Graded gold / tungsten oxide anti-dot array material and preparation method and application thereof
By using self-assembly technology to prepare graded gold/tungsten oxide reverse dot array materials, the problems of long preparation time and high temperature of tungsten oxide array materials were solved, realizing the rapid, safe and low-energy preparation of tungsten oxide array materials and improving gas-sensing performance.
Patent Information
- Application Number
- CN202410676100.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2025-12-02
AI Technical Summary
Existing methods for preparing tungsten oxide array materials suffer from problems such as long synthesis time and high synthesis temperature, and the use of toxic solvents poses safety hazards.
A graded gold/tungsten oxide reverse dot array material was prepared using a self-assembly technique. Polystyrene spheres and gold nanoparticles of different sizes were dried by spin coating twice, combined with tungsten source precursor solution treatment, and finally annealed in a muffle furnace to form a regular honeycomb structure.
The rapid preparation of tungsten oxide array materials has been achieved, reducing energy consumption, improving gas-sensing performance, and is safe to operate with non-toxic solvents, making it suitable for large-scale production.
Smart Images

Figure CN121044629A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor processing technology, specifically to a graded gold / tungsten oxide inverse dot array material, its preparation method, and its application. Background Technology
[0002] Semiconductor metal oxides possess advantages such as high sensitivity, good stability, and ease of preparation, making them significantly superior in the detection of toxic and harmful gases. Nitrogen dioxide is an irritating reddish-brown oxidizing gas, primarily originating from automobile engines and industrial combustion processes. Prolonged exposure to nitrogen dioxide can lead to respiratory diseases. Furthermore, excessive release of nitrogen dioxide can severely pollute the ecological environment. Therefore, the design and fabrication of advanced sensors capable of rapidly detecting nitrogen dioxide gas is crucial.
[0003] As an n-type semiconductor material, tungsten oxide has wide applications in gas sensing, photocatalysis, electrochromism, and battery materials due to its unique physicochemical properties. In recent years, tungsten oxide sensors for detecting gases such as nitrogen dioxide, ethanol, acetone, ammonia, and hydrogen sulfide have been extensively designed and developed.
[0004] Hierarchical structure refers to a material with multi-scale porosity, exhibiting hierarchical pore sizes ranging from nanometers to micrometers and even macroscopic scales. Tungsten oxide's hierarchical structure combines a large specific surface area with carrier transport channels, facilitating gas molecule adsorption reactions and rapid charge transport. Furthermore, employing a plasmonic effect strategy to enhance gas-sensing performance, noble metal-modified tungsten oxide gas sensors not only increase active sites and improve gas-sensing performance but also reduce operating temperature and energy consumption.
[0005] Currently, various methods have been developed and introduced to synthesize tungsten oxide arrays, including hydrothermal / solvothermal, chemical vapor deposition, and electrospinning. However, these growth methods typically require relatively long synthesis times (>24 h), high synthesis temperatures (>400 ° C), complex steps, or expensive preparation facilities.
[0006] Patent CN112062157A discloses a method for preparing inverse opal-structured tungsten trioxide and its application in photo-Fenton co-catalysis. Specifically, it discloses a method using polystyrene microspheres as a template agent, sequentially impregnating the precursor in a methanol bath and a tungsten trioxide precursor solution bath, infusing the precursor into a photonic crystal composed of regularly arranged polystyrene microspheres, and then removing the template by calcination to obtain inverse opal-structured tungsten trioxide. Subsequent application to the visible light co-catalyzing peroxymonosulfate (PMS) / Fe2+ system for the degradation of rhodamine B exhibited highly efficient co-catalytic activity. However, this patent uses highly toxic solvents such as methanol, raising concerns about operational safety during the preparation process. Summary of the Invention
[0007] The purpose of this invention is to provide a graded gold / tungsten oxide inverse dot array material, its preparation method, and its application, in order to solve the technical problems of long synthesis time and high synthesis temperature in the existing tungsten oxide array preparation methods.
[0008] To achieve the above objectives, one embodiment of the present invention provides a graded gold / tungsten oxide reverse dot array material, which is arranged in a regular honeycomb pattern, with tungsten oxide nanopores grown in the gaps between the honeycombs, and gold nanoparticles uniformly distributed in the gaps between the honeycombs.
[0009] In one preferred embodiment of the present invention, the pore diameter of the honeycomb is 1 μm, the diameter of the gold nanoparticles is 45 nm-60 nm, and the diameter of the tungsten oxide nanopores is 85 nm-115 nm.
[0010] Based on the graded gold / tungsten oxide inversion array material disclosed in this invention, this invention also discloses a method for preparing the graded gold / tungsten oxide inversion array material, comprising the following steps:
[0011] Polystyrene spheres are dispersed in a mixture of ethanol and water to form a dispersion solution, which is then injected into the surface of water to self-assemble into a thin film.
[0012] The substrate is bonded to a solution containing a thin film to obtain a single-layer polystyrene spherical template, and the template is then dried.
[0013] The gold nanoparticle solution was spin-coated onto the dried template surface and then dried.
[0014] The polystyrene sphere solution was spin-coated onto the template surface, which had been spin-coated with gold nanoparticle solution and dried, and then dried again.
[0015] The template, after being spin-coated with polystyrene sphere solution and dried, is immersed in tungsten source precursor solution, then removed and dried;
[0016] The template, after being impregnated and dried with a tungsten source precursor solution, was placed in a muffle furnace for annealing to obtain graded gold / tungsten oxide inverse dot array materials.
[0017] In one preferred embodiment of the present invention, the polystyrene spheres have a diameter of 1 μm, the volume ratio of ethanol to water in the mixed solution is 1:1, the injection volume of the dispersion solution is 10 μl-30 μl, and the volume of water is 20 ml-40 ml.
[0018] In one preferred embodiment of the present invention, the method of bonding the substrate with the solution having a thin film is as follows: immersing the substrate in the solution having a thin film.
[0019] In one preferred embodiment of the present invention, the method of bonding the substrate with the solution having a thin film is as follows: the solution having a thin film is dropped onto the substrate.
[0020] In one preferred embodiment of the present invention, the substrate is a silicon wafer or an interdigitated electrode.
[0021] In one preferred embodiment of the present invention, the interdigitated electrode is a 30μm interdigitated electrode.
[0022] In one preferred embodiment of the present invention, the drying temperature of the single-layer polystyrene sphere template is 40℃-60℃, and the drying time is 1h-3h.
[0023] In one preferred embodiment of the present invention, the concentration of the gold nanoparticle solution is 0.1mM-0.3mM, the diameter of the gold nanoparticles is 45nm-55nm, the spin-coating speed of the gold nanoparticle solution is 1000rpm / s-2000rpm / s, and the spin-coating time is 10s-30s; the drying temperature of the template after spin-coating the gold nanoparticle solution is 40℃-60℃, and the drying time is 1h-3h.
[0024] In one preferred embodiment of the present invention, the mass fraction of the polystyrene ball solution is 3%-10%, the diameter of the polystyrene ball solution is 100nm, the spin coating speed of the polystyrene ball solution is 1000rpm / s-2000rpm / s, and the spin coating time is 10s-30s; the template drying temperature after spin coating of the polystyrene ball solution is 40℃-60℃, and the drying time is 1h-3h.
[0025] In one preferred embodiment of the present invention, the tungsten source precursor is silicotungstic acid, the concentration of silicotungstic acid is 2mM-8mM, the immersion time is 1s-6s, and the drying temperature of the template after immersion in the tungsten source precursor solution is 40℃-60℃, and the drying time is 1h-3h.
[0026] In one preferred embodiment of the present invention, the annealing temperature is 380℃-520℃, the heating rate is 5℃ / min, and the holding time is 1h-4h.
[0027] This invention also discloses an application of a graded gold / tungsten oxide inverse dot array material, which is used in a gas sensor.
[0028] In summary, the beneficial effects of the present invention are as follows:
[0029] 1. The method for preparing the graded gold / tungsten oxide reverse dot array material of the present invention involves spin-coating and drying polystyrene spheres of different sizes twice to obtain graded tungsten oxide. The graded tungsten oxide has a large specific surface area and carrier transport channels, which is beneficial to the adsorption reaction of gas molecules and the rapid transport of charges.
[0030] 2. The method for preparing graded gold / tungsten oxide inverse dot array materials of the present invention can prepare graded gold / tungsten oxide inverse dot array materials through self-assembly. The preparation method is simple, the raw materials are inexpensive, and the reproducibility is good. It can become a general method for growing large-scale graded gold / tungsten oxide inverse dot array materials.
[0031] 3. The preparation method of the present invention directly uses a clean silicon wafer or a 30μm interdigitated electrode as a substrate to prepare a graded gold / tungsten oxide inverse dot array by a self-organizing method. The operation is simple and the reproducibility is high.
[0032] 4. The preparation method of the present invention can uniformly distribute gold nanoparticles inside tungsten oxide. The plasmon effect of gold nanoparticles can not only increase active sites and improve the gas-sensing performance of the material, but also reduce the operating temperature and reduce energy consumption.
[0033] 5. The preparation time of the method of the present invention is relatively short, about 12 hours; and the preparation process of the method of the present invention does not use highly toxic solvents such as methanol, and the preparation process is safe, green and friendly. Attached Figure Description
[0034] Figure 1 The images are scanning electron microscope (SEM) images of the graded gold / tungsten oxide reverse dot array material prepared in Example 2 of this invention, where (a) is a 2 μm top view and (b) is a 500 nm top view.
[0035] Figure 2 The X-ray diffraction pattern of the gold / tungsten oxide prepared in Example 2 of this invention;
[0036] Figure 3 This is a graph showing the determination of the optimal operating temperature for 50 ppm NO2 for the graded gold / tungsten oxide reverse dot array material prepared in Example 2 of this invention;
[0037] Figure 4 The graph shows the response curves of the graded gold / tungsten oxide reverse dot array material prepared in Example 2 of this invention to NO2 concentrations of 1ppm-100ppm at three different solar intensities under optimal operating temperature.
[0038] Figure 5 This is a comparison graph showing the response of the graded gold / tungsten oxide reverse dot array material prepared in Example 2 of this invention to NO2, C2H5OH, CH3OH, NH3, CH4, H2 and CH2F2 at the optimal operating temperature and three solar intensities. Detailed Implementation
[0039] This invention discloses a graded gold / tungsten oxide reverse dot array material, which is arranged in a regular honeycomb pattern, with tungsten oxide nanopores grown in the gaps between the honeycombs, and gold nanoparticles uniformly distributed in the gaps between the honeycombs; wherein, the diameter of the honeycomb pores is 1 μm, the diameter of the gold nanoparticles is 45 nm-60 nm, and the diameter of the tungsten oxide nanopores is 85 nm-115 nm.
[0040] This invention also discloses a method for preparing a graded gold / tungsten oxide inverse dot array material, comprising the following steps:
[0041] Step (1): Disperse polystyrene spheres with a diameter of 1 μm in a mixed solution of ethanol and water with a volume ratio of 1:1 to form a dispersion solution. Then inject 10 μl-30 μl of the dispersion solution into the surface of 20 ml-40 ml of water to self-assemble into a thin film.
[0042] Step (2): Combine the clean substrate with the solution containing the thin film to obtain a single-layer polystyrene sphere template, and dry the template at a drying temperature of 40℃-60℃ for 1h-3h; wherein the substrate is combined with the solution containing the thin film by immersing the substrate in the solution containing the thin film, or by dripping the solution containing the thin film onto the substrate to achieve the combination of the substrate and the solution containing the thin film to obtain a single-layer polystyrene sphere template; further, the substrate is a silicon wafer or interdigitated electrodes, and the interdigitated electrodes are 30μm interdigitated electrodes;
[0043] Step (3): Spin-coat a solution of gold nanoparticles with a concentration of 0.1mM-0.3mM and a diameter of 45nm-55nm onto the dried template surface at a spin-coating speed of 1000rpm / s-2000rpm / s for 10s-30s. Then, place the resulting template on a micro-hot plate for curing. The drying temperature is 40℃-60℃ and the drying time is 1h-3h.
[0044] Step (4): Spin coat a polystyrene ball solution with a mass fraction of 3%-10% and a diameter of 100nm onto the template surface after spin coating gold nanoparticle solution and drying for 10s-30s at a spin coating speed of 1000rpm / s-2000rpm / s. Then place the obtained template on a micro hot plate for curing. The drying temperature is 40℃-60℃ and the drying time is 1h-3h.
[0045] Step (5): Immerse the template after spin-coating and drying the polystyrene ball solution into the tungsten source precursor solution, take it out and dry it. The tungsten source precursor is silicotungstic acid with a concentration of 2mM-8mM. The immersion time is 1s-6s. The drying temperature of the template after immersion in the tungsten source precursor solution is 40℃-60℃ and the drying time is 1h-3h.
[0046] Step (6): The template, after being impregnated and dried by the tungsten source precursor solution, is placed in a muffle furnace for annealing to remove the template and crystallized tungsten oxide, thereby obtaining graded gold / tungsten oxide reverse dot array material. The annealing temperature is 380℃-520℃, the heating rate is 5℃ / min, and the holding time is 1h-4h.
[0047] This invention also discloses an application of a graded gold / tungsten oxide inverse dot array material, which is applied to the field of gas sensor technology. Specifically, the graded gold / tungsten oxide inverse dot array material has a sensitivity of 228.3 for identifying 50ppm NO2 gas at a working temperature of 200℃-300℃ and three different sunlight intensities, a recovery time of 52s, and a response time of 5s.
[0048] Example 1
[0049] A method for preparing a graded gold / tungsten oxide inverse dot array material includes the following steps:
[0050] Step (1): Disperse polystyrene spheres with a diameter of 1 μm in a mixed solution of ethanol and water with a volume ratio of 1:1 to form a dispersion solution. Then inject 20 μl of the dispersion solution into the surface of 30 ml of water to self-assemble into a thin film.
[0051] Step (2): Immerse a clean silicon wafer or interdigitated electrode in a solution with a thin film to obtain a single-layer polystyrene ball template by the dip-coating method, and place the template on a micro-hot plate for curing and drying at a drying temperature of 50°C for 2 hours;
[0052] Step (3): Spin-coat a 0.2mM gold nanoparticle solution with a diameter of 50nm onto the dried template surface at a spin coating speed of 1000rpm / s for 30s. Then, place the resulting template on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2h.
[0053] Step (4): A polystyrene ball solution with a mass fraction of 5% and a diameter of 100 nm is spin-coated onto the template surface after spin-coating gold nanoparticle solution and drying for 30 s at a spin-coating speed of 1000 rpm / s. The resulting template is then placed on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2 h.
[0054] Step (5): Prepare a 2mM silicotungstic acid solution using deionized water to obtain a tungsten source precursor solution. Immerse the template, which has been spin-coated with polystyrene spheres and dried, into the tungsten source precursor solution for 2 seconds and then remove it. After removal, place the template on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2 hours.
[0055] Step (6): Place the template, which has been impregnated and dried by the tungsten source precursor solution, into a muffle furnace for calcination at a temperature of 450℃, a heating rate of 5℃ / min, and a holding time of 2h.
[0056] This invention also discloses an application of a graded gold / tungsten oxide inverse dot array material, which is applied to the field of gas sensor technology.
[0057] Nitrogen dioxide gas-sensitive detection is performed according to the following steps:
[0058] The temperature inside the environmental test chamber was raised to the required operating temperature, and the sunlight intensity was set to the required value. An ambient atmospheric pressure and clean, dry air were used as the background gas environment. The prepared graded gold / tungsten oxide inverse dot array gas sensor was placed in the gas-sensitive test chamber and powered on for 15 minutes until the baseline stabilized. The resistance value Ra of the device was recorded. Subsequently, 50 ppm NO2 gas was introduced into the environmental chamber and maintained for 300 seconds, and the resistance value Rg of the device was recorded. The test chamber was then purged with clean air, and the measured gas was expelled until the resistance value stabilized. The sensitivity of the gas-sensitive element to the target gas is defined as: S = Rg / Ra. A correlation curve was plotted between the sensitivity S and time t.
[0059] Example 2
[0060] A method for preparing a graded gold / tungsten oxide inverse dot array material includes the following steps:
[0061] Step (1): Disperse polystyrene spheres with a diameter of 1 μm in a mixed solution of ethanol and water with a volume ratio of 1:1 to form a dispersion solution. Then inject 20 μl of the dispersion solution into the surface of 30 ml of water to self-assemble into a thin film.
[0062] Step (2): Immerse a clean silicon wafer or interdigitated electrode in a solution with a thin film to obtain a single-layer polystyrene ball template by the dip-coating method, and place the template on a micro-hot plate for curing and drying at a drying temperature of 50°C for 2 hours;
[0063] Step (3): Spin-coat a 0.2mM gold nanoparticle solution with a diameter of 50nm onto the dried template surface at a spin coating speed of 1000rpm / s for 30s. Then, place the resulting template on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2h.
[0064] Step (4): A polystyrene ball solution with a mass fraction of 5% and a diameter of 100 nm is spin-coated onto the template surface after spin-coating gold nanoparticle solution and drying for 30 s at a spin-coating speed of 1000 rpm / s. The resulting template is then placed on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2 h.
[0065] Step (5): Prepare a 5mM silicotungstic acid solution using deionized water as the solvent to obtain a tungsten source precursor solution. Immerse the template, which has been spin-coated with polystyrene spheres and dried, into the tungsten source precursor solution for 2 seconds and then remove it. After removal, place the template on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2 hours.
[0066] Step (6): The template, which has been impregnated and dried by the tungsten source precursor solution, is placed in a muffle furnace for calcination at a temperature of 450°C, a heating rate of 5°C / min, and a holding time of 2h to obtain a graded gold / tungsten oxide reverse dot array.
[0067] This invention also discloses an application of a graded gold / tungsten oxide inverse dot array material, which is applied to the field of gas sensor technology.
[0068] Nitrogen dioxide gas-sensitive detection is performed according to the following steps:
[0069] The temperature inside the environmental test chamber was raised to the required operating temperature, and the sunlight intensity was set to the required value. An ambient atmospheric pressure and clean, dry air were used as the background gas environment. The prepared graded gold / tungsten oxide inverse dot array gas sensor was placed in the gas-sensitive test chamber and powered on for 15 minutes until the baseline stabilized. The resistance value Ra of the device was recorded. Subsequently, 50 ppm NO2 gas was introduced into the environmental chamber and maintained for 300 seconds, and the resistance value Rg of the device was recorded. The test chamber was then purged with clean air, and the measured gas was expelled until the resistance value stabilized. The sensitivity of the gas-sensitive element to the target gas is defined as: S = Rg / Ra. A correlation curve was plotted between the sensitivity S and time t.
[0070] Example 3
[0071] A method for preparing a graded gold / tungsten oxide inverse dot array material includes the following steps:
[0072] Step (1): Disperse polystyrene spheres with a diameter of 1 μm in a mixed solution of ethanol and water with a volume ratio of 1:1 to form a dispersion solution. Then inject 20 μl of the dispersion solution into the surface of 30 ml of water to self-assemble into a thin film.
[0073] Step (2): Immerse a clean silicon wafer or interdigitated electrode in a solution with a thin film to obtain a single-layer polystyrene ball template by the dip-coating method, and place the template on a micro-hot plate for curing and drying at a drying temperature of 50°C for 2 hours;
[0074] Step (3): Spin-coat a 0.2mM gold nanoparticle solution with a diameter of 50nm onto the dried template surface at a spin coating speed of 1000rpm / s for 30s. Then, place the resulting template on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2h.
[0075] Step (4): A polystyrene ball solution with a mass fraction of 5% and a diameter of 100 nm is spin-coated onto the template surface after spin-coating gold nanoparticle solution and drying for 30 s at a spin-coating speed of 1000 rpm / s. The resulting template is then placed on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2 h.
[0076] Step (5): Prepare an 8mM silicotungstic acid solution using deionized water to obtain a tungsten source precursor solution. Immerse the template, which has been spin-coated with polystyrene spheres and dried, into the tungsten source precursor solution for 2 seconds and then remove it. After removal, place the template on a micro-hot plate for curing. The drying temperature is 50℃ and the drying time is 2 hours.
[0077] Step (6): The template, which has been impregnated and dried by the tungsten source precursor solution, is placed in a muffle furnace for calcination at a temperature of 450°C, a heating rate of 5°C / min, and a holding time of 2h to obtain a graded gold / tungsten oxide reverse dot array.
[0078] This invention also discloses an application of a graded gold / tungsten oxide inverse dot array material, which is applied to the field of gas sensor technology.
[0079] Nitrogen dioxide gas-sensitive detection is performed according to the following steps:
[0080] The temperature inside the environmental test chamber was raised to the required operating temperature, and the sunlight intensity was set to the required value. An ambient atmospheric pressure and clean, dry air were used as the background gas environment. The prepared graded gold / tungsten oxide inverse dot array gas sensor was placed in the gas-sensitive test chamber and powered on for 15 minutes until the baseline stabilized. The resistance value Ra of the device was recorded. Subsequently, 50 ppm NO2 gas was introduced into the environmental chamber and maintained for 300 seconds, and the resistance value Rg of the device was recorded. The test chamber was then purged with clean air, and the measured gas was expelled until the resistance value stabilized. The sensitivity of the gas-sensitive element to the target gas is defined as: S = Rg / Ra. A correlation curve was plotted between the sensitivity S and time t.
[0081] Experimental testing
[0082] The graded gold / tungsten oxide inverse dot array material prepared in Example 2 was observed under a scanning electron microscope. The observation results are as follows: Figure 1 As shown, (a) is a top view at 2 μm; (b) is a top view at 500 nm. From Figure 1 As can be seen, the graded gold / tungsten oxide reverse dot array material is arranged in a regular honeycomb pattern, with tungsten oxide nanopores grown in the gaps between the honeycombs; the diameter of the honeycomb pores is 1 μm, and the diameter of the tungsten oxide nanopores is about 100 nm.
[0083] The graded gold / tungsten oxide reverse dot array material prepared in Example 2 was examined using an X-ray diffractometer. The test results are as follows: Figure 2 As shown. From Figure 2 As can be seen, the diffraction peaks correspond to orthorhombic tungsten oxide (JCPDS.20-1324) and cubic gold (JCPDS.04-0784), and there are no impurity peaks, which proves the successful preparation of gold / tungsten oxide on the template.
[0084] The optimal temperature for nitrogen dioxide gas-sensitive detection was determined for the graded gold / tungsten oxide inverse dot array material prepared in Example 2. The test results are as follows: Figure 3 As shown. From Figure 3 As can be seen from this, the optimal operating temperature is 200℃.
[0085] The graded gold / tungsten oxide inverse dot array material prepared in Example 2 was subjected to nitrogen dioxide gas-sensitive detection. The detection results are as follows: Figure 4 As shown. From Figure 4 As can be seen, the graded gold / tungsten oxide inverse dot array material has high sensitivity and good linear response to NO2.
[0086] The responses of the graded gold / tungsten oxide inverse dot array material prepared in Example 2 to NO2, C2H5OH, CH3OH, NH3, CH4, H2, and CH2F2 were compared at the optimal operating temperature and under three solar intensities. The comparison results are as follows: Figure 5 As shown. From Figure 5 As can be seen, the graded gold / tungsten oxide inverse dot array material exhibits high selectivity in its response to NO2.
[0087] The morphology and gas-sensing properties of the graded gold / tungsten oxide inverse dot array materials prepared in Examples 1, 2 and 3 are summarized, and the results are shown in Table 1.
[0088] Table 1: Summary Results of Examples 1, 2 and 3
[0089]
[0090]
[0091] As can be seen from Table 1, all three examples (Example 1, Example 2, and Example 3) successfully prepared hierarchical gold / tungsten oxide reverse dot array structures, and the prepared hierarchical gold / tungsten oxide reverse dot array materials exhibited good gas-sensitive response to NO2.
[0092] Although specific embodiments of the present invention have been described in detail with reference to the accompanying drawings, this should not be construed as limiting the scope of protection of this patent. Various modifications and variations that can be made by those skilled in the art without inventive effort within the scope described in the claims still fall within the scope of protection of this patent.
Claims
1. A graded gold / tungsten oxide inverse dot array material, characterized in that: The graded gold / tungsten oxide inverse dot array material is arranged in a regular honeycomb pattern, with tungsten oxide nanopores grown in the gaps between the honeycombs, and gold nanoparticles uniformly distributed in the gaps between the honeycombs.
2. The graded gold / tungsten oxide inverse dot array material as described in claim 1, characterized in that: The honeycomb has a pore diameter of 1 μm, the gold nanoparticles have a diameter of 45 nm-60 nm, and the tungsten oxide nanopores have a diameter of 85 nm-115 nm.
3. A method for preparing a graded gold / tungsten oxide inverse dot array material, characterized in that, Includes the following steps: Polystyrene spheres are dispersed in a mixture of ethanol and water to form a dispersion solution, which is then injected into the surface of water to self-assemble into a thin film. The substrate is bonded to a solution containing a thin film to obtain a single-layer polystyrene spherical template, and the template is then dried. The gold nanoparticle solution was spin-coated onto the dried template surface and then dried. The polystyrene sphere solution was spin-coated onto the template surface, which had been spin-coated with gold nanoparticle solution and dried, and then dried again. The template, after being spin-coated with polystyrene sphere solution and dried, is immersed in tungsten source precursor solution, then removed and dried; The template, after being impregnated and dried with a tungsten source precursor solution, was placed in a muffle furnace for annealing to obtain graded gold / tungsten oxide inverse dot array materials.
4. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that: The polystyrene spheres have a diameter of 1 μm, the volume ratio of ethanol to water in the mixed solution is 1:1, the injection volume of the dispersion solution is 10 μl-30 μl, and the volume of water is 20 ml-40 ml.
5. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that, The method for bonding the substrate to the solution having a thin film is as follows: immersing the substrate in the solution having a thin film.
6. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that, The method for bonding the substrate with the solution having a thin film is as follows: the solution having a thin film is dropped onto the substrate.
7. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, 5, or 6, characterized in that: The substrate is a silicon wafer or interdigitated electrodes.
8. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 7, characterized in that: The interdigitated electrode is a 30μm interdigitated electrode.
9. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that: The drying temperature of the single-layer polystyrene ball template is 40℃-60℃, and the drying time is 1h-3h.
10. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that: The concentration of the gold nanoparticle solution is 0.1mM-0.3mM, the diameter of the gold nanoparticles is 45nm-55nm, the spin coating speed of the gold nanoparticle solution is 1000rpm / s-2000rpm / s, and the spin coating time is 10s-30s; the drying temperature of the template after spin coating of the gold nanoparticle solution is 40℃-60℃, and the drying time is 1h-3h.
11. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that: The polystyrene ball solution has a mass fraction of 3%-10%, a diameter of 100 nm, a spin coating speed of 1000 rpm / s-2000 rpm / s, and a spin coating time of 10 s-30 s; the template drying temperature after spin coating of the polystyrene ball solution is 40℃-60℃, and the drying time is 1 h-3 h.
12. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that: The tungsten source precursor is silicotungstic acid, the concentration of which is 2mM-8mM, the immersion time is 1s-6s, and the drying temperature of the template after immersion in the tungsten source precursor solution is 40℃-60℃, and the drying time is 1h-3h.
13. The method for preparing a graded gold / tungsten oxide inverse dot array material as described in claim 3, characterized in that: The annealing treatment is performed at a temperature of 380℃-520℃, a heating rate of 5℃ / min, and a holding time of 1h-4h.
14. An application of the graded gold / tungsten oxide inverse dot array material according to any one of claims 1-2, wherein it is applied to a gas sensor.
Citation Information
Patent Citations
Preparation method of tungsten trioxide with inverse opal structure and application of tungsten trioxide in photo-Fenton catalysis assistance
CN112062157A
Two-dimensional ordered gold and ITO composite nanometer array and preparation method thereof
CN107089642A
Preparation method of hydrogen sensitive material as well as product and application thereof
CN117740695A