Ultra-flexible robotic cable

By adopting a layered structure and independently developed modifiers, the durability and flame retardancy issues of traditional robot cables under complex dynamic working conditions have been solved, resulting in highly flexible and reliable robot cables suitable for demanding scenarios such as industrial and medical robots.

CN121034721BActive Publication Date: 2026-01-27SICHUAN XINRONG ELECTRIC CABLE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202511538273.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2025-10-27
Publication Date
2026-01-27
Estimated Expiration
2045-10-27

AI Technical Summary

Technical Problem

Traditional robot cables lack durability under complex dynamic working conditions, the conductors are prone to breakage, the sheaths are prone to aging, and the flame retardant properties are insufficient, posing safety hazards and failing to meet the needs of high-end robot systems.

Method used

The cable adopts a symmetrical layered structure. The core is composed of copper wire and polyester fiber, the insulation layer is ethylene-tetrafluoroethylene copolymer, the shielding layer is aluminum foil-tinned copper wire, and the sheath layer is composed of thermoplastic polyurethane elastomer and self-developed modifier. The modifier is prepared by a three-step nucleophilic substitution reaction and contains PN and Si-N bonds to improve flame retardancy and flexibility.

Benefits of technology

It significantly improves the fatigue resistance of cables under repeated bending and twisting, extends service life, enhances flexibility and flame retardancy, reduces signal interference, and improves the reliability and accuracy of robot systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The application discloses a kind of super-high flexible robot cables, belong to robot cable technical field.Symmetrical layered structure is used, from inside to outside in turn: cable core, insulating layer, shielding layer and sheath layer.Cable core uses layered structure of stranding, significantly improve the fatigue resistance of cable, prolongs service life;Insulating layer uses ethylene-tetrafluoroethylene copolymer, with good flexibility, and can adapt to complex working environment;Shielding layer uses aluminum foil-tin coated copper wire, provides good electromagnetic shielding effect, reduces signal interference, improves the operation accuracy and reliability of robot system;Sheath layer uses thermoplastic polyurethane elastomer as matrix, and introduces the modifier of independent research and development, substantially improves the flame retardance and flexibility of cable;Therefore, the cable prepared by the application has high flexibility and flame retardance, and can be widely used in industrial robots, medical manipulators, service robots and other high-demand scenarios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of robot cable technology, specifically, it relates to an ultra-high flexibility robot cable. Background Technology

[0002] As core execution devices in fields such as industrial manufacturing, medical diagnosis, service interaction, and aerospace, robots need to frequently perform complex movements such as bending, twisting, and swinging at their joints. Cables, as key carriers for power transmission and signal interaction, need to accompany these dynamic processes for a long time. The quality of their performance directly determines the reliability, motion accuracy, and service life of the robot system.

[0003] With the rapid development of industrial automation, medical robotic arms, and service robots, the requirements for robot cables are becoming increasingly stringent. Traditional robot cables often exhibit insufficient durability and premature cracking of the outer sheath when dealing with complex and ever-changing dynamic working conditions such as bending, twisting, and stretching, which seriously restricts the further improvement of high-end robot performance and the expansion of application scenarios.

[0004] From a material selection perspective, traditional robot cables mostly use ordinary annealed copper conductors. While these offer some conductivity, repeated bending can cause stress concentration and micro-cracks within the conductor, which expand with each bend, eventually leading to conductor breakage. Cable sheaths are typically made of polyvinyl chloride (PVC) or ordinary nitrile rubber. While these materials are cheaper, they lack flexibility, easily hardening and cracking at low temperatures and aging and deforming at high temperatures or in oily environments, ultimately losing their insulation function. For example, in automotive welding robots, the robot's wrist performs thousands of bending movements daily. Traditional cables typically experience conductor breakage or sheath damage after 3-6 months of use, requiring frequent downtime for replacements, increasing maintenance costs, and potentially causing production interruptions and economic losses due to unexpected malfunctions. Furthermore, most sheaths lack sufficient flame retardant properties, or their flexibility is severely compromised after adding flame retardants. If ignited by an electrical fault or external fire source, the cable itself could become a conduit for fire spread, posing a significant safety hazard. Therefore, it is urgent to address these issues to meet the higher demands of the robot cable technology field. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of the prior art and provide an ultra-high flexibility robot cable.

[0006] The objective of this invention can be achieved through the following technical solutions:

[0007] A highly flexible robot cable adopts a symmetrical layered structure, consisting of, from the inside out: cable core, insulation layer, shielding layer, and sheath layer.

[0008] As a further technical solution, the cable core includes copper wire and polyester fiber.

[0009] As a further technical solution, the material of the insulating layer is an ethylene-tetrafluoroethylene copolymer.

[0010] As a further technical solution, the shielding layer is made of aluminum foil and tin-plated copper wire.

[0011] As a further technical solution, the material of the sheath layer includes the following raw materials in parts by weight: 72-90 parts thermoplastic polyurethane elastomer, 15-20 parts silica, 6-12 parts modifier, and 1-2 parts antioxidant.

[0012] As a further technical solution, the antioxidant is one of antioxidant 3114, antioxidant 1010 and antioxidant 1098.

[0013] As a further technical solution, the modifier is prepared through the following steps:

[0014] A1. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas is introduced as a protective gas. Dichloromethylphosphine and toluene are added in sequence, and stirring is started. After stirring for 10-20 minutes, stearyl alcohol and triethylamine are added in sequence. After the addition is complete, the mixture is heated to 70-75°C in a water bath and reacted at this temperature for 5-6 hours. After the reaction is complete, the product A is obtained through post-processing.

[0015] A2. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas is introduced as a protective gas. Piperazine and toluene are mixed and added to the flask. Stirring is started and after stirring for 10-20 minutes, product A and triethylamine are added in sequence. After the addition is complete, the mixture is heated to 60-65°C in a water bath and reacted at a constant temperature for 7-8 hours. After the reaction is complete, the product B is obtained through post-processing.

[0016] A3. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas is introduced as a protective gas. 1,7-Dichlorooctamethyltetrasiloxane is mixed with toluene and added to the flask. Stirring is started, and product B and triethylamine are added. After the addition is complete, the mixture is heated to 70-80°C in a water bath and reacted at a constant temperature for 8-10 hours. After the reaction is complete, the modifier is obtained through post-treatment.

[0017] As a further technical solution, the ratio of dichloromethylphosphine, toluene, stearyl alcohol and triethylamine in step A1 is 14.2-15.3g:100mL:27.0g:10.1g.

[0018] As a further technical solution, the ratio of piperazine, toluene, product A and triethylamine in step A2 is 9.3-9.9g:120mL:36.6g:10.1g.

[0019] As a further technical solution, the ratio of the amounts of 1,7-dichlorooctamethyltetrasiloxane, toluene, product B and triethylamine in step A3 is 35.1g:200mL:85.5-86.7g:20.2g.

[0020] The reaction formula for preparing the modifier in this invention is as follows:

[0021]

[0022] As can be seen from the above reaction formula, the modifier is prepared through a three-step nucleophilic substitution reaction. In the process of preparing the modifier, it is necessary to strictly control the amount of reactants in each step to reduce the occurrence of side reactions in order to prepare a modifier with the above structure. In step A1, the molar ratio of dichloromethylphosphine to stearyl alcohol should be close to 1:1, and the former should be in excess. In step A2, the molar ratio of piperazine to product A should be close to 1:1, and the former should be in excess. In step A3, the molar ratio of 1,7-dichlorooctamethyltetrasiloxane to product B should be close to 1:2, and the latter should be in excess.

[0023] As can be seen from the above reaction formula, the modifier simultaneously possesses flame-retardant and flexible components. PN and Si-N bonds constitute the flame-retardant component; all three elements exhibit flame-retardant properties and work synergistically to significantly improve the flame-retardant performance of the sheath. Furthermore, silicon-oxygen bonds and long-chain alkyl groups constitute the flexible component. The silicon-oxygen bonds are long, have large bond angles, and extremely low rotation barriers, promoting chain segment movement and improving the sheath's flexibility. The long-chain alkyl groups have numerous rotatable single bonds and a high number of conformations, resulting in excellent flexibility. Similarly, these two components work synergistically to significantly improve the sheath's flexibility, thereby toughening the sheath.

[0024] The beneficial effects of this invention are:

[0025] 1. The cable core of this invention adopts a layered stranded structure, which significantly improves the fatigue resistance of the cable under dynamic working conditions such as repeated bending and twisting, effectively avoids the problem of micro-cracks and fractures caused by stress concentration in the conductor, and extends the service life.

[0026] 2. The insulation layer is made of ethylene-tetrafluoroethylene copolymer, which has good flexibility, heat resistance and corrosion resistance, and can adapt to complex working environments;

[0027] 3. The shielding layer uses aluminum foil and tin-plated copper wire, which provides good electromagnetic shielding, reduces signal interference, and improves the operating accuracy and reliability of the robot system;

[0028] 4. The sheath layer uses thermoplastic polyurethane elastomer as the matrix and introduces a self-developed modifier, which greatly improves the flame retardancy and flexibility of the cable.

[0029] Therefore, the cable produced by this invention has both high flexibility and flame retardancy, and can be widely used in high-requirement scenarios such as industrial robots, medical robotic arms, and service robots. Detailed Implementation

[0030] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0031] Example 1

[0032] Preparation of modifiers:

[0033] A1. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas was introduced as a protective gas. 14.2 g of dichloromethylphosphine and 100 mL of toluene were added sequentially. Stirring was started and after stirring for 10 min, 27.0 g of stearyl alcohol and 10.1 g of triethylamine were added sequentially. After the addition was completed, the mixture was heated to 70 °C in a water bath and reacted at this temperature for 5 h. After the reaction was completed, the reaction solution was cooled to room temperature, the generated triethylamine hydrochloride was removed by filtration, the filter cake was washed with toluene, and the product A was obtained by vacuum distillation.

[0034] A2. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas was introduced as a protective gas. 9.3 g of piperazine and 120 mL of toluene were mixed and added to the flask. Stirring was started and after stirring for 10 min, 36.6 g of product A and 10.1 g of triethylamine were added sequentially. After the addition was completed, the mixture was heated to 60 °C in a water bath and reacted at a constant temperature for 7 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filtrate was washed sequentially with sodium bicarbonate and saturated brine. The organic phase was dried with anhydrous magnesium sulfate, filtered, and toluene was removed by vacuum distillation. The product B was then dried under vacuum.

[0035] A3. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas was introduced as a protective gas. 35.1 g of 1,7-dichlorooctamethyltetrasiloxane was mixed with 200 mL of toluene and added to the flask. Stirring was started, and 85.5 g of product B and 20.2 g of triethylamine were added. After the addition was complete, the mixture was heated to 70 °C in a water bath and reacted at this temperature for 8 h. After the reaction was complete, the mixture was cooled to room temperature, filtered, and the filtrate was washed with anhydrous ethanol. The organic phase was dried with anhydrous sodium sulfate, filtered, and then distilled under reduced pressure. The residue was purified by silica gel column chromatography (using n-hexane and toluene as the developing solvent, with a volume ratio of 3:1) to obtain the modifier.

[0036] An ultra-flexible robot cable is prepared through the following steps:

[0037] B1. The oxygen-free copper rod is drawn into ultra-fine copper wire with a diameter of 0.08mm through multiple drawing dies, and then subjected to soft annealing to eliminate internal stress. After the three copper wires are twisted to the left by a stranding machine, four copper wires are evenly wound and twisted to the right. Polyester fiber is added at the same time, and finally hot air is used for shaping to obtain the cable core.

[0038] B2. The ethylene-tetrafluoroethylene copolymer is melted in an extruder and uniformly extruded onto the surface of the conductor, then cooled and shaped in a water bath to form an insulating layer.

[0039] B3. First, use a wrapping machine to longitudinally wrap a layer of aluminum foil on the insulation layer, and then use a braiding machine to weave 0.05mm tin-plated copper wire into a mesh and wrap it over the insulation layer to form a shielding layer.

[0040] B4. Finally, 72 parts of thermoplastic polyurethane elastomer, 15 parts of silica, 6 parts of modifier and 1 part of antioxidant 3114 are melted in an extruder and uniformly extruded onto the surface of the shielding layer to form a sheath layer. The extruded cable is immediately placed into a cooling water tank for cooling and shaping to obtain an ultra-high flexibility robot cable.

[0041] Example 2

[0042] Preparation of modifiers:

[0043] A1. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas was introduced as a protective gas. 15.3 g of dichloromethylphosphine and 100 mL of toluene were added sequentially. Stirring was started and after 20 min, 27.0 g of stearyl alcohol and 10.1 g of triethylamine were added sequentially. After the addition was completed, the mixture was heated to 75 °C in a water bath and reacted at this temperature for 6 h. After the reaction was completed, the reaction solution was cooled to room temperature, the generated triethylamine hydrochloride was removed by filtration, the filter cake was washed with toluene, and the product A was obtained by vacuum distillation.

[0044] A2. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas was introduced as a protective gas. 9.9 g of piperazine and 120 mL of toluene were mixed and added to the flask. Stirring was started and carried out for 20 min. Then, 36.6 g of product A and 10.1 g of triethylamine were added sequentially. After the addition was completed, the mixture was heated to 65 °C in a water bath and reacted at a constant temperature for 8 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, and the filtrate was washed sequentially with sodium bicarbonate and saturated brine. The organic phase was dried with anhydrous magnesium sulfate, filtered, and toluene was removed by vacuum distillation. The product B was then dried under vacuum.

[0045] A3. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas was introduced as a protective gas. 35.1 g of 1,7-dichlorooctamethyltetrasiloxane was mixed with 200 mL of toluene and added to the flask. Stirring was started, and 86.7 g of product B and 20.2 g of triethylamine were added. After the addition was complete, the mixture was heated to 80 °C in a water bath and reacted at this temperature for 10 h. After the reaction was complete, the mixture was cooled to room temperature, filtered, and the filtrate was washed with anhydrous ethanol. The organic phase was dried with anhydrous sodium sulfate, filtered, and then distilled under reduced pressure. The residue was purified by silica gel column chromatography (using n-hexane and toluene as the developing solvent, with a volume ratio of 3:1) to obtain the modifier.

[0046] An ultra-flexible robot cable is prepared through the following steps:

[0047] B1. The oxygen-free copper rod is drawn into ultra-fine copper wire with a diameter of 0.08mm through multiple drawing dies, and then subjected to soft annealing to eliminate internal stress. After the three copper wires are twisted to the left by a stranding machine, four copper wires are evenly wound and twisted to the right. Polyester fiber is added at the same time, and finally hot air is used for shaping to obtain the cable core.

[0048] B2. The ethylene-tetrafluoroethylene copolymer is melted in an extruder and uniformly extruded onto the surface of the conductor, then cooled and shaped in a water bath to form an insulating layer.

[0049] B3. First, use a wrapping machine to longitudinally wrap a layer of aluminum foil on the insulation layer, and then use a braiding machine to weave 0.05mm tin-plated copper wire into a mesh and wrap it over the insulation layer to form a shielding layer.

[0050] B4. Finally, 81 parts of thermoplastic polyurethane elastomer, 17.5 parts of silica, 9 parts of modifier and 1.5 parts of antioxidant 1010 are melted in an extruder and uniformly extruded onto the surface of the shielding layer to form a sheath layer. The extruded cable is immediately placed into a cooling water tank for cooling and shaping to obtain an ultra-high flexibility robot cable.

[0051] Example 3

[0052] The only difference between this embodiment and Embodiment 2 is that, in this embodiment, an ultra-high flexibility robot cable is prepared through the following steps:

[0053] B1. The oxygen-free copper rod is drawn into ultra-fine copper wire with a diameter of 0.08mm through multiple drawing dies, and then subjected to soft annealing to eliminate internal stress. After the three copper wires are twisted to the left by a stranding machine, four copper wires are evenly wound and twisted to the right. Polyester fiber is added at the same time, and finally hot air is used for shaping to obtain the cable core.

[0054] B2. The ethylene-tetrafluoroethylene copolymer is melted in an extruder and uniformly extruded onto the surface of the conductor, then cooled and shaped in a water bath to form an insulating layer.

[0055] B3. First, use a wrapping machine to longitudinally wrap a layer of aluminum foil on the insulation layer, and then use a braiding machine to weave 0.05mm tin-plated copper wire into a mesh and wrap it over the insulation layer to form a shielding layer.

[0056] B4. Finally, 90 parts of thermoplastic polyurethane elastomer, 20 parts of silica, 12 parts of modifier and 2 parts of antioxidant 1098 are melted in an extruder and uniformly extruded onto the surface of the shielding layer to form a sheath layer. The extruded cable is immediately placed into a cooling water tank for cooling and shaping to obtain an ultra-high flexibility robot cable.

[0057] Comparative Example 1

[0058] The only difference between this comparative example and Example 3 is that in this comparative example, an equal amount of stearyl alcohol (flexibilizer) was used to replace the modifier to obtain the cable.

[0059] Comparative Example 2

[0060] The only difference between this comparative example and Example 3 is that in this comparative example, an equal amount of triphenyl phosphate (flame retardant) was used to replace the modifier to obtain the cable.

[0061] The sheath layer materials from Examples 1, 2, and 3, and Comparative Examples 1 and 2 were extruded separately and subjected to the following performance tests:

[0062] The oxygen index was determined according to GB / T 2406.2-2009 standard;

[0063] The elongation at break and repeated bending life were determined according to GB / T 2951.11-2008 standard.

[0064] Low-temperature flexibility was determined according to GB / T 2951.14-2008 standard;

[0065] The results of the performance tests are shown in Table 1:

[0066] Table 1

[0067]

[0068] As can be seen from the measurement results in Table 1 above, the cable prepared in the embodiments of the present invention has both high flexibility and flame retardancy in its sheath layer. Therefore, the cable prepared in the present invention can be widely used in high-requirement scenarios such as industrial robots, medical robotic arms, and service robots.

[0069] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

Claims

1. A highly flexible robot cable, comprising, from the inside out: a cable core, an insulation layer, a shielding layer, and a sheath layer, characterized in that, The material of the sheath layer includes the following raw materials in parts by weight: 72-90 parts thermoplastic polyurethane elastomer, 15-20 parts silica, 6-12 parts modifier, and 1-2 parts antioxidant. The modifier is prepared through the following steps: A1. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas is introduced as a protective gas. Dichloromethylphosphine and toluene are added in sequence, and stirring is started. After stirring for 10-20 minutes, stearyl alcohol and triethylamine are added in sequence. After the addition is complete, the mixture is heated to 70-75°C in a water bath and reacted at this temperature for 5-6 hours. After the reaction is complete, the product A is obtained through post-processing. A2. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas is introduced as a protective gas. Piperazine and toluene are mixed and added to the flask. Stirring is started and after stirring for 10-20 minutes, product A and triethylamine are added in sequence. After the addition is complete, the mixture is heated to 60-65°C in a water bath and reacted at a constant temperature for 7-8 hours. After the reaction is complete, the product B is obtained through post-processing. A3. In a dry three-necked flask equipped with a mechanical stirrer, nitrogen gas is introduced as a protective gas. 1,7-Dichlorooctamethyltetrasiloxane is mixed with toluene and added to the flask. Stirring is started, and product B and triethylamine are added. After the addition is complete, the mixture is heated to 70-80°C in a water bath and reacted at a constant temperature for 8-10 hours. After the reaction is complete, the modifier is obtained through post-treatment.

2. The ultra-high flexibility robot cable according to claim 1, characterized in that, In step A1, the ratio of dichloromethylphosphine, toluene, stearyl alcohol, and triethylamine is 14.2-15.3 g: 100 mL: 27.0 g: 10.1 g.

3. The ultra-high flexibility robot cable according to claim 1, characterized in that, In step A2, the ratio of piperazine, toluene, product A, and triethylamine is 9.3-9.9 g: 120 mL: 36.6 g: 10.1 g.

4. The ultra-high flexibility robot cable according to claim 1, characterized in that, In step A3, the ratio of 1,7-dichlorooctamethyltetrasiloxane, toluene, product B, and triethylamine is 35.1 g: 200 mL: 85.5-86.7 g: 20.2 g.

5. The ultra-high flexibility robot cable according to claim 1, characterized in that, The antioxidant is one of antioxidant 3114, antioxidant 1010 and antioxidant 1098.

6. The ultra-high flexibility robot cable according to claim 1, characterized in that, The insulating layer is made of ethylene-tetrafluoroethylene copolymer.

7. The ultra-high flexibility robot cable according to claim 1, characterized in that, The shielding layer is made of aluminum foil and tin-plated copper wire.

Citation Information

Patent Citations

  • Irradiation cross-linked rubber-based flame-retardant cable and preparation method thereof

    CN113652077A