves on the surface of the engineered wood panel; then observing whether there are serrated defects on the side of the decorative layer of the groove after milling; and if there are serrated defects, measuring the maximum height of the serrated defects.

[0012] The method of this invention is used to predict whether chipping will occur in the process of using, cutting, sawing, drilling, etc. of the board material.

[0013] The artificial board material is one or more of the following: impregnated paper-faced particleboard, impregnated paper-faced oriented strand board, impregnated paper-faced fiberboard, impregnated paper-faced blockboard, and impregnated paper-faced plywood.

[0014] In particular, a milling cutter is selected to perform the milling groove treatment on the surface of the artificial board.

[0015] In particular, the milling cutter performs the aforementioned groove treatment on the surface of the artificial board on the side of the impregnated paper veneer.

[0016] In particular, the cutting diameter of the milling cutter is 1-3 mm, preferably 2 mm.

[0017] In particular, if the maximum height of the serrated defect is ≥0.5mm, it indicates that the artificial board is unqualified and has chipped edges.

[0018] In particular, the maximum height of the serrated defect is the serration height, that is, the maximum value of the tooth height, which is the maximum length from the junction of the groove and the finishing layer to the outer edge of the serrated defect in the groove direction perpendicular to the milled groove.

[0019] In particular, a milling cutter is selected to perform the "U"-shaped or "circular" milling groove treatment on the surface of the artificial board, preferably the "U"-shaped milling groove treatment.

[0020] In particular, the router bit performs the said "Hui"-shaped or circular grooving treatment on the surface of the impregnated melamine paper decorated side of the artificial board, preferably the "Hui"-shaped grooving treatment.

[0021] In particular, the method further comprises randomly selecting one board from artificial boards of the same shift, same specification base material, same color pattern and same batch of decoration during the artificial board production process, and performing the said "Hui"-shaped grooving treatment.

[0022] In particular, the method further comprises cutting the randomly selected board to obtain a single-side surface area of (800-10000) cm 2 before performing the said "Hui"-shaped grooving treatment to prepare a grooved test piece; preferably 1600-10000 cm 2 , more preferably (2500-3600) cm 2 , still more preferably (2500-2800) cm 2 .

[0023] In particular, the grooved test piece is cut to a size of (40-100) cm × (40-100) cm, preferably (50-60) cm × (50-60) cm, more preferably 50 cm × 50 cm.

[0024] In particular, after cutting into a grooved test piece of 50 cm × 50 cm × board thickness, the said "Hui"-shaped grooving treatment is performed.

[0025] In particular, the size of the grooved test piece is preferably 50 cm × 50 cm × board thickness.

[0026] In another aspect, the present invention provides a method for predicting whether edge chipping occurs in an artificial board, comprising the following steps:

[0027] 1) Randomly select one board from the to-be-predicted artificial boards of the same shift, same specification base material, same color pattern and same batch of decoration during the artificial board production process, as the test piece board for prediction;

[0028] 2) On the decorative layer side of the test piece board for prediction, perform "Hui"-shaped grooving treatment (i.e., cutting treatment) with a router bit;

[0029] 3) Observe the routed groove left after the grooving treatment, and check whether there are serrated defects on the side edge of the decorative layer of the routed groove; if there are no serrated defects, the to-be-predicted artificial board is qualified and has no edge chipping problem; if there are serrated defects, measure the maximum height of the serrated defects; wherein:

[0030] 3A) If the maximum height of the serrated defects on the side edge of the decorative layer of the routed groove is ≥ 0.5 mm, it is predicted that this batch of artificial boards is unqualified and prone to edge chipping;

[0031] 3B) If the maximum height of the serrated defects on the side of the milled groove finishing layer is <0.5mm, then the batch of engineered wood panels is predicted to be qualified and there is no edge chipping problem.

[0032] Wherein, the artificial board mentioned in step 1) is one or more of the following: impregnated paper-faced particleboard, impregnated paper-faced oriented strand board, impregnated paper-faced fiberboard, impregnated paper-faced blockboard, and impregnated paper-faced plywood.

[0033] In particular, the cutting diameter of the milling cutter described in step 2) is 1-3 mm, preferably 2 mm.

[0034] In particular, during the "return" shaped milling process described in step 2), the rotational speed of the milling cutter is controlled to be 10,000-20,000 r / min, preferably 15,000 r / min; the feed speed of the plate is 5-6 m / min, preferably 5.5 m / min; and the milling groove depth is 0.5-1.0 mm, preferably 0.75 mm.

[0035] In particular, the milling path (i.e. the length of the cut groove) of the "return" shaped milling groove described in step 2) is at least 30m, preferably 30-40m.

[0036] In particular, the width of the plate finishing layer of the milled groove after the "return" shaped milling treatment is at least 1.5 mm, preferably 1.5-2.5 mm, and more preferably 2 mm.

[0037] In particular, it also includes placing the pre-test specimen plate in an environment with a temperature of (20±2)℃ and a relative humidity of (65±5)% until the mass is constant before performing the milling process.

[0038] Another aspect of the present invention provides a method for predicting edge chipping of engineered wood panels, comprising the following steps:

[0039] A) Randomly select one board from the same shift, same specification of substrate, same color, and same batch of finishes of the artificial board to be predicted, as the pre-test board.

[0040] B) The randomly selected pre-test specimens are cut to form a surface area (single-sided) of (800-10000) cm². 2 Milled groove test pieces;

[0041] C) On one side of the decorative layer of the milled groove specimen, a "return" shaped milling groove is made using a routing cutter;

[0042] D) Observe the milled grooves left after milling to check for serrated defects on the sides of the decorative layer. If there are no serrated defects, the engineered wood panel is expected to be qualified and there will be no edge chipping. If there are serrated defects, measure the maximum height of the serrated defects.

[0043] D1) If the maximum height of the serrated defects on the side of the finish layer of the milled groove is ≥0.5mm, it is predicted that the batch of artificial board is unqualified and prone to edge chipping.

[0044] D2) If the maximum height of the serrated defects on the side of the milled groove finishing layer is <0.5mm, then the batch of artificial boards is predicted to be qualified and there is no edge chipping problem.

[0045] The surface area of ​​the milled groove specimen in step B) is preferably 1600-10000 cm². 2 Further preferred is (2500-3600) cm 2 Further preferred is (2500-2800) cm 2 .

[0046] In particular, the milled groove specimen described in step B) is cut to a size of (40-100)cm×(40-100)cm, preferably (50-60)cm×(50-60)cm, and more preferably 50cm×50cm.

[0047] In particular, the cutting diameter of the milling cutter described in step C) is 1-3 mm, preferably 2 mm.

[0048] In particular, in step C), during the “return” shaped milling process, the rotational speed of the milling cutter is controlled to be 10,000-20,000 r / min, preferably 15,000 r / min; the feed speed of the plate is 5-6 m / min, preferably 5.5 m / min; and the milling groove depth is 0.5-1.0 mm, preferably 0.75 mm.

[0049] In particular, the milling path (i.e. the length of the cut groove) of the "return" shaped milling groove described in step C) is at least 30m, preferably 30-40m.

[0050] In particular, the width of the plate finishing layer of the milled groove after the "return" shaped milling treatment is at least 1.5 mm, preferably 1.5-2.5 mm, and more preferably 2 mm.

[0051] Edge chipping is a common and emerging quality problem discovered in the production and processing of customized furniture in recent years. Current standards and testing methods lack testing requirements or predictive methods for this defect. It often only becomes apparent after a customer places an order and production begins, when the boards are being cut and sawn. By this time, the boards have already been used, and replacing them at the last minute will cause delays to the customer's order.

[0052] Given the lack of methods for predicting the edge chipping performance of boards, this method can effectively predict whether boards will have edge chipping quality defects, avoid customer complaints caused by the appearance quality defects of finished wooden furniture products due to defective boards after they are put into production, avoid production delays caused by edge chipping quality problems, save costs, and reduce resource waste.

[0053] If there are serrated defects with a maximum height of ≥0.5mm on the side of the milled groove finish layer, it indicates that the batch of artificial boards is unqualified and the boards will have chipping quality problems during use and sawing; if there are no serrated defects or the height of the defects is less than 0.5mm, it indicates that the batch of boards is qualified and the boards will not have chipping during sawing or use.

[0054] The method of this invention provides accurate and rapid prediction results, and can quickly detect whether there are chipped edges in the same batch of boards using only small sample blocks; it avoids lawsuits regarding board quality and economic losses caused by board quality problems; moreover, the equipment used in this invention is simple and can be used by conventional production and processing equipment for artificial board manufacturers, reducing testing costs and the production cost of artificial boards.

[0055] The rapid testing method for chipping edges of boards provided in this paper can not only quickly predict whether a batch of boards will chip using small samples, but also fill the gap in the detection of chipping defects in the quality indicators of engineered wood products and improve the quality inspection standards for engineered wood products.

[0056] Compared with the prior art, the method of the present invention has the following advantages and benefits:

[0057] 1. The method for predicting edge chipping of boards in this invention has a fast detection speed. It can be monitored and tested in real time by the manufacturer after the artificial board is produced, avoiding the problem of edge chipping being discovered by the user during processing or use after the board is delivered. This reduces customer lawsuits about board quality and economic losses caused by quality problems.

[0058] 2. The method of the present invention uses a small amount of material during the testing process. It can use a whole sheet of board for testing or a small-sized board for testing specimens. It does not require a large number of boards to be sawn to determine whether the board of the production batch is qualified and does not have edge chipping defects. The method of the present invention uses small specimens for testing and prediction, without the need for whole board testing, thus saving materials.

[0059] 3. The equipment used for edge chipping detection of boards by the method of the present invention is the conventional production and processing equipment of the artificial board manufacturer (board CNC machining center, cutting machine), which does not require the use of special equipment and saves the production cost of the artificial board manufacturer.

[0060] The invention provides a method for predicting the edge chipping quality of engineered wood products; fills a gap in engineered wood product quality testing methods; provides a basis for product sales and delivery; avoids customer complaints caused by quality problems arising from the processing of defective engineered wood products into customized home furnishing products; and avoids economic disputes caused by defects in engineered wood products. Attached image description:

[0061] Figure 1 This is a surface structure diagram of the milled groove specimen from Example 1 after milling.

[0062] Figure 2 After milling Figure 1 Enlarged view of a portion of the specimen;

[0063] Figure 3 This is a schematic diagram of the structure of the milled groove, the finishing layer, and the serrated defects after milling. Detailed implementation method:

[0064] The present invention will be further described below with reference to specific embodiments, and the advantages and features of the present invention will become clearer as a result. However, these embodiments are merely exemplary and do not constitute any limitation on the scope of the present invention. Those skilled in the art should understand that modifications or substitutions can be made to the details and form of the technical solutions of the present invention without departing from the spirit and scope of the present invention, but all such modifications and substitutions fall within the protection scope of the present invention.

[0065] In this specific embodiment of the invention, an impregnated paper-faced particleboard with a thickness of 18mm is used as an example for illustration. Impregnated paper-faced particleboard, impregnated paper-faced oriented strand board, impregnated paper-faced fiberboard, impregnated paper-faced blockboard, and impregnated paper-faced plywood of other thicknesses are also applicable to this invention.

[0066] Example 1

[0067] 1. Preparation of milled groove specimens

[0068] One sheet of board is randomly selected from all products produced by the board manufacturer according to the customer's order requirements, based on the same production shift, the same specification of base material, the same color, and the same batch of finish for initial inspection. This sheet is then used as the board to be predicted. It is then cut into multiple test pieces with dimensions of 50cm×50cm×board thickness to prepare multiple milled groove (milling) test pieces for later use.

[0069] The surface of the material to be tested should be free of scratches, indentations, abrasions, bubbles, and other appearance defects. The dimensions of the milled (milled) specimens, besides (50cm × 50cm × plate thickness), can also be based on this invention. Other dimensions include (40-100)cm × (40-100)cm × plate thickness, preferably (50-60)cm × (50-60)cm × plate thickness.

[0070] The milled groove specimens of this invention are selected with an area greater than 1600 cm². 2 The dimensions of the milled groove specimens only need to ensure that the cutting path is ≥30m and ≤40m. That is, the milling process of the present invention is performed on the board produced by the artificial board manufacturer to ensure that the milling path is ≥30m and ≤40m; alternatively, the artificial board can be cut into milled groove specimens of the corresponding size, so that the milling path is ≥30m and ≤40m.

[0071] 2. Pretreatment of milled groove specimens

[0072] The prepared milled groove specimens were placed in an environment with a temperature of (20±2)℃ and a relative humidity of (65±5)% to equilibrate until the mass was constant. That is, the weight of the milled groove specimens was weighed once every 24 hours. The difference between two adjacent weighing results should not exceed 0.1% of the mass of the specimen at the last weighing. Pretreated milled groove specimens were obtained for later use.

[0073] Pretreatment, also known as equilibration, is used to prevent the effects of sample storage or different locations.

[0074] 3: Milling groove treatment

[0075] Test equipment: CNC machining center for engineered wood products or other equipment capable of performing milling operations, milling cutter (2mm cutting diameter)

[0076] Test method: Milling cutter speed 15000 r / min, feed rate 5-6 m / min, milling groove depth 0.5-1.0 mm. Use a milling cutter to make a "U" shaped groove on the plate (or specimen) to be tested, with a groove length of about 30 meters.

[0077] 3-1): Place the pre-treated milled groove specimen horizontally on the milling machine and fix it on the horizontal platform of the milling machine;

[0078] In addition to milling on milling machines, milling can also be performed on CNC machining centers, engraving machines, cutting machines, and other existing equipment known in the field capable of milling plates.

[0079] Milling is a process of creating grooves from the top surface downwards, with a groove depth of 0.5-1.5mm. The height of the top surface should be the machine tool height plus the plate thickness. Therefore, during the test, the plate thickness should be accurately measured with calipers first to avoid affecting the milling depth of the subsequent milling process due to measurement deviations in the plate thickness.

[0080] 3-2): Select the carbide cutter for slot milling (or milling) method and slot milling (or milling) parameter settings.

[0081] First: Mount the routing cutter (2mm cutting diameter) on the milling machine and align the cutting edge of the routing cutter with the milling groove test piece;

[0082] In this embodiment, an industrial-grade cutting cutter is selected, model: T201 two-flute straight cutter, with parameters of shank diameter 1 / 2”, cutting diameter 2mm, and cutting length 6mm.

[0083] In addition to using a 2mm cutting diameter cutting cutter, any other cutting cutter with a cutting diameter of 1-3mm is suitable for use in the method of this invention.

[0084] In the actual cutting process of the engineered wood panels tested by the method of this invention, the main concern is the impact of the saw on the surface finish of the panel during sawing. When processing panels using tools such as table saws and panel saws, the kerf width is typically between 1mm and 3mm. Therefore, the milling cutter diameter should not be less than 1mm. Furthermore, through repeated experiments, this invention found that milling cutters with a diameter greater than 3mm have little impact on the edge chipping test results. However, a larger diameter would require larger test materials. Therefore, a milling cutter diameter of 1-3mm is selected.

[0085] Next: Set and adjust the milling cutter speed on the CNC machining center (i.e., CNC machine tool, CNC milling machine) to 15000 r / min (usually below 20000 r / min, preferably 10000-20000 r / min); the feed rate to 5.5 m / min (usually below 8 m / min, preferably 5-6 m / min); the width of the groove cut by the milling cutter to 2 mm (usually 1-3 mm); and the groove depth to 0.75 mm (usually 0.5-1.0 mm, preferably...). 0.75-1mm); and design the milling route for the milling process: perform "return" milling on the surface of the milled groove specimen, that is, select the milling process to form a "return" milled groove, and the length of the "return" milled groove path is 30m (usually at least 30m, preferably 30-40m); the width of the plate finishing layer of the "return" milled groove is 2mm (usually at least 1.5mm, preferably 1.5-2.5mm); the number of "return" milled grooves is 38 turns (usually 25-50 turns, preferably 35-40 turns).

[0086] 3-3) Start the CNC machining center (commonly known as a CNC milling machine). First, move the carbide cutter to the edge of the milling groove test piece, with the cutter perpendicular to the plane of the test piece and the cutting edge 2mm (usually at least 2mm) away from the edge of the test piece. Then, according to the plate size and design, input the "return" shaped milling path into the CNC machining center, ensuring the milling path length is 30m (usually at least 30m, preferably 30-40m); the finishing layer width of the "return" shaped milling groove test piece is 2mm (usually at least 1.5mm, preferably 1.5-2.5mm); the number of "return" shaped milling grooves is 38 turns (usually 25-50 turns, preferably 35-40 turns); then set the milling cutter speed, feed rate, milling groove depth, and other parameters; finally, run the machine.

[0087] The specimen after milling (cutting) with a router bit is as follows: Figure 1 , 2 As shown. Figure 2 After milling Figure 1 A magnified view of a section of the specimen, where the arrow points to a serrated breakage.

[0088] 4. Edge chipping detection

[0089] Edge chipping (dents) refers to the jagged defects on the surface of decorative panels caused during the edge-trimming process. This method is used to predict whether edge chipping will occur on panels after milling the surface of a small sample of the panel to detect jagged defects.

[0090] A schematic diagram of the serrated defect structure of this method is shown below. Figure 3 As shown, Figure 3 In the figure, h represents the height of the serrated defect. If the maximum height (h) of the serrated defect is ≥0.5mm, it indicates that the board will have a chipping problem. If the maximum height of the serrated defect is less than 0.5mm, it indicates that the board will not have a chipping problem.

[0091] After removing the milled specimen from the CNC milling machine, observe the serrated damage (or serrated defects) on the milled groove finish layer. If serrated defects are present, use a steel ruler (accuracy 0.1mm) to measure the maximum height (h, i.e. the height of the serrated tooth, which is the maximum length perpendicular to the groove direction from the junction of the groove and the finish layer to the outer edge of the serrated defect). If the maximum height (maximum serrated height) exceeds 0.5mm, the plate is considered unqualified.

[0092] Measurements showed that the maximum heights of the two serrated breaks in this embodiment were 0.4 mm and 0.3 mm, respectively, neither exceeding 0.5 mm, indicating that edge chipping was not expected.

[0093] When this batch of boards was used to manufacture bookcase shelf panels, no chipping occurred during the sawing process. Furthermore, no damage occurred around the holes in the manufactured shelf panels during drilling. Therefore, the predicted results of the method of this invention are consistent with the actual results.

[0094] Example 2: Screening of Milled Groove Finish Width

[0095] Except for step 3), where the width of the decorative layer of the plate with the "U"-shaped milled groove is 1.0mm, 1.2mm, and 1.5mm respectively, the rest is the same as in Example 1.

[0096] When the width of the milled groove finishing layer was 1.0 mm, the finishing layer of the specimen had multiple defects, including 5 sawtooth defects with a maximum height of more than 0.5 mm, and 2 defects that penetrated the finishing layer between the two milled grooves (the defects were 3 mm and 4.5 mm wide, respectively). This indicates that the predicted edge chipping phenomenon did not match the actual situation.

[0097] When the width of the finishing layer was 1.2mm, the finishing layer of the specimen had multiple defects, including 5 sawtooth defects with a maximum height of more than 0.5mm, and 1 defect that penetrated the finishing layer between two milled grooves (the defect width was 3.5mm). This means that the predicted edge chipping phenomenon did not match the actual situation.

[0098] When the width of the finishing layer is 1.5mm, there are two serrated breaks in the finishing layer of the specimen, with a maximum height of 0.3mm and none exceeding 0.5mm. This indicates that the edge chipping phenomenon was not expected, and the prediction was consistent with the actual situation.

[0099] After repeated testing (through hundreds or thousands of different products), the inventors found that the maximum height of the serrated damage on different boards does not exceed 1.5mm. Therefore, the width of the board surface layer with the milled groove is controlled to be at least 1.5mm.

[0100] Example 3

[0101] In Example 1, the material to be predicted was milled. Except for step 3), the width of the decorative layer of the material with the "U" shaped milled groove was 2.2 mm and 2.5 mm respectively. The rest was the same as in Example 1.

[0102] When the width of the veneer layer is 2.2mm, there are 3 serrated defects on the veneer layer of the board. After measurement, the maximum height of the 3 serrated defects is 0.2mm, 0.3mm and 0.2mm respectively, none of which exceed 0.5mm. Therefore, it is predicted that there will be no edge chipping, and the prediction is consistent with the actual situation.

[0103] When the remaining width of the decorative layer is 2.5mm, 3 serrated damages occur on the decorative layer of the plate. After measurement, the maximum heights of the 3 serrated damages are 0.2mm, 0.2mm, and 0.2mm respectively, none of which exceeds 0.5mm, that is, it is predicted that no edge chipping will occur, and the prediction is consistent with the actual situation.

[0104] After repeated tests by the inventors, in the milling treatment process of the present invention, the remaining width of the decorative layer of the plate with the "loop"-shaped milled groove is greater than 1.5mm, preferably 1.5-2.5mm.

[0105] Example 4

[0106] The rest is the same as Example 1, except that the milling depths in step 3) of the milling treatment process are 0.2mm, 0.4mm, 0.5mm, 1.0mm, 1.5mm, and 2.5mm respectively.

[0107] When the milling depth is 0.2mm, the decorative layer is not worn through, and the base material is not exposed. Multiple continuous serrated or block-shaped damages appear on the decorative layer near the groove, among which the maximum heights of 26 positions exceed 0.5mm, that is, it is predicted that edge chipping will occur, and the prediction is inconsistent with the actual situation;

[0108] When the milling depth is 0.4mm, the decorative layer is not worn through, and the base material is not exposed. Multiple serrated damages appear on the decorative layer near the groove, among which the maximum heights of 5 positions exceed 0.5mm, that is, it is predicted that edge chipping will occur, and the prediction is inconsistent with the actual situation;

[0109] When the milling depth is 0.5mm, there are 4 serrated damages on the decorative layer, with maximum heights of 0.4mm, 0.4mm, 0.3mm and 0.4mm respectively, none of which exceeds 0.5mm, that is, it is predicted that no edge chipping will occur, and the prediction is consistent with the actual situation;

[0110] When the milling depth is 1.0mm, there are 4 serrated damages on the decorative layer, with maximum heights of 0.3mm, 0.3mm, 0.3mm and 0.2mm respectively, none of which exceeds 0.5mm, that is, it is predicted that no edge chipping will occur, and the prediction is consistent with the actual situation;

[0111] When the milling depth is 1.5mm, there are 3 serrated damages on the decorative layer, with maximum heights of 0.3mm, 0.3mm and 0.2mm respectively, none of which exceeds 0.5mm, that is, it is predicted that no edge chipping will occur, and the prediction is consistent with the actual situation;

[0112] When the milling depth is 2.5mm, there are 2 serrated damages on the decorative layer, with maximum heights of 0.2mm and 0.2mm respectively, none of which exceeds 0.5mm, that is, it is predicted that no edge chipping will occur, and the prediction is consistent with the actual situation.

[0113] For practicality in production testing, the milling groove depth of this invention is selected to be greater than 0.5 mm, preferably 0.5-1.0 mm.

[0114] Example 5

[0115] The milling process was performed on the material to be predicted selected in Example 1. Except for step 3), where the milling path was 40m, the process was the same as in Example 1.

[0116] When the milling path is 40m, there are 3 sawtooth-shaped damages in the finishing layer, with maximum heights of 0.4mm, 0.3mm and 0.2mm respectively, none of which exceed 0.5mm, which means that it was predicted that edge chipping would not occur, and the prediction was consistent with the actual situation.

[0117] The invention also tested milling paths of 50m and 60m. The tests revealed serrated damage in both cases, with the maximum height between 0.2mm and 0.4mm. The test plate with a milling path of 50m had 4 serrated damages, and the test plate with a milling path of 60m had 6 serrated damages. Apart from the slightly larger number, the maximum height of the damages was not significantly different. In order to accurately predict edge chipping and save testing time, the inventors chose a milling path of at least 30m, preferably 30-40m.

[0118] Example 6

[0119] Except for step 3), where the feed speed is controlled at 6m / min, 7m / min, and 8m / min during the milling process, the rest is the same as in Example 1.

[0120] When the feed rate is 6m / min, there are 4 serrated breaks in the surface layer, with maximum heights of 0.3mm, 0.3mm, 0.4mm and 0.4mm respectively, none of which exceed 0.5mm. This means that it was predicted that edge chipping would not occur, and the prediction was consistent with the actual situation.

[0121] When the feed rate is 7m / min, there are 5 serrated breaks in the finish layer, with maximum heights of 0.4mm, 0.4mm, 0.4mm, 0.4mm and 0.3mm respectively, none of which exceed 0.5mm, which means that the prediction that edge chipping will not occur is consistent with the actual situation.

[0122] When the feed rate is 8m / min, multiple serrated breaks appear in the surface layer near the groove, with three breaks exceeding 0.5mm in maximum height and one through-break. This indicates that edge chipping was predicted, but the prediction did not match the actual situation.

[0123] In order to accurately predict edge breakage while saving testing time, the inventors chose a feed rate of less than 8 m / min, preferably 5-7 m / min, and more preferably 5-6 m / min.

[0124] Example 7

[0125] Except for step 3), where the milling cutter speed is controlled at 9000 r / min, 17000 r / min, and 25000 r / min respectively during the milling process, the rest is the same as in Example 1.

[0126] When the milling cutter speed was 9000 r / min, there were 3 serrated breaks in the surface layer, with a maximum height of 0.3 mm. None of them exceeded 0.5 mm, so it was predicted that edge chipping would not occur, and the prediction was consistent with the actual situation.

[0127] When the milling cutter speed is 17000 r / min, there are 4 serrated breaks in the surface layer, with maximum heights of 0.3 mm, 0.4 mm, 0.4 mm and 0.4 mm respectively, none of which exceed 0.5 mm. This means that it was predicted that no edge chipping would occur, and the prediction was consistent with the actual situation.

[0128] When the milling cutter speed is 25000 r / min, multiple serrated breaks appear in the surface layer near the groove, including two serrated breaks with a maximum height exceeding 0.5 mm and two through breaks. This indicates that edge chipping was predicted, but the prediction did not match the actual situation.

[0129] The method of this invention tested the milling cutter speed when it exceeded 20,000 r / min. Due to the excessive speed, the milling cutter vibrated, resulting in increased serrated damage and height. In order to improve the detection efficiency and accuracy of the detection results, the inventors selected a milling cutter speed of less than 20,000 r / min, preferably 10,000-20,000 r / min.

[0130] Experimental Example 1

[0131] During the board inspection process, three boards are randomly selected from the same production shift, using the same specification of base material, and with the same color and finish. From each board, one 30cm×40cm×thickness board is made. One board is used for initial inspection, and the other two are used for re-inspection.

[0132] The pretreatment and milling of the sheet metal were carried out according to the method and steps of Example 1, and the process control conditions were the same as those in Example 1.

[0133] If the initial inspection sample is qualified, it is directly judged as qualified; if the initial inspection sample is unqualified, two re-inspections are initiated. If both re-inspections are qualified, it is judged as qualified; otherwise, it is judged as unqualified.

[0134] Experimental Example 2

[0135] Three sheets of board were randomly selected from the same batch of impregnated paper-faced particleboard used in Example 1 and used to make furniture (such as bookcase shelf panels, wardrobe side panels, etc.). No chipping occurred during the sawing process; and no damage occurred around the holes when drilling the boards. This batch of products is qualified.

[0136] No curling, rough edges, breakage, or peeling occurred during the long-term use of the finished furniture (within 2 years).

[0137] This invention provides an innovative surface performance testing method for impregnated paper-faced particleboard, effectively predicting whether edge chipping will occur during use. This method is included as an anti-chipping test method in the group standard project "High-Performance Impregnated Paper-Faceted Particleboard" initiated by the China Forest Products Industry Association. The chipping test method in this standard has been recognized by forestry industry experts, researchers, and enterprise representatives, affirming the testing principle, method, and effectiveness of this invention. This invention is included in the group standard project "High-Performance Impregnated Paper-Faceted Particleboard" initiated by the China Forest Products Industry Association, and this test method also provides a basis for the revision of national standards GB / T 15102 and GB / T 34722.

[0138] The above embodiments of the present invention are merely exemplary and do not constitute any limitation on the scope of the present invention. Those skilled in the art should understand that modifications or substitutions can be made to the details and form of the technical solutions of the present invention without departing from the spirit and scope thereof, but all such modifications and substitutions fall within the protection scope of the present invention.

Claims

1. A method for predicting whether chipping will occur in engineered wood panels, characterized in that, Includes the following steps: 1) Randomly select one board from the artificial boards to be predicted in the same shift, with the same specification of substrate, and the same color and finish in the same batch of artificial board production process, and use it as the pre-test board. 2) On one side of the decorative layer of the pre-test specimen board, a "return" shaped groove is made using a routing cutter; wherein, the length of the "return" shaped groove is at least 30m; the rotational speed of the routing cutter is controlled at 10000-20000 r / min; the feed rate is 5-6 m / min; the groove depth is 0.5-1.0mm; and the width of the decorative layer of the board remaining after the groove is controlled at at least 1.5mm. 3) Observe the milled groove left after the "U"-shaped milling process to see if there are serrated defects on the side of the decorative layer of the milled groove; if there are no serrated defects, the engineered wood panel to be predicted is qualified and there is no edge chipping problem; if there are serrated defects, measure the maximum height of the serrated defects; where: 3A) If the maximum height of the serrated defects on the side of the milled groove finishing layer is ≥0.5mm, it is predicted that the batch of artificial boards is unqualified and prone to edge chipping. 3B) If the maximum height of the serrated defects on the side of the milled groove finishing layer is < 0.5mm, then the batch of engineered wood panels is predicted to be qualified and there is no edge chipping problem.

2. The method as described in claim 1, characterized in that, The cutting diameter of the milling cutter mentioned in step 2) is 1-3mm.

3. The method as described in claim 1, characterized in that, The cutting diameter of the milling cutter mentioned in step 2) is 2mm.

4. The method as described in claim 1 or 2, characterized in that, In step 2), during the "return" shaped milling process, the rotational speed of the milling cutter is controlled at 15000 r / min; the feed rate is 5.5 m / min; and the milling depth is 0.75-1.0 mm.

5. The method as described in claim 1 or 2, characterized in that, The artificial board material is one or more of the following: impregnated paper-faced particleboard, impregnated paper-faced oriented strand board, impregnated paper-faced fiberboard, impregnated paper-faced blockboard, and impregnated paper-faced plywood.

6. A method for predicting whether chipping will occur in engineered wood panels, characterized in that, Includes the following steps: A) Randomly select one board from the same shift, same specification of substrate, same color, and same batch of finishes of the artificial board to be predicted, as the pre-test board. B) The randomly selected pre-test specimens are cut to form a surface area of ​​800-10000 cm². 2 Milled groove test pieces; C) On one side of the decorative layer of the milled specimen, a "return" shaped milling groove is made using a routing cutter, wherein the milling path of the "return" shaped milling groove, i.e., the length of the milled groove, is at least 30m; the rotational speed of the routing cutter is controlled at 10000-20000 r / min; the feed rate is 5-6 m / min; the depth of the milled groove is 0.5-1.0mm; and the width of the decorative layer of the plate after milling is controlled to be at least 1.5mm. D) Observe the milled grooves left after milling to check for serrated defects on the sides of the decorative layer. If there are no serrated defects, the engineered wood panel is expected to be qualified and there will be no edge chipping. If there are serrated defects, measure the maximum height of the serrated defects. D1) If the maximum height of the serrated defects on the side of the finish layer of the milled groove is ≥0.5mm, it is predicted that the batch of artificial board is unqualified and prone to edge chipping. D2) If the maximum height of the serrated defects on the side of the milled groove finishing layer is < 0.5mm, then the batch of artificial boards is predicted to be qualified and there is no edge chipping problem.