High-hardness nitrided steel material and preparation method thereof
By using rare earth catalytic agents and multiple post-oxidation treatments, the hardness and wear resistance of the nitrided layer of 38CrMoAl steel were improved, solving the problem that traditional methods could not meet the performance requirements of modern mechanical parts, and realizing the preparation of high-hardness nitrided steel materials.
Patent Information
- Application Number
- CN202511115276.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-08-11
- Publication Date
- 2025-12-05
AI Technical Summary
After tempering and gas nitriding, the surface hardness and wear resistance of traditional 38CrMoAl steel are no longer sufficient to meet the modern requirements for high strength, high wear resistance and high fatigue strength.
Ion nitriding is performed using rare earth catalytic agents, followed by at least two post-oxidation treatments. Combined with a hydrogen sputtering step, the chemical activation and physical bombardment effects of rare earth elements are utilized to promote the diffusion of nitrogen atoms and refine the nitrided layer, forming a dense nitride layer and improving the hardness and toughness of the material.
It significantly improves the surface hardness and wear resistance of the material, reduces brittleness, optimizes friction performance and aesthetics, and meets the high-performance requirements of modern mechanical parts.
Smart Images

Figure SMS_1
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of nitriding steel material, in particular to a high-hardness nitriding steel material and a preparation method thereof. BACKGROUND
[0002] With the rapid development of modern industrial technology, the performance requirements of mechanical parts are increasingly improved, especially in terms of high strength, high wear resistance, high fatigue strength and good dimensional stability. Among many engineering materials, alloy structural steel is widely used in manufacturing key components that bear heavy load, high-speed friction and complex stress state, such as engine crankshafts, gears, precision shafts and dies, due to its excellent comprehensive mechanical properties and processability. Among them, 38CrMoAl steel, as a typical medium-carbon alloy nitriding steel, has good hardenability, high surface hardness and excellent fatigue resistance due to the presence of alloying elements such as chromium (Cr), molybdenum (Mo) and aluminum (Al), and has been widely used in applications requiring high surface hardness and wear resistance for a long time.
[0003] However, with the development of equipment towards high speed, heavy load and high precision, the surface hardness and wear resistance of conventional 38CrMoAl steel after conventional quenching and tempering treatment and gas nitriding have gradually been difficult to meet the use requirements. Therefore, the applicant prepared a high-hardness nitriding steel material using 38CrMoAl steel as raw material. SUMMARY
[0004] The purpose of the present application is to provide a high-hardness nitriding steel material and a preparation method thereof to solve the technical problems mentioned in the background.
[0005] The technical solution for achieving the purpose of the present application is: In a first aspect, the present application provides a preparation method of a high-hardness nitriding steel material, comprising the following preparation steps: S1. Quenching, cutting, polishing, cleaning and drying the 38CrMoAl steel; S2. Ion nitriding the 38CrMoAl steel treated in step S1 using a rare earth catalyst; S3. Carrying out at least two post-oxidations on the 38CrMoAl steel ion nitrided in step S2 to obtain a high-hardness nitriding steel material.
[0006] Further, the quenching process is as follows: quenching temperature 930-950℃, holding time 1-1.5h, cooling method oil cooling; tempering temperature 600-680℃, tempering time 3-5h, cooling method air cooling.
[0007] Further, the specific steps of step S2 are as follows: Hang the rare earth catalyst in the cathode plate of the ion nitriding furnace, place the 38CrMoAl steel treated by S1 in the ion nitriding furnace, pump the pressure in the furnace to 6*10 -4 Pa, and input the nitriding gas source to perform ion nitriding treatment.
[0008] Further, the rare earth catalyst is lanthanum-cerium alloy, and the main chemical components of the lanthanum-cerium alloy are as follows: 32.4wt% lanthanum, 67.43wt% cerium, 0.15wt% praseodymium, <0.03wt% neodymium, 0.53wt% iron, <0.01 silicon, and <0.01 phosphorus.
[0009] Further, when the loading capacity of the ion nitriding furnace is 240kg, the adding amount of the lanthanum-cerium alloy is 1-2 pieces, and each piece of the lanthanum-cerium alloy is a square of 50mm*50mm*50mm.
[0010] Further, the nitriding gas source is a mixed gas of nitrogen and argon with a volume ratio of (3-4):(1-2).
[0011] Further, the flow of the nitriding gas source of the ion nitriding is 500mL / h, the nitriding gas pressure is 120Pa, the nitriding temperature is 520-560℃, and the holding time is 10-20h.
[0012] Further, one hydrogen sputtering is further performed between the two adjacent post-oxidations.
[0013] Further, the post-oxidation temperature is 390-410℃, the post-oxidation time is 1.5-2.5h, the hydrogen sputtering temperature is 490-510℃, and the hydrogen sputtering time is 3-4h.
[0014] In the second aspect, a high-hardness nitriding steel material is prepared by the preparation method of the high-hardness nitriding steel material in the first aspect.
[0015] By adopting the technical scheme, the present application has the following beneficial effects: (1) In the preparation of the high-hardness nitriding steel material, the 38CrMoAl steel is used as the raw material, and after quenching and tempering, cutting, polishing, cleaning and drying, the ion nitriding is performed by using the rare earth catalyst, and then at least two post-oxidations are performed, so that the hardness and wear resistance of the prepared high-hardness nitriding steel material are better.
[0016] (2) The quenching and tempering process is as follows: the quenching temperature is 930-950℃, the holding time is 1-1.5h, and the cooling mode is oil cooling; the tempering temperature is 600-680℃, the tempering time is 3-5h, and the cooling mode is air cooling. Under the quenching and tempering process, the austenitizing degree of the 38CrMoAl steel is enhanced, the martensite is formed more fully, refined and uniform, and the dislocation density is increased, so that the hardness and impact toughness are better.
[0017] (3) The 38CrMoAl steel of the present application is nitrided by using a mixed gas of nitrogen and argon as the nitriding gas source, and through the synergistic mechanism of "chemical activation + physical bombardment", the efficiency and performance of the nitriding process are realized: on the one hand, argon reduces the ionization energy of nitrogen, and improves the yield of active nitrogen atoms; on the other hand, Ar + bombardment introduces surface defects to promote nitrogen diffusion; under the synergistic effect of the two effects, the 38CrMoAl steel can obtain a thicker, harder and more uniform nitriding layer in a shorter nitriding period, and the surface hardness and wear resistance of the material are significantly improved.
[0018] (4) In the process of ion nitriding of the 38CrMoAl steel, a mixed gas of nitrogen and argon is used as the nitriding medium, and a rare earth lanthanum-cerium alloy (La-Ce) is introduced as a catalyst, and through a triple synergistic mechanism, the hardness, toughness and wear resistance of the steel are significantly improved. First, in terms of gas phase activation and acceleration, lanthanum and cerium elements can destroy the chemical bonds in the nitriding medium, promote the dissociation of nitrogen molecules into active nitrogen atoms, thereby improving the gas phase reaction efficiency and ensuring sufficient supply of active nitrogen source; secondly, in the surface adsorption strengthening mechanism, rare earth atoms preferentially adsorb on the surface of the steel part, remove the oxide film and reduce the system energy, thereby enhancing the adsorption capacity of nitrogen atoms, and at the same time, the rare earth itself also penetrates into the surface layer to form a diffusion channel, further promoting the adsorption process of nitrogen atoms; thirdly, the diffusion kinetics optimization mechanism includes three aspects of lattice distortion effect, concentration gradient driving and diffusion mechanism transformation: large-size rare earth atoms (such as La, with an atomic radius of 1.87 Å, much larger than the 1.24 Å of Fe) penetrate into the grain boundaries and dislocation zones, causing severe lattice distortion, increasing the vacancy and dislocation density, and providing a rapid diffusion channel for small-size nitrogen atoms (atomic radius 0.71 Å); the high surface nitrogen concentration (energy spectrum detection shows that the La mass fraction in the surface layer can reach 2.53%) formed after the adsorption of rare earth and nitrogen atoms establishes a strong concentration gradient from the surface to the center and from the grain boundary to the grain, promoting the inward diffusion of nitrogen; the interaction between rare earth and nitrogen changes the diffusion path and improves the diffusion coefficient of nitrogen. These mechanisms work together to significantly increase the surface hardness, mainly due to the dense nitride (mainly ε-Fe 2-3 N phase) and grain boundary strengthening; at the same time, the rare earth refines the grains and inhibits the nitride network segregation, avoiding stress concentration, thereby optimizing the toughness of the material; in addition, the synergistic effect of the high-hardness surface layer and the tough substrate effectively resists wear, significantly improving the wear resistance of the material.
[0019] (5) The present application carries out multiple post-oxidation treatments after ion nitriding of 38CrMoAl steel, and introduces a hydrogen sputtering step between two adjacent post-oxidations, which significantly improves the hardness, toughness and wear resistance of the material through multiple mechanisms; the post-oxidation treatment refines the nitride particles in the nitriding layer, converting the larger nitride particles formed during the nitriding process into finer oxide particles, which not only significantly improves the surface hardness, but also enhances the wear resistance of the material; at the same time, the post-oxidation treatment improves the residual stress state of the nitriding layer, and the oxide layer formed releases part of the residual stress, which effectively resists external stress, reduces the risk of deformation and cracking, and thus improves the toughness of the material; in addition, the dense oxide layer fills in the surface micro defects, making the surface smoother and more smooth, further optimizing the friction performance and aesthetics; the hydrogen sputtering step reduces the oxide film formed by the previous oxidation, solving the problem of covering and hindering the reaction of active oxygen and nitride layer, so that the subsequent oxidation can continuously decompose the iron nitride (FexN) in the compound layer to generate iron oxide and release active nitrogen atoms, which diffuse to the matrix to form solid solution strengthening effect, significantly increasing the cross-sectional hardness and effective hardening layer thickness; the thinning of the compound layer and the refinement of the nitride particles together reduce the brittleness, while the improvement of the surface hardness combined with the densification of the oxide layer significantly reduces the wear rate and enhances the wear resistance. DETAILED DESCRIPTION
[0020] In order to better understand the above technical solutions, the above technical solutions will be described in detail below in combination with specific embodiments.
[0021] Based on the embodiments in the present application, all other embodiments obtained by those of ordinary skill in the art without creative labor fall within the scope of protection of the present application.
[0022] The following examples are only used to more clearly illustrate the technical solutions of the present application, and cannot be used to limit the protection scope of the present application.
[0024] The main chemical components of 38CrMoAl steel are as follows: 0.38wt% carbon, 0.40wt% silicon, 1wt% aluminum, 0.5wt% manganese, 1.5wt% chromium, 0.2wt% molybdenum, and the balance of iron.
[0025] The main chemical components of lanthanum-cerium alloy are as follows: 32.4wt% lanthanum, 67.43wt% cerium, 0.15wt% praseodymium, <0.03wt% neodymium, 0.53wt% iron, <0.01 silicon, and <0.01 phosphorus. Example 1
[0026] A preparation method of a high-hardness nitriding steel material, comprising the following preparation steps: S1. quenching, cutting, polishing, cleaning and drying 38CrMoAl steel to obtain treated 38CrMoAl steel with a size of 30mm*10mm*10mm; S2. ion nitriding the treated 38CrMoAl steel in step S1 by using a rare earth catalyst; S3. post-oxidizing, hydrogen sputtering, post-oxidizing, hydrogen sputtering and post-oxidizing the 38CrMoAl steel after ion nitriding in step S2 to obtain high-hardness nitrided steel material.
[0027] The quenching process is as follows: quenching temperature is 930℃, holding time is 1.5h, and cooling mode is oil cooling; tempering temperature is 600℃, tempering time is 5h, and cooling mode is air cooling.
[0028] The specific steps of step S2 are as follows: hanging the rare earth catalyst on the cathode disc in the ion nitriding furnace, placing the treated 38CrMoAl steel in the ion nitriding furnace, and pumping the furnace to a vacuum degree of 6*10 -4 Pa, and introducing the nitriding gas source for ion nitriding treatment.
[0029] The rare earth catalyst is lanthanum-cerium alloy, and when the loading capacity of the ion nitriding furnace is 240kg, the addition amount of the lanthanum-cerium alloy is 1 piece, and each piece of lanthanum-cerium alloy is a cube with a size of 50mm*50mm*50mm.
[0030] The nitriding gas source is a mixed gas of nitrogen and argon with a volume ratio of 3:2.
[0031] The flow rate of the nitriding gas source for ion nitriding is 500mL / h, the nitriding gas pressure is 120Pa, the nitriding temperature is 520℃, and the holding time is 20h.
[0032] The post-oxidation temperature is 400℃, the post-oxidation time is 2h, the hydrogen sputtering temperature is 500℃, and the hydrogen sputtering time is 4h. Example 2
[0033] A preparation method of high-hardness nitrided steel material, comprising the following preparation steps: S1. quenching, cutting, polishing, cleaning and drying 38CrMoAl steel to obtain treated 38CrMoAl steel with a size of 30mm*10mm*10mm; S2. ion nitriding the treated 38CrMoAl steel in step S1 by using a rare earth catalyst; S3. post-oxidizing, hydrogen sputtering, post-oxidizing, hydrogen sputtering and post-oxidizing the 38CrMoAl steel after ion nitriding in step S2 to obtain high-hardness nitrided steel material.
[0034] The tempering process is: quenching temperature 940 DEG C, holding time 1h, cooling mode oil cooling; tempering temperature 680 DEG C, tempering time 3h, cooling mode air cooling.
[0035] The specific steps of the step S2 are as follows: the rare earth catalyst is hung on the cathode disc in the ion nitriding furnace, the 38CrMoAl steel treated in S1 is placed in the ion nitriding furnace, the air pressure in the furnace is extracted to a vacuum degree of 6*10 -4 Pa, and the ion nitriding treatment is carried out by introducing the nitriding gas source.
[0036] The rare earth catalyst is lanthanum-cerium alloy, and when the loading capacity of the ion nitriding furnace is 240kg, the adding amount of the lanthanum-cerium alloy is 1 piece, and each piece of the lanthanum-cerium alloy is a cube with a size of 50mm*50mm*50mm.
[0037] The nitriding gas source is a mixed gas of nitrogen and argon with a volume ratio of 3:2.
[0038] The flow of the nitriding gas source of the ion nitriding is 500mL / h, the nitriding gas pressure is 120Pa, the nitriding temperature is 560 DEG C, and the holding time is 10h.
[0039] The post-oxidation temperature is 400 DEG C, the post-oxidation time is 2h, the hydrogen sputtering temperature is 500 DEG C, and the hydrogen sputtering time is 4h. Example 3
[0040] A preparation method of a high-hardness nitriding steel material, comprising the following preparation steps: S1. The 38CrMoAl steel is subjected to quenching and tempering, cutting, polishing, cleaning and drying to obtain the treated 38CrMoAl steel with a size of 30mm*10mm*10mm; S2. The treated 38CrMoAl steel in step S1 is subjected to ion nitriding by using a rare earth catalyst; S3. The 38CrMoAl steel subjected to ion nitriding in step S2 is subjected to post-oxidation, hydrogen sputtering, post-oxidation, hydrogen sputtering and post-oxidation to obtain the high-hardness nitriding steel material.
[0041] The tempering process is: quenching temperature 950 DEG C, holding time 1h, cooling mode oil cooling; tempering temperature 600 DEG C, tempering time 5h, cooling mode air cooling.
[0042] The specific steps of the step S2 are as follows: the rare earth catalyst is hung on the cathode disc in the ion nitriding furnace, the 38CrMoAl steel treated in S1 is placed in the ion nitriding furnace, the air pressure in the furnace is extracted to a vacuum degree of 6*10 -4 Pa, and the ion nitriding treatment is carried out by introducing the nitriding gas source.
[0043] The rare earth catalyst adopts lanthanum-cerium alloy, and when the loading capacity of the ion nitriding furnace is 240 kg, the adding amount of the lanthanum-cerium alloy is 2 pieces, and each piece of the lanthanum-cerium alloy is a cube with a size of 50 mm*50 mm*50 mm.
[0044] The nitriding gas source adopts a mixed gas of nitrogen and argon with a volume ratio of 4:1.
[0045] The nitriding gas source flow of the ion nitriding is 500 mL / h, the nitriding gas pressure is 120 Pa, the nitriding temperature is 540 DEG C, and the holding time is 15 h.
[0046] The post-oxidation temperature is 400 DEG C, the post-oxidation time is 2 h, the hydrogen sputtering temperature is 500 DEG C, and the hydrogen sputtering time is 4 h. Comparative Example 1
[0047] A preparation method of a high-hardness nitriding steel material, comprising the following preparation steps: S1. The 38CrMoAl steel is quenched and tempered, cut, polished, washed, and dried to obtain a treated 38CrMoAl steel with a size of 30 mm*10 mm*10 mm; S2. The treated 38CrMoAl steel in step S1 is subjected to ion nitriding; S3. The 38CrMoAl steel subjected to ion nitriding in step S2 is subjected to post-oxidation, hydrogen sputtering, post-oxidation, hydrogen sputtering, and post-oxidation to obtain a high-hardness nitriding steel material.
[0048] The quenching and tempering process is as follows: the quenching temperature is 940 DEG C, the holding time is 1 h, and the cooling mode is oil cooling; the tempering temperature is 680 DEG C, the tempering time is 3 h, and the cooling mode is air cooling.
[0049] The specific steps of step S2 are as follows: the treated 38CrMoAl steel in step S1 is placed in an ion nitriding furnace, the gas pressure in the furnace is extracted to a vacuum degree of 6*10 -4 Pa, and a nitriding gas source is introduced for ion nitriding treatment.
[0050] The nitriding gas source adopts a mixed gas of nitrogen and argon with a volume ratio of 3:2.
[0051] The nitriding gas source flow of the ion nitriding is 500 mL / h, the nitriding gas pressure is 120 Pa, the nitriding temperature is 560 DEG C, and the holding time is 10 h.
[0052] The post-oxidation temperature is 400 DEG C, the post-oxidation time is 2 h, the hydrogen sputtering temperature is 500 DEG C, and the hydrogen sputtering time is 4 h. Comparative Example 2
[0053] A preparation method of a high-hardness nitriding steel material, comprising the following preparation steps: S1. quenching, cutting, polishing, cleaning and drying 38CrMoAl steel to obtain treated 38CrMoAl steel with a size of 30mm*10mm*10mm; S2. ion nitriding the treated 38CrMoAl steel in step S1 by using a rare earth catalyst; S3. post-oxidizing, hydrogen sputtering, post-oxidizing, hydrogen sputtering and post-oxidizing the 38CrMoAl steel after ion nitriding in step S2 to obtain high-hardness nitrided steel material.
[0054] The quenching process is as follows: quenching temperature is 940℃, holding time is 1h, and cooling mode is oil cooling; tempering temperature is 680℃, tempering time is 3h, and cooling mode is air cooling.
[0055] The specific steps of step S2 are as follows: hanging the rare earth catalyst on the cathode disc in the ion nitriding furnace, placing the treated 38CrMoAl steel in step S1 in the ion nitriding furnace, pumping the gas pressure in the furnace to a vacuum degree of 6*10 -4 Pa, and introducing a nitriding gas source for ion nitriding treatment.
[0056] The rare earth catalyst uses lanthanum-cerium alloy, and when the loading capacity of the ion nitriding furnace is 240kg, the addition amount of the lanthanum-cerium alloy is 1 piece, and each piece of lanthanum-cerium alloy is a cube with a size of 50mm*50mm*50mm.
[0057] The nitriding gas source uses ammonia gas.
[0058] The flow of the nitriding gas source for ion nitriding is 500mL / h, the nitriding gas pressure is 120Pa, the nitriding temperature is 560℃, and the holding time is 10h.
[0059] The post-oxidation temperature is 400℃, the post-oxidation time is 2h, the hydrogen sputtering temperature is 500℃, and the hydrogen sputtering time is 4h. Comparative Example 3
[0060] A preparation method of high-hardness nitrided steel material, comprising the following preparation steps: S1. quenching, cutting, polishing, cleaning and drying 38CrMoAl steel to obtain treated 38CrMoAl steel with a size of 30mm*10mm*10mm; S2. ion nitriding the treated 38CrMoAl steel in step S1 by using a rare earth catalyst; S3. post-oxidizing the 38CrMoAl steel after ion nitriding in step S2 to obtain high-hardness nitrided steel material.
[0061] The tempering process is: quenching temperature 940 DEG C, holding time 1h, cooling mode oil cooling; tempering temperature 680 DEG C, tempering time 3h, cooling mode air cooling.
[0062] The specific steps of the step S2 are as follows: the rare earth catalyst is hung on the cathode disc in the ion nitriding furnace, the 38CrMoAl steel after the treatment of S1 is placed in the ion nitriding furnace, the air pressure in the furnace is extracted to the vacuum degree of 6*10 -4 Pa, and the ion nitriding treatment is carried out by introducing the nitriding gas source.
[0063] The rare earth catalyst adopts lanthanum-cerium alloy, when the loading capacity of the ion nitriding furnace is 240kg, the adding amount of the lanthanum-cerium alloy is 1 piece, and each piece of the lanthanum-cerium alloy is a cube with the size of 50mm*50mm*50mm.
[0064] The nitriding gas source adopts the mixed gas of nitrogen and argon with the volume ratio of 3:2.
[0065] The flow of the nitriding gas source of the ion nitriding is 500mL / h, the nitriding gas pressure is 120Pa, the nitriding temperature is 560 DEG C, and the holding time is 10h.
[0066] The post-oxidation temperature is 400 DEG C, and the post-oxidation time is 2h. Effect example
[0067] Surface hardness: the surface hardness of the high-hardness nitriding steel material obtained in examples 1-3 and comparative examples 1-3 is detected by using the Vickers hardness tester produced by Laizhou Huayin with the model of HV-1000A, the load is 100g, and the holding time is 15s; when the surface hardness is measured, five points of the random area on the surface of the high-hardness nitriding steel material obtained in examples 1-3 and comparative examples 1-3 are selected, and the average value is taken.
[0068] Wear resistance: the wear resistance of the high-hardness nitriding steel material obtained in examples 1-3 and comparative examples 1-3 is tested by using the multifunctional friction and wear testing machine, and the model is CVMT-1000 multifunctional friction tester. The parameters are as follows: the counter-abrasion material is GCr15 steel ball, the radius is 2.5mm, the rotation speed is 200r / min, the radius is 2mm, the load is 200g, and the time is 15min. Then, the wear track is observed by using the optical microscope; the samples before and after the wear test are weighed by using the electronic balance, and the weight ratio wear rate is calculated according to the following formula: W=DeltaM / (F*S); in the formula, W(g*m -1 ·N -1 ) is the weight ratio wear rate, DeltaM(g) is the weight change before and after the treatment, F(N) is the test load, and S(m) is the sliding distance of the ball.
[0069] Brittleness: the surface of the high-hardness nitrided steel material obtained in Examples 1-3 and Comparative Examples 1-3 was subjected to brittleness detection using a Vickers microhardness tester; in the hardness test, the loading load was set to 1000 g, and the loading time was 15 s. After the hardness test was completed, the indentation morphology of the surface of the sample was observed using a metallographic microscope, and the relative brittleness of the sample was evaluated in combination with the shape of the indentation and the cracking condition around the indentation; the brittleness grade 1 was no cracking, and the brittleness grade 4 was serious cracking around the indentation.
[0070] Table 1 below is the surface hardness, impact toughness, and wear resistance test results of the high-hardness nitrided steel material obtained in Examples 1-3 and Comparative Examples 1-3: Table 1
[0071] As can be seen from Table 1, the high-hardness nitrided steel material obtained in Examples 1-3 has good hardness and wear resistance, and low brittleness.
[0072] The difference between Comparative Example 1 and Example 2 is that no rare earth catalyst is used for ion nitriding of the 38CrMoAl steel after step S1, and the high-hardness nitrided steel material obtained has weak hardness and wear resistance, and high brittleness.
[0073] The difference between Comparative Example 2 and Example 2 is that ammonia gas of a traditional process is used as the ion nitriding gas source for the 38CrMoAl steel after step S1, and the high-hardness nitrided steel material obtained has weak hardness and wear resistance, and high brittleness.
[0074] The difference between Comparative Example 3 and Example 2 is that the 38CrMoAl steel is subjected to one post-oxidation treatment after ion nitriding, and the high-hardness nitrided steel material obtained has weak hardness and wear resistance, and high brittleness.
[0075] The above-described specific examples further illustrate the purpose, technical solutions, and beneficial effects of the present application, and it should be understood that the above-described specific examples are only specific embodiments of the present application and are not intended to limit the present application; any modification, equivalent replacement, improvement, etc. made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for producing a high hardness nitrided steel material, characterized by, The preparation method comprises the following steps: S1. quenching, cutting, polishing, cleaning and drying the 38CrMoAl steel; S2. ion nitriding the 38CrMoAl steel treated in step S1 by using a rare earth catalyst; S3. performing at least two post-oxidations on the 38CrMoAl steel ion nitrided in step S2 to obtain a high-hardness nitrided steel material.
2. The method of producing a high-hardness nitrided steel material according to claim 1, characterized by, The quenching process is as follows: quenching temperature is 930-950℃, holding time is 1-1.5h, and cooling mode is oil cooling; tempering temperature is 600-680℃, tempering time is 3-5h, and cooling mode is air cooling.
3. The method for preparing high-hardness nitrided steel material according to claim 1, characterized in that, The specific steps of step S2 are as follows: The rare earth catalyst is hung on the cathode disc in the ion nitriding furnace, the 38CrMoAl steel treated by Si is placed in the ion nitriding furnace, the air pressure in the furnace is extracted to the vacuum degree of 6*10 -4 Pa, the ion nitriding gas source is introduced to carry out ion nitriding treatment.
4. The method of producing a high-hardness nitrided steel material according to claim 3, characterized by, The rare earth catalyst is lanthanum-cerium alloy, and the main chemical components of the lanthanum-cerium alloy are as follows: 32.4wt% lanthanum, 67.43wt% cerium, 0.15wt% praseodymium, <0.03wt% neodymium, 0.53wt% iron, <0.01wt% silicon and <0.01wt% phosphorus.
5. The method of producing a high-hardness nitrided steel material according to claim 4, characterized in that, When the loading capacity of the ion nitriding furnace is 240kg, the adding amount of the lanthanum-cerium alloy is 1-2 pieces, and each piece of the lanthanum-cerium alloy is a cube with a size of 50mm*50mm*50mm.
6. The method of producing a high-hardness nitrided steel material according to claim 3, wherein The nitrogenizing gas source is a mixed gas of nitrogen and argon with a volume ratio of (3-4):(1-2).
7. The method of producing a high-hardness nitriding steel material according to claim 6, characterized in that, The flow rate of the nitrogenizing gas source of the ion nitriding is 500mL / h, the nitrogenizing gas pressure is 120Pa, the nitrogenizing temperature is 520-560℃, and the holding time is 10-20h.
8. The method of producing a high-hardness nitrided steel material according to claim 1, wherein Once hydrogen sputtering is further performed between two adjacent post-oxidations.
9. The method for preparing high-hardness nitrided steel material according to claim 8, characterized in that, The post-oxidation temperature is 390-410℃, the post-oxidation time is 1.5-2.5h, the hydrogen sputtering temperature is 490-510℃, and the hydrogen sputtering time is 3-4h.
10. A high hardness nitrided steel material, characterized by, The high-hardness nitrided steel material is prepared by the preparation method of the high-hardness nitrided steel material according to any one of claims 1-9.